Semiconductor structure and method for manufacturing semiconductor structure
By forming an inverse doping layer opposite to the doping type of active region in the trench of the semiconductor word line transistor, a shallow junction is formed, which solves the problem of hot carrier damage caused by leakage voltage and improves the semiconductor structure. Performance and reliability.
Patent Information
- Application Number
- CN202010816422.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-08-14
AI Technical Summary
In semiconductor word line transistors, due to the combined effect of the drain terminal voltage and the gate voltage, the oxide layer close to the drain forms a strong electric field, resulting in hot carrier damage and device reliability decreases.
The inverse doping layer opposite to the active region doping type is formed in the groove wall of the trench, forming shallow junctions (PN junctions) to offset some leakage voltages, improve the peak electric field of the leakage end depletion region, and thus improve heat Carrier tunneling.
By forming an inverse doping layer, the performance of the semiconductor structure is effectively improved and the reliability and stability of the device are improved.
Smart Images

Figure CN114078852B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor structure and a method for manufacturing the semiconductor structure. Background Art
[0002] Dynamic Random Access Memory (DRAM) is a semiconductor device commonly used in electronic devices such as computers, including a memory cell array for storing data and a peripheral circuit located outside the memory cell array. Each memory cell usually includes a transistor (word line), a bit line, and a capacitor. The word line voltage on the transistor (word line) can control the opening and closing of the transistor, so that the data information stored in the capacitor can be read through the bit line, or the data information can be written into the capacitor.
[0003] With the continuous development of manufacturing technology, the MOS feature size continues to shrink, and the channel lateral electric field strength of MOS devices is constantly increasing. When the semiconductor word line transistor (NMOS) is working, due to the combined effect of the drain voltage (Vdd) and the gate voltage (Vg), a strong electric field is formed near the drain. Therefore, the damage to the device by hot carriers mainly occurs in the oxide layer near the drain, which will cause the transistor switching characteristics to drift and the device reliability to be seriously reduced. Summary of the invention
[0004] The invention provides a semiconductor structure and a method for manufacturing the semiconductor structure to improve the performance of the semiconductor structure.
[0005] According to a first aspect of the present invention, there is provided a semiconductor structure comprising:
[0006] a substrate including an isolation structure and an active region, the active region including ions of a first type;
[0007] A trench, wherein the trench is located in the active area, and an inner surface of the trench includes an inversion doping layer and an oxide layer disposed adjacent to each other, and the inversion doping layer is located above the oxide layer;
[0008] A word line, the word line is located in the trench;
[0009] The inversion doping layer includes ions of a second type, and the first type is opposite to the second type.
[0010] In one embodiment of the present invention, the inner surface of the groove further comprises:
[0011] The protective layer is attached to the inverse doping layer, and the inverse doping layer is sandwiched between the bottom of the protective layer and the top of the oxide layer.
[0012] In one embodiment of the present invention, the inversion doped layer comprises:
[0013] The side wall section, the protective layer is in contact with the side wall section;
[0014] A bottom wall section, wherein the bottom end of the protective layer and the top end of the oxide layer are sandwiched between the bottom wall section, and the side wall section is perpendicular to the bottom wall section;
[0015] The protective layer, the bottom wall section and the oxide layer constitute the inner surface of the groove.
[0016] In one embodiment of the present invention, the bottom end of the protective layer is in contact with the bottom wall section, and the top end of the oxide layer is in contact with the bottom wall section.
[0017] In one embodiment of the present invention, the word line comprises:
[0018] A barrier layer, the barrier layer is located on the surface of the oxide layer;
[0019] The conductive layer is located on the surface of the barrier layer.
[0020] In one embodiment of the present invention, the semiconductor structure further comprises:
[0021] An insulating layer, wherein the insulating layer is located above the barrier layer and the conductive layer, and the top of the barrier layer and the top of the conductive layer are both in contact with the bottom of the insulating layer;
[0022] The barrier layer covers the sidewall and bottom wall of the oxide layer, and the plane where the top of the barrier layer is located is lower than the plane where the bottom of the protection layer is located.
[0023] In one embodiment of the present invention, the plane where the top end of the blocking layer is located is 10 nm to 20 nm lower than the plane where the bottom end of the protective layer is located.
[0024] In one embodiment of the present invention, the top of the barrier layer is flush with the top of the conductive layer.
[0025] According to a second aspect of the present invention, there is provided a method for manufacturing a semiconductor structure, comprising:
[0026] providing a substrate having an isolation structure and an active region, the active region being doped with ions of a first type;
[0027] A trench is formed in the active region, an inversion doping layer and an oxide layer are formed in the trench, and the inversion doping layer is located above the oxide layer;
[0028] forming a word line in the trench;
[0029] The inversion doping layer is doped with ions of a second type, and the first type is opposite to the second type.
[0030] In one embodiment of the present invention, forming a trench in an active area includes:
[0031] forming a first recess in the active region;
[0032] Performing a second type of ion implantation on the inner surface of the first groove to form an ion implantation region;
[0033] Making the protective material layer cover the surface of the ion implantation area;
[0034] Etching the bottom of the protective material layer, the bottom of the ion implantation region and the bottom of the first groove to form a second groove, with the remaining ion implantation region serving as an inversion doping layer and the remaining protective material layer serving as a protective layer;
[0035] forming an oxide layer on an inner surface of the second groove;
[0036] The protection layer, the inversion doping layer and the oxide layer constitute the inner surface of the trench.
[0037] In one embodiment of the present invention, the depth of the first groove is 30 nm to 80 nm, and / or the depth of the second groove is 50 nm to 100 nm.
[0038] In one embodiment of the present invention, after forming the ion implantation region and before forming the second groove, the method further comprises:
[0039] forming a protective material layer to cover the inner surface of the first groove and the surface of the substrate;
[0040] The protective material layer located on the surface of the substrate and the bottom of the first groove is etched to expose the substrate and the ion implantation area.
[0041] In one embodiment of the present invention, forming a word line in a trench includes:
[0042] forming a barrier material layer to cover the inner surface of the trench;
[0043] forming a conductive material layer on the surface of the barrier material layer and filling the groove;
[0044] Etching the conductive material layer and the barrier material layer to expose the protective layer and the inversion doping layer between the protective layer and the oxide layer in sequence to form a third groove, and the remaining conductive material layer and the barrier material layer serve as the conductive layer and the barrier layer respectively;
[0045] forming an insulating material layer on the inner surface of the third groove and on the surface of the substrate;
[0046] Etching the insulating material layer on the surface of the substrate to expose the top of the inversion doping layer and the protection layer, and the remaining insulating material layer serves as an insulating layer;
[0047] The barrier layer and the conductive layer constitute a word line, and the insulating layer is located above the word line.
[0048] In one embodiment of the present invention, the depth of the third groove is greater than the depth of the first groove by 10 nm to 20 nm.
[0049] In one embodiment of the present invention, the implantation dose of the second type of ions is 5E13 cm2-1.5E14 cm2, and the implantation energy of the second type of ions is 0.5 KeV-5 KeV.
[0050] The semiconductor structure of the present invention forms an inversion doping layer with a doping type opposite to that of the active area in the groove wall, thereby forming a shallow junction (i.e., a PN junction) to fix the active area, offset part of the drain voltage, improve the peak electric field in the drain depletion region, and further improve hot carrier tunneling, thereby improving the performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Various objects, features and advantages of the present invention will become more apparent by considering the following detailed description of preferred embodiments of the present invention in conjunction with the accompanying drawings. The accompanying drawings are merely exemplary illustrations of the present invention and are not necessarily drawn to scale. In the accompanying drawings, the same reference numerals always refer to the same or similar parts. Among them:
[0052] Figure 1 is a schematic structural diagram of a semiconductor structure according to an exemplary embodiment;
[0053] Figure 2 yes Figure 1 Schematic diagram of the structure at AA in the middle;
[0054] Figure 3 is a schematic flow chart of a method for manufacturing a semiconductor structure according to an exemplary embodiment;
[0055] Figure 4 is a schematic structural diagram of a substrate provided by a method for manufacturing a semiconductor structure according to an exemplary embodiment;
[0056] Figure 5 is a schematic structural diagram of a method for manufacturing a semiconductor structure after a first groove is formed according to an exemplary embodiment;
[0057] Figure 6 is a schematic structural diagram of a method for manufacturing a semiconductor structure after an ion implantation region is formed according to an exemplary embodiment;
[0058] Figure 7 is a schematic structural diagram of a method for manufacturing a semiconductor structure after covering a protective material layer according to an exemplary embodiment;
[0059] Figure 8is a schematic structural diagram of a method for manufacturing a semiconductor structure after forming a second groove according to an exemplary embodiment;
[0060] Fig. 9 is a schematic structural diagram of a method for manufacturing a semiconductor structure after an oxide layer is formed according to an exemplary embodiment;
[0061] Fig.10 is a schematic structural diagram of a method for manufacturing a semiconductor structure after covering a barrier material layer according to an exemplary embodiment;
[0062] Fig.11 is a schematic diagram of a structure after a conductive material layer is covered in a method for manufacturing a semiconductor structure according to an exemplary embodiment;
[0063] Fig.12 is a schematic structural diagram of a method for manufacturing a semiconductor structure after a third groove is formed according to an exemplary embodiment;
[0064] Fig.13 It is a structural schematic diagram of a method for manufacturing a semiconductor structure covered with an insulating material layer according to an exemplary embodiment.
[0065] The following are the descriptions of the reference numerals:
[0066] 10. Substrate; 11. Isolation structure; 12. Active area; 20. Groove; 30. Inversion doping layer; 31. Side wall segment; 32. Bottom wall segment; 40. Oxide layer; 50. Word line; 51. Barrier layer; 52. Conductive layer; 53. Insulating layer; 60. Protective layer; 70. First groove; 71. Ion implantation area; 72. Second groove; 73. Barrier material layer; 74. Conductive material layer; 75. Third groove; 77. Protective material layer; 76. Insulating material layer. DETAILED DESCRIPTION
[0067] Typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different embodiments without departing from the scope of the present invention, and the descriptions and drawings therein are essentially for illustrative purposes rather than for limiting the present invention.
[0068] In the following description of different exemplary embodiments of the present invention, reference is made to the accompanying drawings, which form a part of the present invention and in which different exemplary structures, systems and steps that can implement various aspects of the present invention are shown by way of example. It should be understood that other specific schemes of components, structures, exemplary devices, systems and steps can be used, and structural and functional modifications can be made without departing from the scope of the present invention. Moreover, although the terms "above", "between", "within", etc. may be used in this specification to describe different exemplary features and elements of the present invention, these terms are used herein only for convenience, such as according to the direction of the examples in the accompanying drawings. Nothing in this specification should be construed as requiring a specific three-dimensional orientation of the structure to fall within the scope of the present invention.
[0069] An embodiment of the present invention provides a semiconductor structure, please refer to Figure 1 The semiconductor structure includes: a substrate 10, the substrate 10 includes an isolation structure 11 and an active area 12, the active area 12 includes a first type of ions; a trench 20, the trench 20 is located in the active area 12, the inner surface of the trench 20 includes an inversion doping layer 30 and an oxide layer 40 arranged adjacent to each other, the inversion doping layer 30 is located above the oxide layer 40; a word line 50, the word line 50 is located in the trench 20; wherein the inversion doping layer 30 includes a second type of ions, and the first type is opposite to the second type.
[0070] The semiconductor structure of one embodiment of the present invention forms an inversion doping layer 30 with a doping type opposite to that of the active region 12 in the groove wall of the groove 20, thereby forming a shallow junction (i.e., a PN junction) to fix the active region 12, offset part of the drain voltage, improve the peak electric field in the drain depletion region, and further improve hot carrier tunneling, thereby improving the performance of the semiconductor structure.
[0071] It should be noted that the inversion doping layer 30 is used to form the sidewalls of the trench 20 , and the oxide layer 40 is used to form the sidewalls and bottom wall of the trench 20 . The word line 50 is filled in the trench 20 , thereby forming a buried word line 50 .
[0072] It should be noted that the opposite doping types can be understood as doping P-type ions and N-type ions respectively, that is, doping P-type ions and N-type ions corresponding to group III elements and group V elements, and whether the first type of ions is P-type ions or N-type ions is consistent with the properties of MOSFET, that is, the first type of NMOS is N-type ions, and the first type of PMOS is P-type ions.
[0073] Specifically, the substrate 10 may be a P-type silicon substrate or an N-type silicon substrate.
[0074] For example, when the substrate 10 is N-type, that is, N-type ions (Group V element ions such as phosphorus P or arsenic As) are injected into the silicon substrate to form an active region 12, the first type of ions are N-type ions, and the second type of ions are P-type ions (Group III element ions such as boron B or gallium Ga), that is, P-type ions are injected into the groove wall of the groove 20 to form an inversion doping layer 30, and the P-type ions can also be boron difluoride BF2.
[0075] Alternatively, when the substrate 10 is of P type, that is, P type ions (group III element ions such as boron B or gallium Ga) are injected into the silicon substrate to form an active region 12, the first type of ions are P type ions, and the second type of ions are N type ions (group V element ions such as phosphorus P or arsenic As), that is, N type ions are injected into the groove wall of the groove 20 to form an inversion doping layer 30.
[0076] In one embodiment, Figure 1 and Figure 2 As shown, a plurality of active regions 12 are provided in the substrate 10, and the active regions 12 are filled between two adjacent isolation structures 11. The depths of the isolation structures 11 may be the same or different. Figure 1 It can be seen that the word line 50 crosses multiple active regions 12. There are multiple word lines 50.
[0077] In one embodiment, in combination Figure 1 , multiple active areas 12 are arranged in multiple rows, and each row is set in parallel, and the word line 50 spans multiple rows of active areas 12, the distance between the sides of two adjacent active areas 12 in two adjacent rows is closer, and the distance between the ends of two adjacent active areas 12 in one row is farther.
[0078] In one embodiment, the active region 12 includes a source region and a drain region. Figure 2 , the drain region is between two adjacent word lines 50 , and the source region is between the isolation structure 11 and the word line 50 .
[0079] In one embodiment, the isolation structure 11 may include silicon oxide, such as SiO 2 .
[0080] In one embodiment, the oxide layer 40 may include SIO2.
[0081] In one embodiment, the thickness of the oxide layer 40 is 3 nm to 8 nm.
[0082] In one embodiment, Figure 2 As shown, the inner surface of the groove 20 further includes: a protective layer 60, the protective layer 60 is in contact with the inverse doping layer 30, and the inverse doping layer 30 is sandwiched between the bottom of the protective layer 60 and the top of the oxide layer 40. The protective layer 60 is used to protect the inverse doping layer 30 to prevent damage to the inverse doping layer 30 during the manufacturing process of the semiconductor structure.
[0083] It should be noted that the protective layer 60 forms the sidewalls of the groove 20, that is, the protective layer 60 covers a portion of the inversion doping layer 30, so that the uncovered inversion doping layer 30 is clamped between the bottom end of the protective layer 60 and the top end of the oxide layer 40, thereby forming the sidewalls of the groove 20.
[0084] In one embodiment, the protection layer 60 may be SIO2, SIN, or a combination of both.
[0085] In one embodiment, the thickness of the protection layer 60 is 3 nm to 10 nm.
[0086] In one embodiment, Figure 2 As shown, the inversion doping layer 30 includes: a side wall segment 31, and the protective layer 60 is in contact with the side wall segment 31; a bottom wall segment 32, and the bottom wall segment 32 is sandwiched between the bottom end of the protective layer 60 and the top end of the oxide layer 40, and the side wall segment 31 is perpendicular to the bottom wall segment 32; wherein the protective layer 60, the bottom wall segment 32 and the oxide layer 40 constitute the inner surface of the groove 20.
[0087] The inversion doping layer 30 is composed of a side wall segment 31 and a bottom wall segment 32 . The protective layer 60 completely covers the side wall segment 31 , and the bottom end of the protective layer 60 is in contact with the bottom wall segment 32 , so that the protective layer 60 , the bottom wall segment 32 and the oxide layer 40 together constitute the inner surface of the groove 20 .
[0088] It should be noted that the inversion doping layer 30 and the oxide layer 40 can be formed in the substrate 10, that is, the inversion doping layer 30 can be formed by injecting the second type of ions into the substrate 10 (the injection dose of the second type of ions is 5E13 per square centimeter to 1.5E14 per square centimeter, and the injection energy of the second type of ions is 0.5KeV to 5KeV), and the oxide layer 40 can be formed in the substrate 10 by an in-situ steam generation (ISSG) method, and the protective layer 60 is formed on the surface of the substrate 10. For example, the protective layer 60 can be formed on the substrate 10 by adopting a physical vapor deposition (PVD) process, a chemical vapor deposition (CVD) process or an atomic layer deposition (ALD) process.
[0089] Alternatively, the inversion doping layer 30 can be formed by injecting a second type of ions into the substrate 10, and the oxide layer 40 is formed on the surface of the substrate 10. For example, the oxide layer 40 can be formed on the substrate 10 by adopting a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process. Accordingly, the protective layer 60 is formed on the surface of the substrate 10. For example, the protective layer 60 can be formed on the substrate 10 by adopting a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process.
[0090] In one embodiment, the bottom end of the protection layer 60 is in contact with the bottom wall section 32 , and the top end of the oxide layer 40 is in contact with the bottom wall section 32 , so that the protection layer 60 , the bottom wall section 32 and the oxide layer 40 completely constitute the inner surface of the groove 20 .
[0091] In one embodiment, the projections of the sidewalls of the protection layer 60 , the sidewalls of the bottom wall section 32 , and the sidewalls of the oxide layer 40 toward the substrate 10 overlap, that is, the word line 50 in the trench 20 is a structure with a fixed cross-sectional area.
[0092] Specifically, for example, when the groove 20 is a circular hole, the diameter of the circular hole remains unchanged along the extension direction of the circular hole, thereby facilitating the manufacture of the semiconductor structure.
[0093] In one embodiment, Figure 2 As shown, the word line 50 includes: a barrier layer 51, which is located on the surface of the oxide layer 40; and a conductive layer 52, which is located on the surface of the barrier layer 51. The barrier layer 51 can prevent the conductive material forming the conductive layer 52 from diffusing.
[0094] In one embodiment, Figure 2 As shown, the semiconductor structure further includes an insulating layer 53, which is located above the barrier layer 51 and the conductive layer 52, and the top of the barrier layer 51 and the top of the conductive layer 52 are both in contact with the bottom of the insulating layer 53. The insulating layer 53 is used to form a good insulating structure.
[0095] In one embodiment, the barrier layer 51 may include Ta, Ti, Ru, TaN, TiN, RuTa, RuTaN, W, or Ir, etc. The barrier layer 51 may be any other material that prevents the conductive material layer from diffusing therethrough.
[0096] In one embodiment, the thickness of the barrier layer 51 may be 2 nm to 7 nm.
[0097] In one embodiment, the conductive layer 52 may be a metal material, such as Cu, Al, W or alloys thereof.
[0098] In one embodiment, the insulating layer 53 may be formed of a material including silicon oxide, silicon nitride, or a combination thereof. For example, the insulating layer 53 may be SiO2, SiO3, or SiO2.
[0099] In one embodiment, the barrier layer 51 covers the sidewalls and the bottom wall of the oxide layer 40 , and the top of the barrier layer 51 is located at a plane lower than the bottom of the protection layer 60 .
[0100] Specifically, the plane where the top end of the blocking layer 51 is located is 10 nm to 20 nm lower than the plane where the bottom end of the protection layer 60 is located.
[0101] In one embodiment, the barrier layer 51 completely covers the side surface and the bottom surface of the conductive layer 52 to ensure an effective barrier effect.
[0102] In the clothes moth embodiment, the top of the conductive layer 52 and the top of the barrier layer 51 are not in the same plane, for example, the top of the conductive layer 52 is higher than the top of the barrier layer 51 .
[0103] In one embodiment, the top of the barrier layer 51 is flush with the top of the conductive layer 52 , that is, the bottom of the insulating layer 53 is a plane, so as to be reliably attached to the top of the barrier layer 51 and the top of the conductive layer 52 .
[0104] Specific, combined Figure 2 After analysis, it is found that the blocking layer 51 is arranged on the oxide layer 40, that is, the blocking layer 51 is located below the inversion doping layer 30, and the top of the blocking layer 51 can be flush with the top of the oxide layer 40, or the top of the blocking layer 51 is lower than the top of the oxide layer 40. Therefore, the insulating layer 53 completely covers the bottom wall section 32 of the inversion doping layer 30 and the protective layer 60.
[0105] An embodiment of the present invention further provides a method for manufacturing a semiconductor structure, please refer to Figure 3 , a method for manufacturing a semiconductor structure comprises:
[0106] S101, providing a substrate 10 having an isolation structure 11 and an active region 12, wherein the active region 12 is doped with first type ions;
[0107] S103, forming a trench 20 in the active region 12, wherein an inversion doping layer 30 and an oxide layer 40 are formed in the trench 20, and the inversion doping layer 30 is located above the oxide layer 40;
[0108] S105, forming a word line 50 in the trench 20;
[0109] The inversion doping layer 30 is doped with ions of the second type, and the first type is opposite to the second type.
[0110] A method for manufacturing a semiconductor structure according to an embodiment of the present invention forms an inversion doping layer 30 with a doping type opposite to that of the active region 12 in the groove wall of the groove 20, thereby forming a shallow junction (i.e., a PN junction) to fix the active region 12, offset part of the drain voltage, improve the peak electric field in the drain depletion region, and further improve hot carrier tunneling, thereby improving the performance of the semiconductor structure.
[0111] It should be noted that if Figure 4 As shown, the provided substrate 10 is a substrate 10 having an isolation structure 11 and an active area 12, that is, regardless of the specific forming method of the isolation structure 11 and the active area 12, a groove 20 is directly formed on the substrate 10, and a word line 50 is formed. Before forming the groove 20, dry etching or chemical mechanical polishing (CMP) can be used to planarize the substrate 10. Among them, a protective structure, such as an oxide layer, can be provided on the upper surface of the substrate 10.
[0112] It should be noted that the word line 50 is a buried word line.
[0113] In one embodiment, a groove 20 is formed in an active area 12, including: forming a first groove 70 in the active area 12; performing a second type of ion implantation on the inner surface of the first groove 70 to form an ion implantation area 71; making a protective material layer 77 cover the surface of the ion implantation area 71; etching the bottom of the protective material layer 77, the bottom of the ion implantation area 71 and the bottom of the first groove 70 to form a second groove 72, the remaining ion implantation area 71 serves as an inversion doping layer 30, and the remaining protective material layer 77 serves as a protective layer 60; forming an oxide layer 40 on the inner surface of the second groove 72; wherein the protective layer 60, the inversion doping layer 30 and the oxide layer 40 constitute the inner surface of the groove 20.
[0114] For the formation of the groove 20 , it is necessary to form a first groove 70 and a second groove 72 in sequence, and treat the inner surface of the first groove 70 with the second type of ions and a protective material layer 77 , and form an oxide layer 40 on the inner surface of the second groove 72 , thereby forming the inner surface of the groove 20 .
[0115] In one embodiment, the depth of the first groove 70 is 30 nm to 80 nm, and / or the depth of the second groove 72 is 50 nm to 100 nm.
[0116] In one embodiment, after forming the ion implantation region 71 and before forming the second groove 72, it also includes: forming a protective material layer 77 to cover the inner surface of the first groove 70 and the surface of the substrate 10; etching the protective material layer 77 located on the surface of the substrate 10 and the bottom of the first groove 70 to expose the substrate 10 and the ion implantation region 71.
[0117] Specific, combined Figures 4 to 9 The formation of the trench 20 will be described.
[0118] like Figure 4 As shown, a substrate 10 having an isolation structure 11 and an active region 12 is provided.
[0119] like Figure 5 As shown, a first groove 70 is formed on the substrate 10, that is, a first groove 70 is formed in the active area 12. The depth of the first groove 70 can be 30nm~80nm, and the width is 30nm~60nm. There is no limitation on the process of forming the first groove 70, and a suitable process in the relevant technology, such as etching, can be used.
[0120] like Figure 6 As shown, the second type of ions are implanted into the substrate 10 through the first groove 70 to form an ion implantation region 71 in the substrate 10, and the ion implantation region 71 constitutes the inner surface of the first groove 70. Wherein, when the substrate 10 is N-type, the second type of ions are P-type ions, such as boron B, gallium Ga, boron difluoride BF2, etc. Alternatively, when the substrate 10 is P-type, the second type of ions are N-type ions, such as phosphorus P or arsenic As, etc.
[0121] like Figure 7 As shown, a protective material layer 77 is formed by a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process, and the protective material layer 77 covers the inner surface of the first groove 70 and the upper surface of the substrate 10. The protective material layer 77 can be SIO2, SIN or a combination of the two, and the thickness of the protective material layer 77 is 3nm to 10nm.
[0122] like Figure 8 As shown, the protective material layer 77 covering the upper surface of the substrate 10 is etched to expose the upper surface of the substrate 10, and the protective material layer 77 is etched along the extension direction of the first groove 70, that is, only the protective material layer 77 extending in the vertical direction is retained, and after the ion implantation area 71 in the horizontal direction is exposed, the etching is continued downward until the second groove 72 is formed, at which time, the remaining ion implantation area 71 serves as the inversion doping layer 30. The second groove 72 is formed below the first groove 70, and the depth of the second groove 72 can be 50nm to 100nm, and the width can be 15nm to 50nm.
[0123] like Fig. 9 As shown, an oxide layer 40 is formed on the inner surface of the second groove 72 by an in-situ water vapor generation method, and a groove 20 is formed. The oxide layer 40 includes SIO2, and the thickness of the oxide layer 40 can be 3nm to 8nm.
[0124] In one embodiment, the implantation dose of the second type of ions is 5E13 cm2-1.5E14 cm2, and the implantation energy of the second type of ions is 0.5 KeV-5 KeV.
[0125] In one embodiment, a word line 50 is formed in a groove 20, including: forming a barrier material layer 73 to cover the inner surface of the groove 20; forming a conductive material layer 74 on the surface of the barrier material layer 73 and filling the groove 20; etching the conductive material layer 74 and the barrier material layer 73 to expose the protective layer 60 and the inversion doping layer 30 located between the protective layer 60 and the oxide layer 40 in turn to form a third groove 75, and the remaining conductive material layer 74 and the barrier material layer 73 serve as the conductive layer 52 and the barrier layer 51 respectively; forming an insulating material layer 76 on the inner surface of the third groove 75 and the surface of the substrate 10; etching the insulating material layer 76 located on the surface of the substrate 10 to expose the top of the inversion doping layer 30 and the protective layer 60, and the remaining insulating material layer 76 serves as the insulating layer 53; wherein the barrier layer 51 and the conductive layer 52 constitute the word line 50, and the insulating layer 53 is located above the word line 50.
[0126] In the process of forming the word line 50 , it is necessary to form a blocking layer 51 , a conductive layer 52 and an insulating layer 53 in sequence.
[0127] In one embodiment, the depth of the third groove 75 is greater than the depth of the first groove 70 by 10 nm to 20 nm.
[0128] In one embodiment, the depth of the third groove 75 is 40 nm to 80 nm.
[0129] Specific, combined Figures 10 to 13 The process of forming the word line 50 will be described.
[0130] like Fig.10 As shown, a barrier material layer 73 is formed by a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process, and the barrier material layer 73 covers the inner surface of the groove 20 and the upper surface of the substrate 10. The barrier material layer 73 may include Ta, Ti, Ru, TaN, TiN, RuTa, RuTaN, W or Ir. The barrier material layer 73 may be any other material that prevents the conductive material layer from diffusing through. The thickness of the barrier material layer 73 may be 2nm to 7nm.
[0131] like Fig.11As shown, a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process is used to form a conductive material layer 74, the conductive material layer 74 fills the space formed by the barrier material layer 73, and covers the barrier material layer 73 located on the upper surface of the substrate 10, and dry etching or chemical mechanical polishing (CMP) is used to flatten the upper surface of the conductive material layer 74. The conductive layer 52 can be a metal material, for example, Cu, Al, W or an alloy thereof.
[0132] like Fig.12 As shown, the conductive material layer 74 and the barrier material layer 73 on the upper surface of the substrate 10 are etched, and the conductive material layer 74 and the barrier material layer 73 in the groove 20 are etched to expose the bottom wall section 32 of the inversion doped layer 30. At this time, the remaining conductive material layer 74 and the barrier material layer 73 serve as the conductive layer 52 and the barrier layer 51, respectively, and a third groove 75 is formed above the conductive layer 52 and the barrier layer 51. The depth of the third groove 75 can be 40nm to 80nm, that is, the bottom end of the third groove 75 needs to be lower than the bottom end of the first groove 70, and the depth of the third groove 75 is greater than the depth of the first groove 70 by 10nm to 20nm.
[0133] like Fig.13 As shown, a physical vapor deposition process, a chemical vapor deposition process or an atomic layer deposition process is used to form an insulating material layer 76, which fills the third groove 75 and covers the upper surface of the substrate 10. The insulating material layer 76 can be SIN, SION or SIO2.
[0134] The insulating material layer 76 is flattened by dry etching or chemical mechanical polishing, and finally the insulating material layer 76 is etched, and the remaining insulating material layer 76 is used as the insulating layer 53, and the following is formed: Figure 2 The semiconductor structure shown.
[0135] It should be noted that a protective structure may be provided on the upper surface of the substrate 10, so the protective structure needs to be removed during the final formation process. Therefore, when removing the insulating material layer 76 located on the upper surface of the substrate 10, the protective structure, as well as the protective material layer 77 and the insulating material layer 76 located inside the protective structure, also need to be removed.
[0136] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. The present invention is intended to cover any variations, uses, or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed by the present invention. The specification and example embodiments are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the preceding claims.
[0137] It should be understood that the present invention is not limited to the exact construction that has been described above and shown in the drawings and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.
Claims
1. A semiconductor structure, characterized in that: include: a substrate comprising an isolation structure and an active region, the active region comprising ions of a first type; A groove, wherein the groove is located in the active area, and an inner surface of the groove includes an inversion doping layer and an oxide layer disposed adjacent to each other, and the inversion doping layer is located above the oxide layer; a word line, the word line being located in the trench; The inversion doping layer includes ions of a second type, and the first type is opposite to the second type.
2. The semiconductor structure according to claim 1, characterized in that: The inner surface of the groove also includes: A protective layer is attached to the inversion doping layer, and the inversion doping layer is sandwiched between the bottom end of the protective layer and the top end of the oxide layer.
3. The semiconductor structure according to claim 2, characterized in that: The inversion doping layer comprises: A side wall section, wherein the protective layer is in contact with the side wall section; A bottom wall section, wherein the bottom wall section is sandwiched between the bottom end of the protective layer and the top end of the oxide layer, and the side wall section is perpendicular to the bottom wall section; The protective layer, the bottom wall segment and the oxide layer constitute the inner surface of the groove.
4. The semiconductor structure according to claim 3, characterized in that: The bottom end of the protective layer is in contact with the bottom wall section, and the top end of the oxide layer is in contact with the bottom wall section.
5. The semiconductor structure according to any one of claims 2 to 4, characterized in that: The word line comprises: A barrier layer, the barrier layer being located on a surface of the oxide layer; A conductive layer is located on the surface of the barrier layer.
6. The semiconductor structure according to claim 5, characterized in that: The semiconductor structure further comprises: An insulating layer, wherein the insulating layer is located above the barrier layer and the conductive layer, and the top of the barrier layer and the top of the conductive layer are both in contact with the bottom of the insulating layer; The barrier layer covers the sidewall and bottom wall of the oxide layer, and the plane where the top of the barrier layer is located is lower than the plane where the bottom of the protective layer is located.
7. The semiconductor structure according to claim 6, characterized in that: The plane where the top end of the blocking layer is located is 10nm to 20nm lower than the plane where the bottom end of the protective layer is located.
8. The semiconductor structure according to claim 5, characterized in that: The top of the barrier layer is flush with the top of the conductive layer.
9. A method for manufacturing a semiconductor structure, characterized in that: include: providing a substrate having an isolation structure and an active region, the active region being doped with ions of a first type; A trench is formed in the active area, wherein an inversion doping layer and an oxide layer are formed in the trench, and the inversion doping layer is located above the oxide layer; forming a word line in the trench; The inversion doping layer is doped with ions of a second type, and the first type is opposite to the second type.
10. The method for manufacturing a semiconductor structure according to claim 9, characterized in that: Forming a trench in the active area, comprising: forming a first groove in the active area; Performing a second type of ion implantation on the inner surface of the first groove to form an ion implantation region; Making the protective material layer cover the surface of the ion implantation area; Etching the bottom of the protective material layer, the bottom of the ion implantation area and the bottom of the first groove to form a second groove, with the remaining ion implantation area serving as the inversion doping layer and the remaining protective material layer serving as a protective layer; forming the oxide layer on the inner surface of the second groove; The protection layer, the inversion doping layer and the oxide layer constitute the inner surface of the trench.
11. The method for manufacturing a semiconductor structure according to claim 10, characterized in that: The depth of the first groove is 30 nm to 80 nm, and / or the depth of the second groove is 50 nm to 100 nm.
12. The method for manufacturing a semiconductor structure according to claim 10, characterized in that: After forming the ion implantation area and before forming the second groove, the method further includes: forming the protective material layer to cover the inner surface of the first groove and the surface of the substrate; The protective material layer located on the surface of the substrate and the bottom of the first groove is etched to expose the substrate and the ion implantation area.
13. The method for manufacturing a semiconductor structure according to claim 10, characterized in that: forming a word line in the trench, comprising: forming a barrier material layer to cover the inner surface of the trench; forming a conductive material layer on the surface of the barrier material layer and filling the groove; Etching the conductive material layer and the barrier material layer to expose the protective layer and the inversion doping layer between the protective layer and the oxide layer in sequence to form a third groove, and the remaining conductive material layer and the barrier material layer serve as a conductive layer and a barrier layer, respectively; forming an insulating material layer on the inner surface of the third groove and the surface of the substrate; Etching the insulating material layer on the surface of the substrate to expose the top of the inversion doping layer and the protection layer, and the remaining insulating material layer serves as an insulating layer; The barrier layer and the conductive layer constitute the word line, and the insulating layer is located above the word line.
14. The method for manufacturing a semiconductor structure according to claim 13, characterized in that: The depth of the third groove is greater than the depth of the first groove by 10 nm to 20 nm.
15. The method for manufacturing a semiconductor structure according to claim 10, characterized in that: The implantation dose of the second type of ions is 5E13 cm2-1.5E14 cm2, and the implantation energy of the second type of ions is 0.5 KeV-5 KeV.
Citation Information
Patent Citations
Method for fabricating side contact in semiconductor device using double trench process
CN102082116A
Semiconductor manufacturing process and semiconductor structure
CN103426825A
Manufacturing method of semiconductor element
CN108269763A
Manufacturing method of embedded type character line structure and structure
CN109427652A