Waterborne cationic polyurethane dispersion

By adding cationic surfactant to the polyurethane resin dispersion, the problem of using high boiling point solvents and toxic reagents in the prior art was solved, and an aqueous cationic polyurethane resin dispersion that meets the Swiss list was prepared, which improved the stability of the dispersion and Safety, suitable for food and beverage contact materials.

CN114144445BActive Publication Date: 2024-11-01AGFA NV
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202080053569.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-25
Filing Date
2020-06-30
Publication Date
2024-11-01
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

The existing aqueous cationic polyurethane resin dispersions require the use of high boiling point solvents and toxic reagents during the preparation process, and it is difficult to obtain solvent-free dispersions, and the raw materials that meet the Swiss list are limited and difficult to use in materials that come into contact with food and beverages.

Method used

By adding cationic surfactant to the organic solvent of the polyurethane resin dispersion, the dispersion of the dispersion in water and colloidal stability are improved, and a water-soluble cationic surfactant is used during the reaction to avoid covalent bonding. , an aqueous cationic polyurethane resin dispersion is formed that is easy to remove.

Benefits of technology

The preparation of aqueous cationic polyurethane resin dispersions without high boiling points or organic solvents is achieved, and it meets the requirements of the Swiss list, is suitable for food and beverage contact materials, and improves the stability and safety of the dispersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure DEST_PATH_IMAGE001
    Figure DEST_PATH_IMAGE001
Patent Text Reader

Abstract

An aqueous polyurethane resin dispersion having a polyalkylene oxide in its side chain and obtainable by reacting a polyisocyanate with a 1,2 or 1,3 polyether diol and with a polymeric diol selected from polyester diol, polyether diol, polycarbonate diol, polyacrylate diol and polyolefin diol in an organic solvent and by adding a cationic surfactant or a cationic surfactant precursor to the organic solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an aqueous polyurethane resin dispersion, and more particularly to use of the polyurethane resin in a treatment liquid for a substrate to be inkjet printed with an aqueous inkjet ink or in an aqueous inkjet ink. Background Art

[0002] In inkjet printing, substrates (e.g., paper or textile fabrics) are sometimes treated with aqueous cationic polymer dispersions to fix the colorant of the ink subsequently applied to the substrate. Among many aqueous cationic polymer dispersions, polyurethane-based resin dispersions are preferred, because one of the properties of polyurethane-based resins is that they ensure good adhesion of the resin to non-porous substrates, as disclosed in US2009 / 0233065.

[0003] Aqueous cationic polyurethane dispersions are typically produced by incorporating tertiary amino diols or polyols into the polyurethane chain, and these may be quaternized by protonation or reaction with an alkyl halide.

[0004] Quaternized amino diols have the disadvantage of poor solubility in typical solvents for polyurethane synthesis such as acetone, acetonitrile or dioxolane, which requires the use of solvents with high boiling points such as NMP, DMF, DMA, NEP, DMSO, sulfolane, TOU, dipropylene glycol dimethyl ether. The presence of these solvents makes it difficult to obtain solvent-free aqueous cationic polyurethane dispersions, as they cannot be easily removed by distillation.

[0005] Furthermore, quaternized aminodiols are commercially available only in limited cases. Those that are commercially available are not listed on the Swiss list, i.e. do not comply with Annex 10 of the FDHA Regulation SR817.023.21 on articles and materials dated May 2017. Compliance with this list is important when using cationic polyurethane resins for materials that come into contact with food and beverages, such as inks and primers.

[0006] JP2009237174 discloses polymers made from quaternized aminodiols, which are prepared and used in organic solvents.

[0007] WO 2019 / 105786 describes aqueous dispersions of polyurethane resins having quaternary N-atoms or tertiary amino groups.

[0008] Another possibility to obtain aqueous cationic polyurethane dispersions with cationic character is to quaternize the amino groups after the polyurethane synthesis has been carried out, as disclosed in US 3686108 and US 7964665 B2. This quaternization must be carried out using reagents such as methyl sulfate or benzyl chloride, which are toxic and must be removed from the aqueous dispersion due to the fact that the quaternization is not complete, especially if these resins are to be used in contact with food and beverages.

[0009] From the foregoing it is apparent that there is a need for a synthesis process for aqueous polyurethane resin dispersions for which the raw materials for the preparation are readily available, comply with the Swiss List, and which does not require the use of organic solvents with high boiling points or purification processes. Summary of the invention

[0010] It is an object of the present invention to provide a solution to the above mentioned problems. This object has been achieved by adding a cationic surfactant to the organic solvent in which the polyurethane resin dispersion is prepared, as defined in claim 1 .

[0011] According to another aspect, the present invention comprises a treating liquid for inkjet recording, the treating liquid comprising the aqueous dispersion as defined in claim 1. The treating liquid is defined in claim 6.

[0012] According to another aspect, the invention comprises an aqueous inkjet ink comprising an aqueous dispersion as defined in claim 1. The inkjet ink is defined in claim 11.

[0013] According to another aspect, the present invention comprises an inkjet recording method using an aqueous dispersion as defined in claim 1. The method is defined in claim 14.

[0014] Other features, elements, steps, characteristics and advantages of the present invention will become more apparent from the following detailed description of preferred embodiments of the present invention. Specific embodiments of the present invention are also defined in the dependent claims. DETAILED DESCRIPTION

[0015] A. Waterborne polyurethane resin dispersion

[0016] A.1. Polyurethane resin

[0017] The polyurethane resin of the aqueous dispersion according to the present invention is characterized by the fact that the polyurethane resin contains polyalkylene oxide in the side chains of the polyurethane backbone. The polyurethane resin of the present invention can be obtained by reacting a polyether diol and a polymeric diol selected from polyester diols, polyether diols, polycarbonate diols, polyacrylate diols and polyolefin diols with a polyisocyanate in an organic solvent. Preferred solvents are acetone, acetonitrile and MEK, because these solvents can be removed after the dispersion step. A cationic surfactant is added to the organic solvent. The cationic surfactant can be added before, during or after the reaction occurs. The cationic surfactant can be added as a solution or can be directly added to the organic solvent. In another embodiment, the cationic surfactant can be added together with the water added to the polyurethane resin solution to obtain an aqueous cationic polyurethane resin dispersion. The first water added does not cause the polyurethane polymer to become insoluble. However, after adding more water, a polyurethane dispersion will be formed due to the insolubility of the polyurethane polymer in water. In order to obtain a good interaction or combination of the surfactant with the dispersion particles, a surfactant is preferably added to the first portion of water added. The first portion of water added preferably contains a quaternary surfactant, while the second portion does not contain a quaternary surfactant and contains only water. Preferably, the first portion is 10-30% of the total water added.

[0018] If the cationic surfactant contains a reactive group toward isocyanate, it is preferred that the surfactant is added when the reaction between the polyisocyanate, polyether diol and polymeric diol is complete. The reaction is considered complete when no more reaction product (polyurethane resin) is formed.

[0019] Both cationic surfactants and polyalkylene oxides incorporated into the polyurethane dispersion improve the dispersibility and colloidal stability of the dispersed resin in water.

[0020] Without being bound by theory, it is speculated that the cationic surfactant is incorporated into the aqueous polyurethane resin dispersion without being covalently bonded to the polyurethane resin. The resulting flexibility of the stabilizing groups from the cationic surfactant increases colloidal stability relative to cationic surfactants that are covalently bound to the resin.

[0021] A.1.1. Polyether diols

[0022] The polyether diols are preferably 1,2 or 1,3 polyether diols. 1,2- and 1,3-polyether diols can be synthesized by alkoxylation of cyclic hydroxy-functional ketals derived from alcohols having at least three hydroxyl groups. The ketals can then be converted to diols under acidic conditions.

[0023] Examples of useful ketals are: 5-ethyl-2,2-dimethyl-1,3-dioxane-5-methanol, CAS Reg. No. 20761-68-6; 2,2-dimethyl-1,3-dioxane-5-methanol, CAS Reg. No. 4728-12-5; 2,2,5-trimethyl-1,3-dioxane-5-methanol, CAS Reg. No. 3663-46-5; 2,2-dimethyl-1,3-dioxane-5,5-dimethanol, CAS Reg. No. 770-74-1; 2,2-dimethyl-1,3-dioxolane-4-methanol, CAS Reg. No. 100-79-8.

[0024] Alternatively to the use of hydroxy-functional ketals, oxetanes can also be used, but these are less stable upon alkoxylation, examples being, for example, 3-methyl-3-oxetanemethanol, CAS Reg. No. 3143-02-0; or 3-ethyl-3-oxetanemethanol = trimethylolpropaneoxetane, CAS Reg. No. 3047-32-3.

[0025] Preferred polyether diols are compounds according to Formula 1.

[0026]

[0027] Where R1 is methyl or ethyl, R2 is H or C 1 -C 4 Alkyl and n represents an integer of 5 to 50, more preferably 10 to 40, most preferably 15 to 30.

[0028] The polyether diols that can be preferably used in the present invention are Ymer N120 or Tegomer D 3403, i.e. α-[2,2-bis(hydroxymethyl)butyl]-ω-methoxy-poly(oxy-1,2-ethanediyl). These diols can be prepared from 5-ethyl-2,2-dimethyl-1,3-dioxane-5-methanol (CAS Reg. No. 20761-68-6) or 3-ethyl-3-oxetanemethanol = trimethylolpropaneoxetane (CAS Reg. No. 3047-32-3).

[0029] A possible synthesis procedure is described in Fock, J.; Möhring, V., Polyether-1,2- and -1,3-diols as macromonomersfor the synthesis of graft copolymers, 1. Synthesis and characterization of the macromonomers. Die Makromolekulare Chemie 1990, 191 (12), 3045-3057.

[0030] Ymer N120 or Tegomer D 3403 is known by CAS Registry Number 131483-27-7, ie α-[2,2-bis(hydroxymethyl)butyl]-ω-methoxy-poly(oxy-1,2-ethanediyl).

[0031] In general, other polyether 1,2- or 1,3-diols can also be used. For good stability, the polyether graft needs to be water-soluble to give good steric stabilization. In the case of Ymer N120, the polyether consists only of ethylene oxide segments, but it can also be a copolymer of different alkylene oxides. In addition, in the current macromonomer diols, the terminal group is a methoxy group, which can also be other terminal groups such as hydrophilic terminal groups (such as anionic groups such as carboxylates, sulfates, phosphates, etc., or cationic groups such as quaternary amine groups, or precursors of cationic groups such as tertiary amino groups) in order to also have an electrosteric stabilization effect.

[0032] The content of polyether diol in the polyurethane resin is preferably 30% by weight or less but greater than 1% by weight relative to the total solid weight of the polyurethane resin; more preferably, the polyether diol content is equal to or less than 15% by weight and greater than 2% by weight relative to the polyurethane resin. A polyether diol content of less than 30% by weight but greater than 1% by weight relative to the polyurethane resin has additional improvements in scratch resistance and solvent resistance of the sprayed and dried image relative to a polyether diol content outside this range. Too high a polyether diol content (exceeding 30% by weight) can result in too high a water solubility and a lower glass transition temperature.

[0033] A.1.2. Polymeric diols

[0034] Preferred polymeric diols include polycarbonate diols, polyether diols, polyacrylate diols, aliphatic polyester diols, polyolefin diols. More preferred diols are polyester diols obtained by reacting polycarboxylic acids with polyols.

[0035] Most preferably, the polyester diol is a resin formed by an esterification reaction or transesterification reaction between at least one aromatic polycarboxylic acid component and at least one polyol component. Specific examples of aromatic polycarboxylic acids include dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid; trivalent or higher polycarboxylic acids such as trimellitic acid and pyromellitic acid; and anhydrides thereof, such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride; and the like. As the aromatic polycarboxylic acid component, one or more dibasic acids selected from the above dibasic acids, lower alkyl ester compounds of these acids, and anhydrides are mainly used. If necessary, monobasic acids such as benzoic acid, crotonic acid or p-tert-butylbenzoic acid may be further used in combination with the polycarboxylic acid component; trivalent or higher polycarboxylic acids such as trimellitic anhydride, methylcyclohexene tricarboxylic acid or pyromellitic anhydride; and the like. It is preferred to use dicarboxylic acids that will provide linear polymer chains to prepare the polyesters, in particular 1,4-terephthalic acid copolymers give better properties with respect to colloidal stability in aqueous media than phthalic anhydride copolymers. In addition to terephthalic acid, other para- or linearly substituted polycarboxylic acids may also be used to obtain the desired properties, such as 2,6-naphthalene dicarboxylic acid or 1,5-naphthalene dicarboxylic acid.

[0036] Preferred carboxylic acids are aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid. The content of aromatic acid in the resin is equal to or higher than 30 mol%, preferably equal to or higher than 50 mol%, relative to the total amount of dicarboxylic acid or anhydride. The treatment liquid containing the polyurethane resin obtained by the reaction of the polyester diol containing aromatic polycarboxylic acid does show improved colloidal stability and produces images with improved solvent resistance and improved dry and wet scratch resistance. The good results obtained with terephthalic acid and isophthalic acid are likely to be related to obtaining a certain amount of polyurethane resin crystallinity or providing linear amorphous chains, which contribute more to the desired physical properties such as scratch resistance and solvent resistance. The introduction of phthalic anhydride or isophthalic acid in terephthalic acid-based polyesters reduces the crystallinity or chain end-to-end distance and improves solubility in organic solvents. For terephthalic acid-based polyester diols, copolymers of terephthalic acid and isophthalic acid are preferably used, more preferably with at least 20 mol% of isophthalic acid. For the same reasons, polyester diols containing only phthalic anhydride are less preferred than copolymers incorporating terephthalic acid. Polyester diols based solely on phthalic anhydride are very soluble in the polymerization solvent used for preparation, but the dried coating will also have low solvent resistance. Therefore, it is preferred that the aromatic polyester diols contain between 20 and 80 mole % of terephthalate groups, based on the total amount of dicarboxylic acid (or anhydride) in the polyester diol.

[0037] Very suitable polyester diols containing terephthalate units and isophthalate units in a 1:1 mol % ratio are: Dynacoll 7150 supplied by Evonik (Marl, Germany), Vylon 220 from Toyobo (Osaka, Japan) and Elitel 1401 obtained from Unitika Ltd (Düsseldorf, Germany).

[0038] In order to obtain the desired properties of polyester diols and use high levels of terephthalic acid, mixtures of dicarboxylic acids can also be used. For example, in order to reduce the crystallinity, a mixture of terephthalic acid and adipic acid can be used. Therefore, polyester diols based on mixtures of aromatic polycarboxylic acids and aliphatic dicarboxylic acids such as adipic acid, succinic acid, methylcyclohexenetricarboxylic acid, fumaric acid and sebacic acid or anhydrides such as tetrahydrophthalic anhydride, hexahydrophthalic anhydride, maleic anhydride and succinic anhydride can also be used.

[0039] Polyester diols with high terephthalic acid content may have poor solubility in the preparation solvent (e.g., acetone) used for preparation or may have too high a crystallinity to obtain good adhesive properties. In particular, this is the case when the polyester diol uses only non-branched diols such as 1,2-ethylene glycol or 1,4-butanediol. When using terephthalic acid-based polyester diols with more than 35 mol % terephthalic acid, a mixture of different non-branched diols (e.g., a mixture of 1,2-ethylene glycol and 1,4-butanediol) or a mixture of non-branched diols (e.g., ethylene glycol) and branched diols (e.g., neopentyl glycol) may be preferably used. When the polyester diol uses a mixture of different diols, a high terephthalic acid content may be used, even up to 100 mol % based on the total dicarboxylic acid content.

[0040] Specific examples of the diol component include diols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,4-hexanediol and 1,6-hexanediol; trivalent or higher polyols such as glycerol, trimethylolethane, trimethylolpropane and pentaerythritol. For the diol component, the above diols are mainly used, and if necessary, trivalent or higher polyols such as glycerol, trimethylolethane, trimethylolpropane and pentaerythritol can be further used in combination with diols. Aliphatic diols containing aromatic units can also be used to increase the content of the aromatic part in the polyester diol. Suitable diols are: p-xylene glycol, 1,5-naphthalenedimethanol, 1,4-naphthalenedimethanol, 4,4'-bis(hydroxymethyl)biphenyl, bis(hydroxyethyl)terephthalate, bis(2-hydroxypropyl)terephthalate, 1,5-bis(2-hydroxyethyl)1,5-naphthalenedicarboxylate, 4,4-bis(hydroxymethyl)diphenylmethane, 2,2-bis(4-β-hydroxyethoxyphenyl)propane (diethoxylated bisphenol A) and bis[p-(2-hydroxyethoxy)phenyl]methane.

[0041] It is preferred to use together with the polyester diol a diol having an Mw of equal to or less than 400. These diols may be used alone or in mixture of two or more kinds.

[0042] In addition to polyester diols, other different polymeric diols can also be used, for example, to adjust physical properties, adhesion, mechanical properties, etc. Examples are, for example, polycarbonate diols, polyether diols, polyacrylate diols, aliphatic polyester diols, polyolefin diols or other polymeric diols. Examples of polycarbonate diols are, for example: Oxymer C112, Oxymer M112 (available via Perstorp); Kuraray diol C-2050, C-2090, C-1090 (available from Kuraray); Converge HMA-1 and Converge HMA-1 (available from Novomer Inc.); Duranol T6002, T6001, T5652, T5651, T5650J, T4672, T4671, T4692 and T4691 (available from Asahi kasei). Further aliphatic polyester diols are, for example, regular (semi)crystalline or amorphous grades, for example based on hexanediol adipate (e.g. Dynacoll 7372 from Evonik), and polyester diols based on natural products, such as those prepared by using dimer acids or dimer diols (e.g. Priplast from Croda), examples being Priplast 3192 and Priplast 1838. The raw materials used to prepare certain Priplast grades, dimer diols sold under the name Pripol, can also be used as monomers in the synthesis to modify the physical and adhesive properties.

[0043] A.1.3. Polyisocyanates

[0044] Specific examples of the organic polyisocyanate compound to be reacted with the polyester diol include aliphatic diisocyanates such as lysine diisocyanate, hexamethylene diisocyanate, 1,5-pentamethylene diisocyanate and trimethylhexane diisocyanate; cyclic aliphatic diisocyanates such as hydrogenated xylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4 (or 2,6)-diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate) and 1,3-(isocyanate). azomethyl)cyclohexane; aromatic diisocyanates such as toluene diisocyanate, xylene diisocyanate and diphenylmethane diisocyanate; organic polyisocyanates themselves, including trivalent or higher-valent polyisocyanates such as lysine triisocyanate; adducts each consisting of such organic polyisocyanates and polyols, a low molecular weight polyester resin; and cyclized polymers (e.g., isocyanurates), biuret-type adducts, and the like, each of which is formed from the above-mentioned various diisocyanate compounds.

[0045] From the perspective of storage stability of the treatment liquid composition, the organic polyisocyanate compound according to the present invention preferably includes at least one selected from non-yellowing polyisocyanate compounds such as isophorone diisocyanate, hexamethylene diisocyanate and lysine diisocyanate, and more preferably the organic polyisocyanate compound includes at least isophorone diisocyanate.

[0046] Furthermore, the organic polyisocyanate compound may be used alone or in mixture of two or more kinds.

[0047] A.1.4. Cationic surfactants

[0048] The cationic surfactants useful in the present invention are preferably soluble or dispersible in water, and may also be soluble or dispersible in an organic solvent, and more preferably soluble or dispersible in a solvent used for the polymerization reaction. The surfactant may be a typical cationic surfactant having one or two alkyl or alkylaryl substituents which are significantly longer than the other alkyl groups substituted on the quaternary amine group. In addition to quaternary ammonium surfactants, quaternary phosphonium, sulfonium or iodonium compounds may also be used.

[0049] Suitable cationic surfactants for use according to the present invention are listed in Table 1.

[0050] Table 1.

[0051]

[0052]

[0053]

[0054] Preferably, the cationic surfactant comprises an ammonium group, more preferably, the cationic surfactant is according to formula II

[0055]

[0056] in

[0057] R1 is hydrogen or a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms

[0058] R2 and R3 are independently a substituted or unsubstituted alkyl group having 1 to 18 carbon atoms, or a benzyl group

[0059] R4 is a substituted or unsubstituted alkyl group having at least 8 carbon atoms.

[0060] One of the advantages of obtaining a cationic polyurethane dispersion according to the present invention is that many cationic surfactants comply with the Swiss list and thus produce dispersions that can be used in inks printed on food and pharmaceutical packaging. In particular, the following cationic surfactants that comply with the Swiss list listed in Table 2 can be used:

[0061] Table 2.

[0062]

[0063]

[0064] Also useful in the present invention is the use of surfactants having tertiary amine groups and the tertiary amine groups can be protonated to become cationic. These are hereinafter referred to as cationic surfactant precursors. In most cases, these tertiary amine surfactants are insoluble in water and become water soluble after protonation. Protonation can be carried out using organic or inorganic acids such as hydrochloric acid, hydrobromic acid, nitric acid, acetic acid, acrylic acid. The tertiary amine surfactant can also be added via the solvent phase, that is, added to the polymerization mixture in, for example, acetone or acetonitrile before adding water. The first portion of water added should preferably be acidified with an organic or inorganic acid to prepare the salt in situ after adding water in the dispersion step. If the pKa of the tertiary amine is low enough, the amine can also be protonated in the water phase without adding acid. Suitable cationic surfactant precursors are listed in Table 3.

[0065] Table 3.

[0066]

[0067] Other suitable tertiary amine surfactants are available, for example, from Akzo under the trade names: Armeen DM12D, i.e. dodecyl dimethylamine = CAS Registry Number 112-8-5; Armeen DM16D, i.e. hexadecyl dimethylamine = CAS Registry Number 112-69-6; Armeen M2C, i.e. dicocoalkyl methylamine = CAS Registry Number 61788-62-3; Ethomeen C12, i.e. ethoxylated (2) coconut alkyl amine = CAS Registry Number 61791-31-9.

[0068] A.1.5. Polyols containing cationic groups

[0069] Polyols containing cationic groups or cationic precursor groups such as amines can also be incorporated into the PU-resins of the present invention to provide additional cationic groups and thus increase the fixing capacity for the colorant. Suitable polyols for obtaining the aqueous dispersions according to the present invention are polyols containing positively charged atoms selected from N, P, S and I. More preferably, the polyol contains groups selected from quaternary ammonium, quaternary phosphonium, tertiary sulfonium and iodonium.

[0070] Preferably, the polyol comprises quaternized ammonium groups. The term "quaternized" means that a positively charged N atom is attached to 4 substituted or unsubstituted alkyl groups. More preferably, the polyol comprising quaternized ammonium groups is a diol.

[0071] Suitable polyols comprising positively charged atoms selected from N, P, S and I are listed in Table 1 of the unpublished patent application EP19188256.2.

[0072] A.2. Reaction conditions

[0073] Regarding the conditions for the reaction between the polyether polyol, the polymeric diol, and the polyisocyanate compound, conventionally used reaction conditions may be used without particular limitation.

[0074] In the reaction between the polymeric diol, the polyether polyol and the polyisocyanate compound, a diol having a Mw of 400 or less may be used, if necessary. Examples of suitable diols are ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,4-hexanediol and 1,6-hexanediol; trivalent or higher polyols such as glycerol, trimethylolethane, trimethylolpropane and pentaerythritol. 1,4-butanediol is most preferred.

[0075] In polyurethane synthesis, in addition to the polyether polyols for stabilizing polyurethane dispersions, different high molar mass polymeric diols can also be reacted with low molecular weight diols. In particular, if polyester diols are used in the reaction, stability polyols and polyester diols (Mw> 400g / mol) react with excessive isocyanates. This allows good reaction conversion. Depending on the molecular weight and copolymer composition, polyester diols may have poor solubility in a reaction solvent (e.g., acetone). After using excessive isocyanate reaction, by adding low molecular weight diols, the excess is offset to a certain NCO / OH molar ratio, which will produce a polyurethane resin with a very small amount of residual isocyanate. In the presence of some residual isocyanates, some urea bonds may be formed. The example of suitable diols is given above.

[0076] Here, examples of organic solvents for the reaction between the polyether glycol and the organic polyisocyanate compound include ketones such as acetone and methyl ethyl ketone, ethers such as tetrahydrofuran and dioxane, acetates such as ethyl acetate and butyl acetate, nitriles such as acetonitrile, and amides such as dimethylformamide, N-methylpyrrolidone and N-ethylpyrrolidone. These can be used alone or in combination of two or more.

[0077] The use of polyether polyols with higher molecular weight than Ymer 120N will give more phase separation, thereby providing better water dispersibility. However, for the preparation of polyurethane resins, it will be more difficult to dissolve these polyols in organic solvents such as acetone. This can be overcome by using a cosolvent during the polycondensation reaction. The preferred cosolvent is 2-pyrrolidone or N-methylpyrrolidone, more preferably 2-pyrrolidone.

[0078] The aqueous polyurethane dispersion of the present invention contains a polyurethane resin having polyalkylene oxide side chains. Therefore, it is preferred that the obtained polyurethane resin is dispersed in water to obtain an aqueous dispersion of the polyurethane resin. Any dispersion technique suitable for preparing an aqueous dispersion can be used. After being dispersed in an aqueous medium, standard separation techniques such as distillation can be used to remove the organic solvent in which the reaction has occurred.

[0079] B. Aqueous treatment fluid

[0080] The aqueous treatment fluid according to the invention contains a polyurethane resin dispersion as described in §A.1. and water. Further components that may be added to the treatment fluid are given below. The amount of polyurethane resin in the treatment fluid is equal to or lower than 30% by weight relative to the total weight of the treatment fluid.

[0081] B.1. Water-soluble organic solvents.

[0082] The treatment liquid of the present invention may contain a water-soluble organic solvent in addition to water as a solvent. Examples of the water-soluble organic solvent include polyhydric alcohols such as diethylene glycol, triethylene glycol, dipropylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2,2-dimethyl-1,3-propylene glycol, 2-methyl-1,3-propylene glycol, 1,2-pentanediol, 2,4-pentanediol, 1,5-pentanediol, 1,6-hexanediol, 2-ethyl-1,3-hexanediol, 1,2-hexanediol and 2,5-hexanediol, polyhydric alcohol alkyl ethers such as dipropylene glycol n-propyl ether, tripropylene glycol methyl ether, tripropylene glycol n-propyl ether, propylene glycol phenyl ether, triethylene glycol methyl ether, triethylene glycol methyl ether, triethylene glycol ethyl ether, diethylene glycol n-hexyl ether and ethylene glycol phenyl ether, and nitrogen-containing heterocyclic compounds such as 2-pyrrolidone and N-methylpyrrolidone.

[0083] Other preferred water-soluble organic solvents include ethylene glycol, propylene glycol, 1,2-butanediol, 2,3-butanediol, 2-methyl-2,4-pentanediol, dipropylene glycol monomethyl ether, propylene glycol n-butyl ether, propylene glycol tert-butyl ether, diethylene glycol methyl ether, ethylene glycol n-propyl ether and ethylene glycol n-butyl ether.

[0084] The content of the water-soluble organic solvent in the treatment liquid is preferably less than 70% by weight. If the content exceeds 70% by mass, the treatment liquid will lose its water-based and therefore greener character.

[0085] B.2. Surfactants

[0086] In the treatment liquid of the present invention, a surfactant may be added to ensure wettability to the substrate. As an active component in the ink, the amount of the surfactant added is preferably 0.1 wt % to 5 wt %.

[0087] If the amount added is less than 0.1% by mass, wettability onto the substrate will be insufficient and result in reduced image quality and adhesion to the substrate. The surfactant that can be used is not particularly limited as long as it satisfies the above-mentioned restrictions.

[0088] Although any amphoteric surfactant, nonionic surfactant or cationic surfactant can be used, nonionic surfactants such as polyoxyethylene alkylphenyl ether, polyoxyethylene alkyl ester, polyoxyethylene alkylamine, polyoxyethylene alkylamide, polyoxyethylene propylene block polymer, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester and ethylene oxide adduct of acetylene alcohol are preferably used in terms of the relationship between dispersion stability and image quality. In addition, fluorine-based surfactants and silicon-based surfactants can be used in combination (or alone) depending on the formulation.

[0089] Suitable surfactants are siloxane-based surfactants such as TegoTwin 4000 from Evonik Industries, Tegowet 270 from Evonik industries, Hydropalat WE3220 from BASF, silane-based surfactants such as Silwet HS312 from Momentive, and fluorosurfactants such as Thetawet FS8150 from Neochem GMBH, Capstone FS3100 from Dupont, Tivida FL2500 from Merck and surfactants from the Dynol, Envirogem and Surfynol series from Air products.

[0090] B.3. Additives

[0091] Along with the polyurethane resin, a flocculant such as a polyvalent metal ion may be included in the treatment solution. Suitable examples are polyvalent metal ions composed of divalent or higher valent metal cations such as magnesium, calcium, strontium, barium, zirconium and aluminum and anions such as fluoride ions (F - ), chloride ion (Cl - ), bromide ion (Br - ), sulfate ion (SO 4 2- ), nitrate ion (NO 3 - ) and acetate ions (CH 3 COO - ) formed by water-soluble metal salts.

[0092] These polyvalent metal ions have the function of aggregating or flocculating the pigment of the ink by acting on anionic groups such as carboxyl groups on the surface of the pigment or on the dispersed polymer of the capsules contained in the ink. As a result, the ink is retained on the surface of the substrate and the color development is improved. Therefore, it is preferred that the surface of the pigment in the ink and / or the dispersed polymer of the capsules contained in the ink have anionic groups selected from carboxyl groups, sulfonate groups and phosphonate groups, and most preferably carboxyl groups.

[0093] Other suitable inorganic flocculants are: polyaluminium hydroxychlorides such as Sylojet A200 from Grace and Drygen from Clariant; zirconium salts; boehms such as the Disperal series; alumina sols such as the Aluminasol series; and barium sulphate.

[0094] The treatment liquid may also contain an organic acid as a flocculant. Preferred examples of organic acids include, but are not limited to, acetic acid, propionic acid, and lactic acid.

[0095] The treatment fluid may also contain a colorant, such as a pigment. Particularly useful for printing on dark substrates are treatment fluids containing white pigments. A preferred pigment for aqueous treatment fluid inks is titanium dioxide. Titanium dioxide (TiO 2 ) The pigment may be in the crystalline form of rutile or anatase. Preparation of TiO 2 The method is described in more detail in "The Pigment Handbook", Volume I, Second Edition, John Wiley & Sons, NY (1988), the relevant disclosure of which is incorporated herein by reference for all purposes as if fully set forth.

[0096] The titanium dioxide particles can have a variety of average particle sizes of about 1 micron or less, depending on the desired end-use application of the treatment fluid. For applications requiring high hiding power or decorative printing applications, the titanium dioxide particles preferably have an average size of less than about 1 μm. Preferably, the particles have an average size of about 50 to about 950 nm, more preferably about 75 to about 750 nm, and even more preferably about 100 to about 500 nm.

[0097] Additionally, a variety of particle sizes can be used to achieve unique advantages, such as opacity and UV protection. These various sizes can be achieved by adding pigment-grade and nano-sized TiO 2 Both to obtain.

[0098] The titanium dioxide pigment may also be provided with one or more metal oxide surface coatings. These coatings may be applied using techniques known to those skilled in the art. Examples of metal oxide coatings include silicon oxide, aluminum oxide, aluminum oxide silicon oxide, boron oxide, and zirconium oxide, among others. These coatings may provide improved properties, including reduced photoreactivity of the titanium dioxide. Metal oxide coatings of aluminum oxide, aluminum oxide silicon oxide, boron oxide, and zirconium oxide result in the titanium dioxide pigment being more oxidized and more oxidized. 2 The surface of the pigments is positively charged and is therefore particularly useful in combination with the cationic polyurethane dispersions of the present invention, since no additional surface treatment of the pigment is required.

[0099] Commercial examples of such coated titanium dioxide include R700 (alumina coated, available from EI DuPont de Nemours (Wilmington, Delaware)), RDI-S (alumina coated, available from Kemira Industrial Chemicals (Helsinki, Finland)), R706 (available from DuPont (Wilmington, Delaware)) and W-6042 (silicon oxide alumina treated nanosized titanium dioxide from Tayco Corporation (Osaka, Japan)). Other suitable white pigments are given in Table 2 in

[0116] of WO 2008 / 074548. White pigments are preferably pigments having a refractive index greater than 1.60. White pigments may be used alone or in combination. Preferably, titanium dioxide is used as the pigment having a refractive index greater than 1.60. Suitable titanium dioxide pigments are those disclosed in

[0117] and

[0118] of WO 2008 / 074548.

[0100] C. Water-based inkjet ink

[0101] The aqueous polyurethane resin dispersion according to the present invention can be incorporated into aqueous inkjet inks. Preferably, the colorant contained in the inkjet ink according to the present invention is a pigment, and more preferably the surface of the pigment is positively charged to avoid aggregation between the polyurethane resin and the pigment.

[0102] In order to obtain a positively charged pigment surface in an aqueous ink formulation, the pigment may be dispersed in an aqueous medium using a dispersant having the formula III:

[0103]

[0104] in

[0105] R 1 is selected from hydrogen, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted alkynyl group, a substituted or unsubstituted aralkyl group, a substituted or unsubstituted alkaryl group and a substituted or unsubstituted (hetero)aryl group

[0106] L represents a divalent linking group containing 2 to 10 carbon atoms

[0107] R 2 , R 3 and R 4 independently selected from substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, substituted or unsubstituted alkynyl groups, substituted or unsubstituted aralkyl groups, substituted or unsubstituted alkaryl groups and substituted or unsubstituted (hetero)aryl groups

[0108] R 5represents a hydrocarbon group containing at least 8 carbon atoms

[0109] R 1 , R 2 , R 3 , R 4 Any of L and L may represent atoms necessary to form a five- to eight-membered ring

[0110] X - represents an anion that counteracts the positive charge of the ammonium group.

[0111] In a preferred embodiment, R 5 represents a substituted or unsubstituted alkyl group containing at least 8 carbon atoms, more preferably at least 10 carbon atoms, most preferably at least 12 carbon atoms. In a particularly preferred embodiment, R 5 In another preferred embodiment, R1 is selected from hydrogen and substituted or unsubstituted alkyl groups, more preferably hydrogen and C1 to C6 unsubstituted alkyl groups, most preferably hydrogen. In a further preferred embodiment, L represents a divalent linking group containing 2 to 8 carbon atoms, more preferably 2 to 6 carbon atoms. In another preferred embodiment, R 2 , R 3 and R 4 independently represents a substituted or unsubstituted alkyl group, more preferably a C1 to C6 unsubstituted alkyl group, most preferably a methyl, ethyl and propyl group.

[0112] Typical dispersants according to the general formula III are given in Table 1 of patent application: WO2019 / 105867.

[0113] The pigment of the dispersion according to the present invention can be any pigment, but preferably a colored pigment. Examples include, but are not limited to, carbon black and colored pigments such as anthraquinone, phthalocyanine blue, phthalocyanine green, diazo compounds, monoazo compounds, pyranthrone, perylene, heterocyclic yellow (heterocyclic yellow), quinacridone, pyrrolopyrrole dione pigment and (sulfur) indigo. Representative examples of phthalocyanine blue include copper phthalocyanine blue and its derivatives (pigment blue 15). Representative examples of quinacridone include pigment orange 48, pigment orange 49, pigment red 122, pigment red 192, pigment red 202, pigment red 206, pigment red 207, pigment red 209, pigment violet 19 and pigment violet 42. Representative examples of anthraquinone include pigment red 43, pigment red 194 (Perlnone Red), pigment red 216 (Brominated Pyrathrone Red) and pigment red 226 (Pyranthrone Red). Representative examples of perylene include Pigment Red 123 (Vermillion), Pigment Red 149 (Scarlet), Pigment Red 179 (Maroon), Pigment Red 190 (Red), Pigment Violet, Pigment Red 189 (Yellow Shade Red), and Pigment Red 224. Representative examples of thioindigo include Pigment Red 86, Pigment Red 87, Pigment Red 88, Pigment Red 181, Pigment Red 198, Pigment Violet 36, and Pigment Violet 38. Representative examples of heterocyclic yellow include Pigment Yellow 117 and Pigment Yellow 138.

[0114] More preferably, the pigment is selected from quinacridone and diketopyrrolopyrrole pigments. Particularly preferred pigments are selected from Pigment Red 122, Pigment Violet 19 and mixed crystals of the above-mentioned specific pigments. A commercially available example is Cinquasia Magenta RT-355-D from Ciba Specialty Chemicals. Examples of other suitable colored pigments are described in the Colour Index 3rd edition (The Society of Dyers and Cikiyrusts, 1982).

[0115] Particularly useful for printing on dark-colored textiles are aqueous inkjet inks with white pigments as pigments containing the dispersions of the invention. A preferred pigment is titanium dioxide. See § B.3.

[0116] In the pigment dispersion, it is desirable that the average particle diameter of the pigment particles is in the range of 0.01 to 1 μm, more preferably in the range of 0.01 to 0.5 μm, and most preferably in the range of 0.01 to 0.2 μm. When the average particle diameter of the pigment particles is 0.2 μm or less, problems related to reliability such as nozzle clogging and storage stability of the ink composition can be effectively minimized. When the average particle diameter of the pigment particles is 0.01 μm or more, the advantages of the pigment used in the present invention, i.e., excellent light resistance and water resistance, can be effectively exhibited, and aggregation of the pigment particles can be prevented.

[0117] The pigment to dispersant ratio (by weight) is preferably from about 0.7 to about 3.2, more preferably from about 1.0 to about 2.8, and most preferably from about 1.8 to about 2.4.

[0118] In order to disperse the pigment, a variety of dispersing devices can be used, for example, a ball mill, a sand mill, a roller mill, a colloid mill, an ultrasonic homogenizer and a high-pressure homogenizer. Using any of the above dispersing devices, the pigment and the water acting as a solvent are mixed and dispersed, and a dispersant as described above is added thereto, thereby obtaining a pigment dispersion of the present invention. Preferably, the dispersant is added in full or in part during the dispersion step.

[0119] The pigment dispersion may contain up to 75% by weight of the pigment, but is generally in the range of about 0.1 to 30% by weight, preferably 0.1 to 15% by weight, and more preferably 0.1 to 10% by weight. When the amount ratio of the pigment is 0.1% by weight or more, sufficient saturation and image density can be obtained. When the amount ratio of the pigment is 30% by weight or less, the color value can be prevented from being reduced and the nozzle of the print head can be prevented from being clogged.

[0120] In addition to the pigment, the inkjet ink according to the present invention may also contain a water-soluble organic solvent and / or a surfactant. Preferred candidates for the water-soluble organic solvent are disclosed in § B.1. Preferred candidates for the surfactant are disclosed in § B.2.

[0121] D. Treatment Fluid Application Method

[0122] The treatment liquid according to the present invention is suitable for treating different substrates, porous and non-porous substrates. The liquid is therefore also referred to as a pre-treatment liquid. Porous substrates include paper, cardboard, white lining particleboard, corrugated board, packaging board, wood, ceramics, stone, leather and textiles. Non-porous substrates include metal, synthetic leather, glass, polypropylene, polyvinyl chloride, PET, PMMA, polycarbonate, polyamide, polystyrene or their copolymers. The treatment liquid according to the present invention is also suitable for treating sprayed images and is generally referred to as a post-treatment liquid.

[0123] All known conventional methods can be used to apply or impregnate the treatment liquid onto the substrate or onto the image formed by spraying the aqueous inkjet ink. Examples of methods include air knife coating, blade coating, roller coating, gravure coating. After applying the treatment liquid to the substrate, the coating is preferably dried before printing the image on the treated substrate.

[0124] The treatment fluid is particularly suitable for treating non-porous substrates before or after printing an image by inkjet printing.

[0125] The treatment liquid is also suitable for treating textile fabrics. The textile fabric used is made of one type of fiber or two or more blended fibers selected from cotton, linen, rayon fiber, acetate fiber, silk, nylon fiber and polyester fiber. The fabric can be in any form, such as woven, knitted or non-woven forms of the above-mentioned fibers. The treatment liquid containing polyurethane resin according to the present invention can be preferably applied to the fabric by spraying, coating, padding or pad printing. Alternatively, the treatment liquid can also be applied to the fabric using an inkjet head or a valve jet head. This measure of applying the treatment liquid has the advantage that the amount of the required treatment liquid is significantly lower than other application methods. Through the jet head, the treatment liquid can be applied to the fabric area where the image should be printed. Suitable inkjet head types for applying the treatment liquid are piezoelectric type, continuous type, thermal printing head type or valve jet type.

[0126] The fabric to which the treatment liquid has been applied may be dried and optionally heat treated prior to the subsequent inkjetting step with the pigmented ink. Examples of heating processes include, but are not limited to, hot pressing, atmospheric steaming, high pressure steaming, and heat setting (THERMOFIX). The heating process may use any heat source; for example, an infrared lamp may be used.

[0127] In another preferred embodiment of the present invention, the treatment liquid is not substantially dried after being applied to the substrate and before being ejected by an aqueous inkjet step to print the image. Example

[0128] 1. Measurement method

[0129] 1.1. Average particle size

[0130] A sample of the PU dispersion was diluted 10 times with a 0.005 M NaCl aqueous solution. 1.0 mL of the diluted PU dispersion was placed in a disposable polystyrene cuvette (DTS0012), and its z-average particle size was measured three times at 23° C. using a Malvern Zetasizer Nano S after a stabilization time of 30 seconds.

[0131] 1.2. Colloidal stability at elevated pH

[0132] The colloidal stability of aqueous cationic polyurethane dispersions at elevated pH was determined by adding 1 drop of 10 wt% NaOH solution to 3 ml of the dispersion in a test tube. The formation of precipitates, agglomerates or aggregates was assessed visually and assigned a numerical value as listed in Table 4.

[0133] Table 4.

[0134] Visual observation of waterborne PU dispersion grade No differences were observed 0 Transparent dispersion with slight sedimentation 1 Slightly turbid dispersion 2 Severely turbid dispersions 3 Agglomerates 4 Severe agglomeration 5

[0135] 2. Materials

[0136] Unless otherwise stated, all materials used in the following examples are readily available from standard sources such as Sigma-Aldrich (Belgium) and Acros (Belgium). The water used was demineralized water.

[0137] Acetone was analytical grade acetone supplied by VWR International

[0138] Dynacoll 7150 is a polyester diol supplied by Evonik

[0139] Ymer N120 is a 1,3 glycol polyether supplied by Perstorp

[0140] Reaxis C708 is the catalyst, supplied by Reaxis BV (Netherlands)

[0141] DBTL is dibutyltin laurate (KEVER-KAT DBTL 162), supplied by Brenntag

[0142] IPDI is Desmodur I, a polyisocyanate supplied by Covestro

[0143] BD is 1,4-butanediol

[0144] Triethylamine is triethylamine

[0145] SP-8 is benzyl dimethyl dodecyl ammonium chloride

[0146] S-13 Dodecyl (benzyl) diethanol ammonium chloride = Benzazonium chloride supplied by Sachem under the trade name BEXOC

[0147] AS-5.HCL: Dodecyldiethanolammonium chloride is obtained by protonation of Ethomeen C12 (CAS Reg. No. 61791-31-9), i.e. N,N-bis(2-hydroxyethyl)(coconut oil alkyl)amine, as supplied by Akzo: 8.79 g of Ethomeen C12 were dissolved in 25.25 mL of 1.2 M HCl (aq.) in a 100 mL conical flask at ambient temperature and atmospheric pressure. To prepare a solution of N,N-bis(2-hydroxyethyl)(coconut oil alkyl)ammonium chloride, which is further used in the preparation of PU dispersions, 34.75 mL of demineralized water were added to the mixture and the mixture was stirred overnight.

[0148] SURF-1 is Capstone FS3100, a surfactant from Dupont

[0149] PYR is 2-pyrrolidone

[0150] HD is 1,2-hexanediol

[0151] COL is CAB-O-JET 450C, a cyan colorant from Cabot

[0152] The PU-9 dispersion is a replica of the PU-9 dispersion disclosed in the published patent application: WO2018 / 077624, with a solid content of 41.9 wt%

[0153] SURF-2 is Tego Wet 270, a surfactant from Evonik Industries.

[0154] 3. Synthesis of the aqueous polyurethane dispersion according to the present invention

[0155] PU-I1

[0156] 111.73 g Dynacoll 7150 and 174.02 g acetone were weighed in a 500 mL conical flask. A solution of Dynacoll 7150 in acetone was stirred at room temperature using a magnetic stirrer for 60 minutes to obtain a colorless, transparent solution. The polyether diol Ymer N120 was preheated in an oven at 80°C to obtain a liquid product, and 16.40 g Ymer N120 was added to the solution. The resulting polyol mixture was then stirred for 15 minutes using a magnetic stirrer to obtain a polyol mixture for the reaction. The polyol mixture was added to a 500 mL three-necked round-bottom flask equipped with a coil condenser and an overhead stirrer under a continuous nitrogen flow, and the conical flask was rinsed with 19.78 g acetone. A solution of 1.07 g Reaxis C708 in 7.84 g acetone was then added to the reaction mixture. The reaction mixture was heated to 55°C within 30 minutes. 19.69 g of IPDI was then added dropwise over 20 minutes via an addition funnel with a pressure balance arm. The amount of isocyanate was in excess relative to the amount of hydroxyl groups, i.e., NCO / OH = 1.53. After the addition of IPDI, the addition funnel was rinsed with 7.84 g of acetone, and the reaction mixture was stirred at 55° C. for 2 hours. A solution of 2.77 g of BD in 3.92 g of acetone was then added. The reaction mixture was reacted at 48° C. for more than 20 hours and then heated at 55° C. for 1 hour to achieve complete conversion.

[0157] 326.10 g of the mixture of the formed nonionic prepolymers was weighed in a stainless steel container. A water-based dispersion was subsequently prepared using a Disperlux apparatus by adding water during high shear mixing. A solution of 10.35 g of SP-8 in 60 mL of demineralized water was added to the prepolymer mixture over 20 minutes using a 5 cm diameter dissolver under stirring at 700 RPM. In order to obtain a dispersion with a solid content of 35% by weight, 207.47 g of water was added and further mixed for 20 minutes under stirring at 1000 RPM. After further stirring at 900 RPM for 35 minutes, the emulsion was transferred to a 2L round-bottom flask to obtain 502.70 g of viscous dispersion. During the mixing process, part of the solvent had evaporated. Residual volatile solvents were removed from the emulsion by rotary vacuum evaporation under reduced pressure at 40 ° C. Evaporation began at a pressure of 400 mbar and the pressure was gradually reduced until 60 mbar, obtaining 368.70 grams of viscous dispersion. The amount of evaporated water was estimated and 42.80 grams of demineralized water were added to obtain a 35 wt% dispersion. The solids content of the resulting dispersion was measured, i.e. 36.85 wt%. The pH of the resulting dispersion was 5.53. The average particle size was measured in a Malvern particle sizer to be 59.88 nm.

[0158] PU-I2

[0159] 111.73g Dynacoll 7150 and 94.92g acetone were weighed in a 500mL conical flask. The solution of Dynacoll 7150 in acetone was stirred at room temperature using a magnetic stirrer for 60 minutes to obtain a colorless and transparent solution. The polyether diol Ymer N120 was preheated in an oven at 80°C to obtain a liquid product, and 16.40g YmerN120 was added to the Dynacoll solution. The resulting polyol mixture was then stirred for 15 minutes using a magnetic stirrer to obtain a polyol mixture for the reaction. 10.35g SP-08 and 78.60g acetonitrile were then added to a 500mL three-necked round-bottom flask equipped with a coil condenser and an overhead stirrer under a continuous nitrogen flow. The reaction mixture was heated to 60°C and stirred within 30 minutes. When the surfactant was dissolved in acetonitrile, a mixture of Dynacoll and Ymer was added to the reaction solution via an addition funnel. The reaction solution was slightly turbid at the beginning and became transparent when the polyol mixture was added within 30 minutes. After the polyol was added, the funnel was rinsed with 15.82g of acetone. A solution of 1.07g of Reaxis C708 in 7.84g of acetone was added to the reaction mixture. Subsequently, 19.69g of IPDI was added dropwise over 20 minutes via an addition funnel with a pressure balance arm. The amount of isocyanate was in excess relative to the amount of hydroxyl groups, i.e., NCO / OH = 1.53. After the addition of IDPI, the addition funnel was rinsed with 7.86g of acetonitrile, and the reaction mixture was stirred at 55°C for 2 hours. Subsequently, a solution of 2.77g of 1,4-butanediol in 3.92g of acetone was added. The reaction mixture was reacted at 48°C for more than 20 hours and then heated at 55°C for 1 hour to achieve complete conversion.

[0160] 348.10g of the formed nonionic prepolymer mixture was weighed in stainless steel. A water-based dispersion was subsequently prepared using a Disperlux device by adding water during high shear mixing. 276.69g of water was added to the prepolymer mixture in 20 minutes using a 5cm diameter dissolver stirrer under stirring at 900RPM. After further stirring for 30 minutes at 800RPM, the emulsion was transferred to a 2L round-bottom flask to obtain 556.50g of viscous dispersion. Residual volatile solvents were removed from the emulsion by rotary vacuum evaporation under reduced pressure at 40°C. Evaporation began at a pressure of 400 mbar and the pressure was gradually reduced until 60 mbar to obtain 377.70 grams of viscous dispersion. The amount of evaporated water was estimated, and 48.0 grams of demineralized water were added to the viscous dispersion to obtain a dispersion of 35% by weight. The solid content of the resulting dispersion was measured, i.e. 36.60% by weight. The pH of the resulting dispersion was 5.82. The average particle size is 55.34 nm.

[0161] PU-I3

[0162] 110.54 g Dynacoll 7150 and 174.02 g acetone were weighed in a 500 mL conical flask. The solution of Dynacoll 7150 in acetone was stirred at room temperature using a magnetic stirrer for 60 minutes to obtain a colorless, transparent solution. The polyether diol Ymer N120 was preheated in an oven at 80°C to obtain a liquid product, and 16.23 g Ymer N120 was added to the solution. The resulting polyol mixture was then stirred for 15 minutes using a magnetic stirrer to obtain a polyol mixture for the reaction. The polyol mixture was added to a 500 mL three-necked round-bottom flask equipped with a coil condenser and an overhead stirrer under a continuous nitrogen flow, and the conical flask was rinsed with 19.78 g acetone. A solution of 1.07 g Reaxis C708 in 7.84 g acetone was added to the reaction mixture. The reaction mixture was heated to 55°C within 30 minutes. 19.48 g of IPDI was then added dropwise over 20 minutes via an addition funnel with a pressure balance arm. The amount of isocyanate was in excess relative to the amount of hydroxyl groups, i.e., NCO / OH = 1.53. After the addition of IDPI, the addition funnel was rinsed with 7.84 g of acetone, and the reaction mixture was stirred at 55° C. for 2 hours. A solution of 2.74 g of BD in 3.92 g of acetone was then added. The reaction mixture was reacted at 48° C. for more than 20 hours and then heated at 55° C. for 1 hour to achieve complete conversion.

[0163] 318.20 g of the formed nonionic prepolymer mixture was weighed in stainless steel. A water-based dispersion was subsequently prepared using a Disperlux apparatus by adding water during high shear mixing. A solution of 11.92 g of S-13 in 60 mL of demineralized water was added to the prepolymer mixture over 20 minutes using a 5 cm diameter dissolver under stirring at 800 RPM. In order to obtain a dispersion with a solid content of 35% by weight, 202.37 g of water was added and further mixed for 20 minutes under stirring at 900 RPM. After further stirring at 900 RPM for 35 minutes, the emulsion was transferred to a 2L round-bottom flask to obtain 477.00 g of viscous dispersion. During the mixing process, part of the solvent had evaporated. Residual volatile solvents were removed from the emulsion by rotary vacuum evaporation under reduced pressure at 40 ° C. Evaporation began at a pressure of 400 mbar and the pressure was gradually reduced until 60 mbar, obtaining 365.80 grams of viscous dispersion. The amount of evaporated water was estimated and 37.80 grams of demineralized water were added to obtain a 35 wt% dispersion. The solid content of the resulting dispersion was measured, which was 37.69 wt%. The pH of the resulting dispersion was 5.39. The average particle size was 57.37 nm.

[0164] PU-I4

[0165] 112.07 g Dynacoll 7150 and 174.02 g acetone were weighed in a 500 mL conical flask. A solution of Dynacoll 7150 in acetone was stirred at room temperature using a magnetic stirrer for 60 minutes to obtain a colorless, transparent solution. The polyether diol Ymer N120 was preheated in an oven at 80°C to obtain a liquid product, and 16.45 g Ymer N120 was added to the solution. The resulting polyol mixture was then stirred for 15 minutes using a magnetic stirrer to obtain a polyol mixture for the reaction. The polyol mixture was added to a 500 mL three-necked round-bottom flask equipped with a coil condenser and an overhead stirrer under a continuous nitrogen flow, and the conical flask was rinsed with 19.78 g acetone. A solution of 1.07 g Reaxis C708 in 7.84 g acetone was then added to the reaction mixture. The reaction mixture was heated to 55°C within 30 minutes. 19.65 g of IPDI was then added dropwise over 20 minutes via an addition funnel with a pressure equalization arm. The amount of isocyanate was in excess relative to the amount of hydroxyl groups, i.e., NCO / OH = 1.53. After the addition of IDPI, the addition funnel was rinsed with 7.84 g of acetone, and the reaction mixture was stirred at 55° C. for 2 hours. A solution of 2.77 g of BD in 3.92 g of acetone was then added. The reaction mixture was reacted at 48° C. for more than 20 hours and then heated at 55° C. for 1 hour to achieve complete conversion.

[0166] 314.60g of the mixture of the formed nonionic prepolymers was weighed in stainless steel. A water-based dispersion was subsequently prepared using a Disperlux device by adding water during high shear mixing. A solution of 60mL AS-5.HCL was added to the prepolymer mixture in 20 minutes using a 5cm diameter dissolver under stirring at 600RPM. In order to obtain a dispersion with a solid content of 35% by weight, 207.92g of water was added and further mixed for 20 minutes under stirring at 900RPM. After further stirring for 35 minutes at 1000RPM, the emulsion was transferred to a 2L round-bottom flask to obtain 485.50g of viscous dispersion. During the mixing process, part of the solvent had evaporated. Residual volatile solvents were removed from the emulsion by rotary vacuum evaporation under reduced pressure at 40°C. Evaporation began at a pressure of 400 mbar and the pressure was gradually reduced until 60 mbar, obtaining 349.20 grams of viscous dispersion. The amount of evaporated water was estimated and 47.60 grams of demineralized water were added to obtain a 35 wt% dispersion. The solid content of the resulting dispersion was measured, which was 39.38 wt%. The pH of the resulting dispersion was 5.59. The average particle size was 52.46 nm.

[0167] 4. Synthesis of Comparative Waterborne Polyurethane Dispersions

[0168] The comparative PU dispersion (PU-C1) corresponds to the dispersion PU-2 mentioned in patent application WO2019 / 105786.

[0169] The comparative PU dispersion (PU-C2) corresponds to the dispersion PU-4 mentioned in patent application WO2019 / 105786.

[0170] 5. Resistance to pH increase

[0171] According to method 1.2, the change in colloidal stability under increased pH simulating the application of inkjet ink to the applied pre-treatment liquid was determined. The test results are summarized in Table 5.

[0172] Table 5.

[0173] PU-resin dispersion Invention / Comparative Cationic surfactants are added to the organic solvent before / after the reaction Colloidal stability at elevated pH PU-I1 The present invention back 1 PU-I2 The present invention forward 1 PU-I3 The present invention back 0 PU-I4 The present invention back 1 PU-C1 Comparative not applicable 4

[0174] As can be seen from the results of Table 5, the PU-resin dispersions according to the invention show better colloidal stability at elevated pH, thus indicating that they better retain their cationic character, which leads to improved fixing ability when used in the pretreatment of substrates prior to inkjet printing.

[0175] Example 2

[0176] This example shows that a treatment liquid in which the PU resin dispersion according to the invention is combined with a white pigment exhibits excellent storage stability.

[0177] Preparation of white pigment dispersion (WIT-1)

[0178] 275 g of white pigment (TRONOX CR 834) were added to a mixture of 68.75 g of Disperbyk 190 and 2.2 g of Proxel K in 204.05 g of water over 30 minutes under high shear with the aid of a Disperlux. 200 g of 0.4 mm yttrium stabilized zirconium oxide beads ("High Wear Resistant Zirconia Grinding Media" from TOSOH Co.) were added and the white pigment was milled in a Dynomill Research Lab at a flow rate of 4500 tons / min for 75 minutes. The zirconium oxide beads were removed by filtration and the dispersion was filtered through a 0.7 μm filter. The average particle size of the dispersion WIT-1 was 183 nm.

[0179] Preparation of treatment liquids PTL-1 and PTL-2

[0180] The treatment liquids PTL-1 and PTL-2 are mixed Table 6 All weight percentages are relative to the total weight of the liquid.

[0181] Table 6.

[0182] PTL-1 PTL-2 Compound Content by weight% Content by weight% PU-C2 33.43 - PU-I4 - 30.47 WIT-1 22.00 22.00 PYR 15.0 15.0 HD 15.0 15.0 SURF-1 0.8 0.8 water Until 100% Until 100%

[0183] PTL-2 showed no aggregates or flocculation when visually inspected by optical transmission microscopy after 1 month storage under standard conditions (temperature, pressure, light). This shows that the PU-resin according to the invention can be combined with white pigments without causing stability problems in the treatment liquid.

[0184] Example 3

[0185] This example illustrates the ability of the cationic polyurethane binder in the treatment solution according to the present invention to fix the colorant.

[0186] Preparation of INK-1

[0187] The cyan ink INK-1 was prepared by mixing the compounds given in Table 7. All weight percentages are relative to the total weight of the inkjet ink.

[0188] Table 7

[0189] INK-1 Compound Content by weight% PU-9 dispersion 28.64 PYR 20.00 HD 20.00 SURF-2 0.60 COL 20.00 water Until 100%

[0190] Evaluation and Results

[0191] The treatment liquids PTL-1 and PTL-2 were applied with a spiral rod coater (from Elcometer) on a piece of black leather cut from black dyed dry hard cowhide leather coated with a black pigment layer from Conceria Nuti Ivo SPA (Italy) using an automatic film applicator (Elcometer 4340 from Elcometer) at a speed of 20 mm / s and a wet thickness of 20 μm. After drying the coating layer in an oven at 60° C. for 5 minutes, the treated substrate sheet was coated with INK-1 by means of the same 20 μm spiral rod. The coated sample was dried at 60° C. for 5 minutes.

[0192] Using X-Rite TM The reflectance spectrum of each coated sample after drying was measured twice by the eXact spectrophotometer in the range of 400 to 700 nm with a step size of 10 nm. The CIEL*a*b* coordinates were determined for a 2° observer and a D50 illuminant.

[0193] The following formula relates the measured color difference to a known set of CIEL*a*b* coordinates. Given two colors (L1, a1, b1) and (L2, a2, b2) in the CIEL*a*b* color space, the CIE76 color difference formula is defined as:

[0194] As explained in Sharma, Gaurav (2003). Digital Color Imaging Handbook (Edition 1.7.2). CRC Press. ISBN 0-8493-0900-X, a value of ΔE ≥ 2.3 corresponds to a JND (Just Noticeable Difference).

[0195] The L*a*b* values ​​are summarized in Table 8. The lower the a* value and the lower the b* value, the more cyan the color.

[0196] Table 8.

[0197] Sample No. Treatment fluid Inkjet ink L* a* b* 1 (Comparative) PTL-1 INK-1 24.13 -3.96 -29.36 2 (the present invention) PTL-2 INK-1 24.45 -5.19 -32.33

[0198] As can be seen from Table 8, the color prints using the pre-treatment liquid according to the invention (PTL-2 + INK-1) give more cyan color values ​​than the color prints using the pre-treatment liquid without the polyurethane dispersion according to the invention. In addition, the ΔE 76 between the two samples can be calculated and observed to be equal to 3.24, which represents a significant visual color difference.

Claims

1. An aqueous polyurethane resin dispersion, the polyurethane resin having polyalkylene oxide in its side chains and obtained by reacting a polyisocyanate with a 1,2 or 1,3 polyether diol and with a polymeric diol selected from polyester diols, polyether diols, polycarbonate diols, polyacrylate diols and polyolefin diols in an organic solvent and by adding a cationic surfactant containing a quaternized ammonium group to the organic solvent, wherein the cationic surfactant is a quaternary ammonium group according to formula II in R1 is hydrogen or an unsubstituted alkyl group having 1 to 4 carbon atoms R2 and R3 are independently a benzyl group or an unsubstituted alkyl group having between 1 and 18 carbon atoms. R4 is an unsubstituted alkyl group having at least 12 carbon atoms.

2. The aqueous polyurethane resin dispersion according to claim 1, wherein the cationic surfactant is added after the reaction is completed.

3. An aqueous treatment liquid for inkjet printing, comprising the polyurethane resin dispersion as defined in claim 1 in an amount of 1 wt% to 30 wt% relative to the total weight of the treatment liquid. 4 . The aqueous treatment liquid for inkjet printing according to claim 3 , further comprising a flocculant. 5 . The aqueous treatment liquid for inkjet printing according to claim 3 , further comprising a pigment. 6 . The aqueous treatment liquid for inkjet printing according to claim 5 , wherein the pigment comprises titanium dioxide.

7. The aqueous treatment liquid for inkjet printing according to claim 4, wherein the flocculant is a multivalent metal salt.

8. An aqueous inkjet ink comprising a pigment dispersion and a polyurethane resin dispersion as defined in claim 1 in an amount of 1 wt % to 30 wt % relative to the total weight of the ink, the pigment dispersion comprising at least one dispersant having formula III in R1 is selected from hydrogen, unsubstituted alkyl groups, unsubstituted alkenyl groups, unsubstituted alkynyl groups, unsubstituted aralkyl groups, unsubstituted alkaryl groups, unsubstituted aryl groups and unsubstituted heteroaryl groups L represents a divalent linking group containing 2 to 10 carbon atoms R2, R3 and R4 are independently selected from unsubstituted alkyl groups, unsubstituted alkenyl groups, unsubstituted alkynyl groups, unsubstituted aralkyl groups, unsubstituted alkaryl groups, unsubstituted aryl groups and unsubstituted heteroaryl groups. Any of R1, R2, R3, R4 and L may represent atoms necessary to form a five- to eight-membered ring. R5 represents a hydrocarbon group containing at least 8 carbon atoms X - represents an anion that counteracts the positive charge of the ammonium group.

9. A method for preparing an aqueous polyurethane resin dispersion, the method comprising the following steps: (i) reacting a polyisocyanate with a 1,2 or 1,3 polyether diol, a polymeric diol selected from polyester diols, polyether diols, polycarbonate diols, polyacrylate diols and polyolefin diols in an organic solvent in the presence of a cationic surfactant containing a quaternized ammonium group as defined in the aqueous polyurethane resin dispersion according to claim 1 to form a solution of a polyurethane resin; and (ii) adding water to the solution to form a polyurethane resin dispersion; and (iv) removing the organic solvent from the dispersion.

10. A method for preparing an aqueous polyurethane resin dispersion, the method comprising the following steps: (i) reacting a polyisocyanate with a 1,2 or 1,3 polyether diol, a polymeric diol selected from polyester diols, polyether diols, polycarbonate diols, polyacrylate diols and polyolefin diols in an organic solvent to form a solution of a polyurethane resin; and (ii) adding to the solution a cationic surfactant comprising a quaternized ammonium group as defined in the aqueous polyurethane resin dispersion according to claim 1; and (iii) adding water to the solution to form a polyurethane resin dispersion; and (iv) removing the organic solvent from the dispersion.

11. An inkjet recording method, comprising the steps of: (i) providing a substrate; and (ii) forming a pretreated substrate by applying a treatment liquid as defined in any one of claims 3 to 7 onto the surface of the substrate, and optionally drying the substrate; and (iii) printing an image by jetting inkjet ink onto the pretreated substrate.

Citation Information

Patent Citations

  • Photosensitive composition, planographic printing plate precursor, and image forming method

    JP2009237174A

  • Ink jet treatment liquid, ink jet recording method, and recorded matter

    US20090233065A1

  • Light fast quaternized or amine salt polyurethanes from 2-alkyl - 2 - dialkylaminomethyl-1,3-propane diols

    US3686108A

  • Cationic polyurethane resin aqueous dispersion, ink-jet receiving agent including the same, and ink-jet recording medium using the same

    US7964665B2

  • White inkjet ink improved for dispersion stability