High permeability soft magnetic alloy and method for producing high permeability soft magnetic alloy

By optimizing the composition and heat treatment process of FeCo alloy, the high cost and manufacturing difficulties of existing soft magnetic materials have been solved, realizing a low-cost, high-permeability FeCo alloy suitable for high power density and miniaturized design in motors.

CN114156079BActive Publication Date: 2024-12-06VACUUMSCHMELZE GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111483709.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-24
Filing Date
2018-10-25
Publication Date
2024-12-06
Estimated Expiration
2038-10-25

AI Technical Summary

Technical Problem

Existing soft magnetic materials such as SiFe and CoFe alloys face high costs and manufacturing challenges in fields such as electric vehicles. In particular, CoFe alloys have high material and manufacturing costs due to their high Co content and additional production steps, and are difficult to mass-produce.

Method used

To develop an FeCo alloy containing a specific range of elements such as Co, V, Cr, Si, Mn, and Al, with a maximum Co content of 25%, by optimizing the alloy composition and heat treatment process to avoid ordered phase transformation, simplify the production process, improve magnetic permeability, and reduce manufacturing costs.

Benefits of technology

A low-cost, high-permeability FeCo alloy has been developed, suitable for high power density and miniaturized designs in motors, reducing motor size and weight while minimizing eddy current and coercive losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114156079B_ABST
    Figure CN114156079B_ABST
Patent Text Reader

Abstract

A soft magnetic alloy is disclosed, which is basically composed of: 5 weight % ≤ Co ≤ 25 weight %, 0.3 weight % ≤ V ≤ 5.0 weight %, 0 weight % ≤ Cr ≤ 3.0 weight %, 0 weight % ≤ Si ≤ 3.0 weight %, 0 weight % ≤ Mn ≤ 3.0 weight %, 0 weight % ≤ Al ≤ 3.0 weight %, 0 weight % ≤ Ta ≤ 0.5 weight %, 0 weight % ≤ Ni ≤ 0.5 weight %, 0 weight % ≤ Mo ≤ 0.5 weight %, 0 weight % ≤ Cu ≤ 0.2 weight %, 0 weight % ≤ Nb ≤ 0.25 weight %, and the balance is Fe and impurities up to 0.2 weight %.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with the application date of October 25, 2018, application number 201880070219.5, and invention name "High magnetic permeability soft magnetic alloy and method for manufacturing high magnetic permeability soft magnetic alloy". Technical Field

[0002] The invention relates to a soft magnetic alloy, in particular to a high magnetic permeability soft magnetic alloy. Background Art

[0003] Non-grain-oriented electrical steel (SiFe) with about 3% by weight of silicon is currently the most widely used crystalline soft magnetic material for the sheet metal stacks (laminated core, lamination stack, Blechpaketen) of electric motors. With the development of electric vehicles, more efficient materials with better properties than SiFe are needed. This means that in addition to having a sufficiently high electrical resistance, a higher induction level is primarily desired to form a high torque and / or a small structural volume.

[0004] For use in some technologies such as the automotive industry and electric vehicles, more efficient materials are desired. Soft magnetic cobalt-iron alloys (CoFe) are also used in electric motors due to their extremely high saturation induction. Commercially available CoFe alloys generally have a composition of 49 wt. % Fe, 49 wt. % Co and 2% V. With this composition, the saturation induction reaches about 2.35 T at a high resistivity of 0.4 μΩm. However, it is desirable to reduce the material and manufacturing costs of CoFe alloys, which are generated, for example, by high Co content, additional production steps and scrap content. Summary of the invention

[0005] Therefore, the problem to be solved in this paper is to provide a FeCo alloy with low material cost and good machinability in order to reduce the manufacturing cost of the alloy until the sheet stack, while achieving high power density.

[0006] This is achieved by the subject matter of the independent claims. Further advantageous solutions are the subject matter of the dependent claims.

[0007] According to the present invention, there is provided a soft magnetic alloy, in particular a high magnetic permeability soft magnetic FeCo alloy, which is basically composed of:

[0008] 5 wt% ≤ Co ≤ 25 wt%

[0009] 0.3 wt% ≤ V ≤ 5.0 wt%

[0010] 0 wt% ≤ Cr ≤ 3.0 wt%

[0011] 0 wt%≤Si≤3.0 wt%

[0012] 0 wt%≤Mn≤3.0 wt%

[0013] 0 wt% ≤ Al ≤ 3.0 wt%

[0014] 0wt%≤Ta≤0.5wt%

[0015] 0 wt% ≤ Ni ≤ 0.5 wt%

[0016] 0 wt%≤Mo≤0.5 wt%

[0017] 0 wt% ≤ Cu ≤ 0.2 wt%

[0018] 0 wt% ≤ Nb ≤ 0.25 wt%

[0019] 0 wt%≤Ti≤0.05 wt%

[0020] 0 wt% ≤ Ce ≤ 0.05 wt%

[0021] 0 wt%≤Ca≤0.05 wt%

[0022] 0 wt%≤Mg≤0.05 wt%

[0023] 0 wt% ≤ C ≤ 0.02 wt%

[0024] 0 wt% ≤ Zr ≤ 0.1 wt%

[0025] 0 wt%≤0≤0.025 wt%

[0026] 0 wt% ≤ S ≤ 0.015 wt%

[0027] The balance is iron, with Cr+Si+Al+Mn≤3.0 wt% and other impurities up to 0.2 wt%. The maximum magnetic permeability of the alloy is μ max ≥5,000, preferably μ max ≥10,000, preferably μ max ≥12,000, preferably μ max ≥17,000. Other impurities include B, P, N, W, Hf, Y, Re, Sc, Be, and other lanthanide elements except Ce.

[0028] Due to the low Co content of the alloy of the invention, the raw material costs are reduced compared to an alloy based on 49 wt. % Fe, 49 wt. % Co, 2 % V. According to the invention, an FeCo alloy with a maximum Co content of 25 wt. % is produced, which has better soft magnetic properties, in particular a significantly higher magnetic permeability than other FeCo alloys with a maximum Co content of 25 wt. %, such as existing and commercially available FeCo alloys such as VACOFLUX 17, AFK 18 or HIPERCO 15. The maximum magnetic permeability of these existing and commercially available alloys is less than 5000.

[0029] The alloy according to the invention has no significant ordering, so that, unlike alloys with more than 30 wt. % Co, this alloy can be cold rolled without an upstream quenching process. The quenching process is difficult to control, especially in the case of large amounts of material, because it is difficult to achieve sufficiently fast cooling rates, so that an ordering occurs, which leads to embrittlement of the alloy. In the alloy according to the invention, the order-disorder transition is omitted, thus simplifying large-scale production.

[0030] A clear order-disorder transition, as in CoFe alloys with a Co content of more than 30 wt. %, can be determined by DSC measurements (differential scanning calorimetry) because it results in a peak in the DSC measurements. For the alloys according to the invention, this peak is not detectable in DSC measurements under the same conditions.

[0031] At the same time, the new alloy has much lower hysteresis losses than previously known and commercially available alloys with Co contents between 10 and 30 wt. %, as well as a higher saturation in addition to significantly higher permeability levels never achieved in such alloys. The FeCo alloy of the invention can also be manufactured cost-effectively on a large scale.

[0032] The alloy of the present invention can be used to reduce the size of the rotor or stator due to its high magnetic permeability in applications such as the rotor or stator of an electric motor, thereby reducing the size of the electric motor and / or increasing the power. For example, higher torque can be generated at the same structural size and / or at the same weight, which is advantageous when used in electric or hybrid vehicles.

[0033] In addition to the maximum magnetic permeability μ max ≥5,000, preferably μ max ≥10,000, preferably μ max ≥12,000, preferably μ max ≥17,000, the alloy may also have a resistivity ρ ≥ 0.25 μΩm, preferably ρ ≥ 0.30 μΩm, and / or a hysteresis loss P Hys ≤0.07J / kg, preferably hysteresis loss P Hys≤0.06J / kg, preferably hysteresis loss P Hys ≤0.05J / kg, both at an amplitude of 1.5T, and / or a coercive field strength H c ≤0.7A / cm, preferably coercive field strength H c ≤0.6A / cm, preferably coercive field strength H c ≤0.5A / cm, preferably coercive field strength H c ≤0.4A / cm, preferably coercive field strength H c ≤0.3A / cm, and / or preferably the induction B at 100A / cm is ≥1.90T, preferably the induction B at 100A / cm is ≥1.95T, preferably the induction B at 100A / cm is ≥2.00T.

[0034] Hysteresis loss P Hys The repetitive magnetization loss P is determined by linear regression from the Y-intercept of the frequency f in the curve P / f at an amplitude of 1.5 T induction. The linear regression is performed on at least 8 measurements that are approximately evenly distributed over the frequency range of 50 Hz to 1 kHz (e.g., at 50, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1,000 Hz).

[0035] In one embodiment, the maximum magnetic permeability μ of the alloy is max ≥μ max ≥10,000, resistivity ρ≥0.28 μΩm, hysteresis loss P Hys ≤0.055J / kg, amplitude is 1.5T, coercive field strength H c ≤0.5A / cm, induction B≥1.95T at 100 A / cm. This combination of properties is particularly advantageous for applications as or for rotors or stators of electric motors to reduce the size of the rotor or stator, thereby reducing the motor and / or increasing the power, or generating higher torque at the same structural size and / or the same weight.

[0036] Therefore, the soft magnetic alloy can be used in electrical machines, for example as or in stators and / or rotors of motors and / or generators, and / or in transformers and / or in electromagnetic actuators. It can be provided in the form of a sheet, for example with a thickness of 0.5 mm to 0.05 mm. Several sheets of the alloy can be stacked into a sheet stack (or laminated core) for use as a stator or rotor.

[0037] The alloy according to the invention has a resistivity of at least 0.25 μΩm, preferably a minimum of 0.3 μΩm. The eddy current losses can be reduced to a lower level by choosing a slightly lower strip thickness.

[0038] In a further embodiment, the composition of the soft magnetic alloy is defined in more detail, wherein 10 weight % ≤ Co ≤ 20 weight %, preferably 15 weight % ≤ Co ≤ 20 weight % and 0.3 weight % ≤ V ≤ 5.0 weight %, preferably 1.0 weight % ≤ V ≤ 3.0 weight %, preferably 1.3 weight % ≤ V ≤ 2.7 weight % and / or 0.1 weight % ≤ Cr+Si ≤ 2.0 weight %, preferably 0.2 weight % ≤ Cr+Si ≤ 1.0 weight %, preferably 0.25 weight % ≤ Cr+Si ≤ 0.7 weight %.

[0039] In one embodiment, the sum is defined in more detail, wherein 0.2 wt % ≤ Cr + Si + Al + Mn ≤ 1.5 wt %, preferably 0.3 wt % ≤ Cr + Si + Al + Mn ≤ 0.6 wt %.

[0040] The soft magnetic alloy may also contain silicon, wherein 0.1 wt %≤Si≤2.0 wt %, preferably 0.15 wt %≤Si≤1.0 wt %, preferably 0.2 wt %≤Si≤0.5 wt %.

[0041] Aluminum and silicon can be interchangeable, so in one embodiment, the sum of Si and aluminum (Si+Al) is 0 wt % ≤ (Si+Al) ≤ 3.0 wt %.

[0042] The alloy according to the invention is virtually carbon-free and has a maximum of 0.02% by weight of carbon, preferably ≤0.01% by weight of carbon. This maximum carbon content is regarded as an unavoidable impurity.

[0043] In the alloy according to the invention, calcium, beryllium and / or magnesium can only be alloyed on a small scale of up to 0.05 wt. % for deoxidation and desulfurization. In order to achieve a particularly good deoxidation effect, up to 0.05 wt. % Cer (cerium) or Cer mixed metals can be alloyed.

[0044] According to the invention, improved magnetic properties can be achieved by heat treatments that are matched to the following compositions. In particular, it has been found that determination of the phase transition temperatures for the selected composition and determination of the heat treatment temperatures and cooling rates relative to these determined phase transition temperatures leads to improved magnetic properties. Furthermore, considering that the alloys according to the invention with a cobalt content of up to 25% by weight do not have an order-disorder transition, no quenching is required during production to avoid ordering and the resulting embrittlement.

[0045] CoFe alloys are usually used in strip thicknesses in the very thin size range of 0.50 mm to 0.050 mm. For strip processing, the material is usually hot-rolled and then cold-rolled to its final thickness. During cooling, after hot rolling, embrittlement occurs at about 730° C., so that a special intermediate annealing and subsequent quenching are necessary to suppress the ordering in order to enable sufficient cold rolling. This quenching is omitted in the alloy according to the invention, since it has no order-disorder transition, which simplifies production.

[0046] In order to obtain magnetic properties, the CoFe alloy is subjected to a final heat treatment, which is also called magnetic final annealing. For this purpose, the material is heated to the annealing temperature, kept at the annealing temperature for a certain time, and then cooled at a specified rate. It is advantageous to carry out the final annealing at the highest possible temperature and in a dry, pure hydrogen atmosphere, because firstly the reduction of impurities by hydrogen becomes more effective, and secondly, the grain structure becomes coarser, thus improving the soft magnetic properties such as coercive field strength and magnetic permeability.

[0047] In practice, there is an upper limit to the annealing temperature in the CoFe system because a phase transformation occurs in the binary system at about 950°C, converting the magnetic and ferrite BCC phase to the non-magnetic and austenitic FCC phase. When alloying occurs, a two-phase region forms between the FCC and BCC phases, where the two phases coexist. The transition temperature between the BCC phase and the two-phase or BCC / FCC mixed region is T ü1 , and the transition temperature between the two-phase region and the FCC phase is T ü2 , where T ü2 >T ü1 . The location and size of the two-phase region also depends on the type and degree of alloying. If annealing occurs in the two-phase region or in the FCC region, the remnants of the FCC phase after cooling and incomplete reversal will damage the magnetic properties. Even if a complete reversal takes place, the destructive effect still exceeds the additionally produced grain boundaries, since the coercive field strength is inversely proportional to the grain diameter. Therefore, known commercial alloys with a Co content of 20 wt. % are final annealed at a temperature below the two-phase region BCC+FCC. For example, for AFK 18, 3h / 850°C and for AFK 1, 3h / 900°C are recommended. For VACOFLUX 17, 10h / 850°C are recommended. At such low final annealing temperatures, due to the relatively high magnetocrystalline anisotropy (K1 is about 45,000 J / m at a Co content of 17 wt. %), the magnetocrystalline anisotropy is increased. 3 ), these FeCo alloys limit the potential for particularly good soft magnetic properties. Thus, for example, when using VACOFLUX 17 strip, only a maximum permeability of 4,000 can be achieved, while the coercive field strength is typically 1 A / cm, which limits the application.

[0048] Compared to these known final annealing processes, the composition according to the invention enables a heat treatment which produces better magnetic properties than the one-step annealing with furnace cooling usually used for FeCo alloys, regardless of the temperature range in which the one-step annealing is carried out. The alloying is selected so that the lower limit of the two-phase region and the BCC / FCC phase transformation are shifted upwards, so that annealing can be carried out at high temperatures, for example above 925° C., in the pure BCC region. Annealing at such high temperatures is not possible with previously known FeCo alloys.

[0049] In addition, due to the composition according to the invention, the width of the two-phase region, i.e., the lower transition temperature T ü1 and a higher transition temperature T ü2 The difference between should be as small as possible. Therefore, a final annealing above the two-phase region, in conjunction with cooling through the two-phase region and subsequent holding time or controlled cooling in the pure BCC region, results in a high final annealing, i.e. the removal of possible magnetically unfavorable textures, the cleaning effect under H2 and the advantages of the growth of large grains, without the risk of magnetically detrimental residues of the FCC phase.

[0050] It has been found that compositions having a phase transition between the pure BCC region and the BCC / FCC mixed region at higher temperatures (e.g., above 925°C) and having a narrow two-phase region (e.g., less than 45 K) show significant improvements in magnetic properties. Compositions having a specific combination of phase diagram features are selected according to the present invention and heat treated accordingly to ensure high permeabilities greater than 5000 or greater than 10,000.

[0051] In Fe-Co alloys, vanadium is considered to be one of the most effective elements, which increases the electrical resistance and simultaneously shifts the two-phase region to higher temperatures. Vanadium is more effective in increasing the transformation temperature at lower cobalt contents. For Fe-17Co alloys, by adding about 2% vanadium, the transformation temperature can even be increased above the value of the binary FeCo composition.

[0052] In the Fe-Co system, starting from about 15% cobalt, the temperature of the BCC / FCC phase transition is at temperatures as low as the Curie temperature. Since the FCC phase is paramagnetic, the magnetic phase transition no longer depends on the Curie temperature, but on the BCC / FCC phase transition. Sufficiently high vanadium contents will shift the BCC / FCC phase transition past the Curie temperature T c , making the paramagnetic BCC phase visible.

[0053] However, if the vanadium content is too high, the width of the mixed zone increases. These compositions have lower maximum permeability values, although the phase transformation between the BCC / FCC mixed zone and the pure BCC zone occurs at a higher temperature. It was found that the composition affects both the temperature at which the phase transformation occurs and the width of the mixed zone, and should be considered when selecting the composition. In order to obtain the highest permeability value, the temperature of the heat treatment can be selected relative to the temperature at which the phase transformation occurs for the composition.

[0054] It has therefore been found that when optimizing a production process, it is advantageous to determine more precisely the temperature at which the phase transition occurs for a specific composition. These can be determined by DSC measurements (differential scanning calorimetry). The DSC measurements can be carried out with a sample mass of 50 mg and a DSC heating rate of 10 K / min, so that the phase transition temperatures determined during sample heating and cooling can be used to determine the temperature of the heat treatment.

[0055] Chromium and other elements can be added to improve electrical resistance or mechanical properties. Chromium, like most other elements, reduces the two-phase region of binary Fe-17Co alloys. Therefore, the alloying proportions other than vanadium are preferably selected in such a way that, in combination with vanadium, the two-phase region is increased compared to binary FeCo alloys. For this purpose, impurities and elements that stabilize austenite in particular, such as nickel, must be kept as low as possible.

[0056] To obtain good magnetic properties, the following contents have proven to be preferred:

[0057] Cobalt, 5 wt% ≤ Co ≤ 25 wt%, preferably 10 wt% ≤ Co ≤ 20 wt%, particularly preferably 15 wt% ≤ Co ≤ 20 wt%

[0058] Vanadium, 0.3 wt % ≤ V ≤ 5.0 wt %, preferably 1.0 wt % ≤ V ≤ 3.0 wt % and the following sum: 0.2 wt % ≤ Cr+Si+Al+Mn ≤ 3.0 wt %.

[0059] The alloy according to the invention is virtually carbon-free and has a maximum of 0.02% by weight of carbon, preferably ≤0.01% by weight of carbon. This maximum carbon content is regarded as an unavoidable impurity.

[0060] In the alloy according to the invention, calcium, beryllium and / or magnesium can only be added in small amounts of not more than 0.05 wt. % for deoxidation and desulfurization. In order to achieve particularly good deoxidation and desulfurization, up to 0.05 wt. % Cer or Cer mixed metals can be alloyed.

[0061] A further improvement is achieved according to the composition of the invention. The diffusion coefficient of cobalt in the paramagnetic BCC phase is higher than that in the ferromagnetic BCC phase. Therefore, vanadium is separated from the two-phase region and the Curie temperature Tc Separation enables self-diffusion over a larger temperature range, so that heat treatment in this region or cooling through this region produces a larger BCC grain structure and therefore better soft magnetic properties. In addition, the two-phase region and the Curie temperature T c The separation of the two phases means that during cooling, the passage through the two-phase region BCC / FCC and the transition to the pure BCC phase occur completely in the paramagnetic state. This also has a positive effect on the soft magnetic properties.

[0062] According to the present invention, there is provided a method for producing a soft magnetic FeCo alloy, wherein the method has the following features: A preform is provided, which is essentially composed of

[0063] 5 wt% ≤ Co ≤ 25 wt%

[0064] 0.3 wt% ≤ V ≤ 5.0 wt%

[0065] 0 wt% ≤ Cr ≤ 3.0 wt%

[0066] 0 wt%≤Si≤3.0 wt%

[0067] 0 wt%≤Mn≤3.0 wt%

[0068] 0 wt% ≤ Al ≤ 3.0 wt%

[0069] 0wt%≤Ta≤0.5wt%

[0070] 0 wt% ≤ Ni ≤ 0.5 wt%

[0071] 0 wt%≤Mo≤0.5 wt%

[0072] 0 wt% ≤ Cu ≤ 0.2 wt%

[0073] 0 wt% ≤ Nb ≤ 0.25 wt%

[0074] 0 wt%≤Ti≤0.05 wt%

[0075] 0 wt% ≤ Ce ≤ 0.05 wt%

[0076] 0 wt%≤Ca≤0.05 wt%

[0077] 0 wt%≤Mg≤0.05 wt%

[0078] 0 wt% ≤ C ≤ 0.02 wt%

[0079] 0 wt% ≤ Zr ≤ 0.1 wt%

[0080] 0 wt%≤0≤0.025 wt%

[0081] 0 wt% ≤ S ≤ 0.015 wt%

[0082] The balance is iron, with Cr+Si+Al+Mn≤3.0 wt. % and up to 0.2 wt. % of other melt-related impurities. Other impurities may include, for example, one or more of the elements B, P, N, W, Hf, Y, Re, Sc, Be, and lanthanides other than Ce. In some embodiments, the preform has a cold rolled texture or a fiber texture.

[0083] The preform or the part made from the preform is subjected to heat treatment. In one embodiment, the preform is heated at a temperature T1 and then cooled from T1 to room temperature.

[0084] In another alternative embodiment, the preform is cooled at temperature T1, then cooled at temperature T2 above room temperature, and further heat treated at temperature T2, wherein T1 > T2. Only after the heat treatment at temperature T2 is the preform cooled to room temperature.

[0085] The preform has a phase transition from the BCC phase region to the BCC / FCC mixed region to the FCC phase region, wherein the phase transition between the BCC phase region and the BCC / FCC mixed region occurs at the first transition temperature T ü1 When the temperature rises, the phase transition between the BCC / FCC mixed region and the FCC phase region occurs at the second transition temperature T ü2 , where T ü2 >T ü1 . Temperature T1 is higher than T ü2 , temperature T2 is lower than T ü1 .

[0086] Transition temperature T ü1 and T ü2 Depends on the composition of the preform. The phase transition temperature T can be determined by DSC measurement ü1 and T ü2 , where the phase transition temperature T is determined during the heating process ü1 , determine the phase transition temperature T during cooling ü2 In one embodiment, when the sample mass is 50 mg and the DSC heating rate is 10 K / min, the transition temperature T ü1 Above 900°C, preferably above 920°C, preferably above 940°C.

[0087] In one embodiment, the solidus temperature of the preform is taken into account when selecting the temperatures T1 and T2. In one embodiment, 900°C ≤ T1 <T m , preferably 930℃≤T1 <T m , preferably 940℃≤T1 <T m , preferably 960℃≤T1 <T mand 700 °C ≤ T2 ≤ 1050 °C and T2 < T1, where T m is the solidus temperature.

[0088] In one embodiment, the difference between T ü2 and T ü1 is less than 45 K, preferably less than 25 K.

[0089] In one embodiment, the cooling rate is at least in the temperature range from T1 to T2 is 10 °C / h to 50,000 °C / h, preferably 10 °C / h to 900 °C / h, preferably 20 °C / h to 1,000 °C / h, preferably 20 °C / h to 900 °C / h, preferably 25 °C / h to 500 °C / h. Such a cooling rate can be used for the above two heat treatments.

[0090] In one embodiment, T ü2 -T ü1 the difference between is less than 45 K, preferably less than 25 K, T1 is higher than T ü2 , T2 is lower than T ü1 , where 940 °C ≤ T1 < T m , 700 °C ≤ T2 ≤ 1050 °C and T2 < T1, where T m is the solidus temperature, and the cooling rate is at least in the temperature range from T1 to T2 is 10 °C / h to 900 °C / h. The properties of the alloy, namely T ü2 and T ü1 , this combination of the heat treatment temperatures T1 and T2 can be used to achieve particularly high permeability values.

[0091] In one embodiment, the preform is heat-treated above T ü2 for a time exceeding 30 minutes and then cooled to T2.

[0092] In one embodiment, the preform is heat-treated at T1 for a period of time t1, where 15 minutes ≤ t1 ≤ 20 hours, and then cooled from T1 to T2. In one embodiment, the preform is cooled from T1 to T2, heat-treated at T2 for a period of time t2, where 30 minutes ≤ t2 ≤ 20 hours, and then cooled from T2 to room temperature.

[0093] In the embodiment of cooling the preform from T1 to room temperature, the preform can then be heated from room temperature to T2 and heat-treated at T2 according to one of the embodiments described herein.

[0094] Since the alloy has no order-disorder transformation, quenching is omitted in the temperature range of 800°C to 600°C. For example, the cooling rate range from 800°C to 600°C can be 100°C / h to 500°C / h. However, slower cooling rates can also be selected in principle. The above cooling rates can also be carried out without problems to room temperature.

[0095] The preform may be cooled from T1 to room temperature at a rate of 10 to 50,000°C / h, preferably 10 to 1,000°C / h, preferably 10 to 900°C / h, preferably 25 to 900°C / h, preferably 25 to 500°C / h.

[0096] The cooling rate from T2 to room temperature has little effect on the magnetic properties, so the preform may be cooled from T2 to room temperature at a rate of 10°C / h to 50,000°C / h, preferably 100°C / h to 1000°C / h.

[0097] In another alternative embodiment, the preform is cooled from T1 to room temperature with a cooling rate of 10°C / h to 900°C / h. In embodiments with slow cooling from T1 to room temperature, for example a cooling rate less than 500°C / h, preferably less than 200°C / h, further heat treatment at temperature T2 may also be avoided.

[0098] After heat treatment, soft magnetic alloys can have one of the following property combinations:

[0099] Maximum magnetic permeability μ max ≥5,000, and / or resistivity ρ ≥0.25μΩm, ​​and / or hysteresis loss P at an amplitude of 1.5T Hys ≤0.07J / kg, coercive field strength H c ≤0.7A / cm, induction B≥1.90T at 100A / cm, or

[0100] Maximum magnetic permeability μ max ≥10,000, and / or resistivity ρ ≥0.25μΩm, ​​and / or hysteresis loss P at an amplitude of 1.5T Hys ≤0.06J / kg, and / or coercive field strength H c ≤0.6A / cm, preferably H c ≤0.5 A / cm and / or induction B≥1.95T at 100A / cm, or

[0101] Maximum magnetic permeability μ max ≥12,000, preferably μ max ≥17,000 and / or resistivity ρ ≥0.30μΩm, and / or hysteresis loss P at 1.5T amplitude Hys≤0.05J / kg, and / or coercive field strength H c ≤0.5A / cm, preferably H c ≤0.4A / cm, preferably H c ≤0.3A / cm and / or induction B≥2.00T at 100A / cm.

[0102] In some embodiments, the soft magnetic alloy has one of the following combinations of properties:

[0103] Maximum magnetic permeability μ max ≥5,000, resistivity ρ ≥0.25μΩm, ​​hysteresis loss P at 1.5T amplitude Hys ≤0.07J / kg, coercive field strength H c ≤0.7A / cm, induction B≥1.90T at 100A / cm, or

[0104] Maximum magnetic permeability μ max ≥10,000, resistivity ρ ≥0.25μΩm, ​​hysteresis loss P at 1.5T amplitude Hys ≤0.06J / kg, coercive field strength H c ≤0.6A / cm, induction B≥1.95T at 100A / cm, or

[0105] Maximum magnetic permeability μ max ≥12,000, resistivity ρ ≥0.28μΩm, hysteresis loss P at 1.5T amplitude Hys ≤0.05J / kg, coercive field strength H c ≤0.5A / cm, induction B≥2.00T at 100A / cm.

[0106] Maximum magnetic permeability μ max ≥17,000, resistivity ρ ≥0.30μΩm, hysteresis loss P at 1.5T amplitude Hys ≤0.05J / kg, coercive field strength H c ≤0.4A / cm, preferably H c ≤0.3A / cm, induction B≥2.00T at 100A / cm.

[0107] In one embodiment, the coercive field strength H after heat treatment measured parallel to the rolling direction, measured diagonally (45°) to the rolling direction, or measured perpendicular to the rolling direction is c The maximum difference is a maximum of 6%, preferably a maximum of 3%. In other words, the coercive field strength H measured parallel to the rolling direction and measured diagonally (45°) to the rolling direction is c 6%, preferably 3%, and / or the coercive field strength H measured parallel to the rolling direction and measured perpendicular to the rolling directionc 6%, preferably 3%, and / or the coercive field strength H between these two directions measured diagonally (45°) to the rolling direction or perpendicular to the rolling direction c The maximum value is 6% maximum, preferably 3% maximum. For soft magnetic FeCo alloys, this very low anisotropy results in uniform properties along the circumference in rotor or stator applications, so there is no need to twist the rotor or stator sheet layers for each layer to ensure sufficient magnetic isotropy in the sheet stack.

[0108] The heat treatment may be performed in a hydrogen-containing atmosphere or in an inert gas atmosphere.

[0109] In one embodiment, the heat treatment is performed in a fixed furnace at T1 and in a fixed furnace or a continuous furnace at T2. In another embodiment, the heat treatment is performed in a continuous furnace at T1 and in a fixed furnace or a continuous furnace at T2.

[0110] The preform may have a cold rolled texture or a fiber texture before heat treatment.

[0111] The preform may be provided in the form of a strip. At least one sheet may be produced from the strip by stamping, laser cutting or water jet cutting. In one embodiment, the stamped, laser cut, etched or water jet cut sheet section made from the strip material is heat treated.

[0112] In one embodiment, after heat treatment, several sheets are bonded into a sheet stack by an insulating adhesive, or the surface is oxidized to adjust the insulating layer and then bonded or laser welded into a sheet stack, or coated with an inorganic-organic hybrid coating and then further processed into a sheet stack.

[0113] In some embodiments, the preform has the shape of a sheet stack, and the sheet stack is heat treated according to one embodiment described herein. Thus, the heat treatment may be performed on a stamped or welded sheet stack made from sheet sections.

[0114] The preform can be produced as follows. The melt can be provided by vacuum induction melting, electroslag remelting or vacuum arc remelting, wherein the melt mainly consists of the following:

[0115] 5 wt% ≤ Co ≤ 25 wt%

[0116] 0.3 wt% ≤ V ≤ 5.0 wt%

[0117] 0 wt% ≤ Cr ≤ 3.0 wt%

[0118] 0 wt%≤Si≤3.0 wt%

[0119] 0 wt%≤Mn≤3.0 wt%

[0120] 0 wt% ≤ Al ≤ 3.0 wt%

[0121] 0 wt% ≤ Ta ≤ 0.5 wt%

[0122] 0 wt% ≤ Ni ≤ 0.5 wt%

[0123] 0 wt% ≤ Mo ≤ 0.5 wt%

[0124] 0 wt% ≤ Cu ≤ 0.2 wt%

[0125] 0 wt% ≤ Nb ≤ 0.25 wt%

[0126] 0 wt% ≤ Ti ≤ 0.05 wt%

[0127] 0 wt% ≤ Ce ≤ 0.05 wt%

[0128] 0 wt% ≤ Ca ≤ 0.05 wt%

[0129] 0 wt% ≤ Mg ≤ 0.05 wt%

[0130] 0 wt% ≤ C ≤ 0.02 wt%

[0131] 0 wt% ≤ Zr ≤ 0.1 wt%

[0132] 0 wt% ≤ O ≤ 0.025 wt%

[0133] 0 wt% ≤ S ≤ 0.025 wt%

[0134] The balance is iron, wherein Cr + Si + Al + Mn ≤ 3.0 wt% and up to 0.2 wt% of other impurities. The other impurities may be one or more of B, P, N, W, Hf, Y, Re, Sc, Be, and lanthanide elements other than Ce. The melt is solidified into an ingot, and the ingot is transformed into a preform of the final size and formed by hot rolling and / or forging and / or cold forming.

[0135] In one embodiment, the ingot is hot rolled at a temperature between 900 °C and 1300 °C to form a slab with a thickness D1, and then cold rolled to form a strip with a thickness D2, where 1.0 mm ≤ D1 ≤ 5.0 mm and 0.05 mm ≤ D2 ≤ 1.0 mm, and D2 < D1. The cold deformation degree by cold rolling can reach > 40%, preferably > 80%.

[0136] In one embodiment, the ingot is formed by hot rolling into a blank at a temperature between 900 °C and 1300 °C, and then transformed into a wire by cold drawing. The cold deformation degree by cold drawing can reach > 40%, preferably > 80%.

[0137] In order to reduce hardening and thus set the desired degree of cold deformation, intermediate annealing of intermediate dimensions can be carried out in continuous or stationary furnaces.

[0138] When selecting the temperature T1 and / or T2, the Curie temperature of the alloy may be considered. ü1 >T c , where T c is the Curie temperature, and T c ≥900℃. In one embodiment, T ü1 >T2>Tc.

[0139] In the two-phase region and Curie temperature T c In the separated composition, there is another temperature range with higher self-diffusion, so by heat treatment in this range or cooling through this range, a larger BCC grain structure can be obtained, thereby obtaining better soft magnetic properties. In addition, the two-phase region and the Curie temperature T c The separation of T2 makes the passage through the two-phase region BCC / FCC and the transformation to the pure BCC phase region occur in a completely paramagnetic state during cooling. ü1 >T2>Tc, the soft magnetic properties are further improved.

[0140] In one embodiment, the average grain size after final annealing is at least 100 μm, preferably at least 200 μm, preferably at least 250 μm.

[0141] In one embodiment, the measured density of the annealed alloy is more than 0.10% lower than the density calculated from the average atomic weight of the metallic elements of the alloy, the average atomic weight of the metallic elements of the corresponding binary FeCo alloy, and the measured density of the annealed binary FeCo alloy.

[0142] Due to the heat treatment, the sulfur content in the finished alloy may be less than that in the melt. For example, the sulfur content in the melt may be limited to 0.025 wt %, while the sulfur content in the finished soft magnetic alloy may be limited to 0.015 wt %.

[0143] In one embodiment, the preform product for electrical insulation is also coated with an oxide layer. This embodiment can be applied, for example, if the preform is used in a stack of sheets. The sheet section or the stack of sheets can be coated with an oxide layer. The preform can be coated with a layer of magnesium methoxide or preferably a layer of zirconium propoxide, which is converted into an insulating oxide layer during the heat treatment. The preform can be heat treated in an oxygen-containing or water vapor-containing atmosphere to form the electrically insulating layer.

[0144] In one embodiment, the sheet sections punched, laser cut or etched from the preform are further subjected to final annealing, and the annealed individual sheets are then bonded into a sheet stack with the aid of an insulating adhesive, or the annealed individual sheets are surface oxidized to adjust the insulating layer and then bonded, welded or laser welded into a sheet stack, or the annealed individual sheets are coated with an inorganic-organic hybrid coating, such as Remisol-C5, and then further processed into a sheet stack.

[0145] A soft magnetic alloy according to one of the aforementioned embodiments can be produced in the method described herein and can be used in stators and / or rotors of electrical machines, such as motors and / or generators, and / or in transformers and / or in electromagnetic actuators. BRIEF DESCRIPTION OF THE DRAWINGS

[0146] Embodiments of the present invention will now be explained in more detail with reference to the accompanying drawings and the following examples.

[0147] Figure 1 A schematic diagram (not to scale) showing three variants of the heat treatment according to the invention.

[0148] Figure 2 The typical course of DSC heating and cooling curves during phase change is shown using batch 930423 as an example.

[0149] Figure 3 Schematic diagram showing the first starting temperature of the phase transformation of the Fe-17Co-Cr-V alloy according to the invention with increasing V content compared to a binary Fe-17Co melt for heating (DSC) and cooling (DSC). Plotted against the second Y-axis is the maximum magnetic permeability μ max direction.

[0150] Figure 4 The coefficients of the induction value B according to multiple linear regression are shown.

[0151] Figure 5 The resistivity from multiple linear regression is shown.

[0152] Figure 6 The coercive field strength H of batch 930329 (Fe-17Co1.5V-0.5Cr) is shown. c As a function of the inverse of the reciprocating grain diameter d for different annealing.

[0153] Figure 7 The transformation temperature T of Fe-17Co special melt with different V contents is shown for different batches ü1 and T ü2 And the best coercive field strength H c These alloys also contain up to 0.6 wt. % Cr and / or Si. Table 29 shows Figure 7 data, including details of individual anneals.

[0154] Figure 8 The maximum permeability and coercive field strength after step annealing in the first annealing stage are shown.

[0155] Fig. 9 The maximum permeability and coercive field strength after step annealing with a first annealing stage of 4h 1000°C above the phase transition and a second annealing stage below the phase transition are shown.

[0156] Fig.10 The coercive field strength H of batches 930329 (Fe-17Co-0.5Cr-1.5V) and 930330 (Fe-17Co-2.0V) depending on the degree of cold deformation is shown. c .

[0157] Fig.11 The (200)-pole figure of batch 93 / 0330 (Fe-17Co-2V) is shown.

[0158] a) Cold deformation: top left.

[0159] b) After final annealing at 910°C for 10 hours: medium to high.

[0160] c) After final annealing at 1050°C for 4 hours: top right.

[0161] d) After final annealing at 1050°C for 4 h and at 910°C for 10 h: bottom.

[0162] Fig.12 The coercive field strength H of batch 930330 (Fe-17Co-2V) measured parallel to the rolling direction (longitudinal), at 45° to the rolling direction, and perpendicular to the rolling direction (transverse) for the specified annealing is shown. c .

[0163] Fig.13 The coercive field strength H of batch 930335 (Fe-23Co-2V) measured parallel to the rolling direction (longitudinal), at 45° to the rolling direction, and perpendicular to the rolling direction (transverse) for the specified annealing is shown. c .

[0164] Fig.14 New curves for batches 930329 (Fe-17Co-1.5V-0.5Cr), 930505 (Fe-17Co-1.4V-0.4Si) and 930330 (Fe-17Co-2V) according to the invention after optimal annealing are shown compared to a typical SiFe (TRAFOPERM N4) and a typical FeCo alloy.

[0165] Fig.15 The permeabilities of batches 930329 (Fe-17Co-1.5V-0.5Cr), 930505 (Fe-17Co-1.4V-0.4Si) and 930330 (Fe-17Co-2V) according to the invention after optimal annealing are shown in comparison with a typical SiFe (TRAFOPERM N4) and a typical FeCo alloy.

[0166] Fig.16 The figures show the losses of the batches 930329 (Fe-17Co-1.5V-0.5Cr) and 930330 (Fe-17Co-2V) according to the invention after optimal annealing at an induction amplitude of 1.5 T compared to typical SiFe (TRAFOPERM N4) and FeCo alloys. The sheet thickness was 0.35 mm in each case.

[0167] Fig.17 Shown is a graph of maximum magnetic permeability as a function of relative density difference Δρ based on Fe-17Co alloys for the data from Table 25. DETAILED DESCRIPTION

[0168] According to the present invention, there is provided a soft magnetic alloy, which is mainly composed of:

[0169] 5 wt% ≤Co ≤25 wt%

[0170] 0.3 wt% ≤V ≤5.0 wt%

[0171] 0 wt% ≤Cr ≤3.0 wt%

[0172] 0 wt% ≤Si ≤3.0 wt%

[0173] 0 wt% ≤Mn≤3.0 wt%

[0174] 0 wt% ≤Al ≤3.0 wt%

[0175] 0 wt% ≤Ni≤0.5 wt%

[0176] 0 wt% ≤Mo ≤0.5 wt%

[0177] 0wt% ≤Ta≤0.5wt%

[0178] 0 wt% ≤Cu ≤0.2 wt%

[0179] 0 wt% ≤Nb ≤0.1 wt%

[0180] 0 wt% ≤Ti ≤0.05 wt%

[0181] 0 wt% ≤Ce≤0.05 wt%

[0182] 0 wt% ≤Ca ≤0.05 wt%

[0183] 0 wt% ≤Mg ≤0.05 wt%

[0184] 0 wt% ≤C ≤0.02 wt%

[0185] 0 wt% ≤ Zr ≤ 0.1 wt%

[0186] 0 wt% ≤0 ≤0.025 wt%

[0187] 0 wt% ≤S ≤0.015 wt%

[0188] The balance is iron,

[0189] and up to 0.2 wt % of other melting-induced impurities. For example, the impurities may be one or more of the elements B, P, N, W, Hf, Y, Re, Sc, Be, and lanthanides other than Ce.

[0190] In order to increase the resistance, in addition to the alloying element vanadium, one or more of Cr, Si, Al and Mn may be alloyed to a certain extent, wherein the following sum is satisfied:

[0191] 0.05 wt% ≤ Cr+Si+Al+Mn ≤ 3.0 wt%

[0192] The alloy according to the invention is preferably melted in a vacuum induction furnace. However, vacuum arc remelting and electroslag remelting are also feasible. The melt is first solidified into a block (or ingot, block) from which the oxide scale is removed, and then forged or hot rolled at a temperature between 900°C and 1300°C. Alternatively, the removal of the oxide scale can also be first carried out on the forged or hot-rolled rod. The required size can be achieved by hot forming of the strip, billet or rod. The hot-rolled material can be sandblasted, polished or peeled to remove the surface oxide. However, the favorable final size can also be achieved by cold forming of the strip, rod or wire. In the case of cold-rolled strip, a polishing process can be carried out to remove the oxide in the hot rolling process. If the hardening is too high after cold forming, one or more intermediate anneals can be carried out at a temperature between 400°C and 1300°C for recovery and recrystallization. The thickness or diameter of the intermediate annealing should be selected so that preferably a cold deformation of >40% is achieved until the final thickness, in particular a cold deformation of >80%.

[0193] The last processing step is at 700°C and the solidus temperature T mThe heat treatment is carried out at a temperature between 100°C and 200°C (usually up to 1200°C), which is also called magnetic final annealing. The final annealing is preferably carried out in a pure dry hydrogen atmosphere. Annealing can also be carried out in a protective gas or in a vacuum.

[0194] Figure 1 A schematic diagram of three variants of the heat treatment according to the invention with regard to phase transformations, in particular the FCC, FCC+BCC and BCC regions, is shown.

[0195] For Figure 1 In the scheme 1 shown by the solid line in FIG, the first annealing stage in the FCC zone is directly followed by a second annealing stage in the BCC zone. The second annealing stage is optional and can be used to further improve the soft magnetic properties, especially the magnetic permeability and hysteresis losses. Figure 1 In the case of scheme 2, which is represented by the dashed line in FIG, the first annealing stage in the FCC zone is first cooled to room temperature. The second annealing stage in the BCC zone occurs at a later point in time. Figure 1 In the embodiment 3, which is indicated by the dotted line in FIG. 1 , controlled cooling from the annealing stage in the FCC zone to room temperature is performed. This type of controlled cooling can also be performed in the cooling from the first stage to the second stage in embodiment 1 ( Figure 1 not shown).

[0196] Thus, according to the invention, annealing can be carried out in two stages or by controlled cooling from a temperature above the upper transformation temperature. Controlled cooling means that there is a defined cooling rate to optimally adjust the soft magnetic properties. In any case, one of the annealing stages takes place in the FCC zone. Annealing according to the invention can be carried out in a continuous furnace or in a fixed furnace.

[0197] In the annealing of the present invention, at 900°C (if T ü2 >900℃, higher than T ü2 ) and T m Between higher than T ü2 At a temperature above T, the alloy is annealed at least once in the austenitic FCC region to produce large grains, take advantage of the cleaning effect of hydrogen, and remove possible textures that are unfavorable to magnetic properties. ü2 The final annealing stage is carried out in a stationary annealing or in a continuous furnace. Alternatively, this stage of heat treatment can also be carried out on the strip in a continuous furnace. The alloy is then cooled in the BCC zone at a rate of 10-50,000°C per hour, preferably 20-1,000°C per hour, to room temperature or a temperature between 700°C and 1,000°C.

[0198] The second annealing stage can be carried out in the ferrite BCC zone by heating or by heating at 700°C to 1000°C (if T ü1 <1000℃, then lower than Tü1 ) to remove possible remnants of the FCC phase. Then, after the magnetic final annealing, the alloy is cooled from the annealing temperature at a rate of 10 to 50,000° C. per hour, preferably at a rate of 20 to 1,000° C. per hour.

[0199] The alloy according to the present invention has a phase transition from the BCC phase region to the BCC / FCC mixed region, and at a slightly higher temperature also has a phase transition from the BCC / FCC mixed region to the FCC phase region, wherein as the temperature increases, the phase transition between the BCC phase region and the BCC / FCC mixed region occurs at the first transformation temperature T ü1 As the temperature further increases, the phase transition between the BCC / FCC mixed region and the FCC phase region occurs at the second transition temperature T ü2 Where Figure 2 shown.

[0200] The temperature at which the phase transition from the BCC phase region to the BCC / FCC mixed region and from the BCC / FCC mixed region to the FCC phase region occurs can be determined by DSC measurement. Taking batch 930423 as an example, Figure 2 A typical DSC heating and cooling curve for a phase transition is shown in Figure 1. The Curie temperature and first onset temperature of the phase transition are also shown in Figure 2. Figure 2 middle.

[0201] The figure below shows the results of a DSC measurement carried out with a dynamic heat flow differential calorimeter from NETZSCH. Two identical corundum crucibles (Al2O3) are placed in a furnace, one of which contains the actual sample and the other a calibration sample used as a reference. Both crucibles undergo the same temperature program, which can include a combination of heating, cooling or isothermal sections. The heat flow difference is quantitatively obtained by measuring the temperature difference between the sample and the reference sample at a defined heat conduction path. The various maxima and minima (peaks) determined in the DSC measurement can be assigned to specific types of phase transitions based on their curve shape. Typical curves are plotted, but material characteristic curves also depend on the measurement conditions, in particular the sample mass as well as the heating and cooling rates. In order to ensure comparability of the measurements, the heating and cooling rates of the measuring instruments and the sample mass of the samples investigated here were chosen to be identical. The heating and cooling rates used in the experiments were 10 K / min and the sample mass was 50 mg.

[0202] The transition temperature T is determined by means of DSC measurements by heating a defined mass of sample at a defined heating rate. ü1 and T ü2. In this measurement, the transition temperature is represented by the first onset. This parameter defined in DIN 51005 ("Thermal Analysis") is also called the extrapolated peak onset temperature, which represents the beginning of the phase change and is defined as the intersection of the extrapolated initial baseline with the tangent line through the linear part of the rising or falling peak side edge. The advantage of this parameter is that it is independent of the sample mass and the heating rate or cooling rate. The difference between the first onset temperatures is defined as the width of the two-phase region:

[0203] T 第一起始 (BCC+FCC→FCC)–T 第一起始 (BCC+FCC→BCC)=T ü2 –T ü1

[0204] (from DSC heating) (from DSC cooling)

[0205] Composition and transition temperature T ü1 and T ü2 The effect of is determined by means of DSC.

[0206] Figure 3 The first starting temperature of the phase transformation for the Fe-17Co-Cr-V alloy (circles) with increased V content compared to the binary Fe-17Co alloy (squares) for heating (solid symbols) and cooling (open symbols) is shown. The composition of the alloys is given in Tables 1 to 4.

[0207] The peak-Curie temperatures Tc for heating (DSC) and cooling (DSC) are indicated by diamonds. For a particular melt with a lower V content, T c Corresponds to the phase transition temperature. The highest maximum permeability μ is plotted on the minor axis. max (Triangles) V contents between 1 and 3 wt. % achieve the highest maximum permeabilities.

[0208] Figure 3 It shows that with the increase of V content, the phase transition T ü2 and T ü1 occurs at high temperatures, and the width of the two-phase region BCC+FCC (i.e., T ü2 -T ü1 )Increase.

[0209] In order to adjust the soft magnetic properties, a final annealing is performed. In this experiment, this is always carried out under a H2 protective atmosphere. The H2 mass used is always hydrogen 3.0 (or industrial grade hydrogen), and the H2 content is >99.9%, where H2O≤40ppm-mol, O2≤10ppm-mol, and N2≤100ppm-v.

[0210] The magnetic properties of the alloy were studied using strips made from ingots weighing 5 kg. The alloy was melted under vacuum and then poured into a flat mold at about 1500°C. After grinding off the oxide scale from the individual ingots, these ingots were hot rolled into 3.5 mm thick strips at temperatures ranging from about 1000°C to 1300°C. The resulting hot-rolled strips were then pickled to remove the oxide scale and then cold rolled to a thickness of 0.35 mm. To characterize the magnetic properties, sample rings were punched out of the strips and resistor strips were cut. The resistance ρ was determined on the resistor strips. The maximum magnetic permeability μ was measured on sample rings produced in the annealed state at room temperature. max , coercive field strength H c , induction B, remanence B at field strengths of 20, 25, 50, 90, 100 and 160 A / cm r and hysteresis loss P Hyst The hysteresis losses are determined by measuring the losses at different frequencies with an induction amplitude of 1.5 T. The intercept of the curve P / f versus f determined by linear regression gives the hysteresis losses.

[0211] Discs were sawn from the ingots for elemental analysis. The results of the analyses are shown in Tables 1 to 4. Table 1 shows the wet chemical analysis of the metallic elements to determine their basic composition. The balance is iron, other elements <0.01% are not given, where the data are in weight %. Table 2 shows the analysis of non-metallic impurities in the batches of Table 1 by hot gas extraction, where the data are in weight %. Table 3 shows the wet chemical analysis of the metallic elements to fine-tune the basic composition and limit the composition range and impurities. The balance is iron, other elements <0.01% are not specified. The data are in weight %. In batches 930502 and 930503, iron raw materials with a higher degree of impurities were used. Table 4 shows the analysis of non-metallic impurities in the batches of Table 3 by hot gas extraction, where the data are in weight %.

[0212] Table 3 continues with the analysis of the metallic elements of the two large melts. The balance is iron, the P content of the 76 / 4988 large melt is 0.003 wt.%, the P content of the 76 / 5180 large melt is 0.002 wt.%, and other elements <0.01% are not given. Table 4 also shows the analysis of the non-metallic impurities of the two large melts of Table 3 by hot gas extraction, the data are in wt.%.

[0213] Figure 4 and Figure 5 A statistical evaluation of the influence of the main alloying elements cobalt, vanadium and chromium on the induction values ​​and resistance of the optimum annealing by means of multiple linear regression is shown.

[0214] Figure 4The coefficients of the induction values ​​B according to the multiple linear regression are shown. The number after the B value (such as B20) indicates the field strength (A / cm). The bar graph shows the change in induction value when adding 1 wt%. Only those elements whose regression values ​​are larger than the regression error are shown.

[0215] Figure 5 The resistivity after multiple linear regression is shown. The bar graph indicates the change in resistance upon alloying with 1 wt% of each element.

[0216] From these figures, it can be seen that vanadium reduces low induction more than chromium. For this reason, chromium increases resistance more than vanadium at the same saturation (B160). Co increases saturation (B160) but has little effect on low induction values ​​and resistance.

[0217] Table 7 shows the annealing schedule according to the invention for batch 93 / 0330 with a strip thickness of 0.35 mm compared to an annealing schedule not according to the invention, see Figure 1 Unless otherwise specified, the cooling rate was 150 °C / h. No demagnetization treatment was performed before the measurement.

[0218] Figure 6 The coercive field strength H of batch 930329 (Fe-17Co1.5V-0.5Cr) is shown for different annealing conditions. c As a function of the inverse of the grain diameter d. Table 5 shows the average grain size d and the coercive field strength H after the specified annealing. c And the maximum magnetic permeability μ max ,See Figure 4 The cooling rate was 150°C / h.

[0219] Table 6 shows the DSC transition temperature and Curie temperature T C The unit is °C. #NV means that no signal can be detected in the DSC measurement.

[0220] One of the reasons for the very good soft magnetic properties of Fe-Co alloys is the unusually large grain structure, which is achieved after annealing in the FCC zone. After a short annealing of batch 93 / 0330 (Fe-17Co-2V) at 1050°C for 4 hours, the grain size was determined to be 354-447μm. After continuous annealing for several days, similar grain sizes were only obtained by annealing in the BCC zone. Figure 6 The coercive field strength H is schematically shown with the aid of batch 930329. c The relationship with the inverse of the grain size shows a linear relationship.

[0221] In order to compare the above annealing schemes, batch 930330 was tested as an example. Table 8 shows the results after step annealing in the first annealing stage (batch 93 / 0330), see Figure 6 The cooling rate was 150°C / h. As long as the first annealing took place in the lower FCC zone (here at 1050°C), all annealing schemes showed very good soft magnetic properties, much better than annealing in the pure BCC zone. A second annealing stage in the higher BCC zone after the previous first annealing stage in the FCC zone further improved the above values.

[0222] Figure 7 The transformation temperature T of a specific Fe-17Co melt with different V contents is shown. ü1 and T ü2 , as the optimal coercive field strength H achieved c These labels reflect the content of V. Figure 7 It shows that the V content is decisive for the adjustment of soft magnetic properties. If the V content is too low, T ü1 If the V content is too high, the two-phase region (T ü2 -T ü1 ) becomes wider, the soft magnetic properties deteriorate, see also Figure 3 and Table 6. This results in a coercive field strength H at about 1.4 to 2 wt. % vanadium. c The minimum value of .

[0223] To find the optimum annealing temperature, the samples are annealed at different annealing temperatures and then measured. If the number of necessary annealings is greater than the number of samples available, the same sample group is usually annealed at different temperatures. In this so-called "step annealing", one starts with a lower starting temperature and anneals stepwise at higher temperatures. Step annealing can be used, for example, to track elimination regions, recrystallization temperatures or phase transitions that have a direct influence on magnetic properties.

[0224] Figure 8 The maximum permeability and coercive field strength after the first annealing stage step annealing are shown. Table 9 shows the results of the step annealing of batch 93 / 0330 below the phase transition after the previous first annealing stage of 4h 1000℃ above the phase transition. The cooling rate is 150℃ / h. An extended maximum around 1000℃ can be seen. The corresponding DSC measurements are also shown for comparison with the phase position.

[0225] Fig. 9The maximum permeability and coercive field strength (circles) after a step annealing with a second annealing stage below the phase transition are shown, after a previous first annealing stage of 4h 1000°C above the phase transition (diamonds). Do not demagnetize before measuring the static values. The maximum value is visible at 950°C. After the last annealing of the step annealing at 1000°C, the sample is annealed at 950°C for 10h (triangles). The original values ​​of the step annealing at 950°C are no longer present. Passing through the two-phase region BCC+FCC again will damage the soft magnetic properties.

[0226] The magnetic properties of alloys with different compositions after different annealing were measured. The results are summarized in Tables 10 to 24. The values ​​B are given. 20 , B 25 , B 50 , B 90 , B 100 , B 160 (T)H c (A / cm), μ max , B r (T) and P Hyst 1.5T(Ws / kg).

[0227] Table 10 shows the results of selected batches after annealing at 850° C. for 4 h at a cooling rate of 150° C. / h. These examples are not according to the invention.

[0228] Table 11 shows the results of selected batches after annealing at 910° C. for 10 h at a cooling rate of 150° C. / h. No demagnetization was performed before measuring the static values. These examples are not according to the invention.

[0229] Table 12 shows the results of selected batches after annealing at 910° C. for 10 h and cooling to room temperature followed by annealing at 930° C. for 70 h. The cooling rate was 150° C. / h. No demagnetization was performed before measuring the static values.

[0230] These embodiments are not according to the invention.

[0231] Table 13 shows the results of selected batches after annealing at 1000°C for 4 h. The cooling rate was 150°C / h. No demagnetization was performed before measuring the static values.

[0232] Table 14 shows the results of selected batches annealed at 1000° C. for 4 h in a first annealing stage and cooled to room temperature and then annealed at 910° C. for 10 h in a second annealing stage. The cooling rate was 150° C. / h. No demagnetization was performed before measuring the static values.

[0233] Table 15 shows the results for all Fe-Co-V-Cr batches after annealing at 1050°C for 4 h. The cooling rate was 150°C / h. No demagnetization was performed before measuring the static values. The resistance of batches 930322 to 930339 was measured after annealing at 850°C for 4 h. For V-rich batches 930422 and 930423, T ü2 Slightly below 1050 °C. The adjusted annealing stages can be found in Table 18.

[0234] Table 16 shows the results for all Fe-Co-V-Cr batches after annealing at 1050°C for 4 h in the first annealing stage and cooling to room temperature and then annealing at 910°C for 10 h in the second annealing stage. The cooling rate was 150°C / h. Demagnetization before measurement. For the batches marked in grey, T ü1 Not enough above 910° C., or too much above 910° C. The adjusted annealing stage can be found in Table 17.

[0235] Table 17 shows the results after adjusting the annealing of these batches, where the transition temperature measured by DSC (Table 6) does not correspond, or only slightly, to the annealing of 4h 1050°C + 10h 910°C (Tables 15 and 16) according to the invention. The cooling rate was 150°C / h. For the annealing of 4h 1050°C, no demagnetization was performed before the measurement, while for all other anneals, demagnetization was performed before the measurement.

[0236] Table 18 shows the results of batch 930423 after annealing in different phase regions to illustrate the influence of ferromagnetic BCC region and paramagnetic BCC on magnetic properties, see also Figure 2 The cooling rate was 150°C / h. For the 4h 1050°C annealing, no demagnetization was performed before the measurement, while for all other anneals, demagnetization was performed before the measurement.

[0237] Table 19 shows the results for selected batches after annealing at 1050°C for 4 h followed by slow cooling to room temperature at 50°C / h. No demagnetization was performed before measuring the static values.

[0238] Table 20 shows the results of selected batches after a second annealing stage of annealing at 1050°C for 4 h and slow cooling to room temperature at 50°C / h and furnace cooling at about 150°C / h. No demagnetization was performed before measuring the static values.

[0239] Table 21 shows the results of selected batches after annealing at 1100°C for 4 h. The cooling rate was 150°C / h. Except for batches 930422 and 930423, no demagnetization was performed before measuring the static values.

[0240] Table 22 shows the results of selected batches after annealing at 1100° C. for 4 h and cooling to room temperature in a first annealing stage and a second annealing stage at 910° C. for 10 h. The cooling rate was 150° C. / h. No demagnetization was performed before measuring the static values.

[0241] Table 23 shows the results for selected batches after annealing at 1150°C for 4 h with a cooling rate of 150°C / h. Except for batch 930442, no demagnetization was performed before measuring the static values.

[0242] Table 24 shows the results of selected batches after annealing at 1150° C. for 4 h and cooling to room temperature in a first annealing stage and a second annealing stage at 910° C. for 10 h. The cooling rate was 150° C. / h. No demagnetization was performed before measuring the static values.

[0243] Table 25 shows the maximum permeability and density data for various Fe-17Co alloy compositions with various additives. From the binary alloy Fe-16.98Co (whose measured density is 7.942 g / cm 3 , whose average atomic weight is 56.371 g / mol (calculated based on the analyzed content of metal alloying elements)). For Fe-17Co alloys with added V, Cr, Mn, Si, Al and other metal elements, their virtual density is calculated with the help of their average atomic weight and compared with the measured density. For example, for Fe-17.19Co-1.97V alloy (batch 93 / 0330), the average atomic weight is 56.281 g / mol. Now we can calculate the virtual density based on the ratio method (7.942 g / cm 3 ×56.281 / 56.371=7.929g / cm 3 ) to calculate the virtual density that the Fe-17.19Co-1.97V alloy should have if its lattice constant remains the same as that of the binary Fe-16.98Co alloy. However, in reality, the density measured on this alloy is 7.909 g / cm 3 , virtual density 7.929g / cm 3 This means that the lattice constant of the alloy must be about 0.085% greater than that of the binary alloy.

[0244] Table 26 shows data for selected batches and anneals that simultaneously exhibit exceptionally high maximum permeability and low hysteresis losses, and exhibit an induction B (B 100 ) level is very high.

[0245] Table 27 shows data in ppm for impurities C and S for selected batches and anneals. These impurities were effectively reduced by annealing at 1050°C under hydrogen.

[0246] Table 28 shows the magnetic values ​​of two large melts 76 / 4988 and 76 / 5180. The notation A or B means from ingot A or ingot B - the melt was poured into two molds respectively. The resistivity of batch 76 / 4988 is 0.306 μΩm and the resistivity of batch 76 / 5180 is 0.318 μΩm.

[0247] Table 29 shows the transformation temperatures T obtained for different batches of Fe-17Co special melts with different V contents. ü1 and T ü2 And the optimal coercive field strength H c , including details of the corresponding annealing treatments. These alloys also contain up to a total of 0.6 wt. % Cr and / or Si. A graphic representation of these data is given in Figure 7 .

[0248] Figure 8 and Fig. 9 It is shown that the BCC / FCC phase transformation present in the alloy 930330 according to the present invention has a great influence on the maximum magnetic permeability and the coercive field strength.

[0249] In the first annealing stage ( Figure 8 ), the first cooling starts (=T ü1 , the lower boundary of the two-phase region) and μ max The increase is consistent with that at the beginning of the first heating (=T ü2 , the upper boundary of the two-phase region), μ max At higher temperatures in the FCC zone, the magnetic properties deteriorate again.

[0250] In the second annealing stage ( Fig. 9 ), μ max In T ü1 The following becomes the maximum value and decreases as it enters the two-phase region. If it crosses the two-phase region and at T ü1 (here 950℃) and annealed again, μ max This may be due to the fact that the sample has passed through the BCC+FCC mixed zone twice and the resulting grain boundaries.

[0251] In summary, it can be determined that if the first annealing stage occurs above T ü2 , while the second annealing stage occurs less than T ü1 , the best magnetic properties can be obtained.

[0252] The effect of cold deformation degree on magnetic properties was studied.

[0253] Fig.10The coercive field strength H of batches 930329 (Fe-17Co-0.5Cr-1.5V) and 930330 (Fe-17Co-2.0V) depending on the degree of cold deformation is shown. c In the case of “without intermediate annealing”, the hot-rolled thickness corresponds to 0% KV, and in the case of “with intermediate annealing”, the intermediate annealed thickness corresponds to 0% KV.

[0254] The degree of cold deformation KV of the strip with a final thickness D2 is defined as the percentage reduction in thickness relative to the non-cold-deformed initial thickness D1 due to negligible width during rolling. The non-cold-deformed initial thickness D1 can be achieved, for example, by hot rolling or by intermediate annealing (ZGL).

[0255] KV[%]=[(D1-D2) / D1]x100

[0256] exist Fig.10 For example, from the coercive field strength H c It can be seen that when KV is increased (achieved by intermediate annealing at different D1 = 1.3 mm; 1.0 mm; 0.60 mm and the same final thickness D2 = 0.35 mm), the magnetic properties improve by a maximum of about 90% KV.

[0257] If we start from a constant D1 (hot rolled thickness) of 3.5 mm and cold forming is carried out with high rolling rates of 0.20 mm and 0.10 mm, then H c will increase again, as shown by the dotted line. This can be explained by the following: at the highest degree of cold deformation, there are too many nucleation points for the grains and the grains interfere with each other's growth during annealing. After final annealing at T1 = 1000°C for 4h and at T2 = 910°C for 10h, without intermediate annealing, the alloy of batch 930329 (Fe-17Co-0.5Cr-1.5V) (all in weight %) was prepared with an average grain size of 0.25mm at a final thickness of 0.35mm, an average grain size of 0.21mm at a final thickness of 0.20mm, and an average grain size of 0.15mm at a final thickness of 0.10mm. Therefore, there is an optimal degree of cold deformation, which is about 90%.

[0258] In order to investigate whether the formation of texture plays a decisive role in the magnetic properties, the texture was determined by X-ray diffraction on 50 mm × 45 mm sheets.

[0259] Fig.11The (200) pole figures of batch 93 / 0330 (Fe-17Co-2V) are shown. The results on the left are those of an unannealed plate with rolling texture. The results for the plate in the middle are annealed at 910°C for 10 h and have only very weak texture. The results for the plate on the right are annealed at 1050°C for 4 h and have no texture. The results for the plate on the bottom are annealed at 1050°C for 4 h and annealed at 910°C for 10 h and have no texture.

[0260] Here, Cu-K α = 0.154059295 nm was irradiated onto the sample, and the diffraction intensity was measured with a 2 mm perforated plate. A Lynxexe semiconductor strip detector with an angle range of 2° and energy dispersion operation was used as a detector. As shown in the (200) pole figure, rolling texture appeared in the hard-rolled state without annealing, and the rolling texture was completely dissolved after annealing at 1050°C in H2 for 4 h in the FCC zone.

[0261] Lack of texture and direction-dependent H c To this end, five H measurements were taken in each direction relative to the rolling direction (longitudinal = 0°, diagonal = 45°, transverse = 90°). c The size of each belt is 50mm×10mm, and Measurements are taken in

[0262] Fig.12 The coercive field strength H of batch 930330 (Fe-17Co-2V) measured parallel to the rolling direction (longitudinal), at 45° to the rolling direction, and perpendicular to the rolling direction (transverse) for the specified annealing is shown. c Each point is the mean of 5 measurements. Error bars represent standard deviation.

[0263] Fig.13 The coercive field strength H of batch 930335 (Fe-23Co-2V) measured parallel to the rolling direction (longitudinal), at 45° to the rolling direction, and perpendicular to the rolling direction (transverse) for the specified annealing is shown. c Each point is the mean of 5 measurements. Error bars represent standard deviation.

[0264] After annealing at 910℃ for 4h, the average values ​​show anisotropy, but considering the statistical error, the anisotropy is not obvious. However, this slight anisotropy coincides with the remnant of the texture from the corresponding pole figure ( Fig.11 After annealing at 1050℃ for 4h and 1010℃ for 4h, H cThe average values ​​of are almost the same. Annealing in the FCC zone at 1050°C completely eliminates the existing texture, and the subsequent second annealing stage in the BCC zone at 910°C does not generate any new texture.

[0265] In the following, the magnetic properties of the alloys according to the invention are compared by way of example with reference to the batches 930329 (Fe-17Co-1.5V-0.5Cr) and 930330 (Fe-17Co-2.0V) according to the invention with reference to comparative alloys. As comparative alloys there are the typical Elektroblech TRAFOPERM N4 (Fe-2.5Si-Al-Mn) and the three FeCo alloys VACOFLUX 17 (Fe-17Co-2Cr-Mo-V-Si), VACOFLUX 48 (Fe-49Co-1.9V) and HYPOCORE special melt. The HYPOCORE special melt was melted according to the composition published by Carpenter Technologies (Fe-5Co-2.3Si-1Mn-0.3Cr, data given in wt. %).

[0266] Fig.14 New curves are shown for batches 930329 (Fe-17Co-1.5V-0.5Cr), 930505 (Fe-17Co-1.4V-0.4Si) and 930330 (Fe-17Co-2V) according to the invention after optimal annealing compared to SiFe (TRAFOPERM N4) and FeCo comparative alloys.

[0267] Fig.15 The permeabilities of batches 930329 (Fe-17Co-1.5V-0.5Cr), 930505 (Fe-17Co-1.4V-0.4Si) and 930330 (Fe-17Co-2V) according to the invention after optimal annealing are shown compared to pSiFe (TRAFOPERM N4) and a FeCo comparative alloy.

[0268] Fig.16 The losses of batches 930329 (Fe-17Co-1.5V-0.5Cr) and 930330 (Fe-17Co-2V) according to the invention after optimal annealing at an amplitude of 1.5 T are shown compared to SiFe (TRAFOPERM N4) and FeCo comparative alloys. The hysteresis losses (y-intercept) of 930329, 930330 and TRAFOPERM N4 are similar. The sheet thickness is 0.35 mm in each case.

[0269] Fig.17The maximum magnetic permeability of Fe-17Co based alloys is shown as a function of the relative density difference Δρ (data in Table 25). It can be seen that alloys with a relative density difference of -0.10% to -0.35% achieve higher maximum magnetic permeabilities, and alloys with a relative density difference of -0.20% to -0.35% achieve particularly high maximum magnetic permeabilities. The relative density difference of binary Fe-17Co alloys ultimately means that the lattice constant of these alloys must be somewhat larger than that of binary alloys. A larger lattice constant means better diffusivity due to the larger atomic distances in the lattice and lower activation energy for the transposition process. This also contributes to grain growth, and therefore helps to reduce the coercive field strength or increase the magnetic permeability.

[0270] In order to investigate the properties of the alloy according to the invention on a production scale, two large melts were carried out in normal production. For this purpose, 2.2 t of the desired composition were melted in a vacuum induction furnace and, after setting and analyzing the exact composition, poured into two round molds with a diameter of 340 mm. After solidification and cooling, the round blocks were removed from the molds and hot-rolled in a gas-fired rotary furnace at a temperature of 1170 ° C. The fully heated blocks were then hot-rolled on the blooming rolls to a cross-section of 231 x 96 mm. 2 Then all the surfaces of these slabs are ground into 226x93mm 2 size to remove the oxide scale.

[0271] The two slabs thus obtained from batch 76 / 4988 were rolled into hot-rolled strips on a hot rolling mill. To this end, the slabs were first heated at a temperature of 1130°C and then rolled into hot-rolled strips after sufficient heating. The final thickness of the strip was 2.6 mm. The final rolling temperature of the strip was 900°C and the coil temperature was 828°C. The final thickness of the other strip was selected to be 1.9 mm. The final rolling temperature of the strip was 871°C and the coil temperature was 718°C. The two hot-rolled strips were then sandblasted to remove the oxide scale. Part of the hot-rolled strip was intermediately annealed at 750°C for 1 hour under a H2 protective gas atmosphere. Another part of the hot-rolled strip was intermediately annealed at 1050°C for 1 hour under a H2 protective gas atmosphere. The rest of the hot-rolled strip remained intact without intermediate annealing. It was then rolled to the final thickness, wherein the strips were all deoxidized from both sides at the intermediate thickness. Before the hot rolling of the strip, sections with a thickness of 15 mm were additionally sawn from the slab and stripped by hot rolling (thickness 3.5 mm), pickling the obtained hot rolled strip and then cold rolling in the technical center, thereby producing the strip. The obtained results are listed for comparison.

[0272] 15 mm thick discs were sawn from the two slabs at both ends of batch 76 / 5180. These discs were heated at 1200°C and then hot rolled into 3.5 mm thick strips. The hot rolled strips thus obtained were pickled to remove oxides. They were then cold rolled to a thickness of 0.35 mm.

[0273] All the strips thus obtained were made into punched rings and subjected to a final annealing treatment. Table 28 shows the results of the magnetic values. The resistivity of batch 76 / 4988 was 0.306 μΩm and that of batch 76 / 5180 was 0.318 μΩm.

[0274] As can be seen from Table 28, the magnetic properties of large melt samples measured for commercial alloys with a Co content of less than 30 wt. % are better than those of VACOFLUX 17. The maximum magnetic permeability measured for large melt samples of 76 / 5180B is greater than 20,000. Therefore, the alloy according to the invention is suitable for large-scale industrial production of ribbon material with improved magnetic properties.

[0275] The alloy according to the invention shows a higher induction than VACOFLUX 17 for every field strength. At the induction above the breakpoint, the new alloy lies between TRAFOPERM N4 and VACOFLUX 48. The air flow corrected induction B at a field strength of 400 A / cm close to magnetic saturation is 2.264 T for both batches (this corresponds to a polarization J of 2.214 T). Therefore, in the operating area of ​​typical motors and generators, the new alloy will have a higher torque than VACOFLUX 17 and TRAFOPERM N4.

[0276] As can be seen from the comparison of 930329 and 930330, vanadium, in combination with the above heat treatment, increases the rectangularity of the hysteresis loop to a point where, depending on the alloy, the maximum permeability is almost as great as that of VACOFLUX 48. This is surprising and extremely unexpected, since at about 50% Co the anisotropy constant K1 passes through zero, while at 17% Co it does not exist. In contrast, at 17% Co the anisotropy constant K1 in the Fe-Co system is very high.

[0277] Very good soft magnetic properties are also shown at hysteresis losses at a level comparable to that of TRAFOPERM N4. However, with increasing frequency, the losses of TRAFOPERM N4 increase much less than those of the new alloy at the same strip thickness due to the higher electrical resistance of the new alloy. However, this effect can be compensated by choosing a slightly lower strip thickness and correspondingly lower eddy current losses.

[0278] In summary, a high permeability soft magnetic alloy with improved soft magnetic properties is provided, for example, having significantly higher permeability and lower hysteresis losses than existing and commercially available FeCo alloys, while providing a higher saturation. At the same time, this new alloy provides significantly lower hysteresis losses than previously known and commercially available alloys with a Co content between 10 and 30 wt. %, and in particular significantly higher permeability levels that have never been achieved by such alloys. The alloy of the invention can also be produced on an industrial scale and inexpensively.

[0279]

[0280] Table 1

[0281] Batch 93 / C S O N 0322 0.0050 0.0012 0.0016 0.0012 0323 0.0045 0.0010 0.0150 0.0011 0324 0.0038 0.0010 0.0130 0.0009 0325 0.0031 0.0011 0.0100 0.0011 0326 0.0032 0.0011 0.0085 0.0012 0327 0.0032 0.0011 0.0097 0.0011 0328 0.0029 0.0011 0.0100 0.0013 0329 0.0028 0.0012 0.0093 0.0013 0330 0.0024 0.0011 0.0092 0.0014 0331 0.0030 0.0011 0.0087 0.0011 0332 0.0022 0.0011 0.0068 0.0012 0333 0.0040 0.0011 0.0014 0.0011 0334 0.0036 0.0010 0.0022 0.0013 0335 0.0034 0.0010 0.0120 0.0016 0336 0.0040 0.0010 0.0088 0.0014 0337 0.0039 0.0010 0.0058 0.0012 0338 0.0036 0.0011 0.0082 0.0012 0339 0.0025 0.0009 0.0026 0.0010

[0282] Table 2

[0283]

[0284] Table 3

[0285]

[0286] Table 4

[0287]

[0288] Table 5

[0289]

[0290] Table 6

[0291]

[0292]

[0293] Table 7

[0294]

[0295] Table 8

[0296]

[0297]

[0298] Table 9

[0299]

[0300] Table 10

[0301]

[0302] Table 11

[0303]

[0304] Table 12

[0305]

[0306] Table 13

[0307]

[0308] Table 14

[0309]

[0310] Table 15

[0311]

[0312] Table 16

[0313]

[0314] Table 17

[0315]

[0316] Table 18

[0317]

[0318] Table 19

[0319]

[0320] Table 20

[0321]

[0322] Table 21

[0323]

[0324] Table 22

[0325]

[0326] Table 23

[0327]

[0328] Table 24

[0329]

[0330] Table 25

[0331]

[0332] Table 26

[0333]

[0334] Table 27

[0335]

[0336]

[0337] Table 28

[0338]

[0339] Table 29.

Claims

1. A method for manufacturing a soft magnetic alloy, the method comprising: A preform is provided, the composition of which consists of the following The balance is iron, of which 0.1 wt. % ≤ Cr + Si + Al + Mn ≤ 1.5 wt. % and other impurities up to 0.2 wt. %, The preform is subjected to final annealing, wherein the final annealing comprises: The preform is heat treated at a temperature T1 and then cooled from T1 to room temperature, The preform has a phase transition from the BCC phase region to the BCC / FCC mixed region to the FCC phase region, wherein as the temperature increases, the phase transition between the BCC phase region and the BCC / FCC mixed region occurs at a first transition temperature. As the temperature further increases, the phase transition between the BCC / FCC mixed region and the FCC phase region occurs at the second transition temperature. in T1 is higher than and Wherein, after the heat treatment, the hysteresis loss P of the soft magnetic alloy at an amplitude of 1.5T is Hys ≤0.07J / kg.

2. The method according to claim 1, wherein: When the sample mass is 50 mg and the DSC heating rate is 10 K / min, the transition temperature Above 900℃.

3. The method according to claim 2, wherein: The transition temperature Above 920℃.

4. The method according to claim 2, wherein: The transition temperature Above 940℃.

5. The method according to claim 1, wherein: 900℃≤T1 <T m , where T m is the solidus temperature.

6. The method according to claim 1, wherein: 930℃≤T1 <T m , where T m is the solidus temperature.

7. The method according to claim 1, wherein: 940℃≤T1 <T m , where T m is the solidus temperature.

8. The method according to claim 1, wherein: 960℃≤T1 <T m , where T m is the solidus temperature.

9. The method according to claim 1, wherein: Difference Less than 45K.

10. The method according to claim 1, wherein: Difference Less than 25K.

11. The method according to claim 5, wherein: The cooling rate from T1 to room temperature is at least from T1 to less than The temperature range of T2 is from 10℃ / h to 50,000℃ / h.

12. The method according to claim 5, wherein: The cooling rate from T1 to room temperature is at least from T1 to less than The temperature range of T2 is 10℃ / h to 900℃ / h.

13. The method according to claim 5, wherein: The cooling rate from T1 to room temperature is at least from T1 to less than The temperature range of T2 is from 25℃ / h to 500℃ / h.

14. The method according to claim 1, wherein the preform is cooled from T1 to room temperature at a rate of 10°C / h to 50,000°C / h. 15 . The method according to claim 1 , wherein the preform is cooled from T1 to room temperature at a rate of 10° C. / h to 900° C. / h. 16 . The method according to claim 1 , wherein the preform is cooled from T1 to room temperature at a rate of 25° C. / h to 500° C. / h.

17. The method according to claim 11, wherein: The preform is above The heat treatment is carried out over a period of 30 minutes and then cooled to T2.

18. The method according to claim 1, wherein the preform is heat treated at T1 for a time t1, wherein 15 minutes ≤ t1 ≤ 20 hours, and then cooled from T1 to T2, wherein, Temperature T2 is lower than 19. The method according to claim 1, wherein: After the heat treatment, the maximum magnetic permeability μ of the soft magnetic alloy is max ≥5000, and / or resistivity ρ≥0.25μΩm, ​​and / or coercive field strength H c ≤0.7A / cm and / or induced B≥1.90T at 100A / cm.

20. The method according to claim 19, wherein: After the heat treatment, the maximum magnetic permeability μ of the soft magnetic alloy is max ≥10,000, and / or resistivity ρ ≥0.25μΩm, ​​and / or hysteresis loss P at an amplitude of 1.5T Hys ≤0.06J / kg, and / or coercive field strength H c ≤0.6A / cm and induced B≥1.95T at 100A / cm.

21. The method according to claim 20, wherein: After the heat treatment, the maximum magnetic permeability μ of the soft magnetic alloy is max ≥12,000, and / or resistivity ρ ≥0.30μΩm, and / or hysteresis loss P with amplitude of 1.5T Hys ≤0.05J / kg, and / or coercive field strength H c ≤0.5A / cm, and / or induction B≥2.00T at 100A / cm.

22. The method according to claim 21, wherein: The maximum magnetic permeability μ of the soft magnetic alloy max ≥17,000.

23. The method according to claim 21, wherein: Coercive field strength H c ≤0.4A / cm.

24. The method according to claim 21, wherein: Coercive field strength H c ≤0.3A / cm.

25. The method of claim 1, wherein: The coercive field strength H measured parallel to the rolling direction, diagonally to the rolling direction (45°), or perpendicular to the rolling direction between these two directions c The maximum difference is a maximum of 6%.

26. The method of claim 1, wherein: The coercive field strength H measured parallel to the rolling direction, diagonally to the rolling direction (45°), or perpendicular to the rolling direction between these two directions c The maximum difference is a maximum of 3%.

27. The method of claim 1, wherein: The heat treatment is performed in a hydrogen-containing atmosphere or under an inert gas.

28. The method of claim 1, wherein: The heat treatment is carried out in a fixed furnace or a continuous furnace at T1.

29. The method of claim 1, wherein: Before heat treatment, the preform has a cold rolled texture or a fiber texture.

30. The method of claim 1, wherein: The preform has the shape of one or more sheets or a stack of one or more sheets.

31. The method of claim 1, wherein: The preform first has the form of a strip from which at least one sheet is produced by punching, laser cutting or water jet cutting, wherein the heat treatment is carried out on one or more sheets.

32. The method according to claim 31, wherein: After the heat treatment, several sheets are bonded to form a sheet stack by means of an insulating adhesive, or Surface oxidation to form an insulating layer and subsequent bonding or laser welding to form a sheet stack, or Coating with an inorganic-organic hybrid coating and subsequent further processing to form a sheet stack.

33. The method of claim 1, wherein: The preform firstly has the shape of a sheet stack and the heat treatment is carried out on one or more sheet stacks.

34. The method of claim 1, further comprising: The melt is provided by vacuum induction melting, electroslag remelting or vacuum arc remelting, the melt consisting of: The balance is iron, of which 0.1 wt% ≤ Cr + Si + Al + Mn ≤ 1.5 wt% and a maximum of 0.2 wt% of other impurities, Solidify the melt into an ingot, The ingot is shaped, wherein the shaping is carried out by means of hot rolling and / or forging and / or cold forming.

35. The method of claim 34, wherein: The ingot is hot rolled into a slab at a temperature between 900°C and 1300°C, then formed into a hot strip with a thickness of D1, and then formed into a strip with a thickness of D2 by cold rolling, wherein 0.05 mm ≤ D2 ≤ 1.0 mm, and D2 <D1。 36. The method of claim 34, wherein: First, a hot strip with a thickness of D1 is produced by continuous casting, and then formed into a strip with a thickness of D2 by cold rolling, where 0.05 mm ≤ D2 ≤ 1.0 mm, and D2 <D1。 37. The method of claim 35, wherein: The cold deformation degree by cold rolling is >40%.

38. The method of claim 35, wherein: The cold deformation degree by cold rolling is >80%.

39. The method of claim 34, wherein: The ingot is formed into a blank by hot rolling at a temperature between 900° C. and 1300° C. and then formed into a wire by cold drawing.

40. The method of claim 39, wherein: The cold deformation degree by cold drawing is >40%.

41. The method of claim 39, wherein: The cold deformation degree by cold drawing is >80%.

42. The method of claim 37, further comprising an intermediate annealing.

43. The method of claim 1, wherein: Where T c is the Curie temperature, and T c ≥900℃.

44. The method of claim 1, wherein: After said heat treatment, the average grain size is at least 100 μm.

45. The method of claim 1, wherein: After said heat treatment, the average grain size is at least 200 μm.

46. ​​The method of claim 1, wherein: After said heat treatment, the average grain size is at least 250 μm.

47. The method of claim 34, wherein: The sulfur content is reduced during the heat treatment in a H2-containing protective gas atmosphere.

48. The method of claim 1 further comprising coating the preform with an oxide layer for electrical insulation.

49. The method of claim 48, wherein: The preform is coated with a layer made of magnesium methoxide or zirconium propoxide, which is transformed into an insulating oxide layer during a heat treatment.

50. The method of claim 48, wherein: The preform is heat-treated in an atmosphere containing oxygen or water vapor to form an electrical insulating layer.

51. The method of claim 11, wherein: 700℃≤T2≤1050℃。 52. A soft magnetic alloy, the soft magnetic alloy consisting of: The balance is iron, of which 0.1 wt% ≤ Cr + Si + Al + Mn ≤ 1.5 wt% and a maximum of 0.2 wt% of other impurities, and it has a maximum magnetic permeability μ max ≥5,000, The hysteresis loss P of the soft magnetic alloy at an amplitude of 1.5 T is Hys ≤0.07J / kg.

53. The soft magnetic alloy according to claim 52, wherein the maximum magnetic permeability μmax ≥ 10,000.

54. The soft magnetic alloy according to claim 52, wherein the maximum magnetic permeability μmax ≥ 12,000.

55. The soft magnetic alloy according to claim 52, having a maximum magnetic permeability μmax ≥ 17,000.

56. The soft magnetic alloy according to claim 52, having a resistivity ρ ≥ 0.25 μΩm, and / or a hysteresis loss P at an amplitude of 1.5 T. Hys ≤0.06J / kg, coercive field strength H c ≤0.7A / cm, and / or induction B≥1.90T at 100A / cm.

57. The soft magnetic alloy according to claim 56, having a resistivity of ρ ≥ 0.30 μΩm.

58. The soft magnetic alloy according to claim 56, wherein the hysteresis loss P at an amplitude of 1.5 T is Hys ≤0.05J / kg.

59. The soft magnetic alloy according to claim 56, wherein the coercive field strength H c ≤0.5A / cm.

60. The soft magnetic alloy according to claim 56, wherein the coercive field strength H c ≤0.4A / cm.

61. The soft magnetic alloy according to claim 56, the coercive field strength H c ≤0.3A / cm.

62. The soft magnetic alloy according to claim 56, wherein the induction B at 100 A / cm is ≥ 1.95 T.

63. The soft magnetic alloy according to claim 56, wherein the induction B at 100 A / cm is ≥ 2.00 T.

64. The soft magnetic alloy according to claim 52, wherein: 10 wt%≤Co≤20 wt%.

65. The soft magnetic alloy according to claim 52, wherein: 15 wt%≤Co≤20 wt%.

66. The soft magnetic alloy according to claim 52, wherein: 0.5 wt% ≤ V ≤ 4.0 wt%.

67. The soft magnetic alloy according to claim 52, wherein: 1.0 wt% ≤ V ≤ 3.0 wt%.

68. The soft magnetic alloy according to claim 52, wherein: 1.3 wt% ≤ V ≤ 2.7 wt%.

69. The soft magnetic alloy according to claim 52, wherein: 0.1 wt%≤Cr≤2.0 wt%.

70. The soft magnetic alloy according to claim 52, wherein: 0.2 wt%≤Cr≤1.0 wt%.

71. The soft magnetic alloy according to claim 52, wherein: 0.3 wt% ≤ Cr ≤ 0.7 wt%.

72. The soft magnetic alloy according to claim 52, wherein: 0.1 wt%≤Si≤2.0 wt%.

73. The soft magnetic alloy according to claim 52, wherein: 0.15 wt%≤Si≤1.0 wt%.

74. The soft magnetic alloy according to claim 52, wherein: 0.2 wt%≤Si≤0.5 wt%.

75. The soft magnetic alloy according to claim 52, wherein: 0.2 wt%≤Cr+Si+Al+Mn≤0.6 wt%.

76. Use of the soft magnetic alloy according to claim 52 in an electric machine, and / or in a transformer, and / or in an electromagnetic actuator.

77. Use of the soft magnetic alloy according to claim 52 as or for a stator and / or rotor of an electric motor and / or a generator.