A thixotropic early-strength water-reducing agent and its preparation method and application
Through the combination of polyethylene glycol divinyl ether and polyethylene glycol dicrylate functional monomer, a water-reducing agent with dual barrier effects is formed, which solves the problem that the existing technology cannot meet the needs of high-slope construction and subway segments. The issue of concrete requirements achieves high compressive strength and early strength of concrete and improves the overall performance.
Patent Information
- Application Number
- CN202111580834.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-22
AI Technical Summary
The existing thixotropic early-strength polycarboxylate superplasticizer cannot meet the high construction design requirements of ultra-high slope construction and subway segment concrete, and cannot guarantee the high slope rate, service strength and early strength of the concrete, resulting in the failure to achieve the comprehensive performance of the concrete. breakthrough.
Polyethylene glycol divinyl ether macromonomer is combined with polyethylene glycol dicrylate functional monomer to form highly active polyether and carboxylate side chain groups, combined with specific functional monomer B, It forms a water-reducing agent with dual barrier effects to improve the water-reducing property and early strength of concrete. Through specific preparation methods and component ratios, a uniform network structure is formed to achieve a balance of thixotropy, early strength, and water-reducing effects.
It achieves high compressive strength, yield strength and good slump of concrete, meets the construction design requirements of steep slope sections, facades, roofs and subway segments, and improves the comprehensive performance and construction efficiency of concrete.
Smart Images

Figure BDA0003425993330000021 
Figure BDA0003425993330000031 
Figure BDA0003425993330000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a thixotropic early-strength water reducing agent and a preparation method and application thereof. Background Art
[0002] The thixotropy of fresh concrete refers to the fact that under the action of external shear, the consistency of the concrete decreases and it can change from a solid form to a flowable form. The flocculation components of the mixture undergo structural changes due to shear strain, causing the paste in the concrete to undergo thixotropic shear thinning, which is convenient for pouring, vibrating and plastering. The mechanism of thixotropy is: as the shear rate increases, the structure of the bonding between concrete particles is destroyed and the viscosity decreases. When the shear stops for a period of time, the structure of the bonding between particles gradually returns to its original state, and the consistency returns to its original state. Thixotropic early-strength water reducers are mainly used in the construction of super-high sections with large slopes, facades, and top surface defect repairs, etc., to ensure that the fresh concrete maintains the required slope after construction, and the concrete in the drainage slope maintains the slope for smooth drainage.
[0003] The characteristics of subway segment concrete are large amount of adhesive, low water-binder ratio, small slump, and difficulty in pouring. Therefore, it needs to have good thixotropy and be sheared and thinned before construction. In order to improve production efficiency, high early strength is required after construction so that the hardened concrete in the formwork can be demolded as soon as possible. However, the existing thixotropic early-strength polycarboxylate water-reducing agent cannot meet the above concrete conditions to ensure that the concrete has a high slope rate and service strength after static placement, and cannot meet the high construction design requirements of steep slope sections, facades, top surfaces and subway segment concrete, resulting in the comprehensive performance of existing concrete still unable to achieve a major breakthrough and progress. Summary of the invention
[0004] In view of the above-mentioned problems existing in the existing thixotropic early-strength water-reducing agent, the present invention provides a thixotropic early-strength water-reducing agent and a preparation method and application thereof. The thixotropic early-strength water-reducing agent can achieve a balance among water-reducing, thixotropic and early-strength effects, and can effectively ensure the construction design requirements of concrete parts for steep slope sections, facades, top surfaces and subway segments while improving the workability and working performance of concrete, and improve the comprehensive properties of concrete such as compressive strength, yield strength, thixotropy and good slump, and has broad application prospects in concrete construction projects.
[0005] In order to achieve the above-mentioned object of the invention, the embodiment of the present invention adopts the following technical solution:
[0006] A thixotropic early strength water reducing agent, comprising the following components in parts by weight:
[0007] 150-170 parts of polyethylene glycol divinyl ether macromonomer, 22-30 parts of unsaturated carboxylic acid small monomer, 3-5 parts of functional monomer A, 1-2 parts of functional monomer B, 1-4 parts of initiator, 0.4-0.9 parts of chain transfer agent, 2-5 parts of pH adjuster, add water to make up to 250-300 parts;
[0008] The functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer comprises: adding maleic anhydride to polyethylene glycol and simultaneously adding a NaOH aqueous solution, performing an esterification reaction under reduced pressure, and naturally cooling after the reaction is completed, washing, and drying to obtain the polyethylene glycol dibutyl ester functional monomer;
[0009] The functional monomer B is at least one of allyltrimethylammonium chloride, dimethyldiallylammonium chloride and hydroxymethylcellulose.
[0010] Wherein, the structural formula of polyethylene glycol divinyl ether macromonomer is as follows:
[0011]
[0012] Compared with the prior art, the thixotropic early-strength water-reducing agent provided by the present invention adds a hexacarbon macromonomer diethylene glycol divinyl ether, which is polymerized with a polyethylene glycol dibutyl ester functional monomer to form a large number of highly active and specially arranged polyether and carboxylate side chain groups in the water-reducing agent system. These side chain groups can form a dual barrier effect, which can reduce the adsorption and wrapping of water molecules, thereby effectively reducing the aggregation of concrete particles, improving the surface adsorption state of cement particles, reducing the water-cement ratio, reducing water bleeding, and improving the water-reducing property and working performance of concrete.
[0013] At the same time, the unsaturated bonds in the polyethylene glycol divinyl ether macromonomer of the present invention can also react with the unsaturated groups in the polyethylene glycol dibutyl ester functional monomer, thereby improving the adsorption capacity of the water reducer and increasing the workability of the water reducer with different aggregates. The polyethylene glycol dibutyl ester functional monomer prepared by the above preparation method has a certain emulsification and softening effect in the water reducer system, and the carboxylate group therein can form a physical adsorption effect with concrete particles, and the physical adsorption force is related to the shear force. Under the shear force, the functional monomer A (polyethylene glycol dibutyl ester functional monomer) destroys the adsorption force between concrete particles and reduces the viscosity. When the shearing stops for a period of time, the bonding force between the carboxylate group and the concrete particles is quickly restored, and the adsorption force is significantly enhanced, giving the concrete good thixotropy, which is conducive to improving the early strength of the concrete.
[0014] The specific functional monomer B in the present invention can be adsorbed on the surface of clay after being mixed with concrete in the above-mentioned water-reducing agent system, and can neutralize part of the negative charge of the clay, thereby inhibiting the expansion of the clay, and achieving the effect of tightening and stabilizing the expansion of concrete, that is, the above-mentioned functional monomer B is combined with the polyethylene glycol divinyl ether macromonomer, unsaturated carboxylic acid small monomer and functional monomer A in the water-reducing agent to improve the stability of concrete.
[0015] The combination of the above macromonomer, micromonomer and functional monomer in the present invention forms a water reducer, in which the main chain structure contains sufficient carboxyl and amino groups, and the long side chain contains amino, ester and polyether structures. The combination enables the water reducer and the cement component in the concrete to form a uniform network structure through the filling barrier, adsorption, analysis and electrostatic interaction of the side chain groups, and achieve a balanced state of thixotropy, early strength and water reduction effects. While improving the workability and working performance of concrete, it can effectively ensure the design requirements for the construction of steep slope sections, facades, top surfaces and subway pipe segments, and improve the comprehensive performance of concrete.
[0016] Preferably, the unsaturated carboxylic acid small monomer is at least one of sodium methyl propylene sulfonate, methyl acrylamide, 2-amino-butenoic acid (2-amino-2-butenoic acid) and 2-aminomalic acid. The structural formula of 2-aminomalic acid is as follows:
[0017]
[0018] Preferably, the initiator is at least one of azobisisobutyronitrile, azobisisoheptylnitrile, ammonium persulfate, benzoyl peroxide and diisopropyl peroxydicarbonate.
[0019] Preferably, the chain transfer agent is at least one of mercaptoethanol, 3-mercaptopropionic acid, sodium aluminum phosphate and sodium hypophosphite.
[0020] Preferably, the pH regulator is a sodium hydroxide solution with a mass fraction of 20%-30%.
[0021] Preferably, the mass ratio of the polyethylene glycol to maleic anhydride is 20:1-2.5.
[0022] Preferably, the concentration of the NaOH aqueous solution is 0.1 wt.%-0.25 wt.%, and the added amount is 10%-15% of the total mass of maleic anhydride.
[0023] Preferably, the esterification reaction is carried out at a temperature of 80°C-100°C and a stirring speed of 400-500 r / min for 6-8 hours.
[0024] Directly adding maleic anhydride to polyethylene glycol without adding a reaction solvent to carry out an esterification reaction can significantly improve the esterification reaction activity and the conversion rate of the product, thereby forming a functional monomer with thixotropic early strength function; at the same time, by optimizing the above-mentioned reaction temperature, reaction time and the amount of raw material added, the prepared polyethylene glycol dibutyl ester functional monomer can have a controllable molecular weight, high stability and good water solubility, and is suitable for the synthesis of thixotropic early strength water reducer.
[0025] Preferably, the washing method is washing with deionized water 3-5 times.
[0026] Preferably, the drying method is drying under vacuum conditions for 2-4 hours.
[0027] Preferably, the number average molecular weight of the polyethylene glycol dibutyl acrylate functional monomer is 2150-3100 g / mol.
[0028] The present invention also provides a method for preparing the thixotropic early-strength water-reducing agent, which comprises at least the following steps:
[0029] a. Add the polyethylene glycol divinyl ether macromonomer to 10-20 parts of water according to the mass fraction, stir evenly, and obtain a macromonomer aqueous solution;
[0030] b. adding the functional monomer A, the functional monomer B, the chain transfer agent and 5-7 parts of the unsaturated carboxylic acid small monomer into 5-10 parts of water to obtain a mixed solution;
[0031] c. Add the mixed solution dropwise to the aqueous solution of the macromonomer, then add the initiator, stir evenly, then add the remaining unsaturated carboxylic acid small monomer dropwise, stir and react for 2-3 hours, then add the pH adjuster, cool naturally, add water to make up to 250-300 parts, mix evenly, and obtain the thixotropic early strength water reducer.
[0032] Compared with the prior art, the preparation method of the thixotropic early strength water reducer provided by the present invention adds the unsaturated carboxylic acid small monomer through the dropwise addition process, which can make the reaction process smooth, ensure that the polyethylene glycol divinyl ether macromonomer and the unsaturated carboxylic acid small monomer, the functional monomer A and the functional monomer B can react smoothly and completely, and make the average molecular weight distribution range of the polymer generated by the reaction narrower, and the polymerization reaction is more complete.
[0033] In the above reaction process, the polyethylene glycol divinyl ether macromonomer is polymerized with the unsaturated carboxylic acid micromonomer, the functional monomer A and the functional monomer B under the action of the initiator, and the chain transfer agent can transfer the chain growth free radicals to obtain a thixotropic early strength water reducing agent through free radical polymerization. The entire preparation process is safe and reliable, easy to operate, and safe to the environment, and has a wide range of application prospects in concrete construction projects.
[0034] Preferably, in step c, the dropping speed of the mixed solution is 0.05-0.1 mL / min.
[0035] Preferably, in step c, the remaining unsaturated carboxylic acid small monomer is added dropwise at a rate of 0.08-0.15 mL / min.
[0036] The preferred dropping speed of the unsaturated carboxylic acid small monomer can further narrow the molecular weight distribution range of the polymer produced by the reaction.
[0037] Preferably, in step c, the stirring reaction is carried out at a speed of 400-500 r / min and a temperature of 40-50°C.
[0038] The invention provides application of the thixotropic early-strength water-reducing agent as a concrete admixture. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] Example 1
[0041] A thixotropic early strength water reducing agent, comprising the following components in parts by weight:
[0042] 150 parts of polyethylene glycol divinyl ether macromonomer, 22 parts of unsaturated carboxylic acid small monomer, 3 parts of functional monomer A, 1 part of functional monomer B, 1 part of initiator, 0.4 parts of chain transfer agent, 2 parts of pH adjuster, add water to make up to 250-300 parts;
[0043] Among them, the functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer is: adding butyric anhydride to polyethylene glycol at one time (the mass ratio of polyethylene glycol to butyric anhydride is 20:1), and adding 0.1wt.% NaOH aqueous solution at the same time, the addition amount is 15% of the total mass of butyric anhydride, and esterification reaction is carried out for 6 hours under reduced pressure, temperature of 80°C, and stirring speed of 400r / min. After the reaction is completed, it is naturally cooled, washed with deionized water for 3 times, and then dried under vacuum conditions for 2 hours to obtain the polyethylene glycol dibutyl ester functional monomer, and the number average molecular weight of the polyethylene glycol dibutyl ester functional monomer is 2150g / mol;
[0044] Functional monomer B is allyltrimethylammonium chloride;
[0045] The unsaturated carboxylic acid small monomer is sodium methyl methacrylate sulfonate;
[0046] The initiator is azobisisobutyronitrile;
[0047] The chain transfer agent is mercaptoethanol;
[0048] The pH regulator is a sodium hydroxide solution with a mass fraction of 20%.
[0049] The preparation method of the above-mentioned thixotropic early strength water reducing agent comprises the following steps:
[0050] a. Weigh each component according to the mass fraction of each component in the above water reducer; first add polyethylene glycol divinyl ether macromonomer to 10 parts of water and stir evenly to obtain a macromonomer aqueous solution;
[0051] b. Then, functional monomer A, functional monomer B, chain transfer agent and 5 parts of unsaturated carboxylic acid small monomer are added to 5 parts of water to obtain a mixed solution;
[0052] c. Add the mixed solution to the aqueous solution of the large monomer at a dropping speed of 0.05 mL / min. After the addition is completed, stir for 15 minutes, add the initiator, continue stirring for 10 minutes, and then add the remaining unsaturated carboxylic acid small monomer at a dropping speed of 0.08 mL / min. After the addition is completed, stir the reaction for 2 hours at a stirring speed of 400 r / min and a reaction temperature of 40°C. Add a pH adjuster, cool naturally, add water to make up to 250 parts, mix well, and obtain the above-mentioned thixotropic early strength water reducer.
[0053] Example 2
[0054] A thixotropic early strength water reducing agent, comprising the following components in parts by weight:
[0055] 160 parts of polyethylene glycol divinyl ether macromonomer, 25 parts of unsaturated carboxylic acid micromonomer, 4 parts of functional monomer A, 1.5 parts of functional monomer B, 2 parts of initiator, 0.6 parts of chain transfer agent, 3 parts of pH adjuster, add water to make up to 280 parts;
[0056] Among them, the functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer is: adding butyric anhydride to polyethylene glycol at one time (the mass ratio of polyethylene glycol to butyric anhydride is 20:1.5), and adding 0.15wt.% NaOH aqueous solution at the same time, the addition amount is 12.5% of the total mass of butyric anhydride, and esterification reaction is carried out for 7 hours under reduced pressure, temperature of 90°C, and stirring speed of 450r / min. After the reaction is completed, it is naturally cooled, washed with deionized water for 4 times, and then dried under vacuum conditions for 3 hours to obtain the polyethylene glycol dibutyl ester functional monomer, and the number average molecular weight of the polyethylene glycol dibutyl ester functional monomer is 2400g / mol;
[0057] Functional monomer B is dimethyldiallylammonium chloride;
[0058] The unsaturated carboxylic acid small monomer is methacrylamide;
[0059] The initiator is azobisisoheptanonitrile;
[0060] The chain transfer agent is 3-mercaptopropionic acid;
[0061] The pH regulator is a sodium hydroxide solution with a mass fraction of 25%.
[0062] The preparation method of the above-mentioned thixotropic early strength water reducing agent comprises the following steps:
[0063] a. Weigh each component according to the mass fraction of each component in the above water reducer; first add polyethylene glycol divinyl ether macromonomer to 15 parts of water and stir evenly to obtain a macromonomer aqueous solution;
[0064] b. Then, functional monomer A, functional monomer B, chain transfer agent and 6 parts of unsaturated carboxylic acid small monomer are added to 7 parts of water to obtain a mixed solution;
[0065] c. Add the mixed solution dropwise to the aqueous solution of the large monomer at a dropping speed of 0.08 mL / min. After the dropping is completed, stir for 15 minutes, add the initiator, continue stirring for 15 minutes, and then add the remaining unsaturated carboxylic acid small monomer at a dropping speed of 0.1 mL / min. After the dropping is completed, stir the reaction at a stirring speed of 450 r / min and a reaction temperature of 45°C for 2.5 hours. Add a pH adjuster, cool naturally, add water to make up to 280 parts, mix well, and obtain the above-mentioned thixotropic early strength water reducer.
[0066] Example 3
[0067] A thixotropic early strength water reducing agent, comprising the following components in parts by weight:
[0068] 170 parts of polyethylene glycol divinyl ether macromonomer, 30 parts of unsaturated carboxylic acid micromonomer, 5 parts of functional monomer A, 2 parts of functional monomer B, 4 parts of initiator, 0.9 parts of chain transfer agent, 5 parts of pH adjuster, add water to make up to 300 parts;
[0069] Among them, the functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer comprises: adding butyric anhydride to polyethylene glycol at one time (the mass ratio of polyethylene glycol to butyric anhydride is 20:2.5), and adding 0.25wt.% NaOH aqueous solution at the same time, the addition amount is 10% of the total mass of butyric anhydride, and esterification reaction is carried out for 8 hours under reduced pressure, temperature of 100°C, and stirring speed of 500r / min. After the reaction is completed, it is naturally cooled, washed with deionized water for 5 times, and then dried under vacuum conditions for 4 hours to obtain the polyethylene glycol dibutyl ester functional monomer, and the number average molecular weight of the polyethylene glycol dibutyl ester functional monomer is 3100g / mol;
[0070] Functional monomer B is hydroxymethyl cellulose;
[0071] The unsaturated carboxylic acid small monomer is 2-amino-butenoic acid;
[0072] The initiator is ammonium persulfate;
[0073] The chain transfer agent is sodium aluminum phosphate;
[0074] The pH regulator is a sodium hydroxide solution with a mass fraction of 30%.
[0075] The preparation method of the above-mentioned thixotropic early strength water reducing agent comprises the following steps:
[0076] a. Weigh each component according to the mass fraction of each component in the above water reducer; first add polyethylene glycol divinyl ether macromonomer to 20 parts of water and stir evenly to obtain a macromonomer aqueous solution;
[0077] b. Then, functional monomer A, functional monomer B, chain transfer agent and 7 parts of unsaturated carboxylic acid small monomer are added to 10 parts of water to obtain a mixed solution;
[0078] c. Add the mixed solution dropwise to the aqueous solution of the large monomer at a dropping speed of 0.1 mL / min. After the dropping is completed, stir for 15 min. Then add the initiator and continue stirring for 20 min. Then add the remaining unsaturated carboxylic acid small monomer at a dropping speed of 0.15 mL / min. After the dropping is completed, stir the reaction for 3 h at a stirring speed of 500 r / min and a reaction temperature of 50°C. Add a pH adjuster, cool naturally, add water to make up to 300 parts, mix well, and obtain the above-mentioned thixotropic early strength water reducer.
[0079] Example 4
[0080] A thixotropic early strength water reducing agent, comprising the following components in parts by weight:
[0081] 160 parts of polyethylene glycol divinyl ether macromonomer, 28 parts of unsaturated carboxylic acid micromonomer, 4 parts of functional monomer A, 1.5 parts of functional monomer B, 2 parts of initiator, 0.7 parts of chain transfer agent, 4 parts of pH adjuster, add water to make up to 280 parts;
[0082] The functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer comprises: adding maleic anhydride to polyethylene glycol at one time (the mass ratio of polyethylene glycol to maleic anhydride is 20:2), and adding 0.2wt.% NaOH aqueous solution at the same time, the addition amount is 12% of the total mass of maleic anhydride, and esterification reaction is carried out for 7 hours under reduced pressure, temperature of 85°C, and stirring speed of 450r / min. After the reaction is completed, it is naturally cooled, washed with deionized water for 4 times, and then dried under vacuum conditions for 3 hours to obtain the polyethylene glycol dibutyl ester functional monomer, and the number average molecular weight of the polyethylene glycol dibutyl ester functional monomer is 2600g / mol;
[0083] Functional monomer B is allyltrimethylammonium chloride;
[0084] The unsaturated carboxylic acid small monomer is 2-aminomalic acid;
[0085] The initiator is benzoyl peroxide;
[0086] The chain transfer agent is sodium hypophosphite;
[0087] The pH regulator is a sodium hydroxide solution with a mass fraction of 28%.
[0088] The preparation method of the above-mentioned thixotropic early strength water reducing agent comprises the following steps:
[0089] a. Weigh each component according to the mass fraction of each component in the above water reducer; first add polyethylene glycol divinyl ether macromonomer to 18 parts of water and stir evenly to obtain a macromonomer aqueous solution;
[0090] b. Then, functional monomer A, functional monomer B, chain transfer agent and 6 parts of unsaturated carboxylic acid small monomer are added to 7 parts of water to obtain a mixed solution;
[0091] c. Add the mixed solution dropwise to the aqueous solution of the large monomer at a dropping speed of 0.06 mL / min. After the dropping is completed, stir for 15 minutes, add the initiator, continue stirring for 12 minutes, and then add the remaining unsaturated carboxylic acid small monomer at a dropping speed of 0.12 mL / min. After the dropping is completed, stir the reaction at a stirring speed of 450 r / min and a reaction temperature of 48°C for 2.5 hours. Add a pH adjuster, cool naturally, add water to make up to 280 parts, mix well, and obtain the above-mentioned thixotropic early strength water reducer.
[0092] Example 5
[0093] A thixotropic early strength water reducing agent, comprising the following components in parts by weight:
[0094] 165 parts of polyethylene glycol divinyl ether macromonomer, 28 parts of unsaturated carboxylic acid small monomer, 4 parts of functional monomer A, 1.5 parts of functional monomer B, 2 parts of initiator, 0.8 parts of chain transfer agent, 3 parts of pH adjuster, add water to make up to 260 parts;
[0095] Among them, the functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer comprises: adding maleic anhydride to polyethylene glycol at one time (the mass ratio of polyethylene glycol to maleic anhydride is 20:2.2), and adding 0.2wt.% NaOH aqueous solution at the same time, the addition amount is 13% of the total mass of maleic anhydride, and esterification reaction is carried out for 7 hours under reduced pressure, temperature of 95°C, and stirring speed of 400r / min. After the reaction is completed, it is naturally cooled, washed with deionized water for 4 times, and then dried under vacuum conditions for 3 hours to obtain the polyethylene glycol dibutyl ester functional monomer, and the number average molecular weight of the polyethylene glycol dibutyl ester functional monomer is 3050g / mol;
[0096] Functional monomer B is dimethyldiallylammonium chloride;
[0097] The unsaturated carboxylic acid small monomer is sodium methyl methacrylate sulfonate;
[0098] The initiator is diisopropyl peroxydicarbonate;
[0099] The chain transfer agent is mercaptoethanol;
[0100] The pH regulator is a sodium hydroxide solution with a mass fraction of 22%.
[0101] The preparation method of the above-mentioned thixotropic early strength water reducing agent comprises the following steps:
[0102] a. Weigh each component according to the mass fraction of each component in the above water reducer; first add polyethylene glycol divinyl ether macromonomer to 15 parts of water and stir evenly to obtain a macromonomer aqueous solution;
[0103] b. Then, functional monomer A, functional monomer B, chain transfer agent and 6 parts of unsaturated carboxylic acid small monomer are added to 6 parts of water to obtain a mixed solution;
[0104] c. Add the mixed solution dropwise to the aqueous solution of the large monomer at a dropping speed of 0.09 mL / min. After the dropping is completed, stir for 15 minutes, add the initiator, continue stirring for 18 minutes, and then add the remaining unsaturated carboxylic acid small monomer at a dropping speed of 0.1 mL / min. After the dropping is completed, stir the reaction at a stirring speed of 500 r / min and a reaction temperature of 45°C for 2.5 hours. Add a pH adjuster, cool naturally, add water to make up to 260 parts, mix well, and obtain the above-mentioned thixotropic early strength water reducer.
[0105] Test example
[0106] The thixotropic early strength water reducer obtained in Example 1-5 was compared with the commercially available polycarboxylate water reducer FDN-C with a solid content of 40wt.%, and the test was carried out in accordance with the national standard GB 8076-2008 "Concrete Admixtures". The cement was Dinglu PO 42.5, the fineness modulus was in the range of medium sand river sand, the gravel was 5-32.5mm continuous gradation, the admixture was the thixotropic early strength water reducer in Example 1-5 and the commercially available polycarboxylate water reducer FDN-C with a solid content of 40wt.%, and the admixture was 1.0wt.% of the total mass of the cementitious material. The test was carried out according to the following mix ratio: cement: fly ash: mineral powder: river sand: gravel: water: admixture = 240: 60: 80: 777: 988: 195: 7.8 (unit: kg / m 3 ), so that the initial slump of concrete is controlled within the range of (220±20) mm. According to the standard of "Concrete Strength Test and Evaluation Standard" (GB / T 50107-2010), the maximum yield force of fresh concrete is measured by RHM-3000ICAR rheometer to analyze the thixotropy of concrete. The early strength performance of water reducer is examined by concrete thixotropy evaluation and 1d, 3d and 7d compressive strength tests. The test results are shown in Table 1.
[0107] Table 1 Concrete performance test results
[0108]
[0109]
[0110] From the test data in Table 1, the thixotropic early strength water reducer provided by the embodiment of the present invention has a higher maximum yield moment after being added to concrete at a low dosage than the commercial polycarboxylate water reducer FDN-C (Wanshan Chemical). The concrete becomes thinner after the shear force is applied, and recovers its original dense adhesion after the shear force stops, showing good thixotropic properties. Moreover, the concrete mixed with the thixotropic early strength water reducer of the present invention has higher early strength than the concrete mixed with the ordinary commercial water reducer, showing significant early strength performance. At the same time, the water reducer has good adsorption and dispersion properties for cement, and the slump loss of the concrete in 2h is less than 10%, showing a high water reduction rate.
[0111] In summary, the thixotropic early strength type water reducing agent provided by the present invention has obvious thixotropic properties and early strength properties, and has relatively good collapse retention and water reduction effects. In addition, the preparation method of the thixotropic early strength type water reducing agent provided by the present invention is simple and easy to operate, has strong operability, is environmentally friendly, and the reaction process is easy to control.
[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A thixotropic early strength water reducing agent, characterized in that: The composition includes the following components in parts by weight: 150-170 parts of polyethylene glycol divinyl ether macromonomer, 22-30 parts of unsaturated carboxylic acid small monomer, 3-5 parts of functional monomer A, 1-2 parts of functional monomer B, 1-4 parts of initiator, 0.4-0.9 parts of chain transfer agent, 2-5 parts of pH adjuster, add water to make up to 250-300 parts; The functional monomer A is a polyethylene glycol dibutyl ester functional monomer, and the preparation method of the polyethylene glycol dibutyl ester functional monomer comprises: adding maleic anhydride to polyethylene glycol and simultaneously adding a NaOH aqueous solution, performing an esterification reaction under reduced pressure, and naturally cooling after the reaction is completed, washing, and drying to obtain the polyethylene glycol dibutyl ester functional monomer; The mass ratio of the polyethylene glycol to maleic anhydride is 20:1-2.5; The number average molecular weight of the polyethylene glycol dibutyl acrylate functional monomer is 2150-3100 g / mol; The functional monomer B is at least one of allyltrimethylammonium chloride, dimethyldiallylammonium chloride and hydroxymethylcellulose.
2. The thixotropic early strength water reducing agent according to claim 1, characterized in that: The unsaturated carboxylic acid small monomer is at least one of sodium methyl propylene sulfonate, methyl acrylamide, 2-amino-butenoic acid and 2-aminomalic acid.
3. The thixotropic early strength water reducing agent according to claim 1, characterized in that: The initiator is at least one of azobisisobutyronitrile, azobisisoheptylnitrile, ammonium persulfate, benzoyl peroxide and diisopropyl peroxydicarbonate.
4. The thixotropic early strength water reducing agent according to claim 1, characterized in that: The chain transfer agent is at least one of mercaptoethanol, 3-mercaptopropionic acid, sodium aluminum phosphate and sodium hypophosphite.
5. The thixotropic early strength water reducing agent according to claim 1, characterized in that: The pH regulator is a sodium hydroxide solution with a mass fraction of 20%-30%.
6. The thixotropic early strength water reducing agent according to claim 1, characterized in that: The concentration of the NaOH aqueous solution is 0.1 wt.%-0.25 wt.%, and the added amount is 10%-15% of the total mass of maleic anhydride.
7. The thixotropic early strength water reducing agent according to claim 1, characterized in that: The esterification reaction is carried out at a temperature of 80°C-100°C and a stirring speed of 400-500 r / min for 6-8 hours; And / or the washing method is washing with deionized water 3-5 times; And / or the drying method is drying under vacuum conditions for 2-4 hours.
8. The method for preparing the thixotropic early strength water reducing agent according to any one of claims 1 to 7, characterized in that: The following steps are involved: a. Add the polyethylene glycol divinyl ether macromonomer to 10-20 parts of water according to the mass fraction, stir evenly, and obtain a macromonomer aqueous solution; b. adding the functional monomer A, the functional monomer B, the chain transfer agent and 5-7 parts of the unsaturated carboxylic acid small monomer into 5-10 parts of water to obtain a mixed solution; c. Add the mixed solution dropwise to the aqueous solution of the macromonomer, then add the initiator, stir evenly, then add the remaining unsaturated carboxylic acid small monomer dropwise, stir and react for 2-3 hours, then add the pH adjuster, cool naturally, add water to make up to 250-300 parts, mix evenly, and obtain the thixotropic early strength water reducer.
9. The method for preparing the thixotropic early strength water reducing agent according to claim 8, characterized in that: In step c, the dropwise addition rate of the mixed solution is 0.05-0.1 mL / min; and / or in step c, the remaining unsaturated carboxylic acid small monomer is added dropwise at a rate of 0.08-0.15 mL / min; And / or in step c, the rotation speed of the stirring reaction is 400-500 r / min and the temperature is 40-50°C.
10. Use of the thixotropic early strength water reducing agent according to any one of claims 1 to 7 as a concrete admixture.
Citation Information
Patent Citations
Polyether mixed concrete water reducer, and preparation method and application thereof
CN103588412A
Early-strength polycarboxylate superplasticizer having slump-loss prevention function and preparation method thereof
CN105218757A
Preparation method of high-thixotropy early-strength type polycarboxylate superplasticizer
CN105504180A
Concrete workability regulator with water reducing function and preparation method of concrete workability regulator
CN107828027A
Polycarboxylate superplasticizer with high adsorption and mud blocking functions and preparation method of polycarboxylate superplasticizer
CN112708051A