Positive electrode active material, positive electrode and secondary battery
By forming an organic-inorganic hybrid coating composed of a variety of metal alkoxides on the surface of the positive electrode active material, the problem of insufficient softness and adhesion of the coating in the existing technology is solved, and the filling and loading characteristics of the positive electrode active material are improved. , improved battery performance.
Patent Information
- Application Number
- CN202080053885.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-06
- Filing Date
- 2020-08-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-08-05
AI Technical Summary
In the existing technology, when metal alkoxides are used for surface treatment of positive electrode active materials, the coating lacks flexibility and adhesion, resulting in reduced cycle characteristics, and increasing the calendering pressure will cause cracks in the positive electrode layer and damage to the current collector, affecting the battery. performance.
An organic-inorganic hybrid coating composed of the first metal alkoxide, the second metal alkoxide and the third metal alkoxide is used to form a mesh structure, enhance the softness and adhesion of the coating, prevent the coating from peeling off, and improve the positive electrode Filling and loading characteristics of active substances.
It effectively prevents the degradation of cycle characteristics, improves the filling and load characteristics of the positive active material, prolongs the service life of the battery and improves the battery performance.
Smart Images

Figure CN114175308B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a positive electrode active material, a positive electrode and a secondary battery. Background Art
[0002] Secondary batteries have long been used as power sources for various electronic devices. Secondary batteries generally have a structure in which an electrode assembly (electrode body) and an electrolyte are housed in an outer body (housing), and are provided with external terminals (or electrode leads) for realizing electrical connection of the secondary battery. The electrode assembly has a structure in which a positive electrode and a negative electrode are arranged with a separator therebetween.
[0003] The positive electrode and the negative electrode respectively have a positive electrode layer containing a positive electrode active material and a negative electrode layer containing a negative electrode active material. In a secondary battery, ions are provided to the electrolyte by the "positive electrode active material contained in the positive electrode layer" and the "negative electrode active material contained in the negative electrode layer", and the ions move between the positive electrode and the negative electrode to transfer electrons, thereby performing charging and discharging. In recent years, lithium-ion secondary batteries using lithium ions as ions have attracted much attention due to their battery capacity.
[0004] The positive electrode for lithium ion secondary battery is manufactured as follows using lithium cobalt oxide and the like as the positive electrode active material. First, the positive electrode active material and the binder are mixed in a dispersion medium to prepare a positive electrode layer slurry. Next, the positive electrode layer slurry is applied to a positive electrode collector such as aluminum foil and then dried to form a coating of the positive electrode active material. Next, the coating of the positive electrode active material is rolled by a calendering roller or the like to form a positive electrode layer. Finally, the positive electrode current collector loaded with the positive electrode layer formed in this way is cut into a specified shape to obtain a positive electrode. When manufacturing the positive electrode, from the viewpoint of increasing the battery capacity, in order to improve the filling property of the positive electrode active material, the positive electrode layer coating is rolled.
[0005] On the other hand, attempts have been made to improve various characteristics of the positive electrode by surface-treating the positive electrode active material with a metal alkoxide (for example, Patent Documents 1 to 4).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2012-199101
[0009] Patent Document 2: Japanese Patent Application Publication No. 2012-169249
[0010] Patent Document 3: Japanese Patent Application Publication No. 2011-49161
[0011] Patent Document 4: Japanese Patent Application Publication No. 2013-191539. Summary of the invention
[0012] Problems to be solved by the invention
[0013] The inventors of the present invention have found that in the surface treatment technology of the positive electrode active material using metal alkoxides in the prior art, problems will arise in the cycle characteristics as follows. In the prior art, the metal alkoxide-based coating formed on the surface of the positive electrode active material does not have sufficient flexibility and / or does not have sufficient close contact with the positive electrode active material. Therefore, the coating does not have sufficient strength and is more likely to peel off due to repeated charge and discharge, resulting in reduced cycle characteristics. The peeling of the coating can cause the electrolyte (or electrolyte) to deteriorate, causing the cycle characteristics to further decrease.
[0014] The inventors of the present invention have also found that the following problems may occur when manufacturing the positive electrode. From the viewpoint of further improving the filling property of the positive electrode active material in the positive electrode layer, if the pressure is increased for rolling, the rate characteristics are reduced due to cracks along the grain boundaries of the positive electrode active material. In addition, the collector may be concave and convex, damaged, and / or the positive electrode layer may be peeled off from the collector. These problems are the cause of further reduction in cycle characteristics.
[0015] Therefore, the inventors of the present invention attempted to improve the filling property of the positive electrode active material by surface treating the positive electrode active material with a metal alkoxide, and found that a new problem of reduced battery characteristics such as load characteristics in the obtained positive electrode would occur. In detail, even if the filling property of the positive electrode active material is more fully improved, the ion conductivity (especially Li ion conductivity) on the surface of the positive electrode active material will also decrease, thus generating a new problem of reduced battery characteristics such as load characteristics.
[0016] An object of the present invention is to provide a positive electrode active material that can more fully prevent reduction in cycle characteristics even if it has a coating film based on a metal alkoxide on the surface. Hereinafter, the present invention that solves this object may be referred to as "present invention A".
[0017] The present invention also aims to provide a positive electrode active material that can more fully prevent the reduction of cycle characteristics even if it has a metal alkoxide coating on the surface, and also has better battery characteristics such as filling property and load characteristics. Hereinafter, the present invention that solves this purpose is sometimes referred to as "present invention B".
[0018] The problems related to the cycle characteristics are the problems to be solved by the present invention.
[0019] The problems related to filling properties and battery characteristics (for example, load characteristics) are not problems that must be solved by the present invention, but are problems that may not be solved but are preferably solved.
[0020] Technical solutions to solve problems
[0021] The present invention A relates to a positive electrode active material having:
[0022] Positive electrode active material core material; and
[0023] A coating formed on the surface of the positive electrode active material core material,
[0024] The coating is an organic-inorganic hybrid coating composed of reactants, and the reactants at least include:
[0025] A first metal alkoxide that does not contain any metal atom-carbon atom bonds in one molecule; and
[0026] A second metal alkoxide comprising two or more metal atom-carbon atom bonds in one molecule.
[0027] The present invention B relates to a positive electrode active material having:
[0028] Positive electrode active material core material; and
[0029] A coating formed on the surface of the positive electrode active material core material,
[0030] The coating is an organic-inorganic hybrid coating composed of reactants, and the reactants at least include:
[0031] a first metal alkoxide that does not contain any metal atom-carbon atom bonds in one molecule;
[0032] A second metal alkoxide containing two or more metal atom-carbon atom bonds in one molecule; and
[0033] A third metal alkoxide containing one metal atom-carbon atom bond in one molecule.
[0034] In this specification, unless otherwise specified, "the present invention" includes the present invention A and the present invention B. The present invention A includes the present invention B.
[0035] Effects of the Invention
[0036] Even if the positive electrode active material of the present invention A has a coating film based on a metal alkoxide on the surface, it can constitute a positive electrode capable of more fully preventing a decrease in cycle characteristics.
[0037] Even if the positive electrode active material of the present invention B has a coating film based on a metal alkoxide on the surface, it can constitute a positive electrode that can more fully prevent the cycle characteristics from being deteriorated and has more excellent battery characteristics such as filling property and load characteristic. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a schematic cross-sectional view of the positive electrode active material of the present invention (particularly the present inventions A and B).
[0039] Figure 2 This is a schematic conceptual diagram showing the main bonding state at the interface between the organic-inorganic hybrid coating and the positive electrode active material core material in the positive electrode active material of the present invention (particularly the present inventions A and B).
[0040] Figure 3 This is a schematic conceptual diagram showing the main structure of the organic-inorganic hybrid film in the positive electrode active material of the present invention (particularly the present inventions A and B).
[0041] Figure 4 This is a schematic conceptual diagram showing the main surface state of the organic-inorganic hybrid film in the positive electrode active material of the present invention (particularly the present invention B).
[0042] Figure 5 Schematic conceptual diagram showing the main structure of a coating on the surface of a positive electrode active material in the prior art. DETAILED DESCRIPTION
[0043] [Positive electrode active material]
[0044] like Figure 1 As shown, the positive electrode active material 10 of the present invention includes a positive electrode active material core material 1 and a coating 2 formed on the surface of the positive electrode active material core material 1 . Figure 1 It is a schematic cross-sectional view of the positive electrode active material of the present invention.
[0045] The positive electrode active material core material is a substance that helps to move between the positive electrode and the negative electrode to be responsible for the adsorption and release of ions responsible for electron transfer. From the viewpoint of increasing the battery capacity, it is preferably a substance that helps to adsorb and release lithium ions. From this point of view, the positive electrode active material core material is preferably, for example, a lithium-containing composite oxide. More specifically, the positive electrode active material core material is preferably a lithium transition metal composite oxide containing lithium and at least one transition metal selected from the group consisting of cobalt, nickel, manganese and iron. That is, it is preferred that such a lithium transition metal composite oxide is included as a positive electrode active material core material in the positive electrode active material of the present invention. For example, the positive electrode active material core material can be lithium cobaltate, lithium nickelate, lithium manganate, lithium iron phosphate or a part of their transition metals replaced by other metals. This positive electrode active material core material can be included as a single species, or it can be included in combination of two or more. In a more preferred embodiment, the positive electrode active material core material contained in the positive electrode active material is lithium cobaltate.
[0046] The average primary particle size of the positive electrode active material core material is not particularly limited, and may be, for example, 1 μm or more and 50 μm or less, particularly 3 μm or more and 30 μm or less.
[0047] In this specification, the average primary particle size is the average value calculated by observing the positive electrode active material core material through an optical microscope or an electron microscope, measuring the length of 50 randomly selected particles. In the microscope image, a line is drawn from the end to the end of each particle, and the distance between the two points with the maximum length is taken as the particle size.
[0048] The film 2 is an organic-inorganic hybrid film, and is formed of a composite of an organic component and an inorganic component.
[0049] In the present invention, the coating 2 is formed by a reactant containing at least a first metal alkoxide and a second metal alkoxide as monomer components. Such the present invention corresponds to the present invention A. In detail, in the present invention (especially the present invention A), the coating 2 is not formed by stacking a plurality of layers formed by the above-mentioned metal alkoxides, but has a mesh structure (single-layer structure) composed of reactants of a mixture of the above-mentioned metal alkoxides. The coating 2 of the present invention A has a mesh structure of moderate thickness and therefore has more sufficient flexibility. The coating 2 further has more sufficient adhesion to the positive electrode active material core 1. Therefore, it is believed that the coating 2 has more sufficient strength, and as a result, even if it is repeatedly charged and discharged, it can more fully prevent the peeling of the coating, and the cycle characteristics are improved. In the case where the coating does not contain at least one of the first metal alkoxide or the second metal alkoxide, the coating does not have sufficient flexibility and / or does not have sufficient adhesion to the positive electrode active material core. Therefore, the coating does not have sufficient strength and is more likely to peel off due to repeated charging and discharging, which leads to reduced cycle characteristics. The cycle characteristics refer to the characteristics that prevent the discharge capacity from decreasing even after repeated charge and discharge.
[0050] In the present invention, the coating 2 is formed by a reactant containing not only the first metal alkoxide and the second metal alkoxide, but also at least the third metal alkoxide as a monomer component, thereby further obtaining the effect of improving the filling property and the battery characteristics (for example, load characteristics). Such the present invention corresponds to the present invention B. In the present invention (especially the present invention B), in detail, the coating 2 is formed by a reactant containing at least the first metal alkoxide, the second metal alkoxide and the third metal alkoxide as monomer components. In the present invention B, the first metal alkoxide and the second metal alkoxide are respectively the same as the first metal alkoxide and the second metal alkoxide in the present invention A. In detail, in the present invention B, the coating 2 is not formed by stacking a plurality of layers formed by the above-mentioned metal alkoxides, but has a mesh structure (single-layer structure) composed of reactants of a mixture of the above-mentioned metal alkoxides. In the present invention B, the coating contains the first metal alkoxide and the second metal alkoxide, so it has the same effect of improving the cycle characteristics as the present invention A. In the present invention B, the coating 2 further contains the third alkoxide, so it not only has a mesh structure of moderate coarseness and fineness, but also has a more sufficient lubricity on the surface. Therefore, it is believed that the positive electrode active material of the present invention B has a more sufficient and excellent filling property, and the ion conductivity of the ions (especially lithium ions) responsible for electron transfer is sufficiently improved when passing through the coating, and the battery characteristics such as load characteristics are sufficient. In the case where the coating does not contain the third metal alkoxide, the filling property of the positive electrode active material is reduced and the volume density is reduced. In the case where the coating does not contain the second metal alkoxide, the mesh in the mesh structure of the coating becomes smaller, so the ion conductivity is reduced and the load characteristics are reduced. In the case where the coating does not contain the first metal alkoxide, the coating will not be fully fixed to the surface of the positive electrode active material core material, so the filling property of the positive electrode active material is reduced and the volume density is reduced.
[0051] The coating 2 generally has an average film thickness of, for example, 0.1 nm to 20 nm (particularly 0.5 nm to 15 nm).
[0052] The first metal alkoxide is a metal alkoxide that does not contain any metal atom-carbon atom bonds in one molecule, and all the bonds that the metal has to alkoxy groups (-OR 1 ) bonded metal alkoxide. In the first metal alkoxide, the metal atom-carbon atom bond refers to a direct covalent bond between a metal atom and a carbon atom. In the first metal alkoxide, the carbon atom constituting the metal atom-carbon atom bond refers to a carbon atom constituting a monovalent hydrocarbon group (e.g., an alkyl group and an alkenyl group) or a carbon atom constituting a divalent hydrocarbon group (e.g., an alkylene group). The first metal alkoxide does not have any such metal atom-carbon atom bond in one molecule. Therefore, the first metal alkoxide has a high reactivity, such as Figure 2 As shown, at the interface between the coating 2 and the positive electrode active material core material 1 , the coating 2 is fixed mainly by relatively strong bonding with the positive electrode active material core material 1 . Figure 2This is a schematic conceptual diagram showing the main bonding state at the interface between the organic-inorganic hybrid coating and the positive electrode active material core material in the positive electrode active material of the present invention (particularly the present inventions A and B).
[0053] Specifically, the first metal alkoxide is a compound represented by the following general formula (1).
[0054]
Chemical formula 1
[0055] M 1 (OR 1 ) x (1)
[0056] In formula (1), M 1 It is a metal atom Si, Ti, Al or Zr. From the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, Si or Ti is preferred, and Si is more preferred.
[0057] x is M 1 The valence number. 1 When M is Si, Ti or Zr, x is 4. 1 When it is Al, x is 3.
[0058] R 1 Each independently represents an alkyl group having 1 to 10 carbon atoms or a general formula: -C(R 2 )=CH-CO-R 3 The group represented by (wherein R 2 and R 3 As described below), from the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, an alkyl group having 1 to 5 carbon atoms is preferred. 1 As for the alkyl group, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, etc. can be mentioned. 1 , all R 1 can be independently selected from the above alkyl groups, or all R 1 The alkyl groups may be the same as each other and are selected from the above-mentioned alkyl groups.
[0059] R 2 is an alkyl group having 1 to 10 carbon atoms, and preferably an alkyl group having 1 to 5 carbon atoms from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 2 As for the alkyl group of R, there can be mentioned 1 The alkyl group is the same as the alkyl group.
[0060] R 3It is an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, or an alkenyloxy group having 1 to 30 carbon atoms. From the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material, it is preferably an alkyl group having 1 to 20 carbon atoms (more preferably 1 to 10, and further preferably 1 to 5), an alkoxy group having 10 to 30 carbon atoms (especially 14 to 24), or an alkenyloxy group having 10 to 30 carbon atoms (especially 14 to 24). 3 As for the preferred alkyl group of R, there can be mentioned: 1 The alkyl group of R is the same as that of alkyl, and undecyl, dodecyl, tridecyl, myristyl, pentadecyl, hexadecyl, heptadecyl, stearyl, nonadecyl, eicosyl, etc. 3 For example, the alkoxy group of formula: -OC p H 2p+1 (wherein p is an integer from 1 to 30). 3 For example, the alkenyloxy group of the formula: -OC q H 2q-1 (wherein q is an integer of 1 to 30).
[0061] In formula (1), multiple R 1 In the example, two adjacent R 1 When they are alkyl groups, they can be bonded to each other, and the two R 1 The oxygen atom to which it is bonded and the M to which the oxygen atom is bonded 1 The atoms together form a ring (e.g., a 5- to 8-membered ring, especially a 6-membered ring). 1 The ring formed by bonding together is, for example, a 6-membered ring represented by the general formula (1X).
[0062]
Chemical formula 1X
[0063]
[0064] In formula (1X), R 4 , R 5 and R 6 Each of R is independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and is preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 4 , R 5 and R 6 The total number of carbon atoms is usually 0 to 12, and preferably 2 to 8 from the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material. 4 , R 5and R 6 As for the alkyl group of R, there can be mentioned 1 The alkyl group is the same as the alkyl group.
[0065] As the first metal alkoxide, for example, compounds represented by the following general formulae (1A), (1B), (1B′), (1C) and (1D) can be cited. From the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, the first metal alkoxide is preferably a compound represented by the general formula (1A), (1B), (1C) or (1D) or a mixture thereof, more preferably a compound represented by the general formula (1A) or (1B) or a mixture thereof, and further preferably a compound represented by the general formula (1A) or a mixture thereof.
[0066]
Chemical formula 1A
[0067] Si(OR 1 )4 (1A)
[0068] In formula (1A), R 1 are independently the same as R in formula (1) 1 Same R 1 From the perspective of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, R 1 Each independently is preferably an alkyl group having 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms.
[0069] Specific examples of the compound (1A) represented by the general formula are shown in the following table.
[0070]
Table 1A
[0071] Specific examples of compound (1A)
[0072] Compound <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> 1A-1 Ethyl Ethyl Ethyl Ethyl 1A-2 methyl methyl methyl methyl 1A-3 Butyl Butyl Butyl Butyl 1A-4 Isopropyl Isopropyl Isopropyl Isopropyl
[0073]
Chemical formula 1B1
[0074] Ti(OR 1 )4 (1B)
[0075] In formula (1B), R 1 are independently the same as R in formula (1) 1 Same R 1 From the perspective of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, R 1 Each of them is independently preferably an alkyl group having 1 to 10 carbon atoms or the general formula: -C(R 2 )=CH-CO-R 3 The group represented by (wherein R 2 and R 3and R in the general formula (1) 2 and R 3 The same), more preferably an alkyl group having 1 to 10 carbon atoms (particularly 1 to 5).
[0076] In formula (1B), from the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, R 2 and R 3 The following groups are preferred. 2 is an alkyl group having 1 to 10 carbon atoms, preferably an alkyl group having 1 to 5 carbon atoms. 2 As for the alkyl group of R, there can be mentioned 1 The alkyl group of R is the same as the alkyl group of 3 is an alkyl group having 1 to 30 carbon atoms, preferably an alkyl group having 1 to 20 carbon atoms (more preferably 1 to 10, and even more preferably 1 to 5). 3 As for the preferred alkyl group of R, there can be mentioned: 1 The alkyl group having the same alkyl group as the alkyl group, as well as undecyl, dodecyl, tridecyl, myristyl, pentadecyl, hexadecyl, heptadecyl, stearyl, nonadecyl, eicosyl and the like.
[0077] Specific examples of the compound (1B) represented by the general formula are shown in the following table.
[0078]
Table 1B1
[0079] Specific examples of compound (1B)
[0080]
[0081]
Chemical formula 1B2
[0082]
[0083] In formula (1B'), Ra 1 , Ra 2 , Ra 3 , Ra 4 , Ra 5 and Ra 6 Each of Ra is independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and preferably an alkyl group having 1 to 5 carbon atoms from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 1 , Ra 2 , Ra 3 , Ra 4 , Ra 5 and Ra 6 The alkyl group with 1 The alkyl groups are the same.
[0084] Specific examples of the compound (1B') represented by the general formula are shown in the following table.
[0085]
Table 1B2
[0086] Specific examples of compound (1B')
[0087] Compound <![CDATA[Ra 1 ]]> <![CDATA[Ra 2 ]]> <![CDATA[Ra 3 ]]> <![CDATA[Ra 4 ]]> <![CDATA[Ra 5 ]]> <![CDATA[Ra 6 ]]> 1B’-1 n-propyl Ethyl Hydrogen Atom n-propyl Ethyl Hydrogen Atom
[0088]
Chemical formula 1C
[0089] Al(OR 1 )3 (1C)
[0090] In formula (1C), R 1 are independently the same as R in formula (1) 1 Same R 1 From the perspective of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, R 1 Each of them is independently preferably an alkyl group having 1 to 10 carbon atoms or the general formula: -C(R 2 )=CH-CO-R 3 The group represented by (wherein R 2 and R 3 respectively with R in the general formula (1) 2 and R 3 The same), more preferably an alkyl group having 1 to 10 carbon atoms (particularly 1 to 5).
[0091] In formula (1C), from the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, R 2 and R 3 The following groups are preferred. 2 is an alkyl group having 1 to 10 carbon atoms, preferably an alkyl group having 1 to 5 carbon atoms. 2 As for the alkyl group of R, there can be mentioned 1 The alkyl group of R is the same as the alkyl group of 3 It is an alkoxy group having 1 to 30 carbon atoms or an alkenyloxy group having 1 to 30 carbon atoms, preferably an alkoxy group having 10 to 30 carbon atoms (particularly 14 to 24 carbon atoms) or an alkenyloxy group having 10 to 30 carbon atoms (particularly 14 to 24 carbon atoms). 3 For the alkoxy group, for example, the formula: -OC p H 2p+1 (wherein p is an integer from 1 to 30). 3 For the alkenyloxy group, for example, the formula: -OC q H 2q-1(wherein q is an integer of 1 to 30).
[0092] Specific examples of the compound (1C) represented by the general formula are shown in the following table.
[0093]
Table 1C
[0094] Specific examples of compound (1C)
[0095] Compound <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> 1C-1 Isopropyl Isopropyl Isopropyl 1C-2 sec-butyl sec-butyl sec-butyl 1C-3 Ethyl Ethyl Ethyl 1C-4 methyl methyl methyl 1C-5 Isopropyl Isopropyl <![CDATA[-C(CH3)=CH-CO-C 18 H 35 ]]> 1C-6 Isopropyl Isopropyl <![CDATA[-C(CH3)=CH-CO-C 18 H 37 ]]> 1C-7 sec-butyl sec-butyl <![CDATA[-C(CH3)=CH-CO-C 18 H 35 ]]> 1C-8 sec-butyl sec-butyl <![CDATA[-C(CH3)=CH-CO-C 18 H 37 ]]> 1C-9 Ethyl Ethyl <![CDATA[-C(CH3)=CH-CO-C 18 H 35 ]]> 1C-10 Ethyl Ethyl <![CDATA[-C(CH3)=CH-CO-C 18 H 37 ]]> 1C-11 methyl methyl <![CDATA[-C(CH3)=CH-CO-C 18 H 35 ]]> 1C-12 methyl methyl <![CDATA[-C(CH3)=CH-CO-C 18 H 37 ]]>
[0096]
Chemical formula 1D
[0097] Zr(OR 1 )4 (1D)
[0098] In formula (1D), R 1 are independently the same as R in formula (1) 1 Same R 1 From the perspective of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, R 1 Each independently is preferably an alkyl group having 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms.
[0099] Specific examples of the compound (1D) represented by the general formula are shown in the following table.
[0100]
Table 1D
[0101] Specific examples of compound (1D)
[0102] Compound <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> <![CDATA[R 1 ]]> 1D-1 Isopropyl Isopropyl Isopropyl Isopropyl 1D-2 Butyl Butyl Butyl Butyl 1D-3 Ethyl Ethyl Ethyl Ethyl 1D-4 methyl methyl methyl methyl
[0103] The compound (1) represented by the general formula (1) can also be obtained as a commercial product or can be produced by a known method.
[0104] For example, compound (1A) can be obtained as a commercial product, tetraethyl orthosilicate (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0105] For another example, compound (1B) can be obtained as commercially available products such as tetrabutyl orthotitanate (manufactured by Tokyo Chemical Industry Co., Ltd.) and T-50 (manufactured by Nippon Soda Co., Ltd.).
[0106] For another example, compound (1B') can be obtained as a commercial product TOG (manufactured by Nippon Soda Co., Ltd.).
[0107] For another example, compound (1C) can be obtained as a commercial product, aluminum triisopropoxide (manufactured by Kanto Chemical Co., Ltd.).
[0108] For another example, compound (1D) can be obtained as commercially available products such as zirconium (IV) tetrabutoxide (trade name: TBZR, manufactured by Nippon Soda Co., Ltd.) and ZR-181 (manufactured by Nippon Soda Co., Ltd.).
[0109] The content of the first metal alkoxide in the coating 2 (i.e., the reactant constituting the coating) is usually 5% by weight or more and 85% by weight or less relative to its total weight (e.g., the total weight of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide). From the perspective of further improving the cycle characteristics, filling properties, and load characteristics of the positive electrode active material, it is preferably 5% by weight or more and 70% by weight or less, more preferably 5% by weight or more and 60% by weight or less, and further preferably 5% by weight or more and 55% by weight or less. The coating may include two or more first metal alkoxides, in which case their total amount is within the above range. The content of the first metal alkoxide in the coating 2 is the ratio of the amount of the first metal alkoxide to the total amount of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide.
[0110] The second metal alkoxide is a metal alkoxide containing two or more (for example, two or more and less than 20, in particular, two or more and less than 12) metal atom-carbon atom bonds in one molecule. In the second metal alkoxide, the carbon atoms constituting the two or more metal atom-carbon atom bonds are carbon atoms constituting a monovalent hydrocarbon group (for example, an alkyl group and an alkenyl group) and / or carbon atoms constituting a divalent hydrocarbon group (for example, an alkylene group). In the second metal alkoxide, from the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, the carbon atoms constituting all of the two or more metal atom-carbon atom bonds are preferably carbon atoms constituting a divalent hydrocarbon group (for example, an alkylene group). The metal atom of the second metal alkoxide is silicon. The second metal alkoxide contains two or more such metal atom-carbon atom bonds in one molecule. Therefore, the second metal alkoxide prevents the formation of a tight mesh structure and forms a coating 2 by a mesh structure of moderate thickness with flexibility. Specifically, for example, in the case where the carbon atom constituting the metal atom-carbon atom bond in the second metal alkoxide is a carbon atom constituting a divalent hydrocarbon group (e.g., an alkylene group), the "flexibility" and "appropriate thickness" of the coating 2 are considered to be as follows: Figure 3 As shown, it is based on the divalent hydrocarbon group 30 possessed by the second metal alkoxide. For another example, in the second metal alkoxide, when the carbon atom constituting the metal atom-carbon atom bond is a carbon atom constituting a monovalent hydrocarbon group (for example, an alkyl group and an alkenyl group), the second metal alkoxide promotes the formation of the end of the metal atom-oxygen atom skeleton (for example, a polysiloxane skeleton), and it is believed that the "moderate coarseness" of the coating 2 is based on the monovalent hydrocarbon group possessed by the second metal alkoxide. As a result, it is believed that the ion conductivity of the ions (especially lithium ions) responsible for electron donation and acceptance in the positive electrode active material of the present invention is sufficiently improved when passing through the coating. In the case where the coating does not contain the second metal alkoxide, for example Figure 5As shown, the film forms a relatively dense mesh structure, resulting in reduced cycle characteristics and ion conductivity. Figure 3 This is an example of a schematic conceptual diagram showing the main structure of the organic-inorganic hybrid film in the positive electrode active material of the present invention (particularly the present inventions A and B). Figure 3 This is a schematic conceptual diagram showing the main structure of an organic-inorganic hybrid film when 1,2-bis(triethoxysilyl)ethane (BTESE) is used as the second metal alkoxide. Figure 5 1 is a schematic conceptual diagram showing the main structure of a coating on the surface of a positive electrode active material in the related art.
[0111] When the carbon atom constituting the metal atom-carbon atom bond in the second metal alkoxide is a carbon atom constituting a divalent hydrocarbon group, the second metal alkoxide is a compound having two or more trialkoxysilyl groups represented by the following general formula (2) in one molecule.
[0112]
Chemical formula 2
[0113] -Si(OR 21 )3 (2)
[0114] In formula (2), R 21 Each independently represents an alkyl group having 1 to 10 carbon atoms. From the viewpoint of further improving the cycle characteristics, filling properties, and load characteristics of the positive electrode active material, an alkyl group having 1 to 5 carbon atoms is preferred, and an alkyl group having 1 to 3 carbon atoms is more preferred. Examples of such alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl. 21 , all R 21 Can be independently selected from the above alkyl groups, or all R 21 The alkyl groups may be the same as each other and are selected from the above-mentioned alkyl groups.
[0115] The trialkoxysilyl groups contained in the second metal alkoxide may be independently selected from the trialkoxysilyl groups of the above general formula (2), or may be the same groups.
[0116] Specific examples of the trialkoxysilyl group represented by the general formula (2) are shown in the following table.
[0117]
Table 2
[0118] Specific examples of the group of general formula (2)
[0119] Group <![CDATA[R 21 ]]> <![CDATA[R 21 ]]> <![CDATA[R 21 ]]> 2A-1 methyl methyl methyl 2A-2 Ethyl Ethyl Ethyl 2A-3 Isopropyl Isopropyl Isopropyl 2A-4 Butyl Butyl Butyl
[0120] In the case where the carbon atoms constituting two or more of all metal atom-carbon atom bonds in the second metal alkoxide are carbon atoms constituting a divalent hydrocarbon group, the second metal alkoxide may be, for example, a compound represented by the following general formula (2A), (2B), (2C), (2E) or (2F) or a mixture thereof. Among them, from the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, the second metal alkoxide is preferably a compound represented by the general formula (2A), (2B) or (2C) or a mixture thereof, more preferably a compound represented by the general formula (2A) or (2B) or a mixture thereof, and further preferably a compound represented by the general formula (2A).
[0121] When all of the carbon atoms constituting two or more metal atom-carbon atom bonds in the second metal alkoxide are carbon atoms constituting a monovalent hydrocarbon group, the second metal alkoxide may be, for example, a compound represented by the following general formula (2D) or a mixture thereof.
[0122]
Chemical formula 2A
[0123] (R 211 O)3Si-R 31 -Si(OR 212 )3 (2A)
[0124] In formula (2A), R 211 and R 212 are independently the same as R in formula (2) 21 Specifically, the three R 211 and the three Rs 212 Each of the three R is independently an alkyl group having 1 to 10 carbon atoms, and is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 211 and the three Rs 212 R can be independently selected from the above general formula (2): 21 , or may be the same groups as each other.
[0125] R 31 It is a divalent hydrocarbon group having 1 to 20 carbon atoms, and is preferably a divalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a divalent hydrocarbon group having 2 to 8 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 31 The divalent hydrocarbon group of R may be a divalent saturated aliphatic hydrocarbon group (e.g., an alkylene group), or may be a divalent unsaturated aliphatic hydrocarbon group (e.g., an alkenylene group). 31The divalent hydrocarbon group is preferably a divalent saturated aliphatic hydrocarbon group (especially an alkylene group). 31 As for the divalent saturated aliphatic hydrocarbon group (especially alkylene group), for example, -(CH2) p - (wherein p is an integer of 1 to 10, more preferably 2 to 8), etc.
[0126] Specific examples of the compound (2A) represented by the general formula are shown in the following table.
[0127]
Table 2A
[0128] Specific examples of compound (2A)
[0129] Compound <![CDATA[R 211 ]]> <![CDATA[R 211 ]]> <![CDATA[R 211 ]]> <![CDATA[R 31 ]]> <![CDATA[R 212 ]]> <![CDATA[R 212 ]]> <![CDATA[R 212 ]]> 2A-1 methyl methyl methyl <![CDATA[-CH2CH2-]]> methyl methyl methyl 2A-2 methyl methyl methyl <![CDATA[-CH2CH2CH2CH2CH2CH2-]]> methyl methyl methyl 2A-3 Ethyl Ethyl Ethyl <![CDATA[-CH2CH2-]]> Ethyl Ethyl Ethyl 2A-4 Ethyl Ethyl Ethyl <![CDATA[-CH2CH2CH2CH2CH2CH2-]]> Ethyl Ethyl Ethyl
[0130]
Chemical formula 2B
[0131]
[0132] In formula (2B), R 211 , R 212 , R 213 and R 214 is the same as R in formula (2) 21 Specifically, the three R 211 , Three Rs 212 , Three Rs 213 and the three Rs 214 Each of the three R is independently an alkyl group having 1 to 10 carbon atoms, and is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 211 , Three Rs 212 , Three Rs 213 and the three Rs 214 R can be independently selected from the above general formula (2): 21 , or may be the same groups as each other.
[0133] R 32 Each of R is independently a divalent hydrocarbon group having 1 to 20 carbon atoms, and is preferably a divalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a divalent hydrocarbon group having 6 to 10 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 32 The divalent hydrocarbon group of R may be a divalent saturated aliphatic hydrocarbon group (e.g., an alkylene group), or may be a divalent unsaturated aliphatic hydrocarbon group (e.g., an alkenylene group). 32The divalent hydrocarbon group is preferably a divalent saturated aliphatic hydrocarbon group (especially an alkylene group). 32 As for the divalent saturated aliphatic hydrocarbon group (especially alkylene group), for example: -(CH2) q - (wherein q is an integer of 1 to 10, more preferably an integer of 6 to 10). All R 32 can be independently selected from the R 32 , or may be the same groups as each other.
[0134] R 33 Each of R is independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, and is preferably a monovalent hydrocarbon group having 1 to 5 carbon atoms, and more preferably a monovalent hydrocarbon group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 33 The monovalent hydrocarbon group of R may be a saturated aliphatic hydrocarbon group (e.g., an alkyl group) or an unsaturated aliphatic hydrocarbon group (e.g., an alkenyl group). 33 The monovalent hydrocarbon group is preferably a saturated aliphatic hydrocarbon group (particularly an alkyl group). 33 As for the monovalent saturated aliphatic hydrocarbon group (especially alkyl), for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, etc. can be mentioned. All R 33 can be independently selected from the R 33 , or may be the same groups as each other.
[0135] Specific examples of the compound (2B) represented by the general formula are shown in the following table.
[0136]
Table 2B
[0137] Specific examples of compound (2B)
[0138]
[0139]
Chemical formula 2C
[0140] (R 211 O)3Si-R 34 -NH-R 35 -NH-R 36 -Si(OR 212 )3 (2C)
[0141] In formula (2C), R 211 and R 212 is the same as R in formula (2) 21 Specifically, the three R211 , and three R 212 Each of the three R is independently an alkyl group having 1 to 10 carbon atoms, and is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 211 and the three Rs 212 R can be independently selected from the above general formula (2): 21 , or may be the same groups as each other.
[0142] R 34 , R 35 , and R 36 Each of R is independently a divalent hydrocarbon group having 1 to 10 carbon atoms, and preferably a divalent hydrocarbon group having 1 to 5 carbon atoms from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 34 , R 35 , and R 36 The divalent hydrocarbon group of R may be a divalent saturated aliphatic hydrocarbon group (e.g., an alkylene group), or may be a divalent unsaturated aliphatic hydrocarbon group (e.g., an alkenylene group). 34 , R 35 , and R 36 The divalent hydrocarbon group is preferably a divalent saturated aliphatic hydrocarbon group (especially an alkylene group). 34 , R 35 and R 36 As for the divalent saturated aliphatic hydrocarbon group (especially alkylene group), for example, -(CH2) r - (wherein r is an integer of 1 to 10, more preferably an integer of 1 to 5). All R 34 , R 35 , and R 36 The above divalent hydrocarbon groups may be independently selected from the above divalent hydrocarbon groups, or may be the same group. From the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, R 34 , R 35 , and R 36 The total number of carbon atoms is preferably 3-20, more preferably 6-10.
[0143] Specific examples of the compound (2C) represented by the general formula are shown in the following table.
[0144]
Table 2C
[0145] Specific examples of compound (2C)
[0146]
[0147]
Chemical Formula 2D
[0148] (R 211 )2-Si(OR 212 )2 (2D)
[0149] In formula (2D), R 211 and R 212 are independently the same as R in formula (2) 21 Specifically, the two R 211 and two R 212 Each independently represents an alkyl group having 1 to 10 carbon atoms, and preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 211 and two R 212 R can be independently selected from the above general formula (2): 21 , or may be the same groups as each other.
[0150] Specific examples of the compound (2D) represented by the general formula are shown in the following table.
[0151]
Table 2D
[0152] Specific examples of compound (2D)
[0153] Compound <![CDATA[Two Rs 211 > <![CDATA[Two Rs 212 <!-- 12 -->]]> 2D-1 methyl methyl 2D-2 methyl Ethyl
[0154]
Chemical formula 2E
[0155]
[0156] In formula (2E), R 212 and R 213 is the same as R in formula (2) 21 Specifically, the three R 212 and the three Rs 213 Each of the three R is independently an alkyl group having 1 to 10 carbon atoms, and is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 212 and the three Rs 213 R can be independently selected from the above general formula (2): 21 , or may be the same groups as each other.
[0157] R 32Each of R is independently a divalent hydrocarbon group having 1 to 20 carbon atoms, and is preferably a divalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a divalent hydrocarbon group having 4 to 8 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 32 The divalent hydrocarbon group of R may be a divalent saturated aliphatic hydrocarbon group (e.g., an alkylene group), or may be a divalent unsaturated aliphatic hydrocarbon group (e.g., an alkenylene group). 32 The divalent hydrocarbon group is preferably a divalent saturated aliphatic hydrocarbon group (especially an alkylene group). 32 As for the divalent saturated aliphatic hydrocarbon group (especially alkylene group), for example: -(CH2) q - (wherein q is an integer of 1 to 20, preferably 1 to 10, and more preferably 4 to 8). All R 32 can be independently selected from the R 32 , or may be the same groups as each other.
[0158] R 33 Each of R is independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, and is preferably a monovalent hydrocarbon group having 1 to 5 carbon atoms, and more preferably a monovalent hydrocarbon group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 33 The monovalent hydrocarbon group of R may be a saturated aliphatic hydrocarbon group (e.g., an alkyl group) or an unsaturated aliphatic hydrocarbon group (e.g., an alkenyl group). 33 The monovalent hydrocarbon group is preferably a saturated aliphatic hydrocarbon group (particularly an alkyl group). 33 As for the monovalent saturated aliphatic hydrocarbon group (especially alkyl), for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, etc. can be mentioned. All R 33 can be independently selected from the R 33 , or may be the same group as each other.
[0159] R 34 Each of R is independently a monovalent hydrocarbon group having 1 to 30 carbon atoms, and is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a monovalent hydrocarbon group having 1 to 5 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 34The monovalent hydrocarbon group of R may be a saturated aliphatic hydrocarbon group (e.g., an alkyl group) or an unsaturated aliphatic hydrocarbon group (e.g., an alkenyl group). 34 The monovalent hydrocarbon group is preferably a saturated aliphatic hydrocarbon group (particularly an alkyl group). 34 As for the monovalent saturated aliphatic hydrocarbon group (especially alkyl), for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, etc. All R 34 can be independently selected from the R 34 , or may be the same group as each other.
[0160] Specific examples of the compound (2E) represented by the general formula are shown in the following table.
[0161]
Table 2E
[0162] Specific examples of compound (2E)
[0163] Compound <![CDATA[Three Rs 212 and three Rs 213 > <![CDATA[Two Rs 32 > <![CDATA[Four Rs 33 > <![CDATA[Two Rs 34 > 2E-1 methyl <![CDATA[-CH2CH2CH2CH2CH2CH2-]]> methyl Ethyl 2E-2 Ethyl <![CDATA[-CH2CH2CH2CH2CH2CH2-]]> methyl Ethyl
[0164]
Chemical formula 2F
[0165]
[0166] In formula (2F), R 212 , R 213 and R 214 are independently the same as R in formula (2) 21 Specifically, the three R 212 , Three Rs 213 and the three Rs 214 Each of the three R is independently an alkyl group having 1 to 10 carbon atoms, and is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading properties of the positive electrode active material. 212 , Three Rs 213 and the three Rs 214 R can be independently selected from the above general formula (2): 21 , or may be the same groups as each other.
[0167] R 32Each of R is independently a divalent hydrocarbon group having 1 to 20 carbon atoms, and is preferably a divalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a divalent hydrocarbon group having 1 to 5 carbon atoms, from the viewpoint of further improving the cycle characteristics, filling properties, and loading characteristics of the positive electrode active material. 32 The divalent hydrocarbon group of R may be a divalent saturated aliphatic hydrocarbon group (e.g., an alkylene group), or may be a divalent unsaturated aliphatic hydrocarbon group (e.g., an alkenylene group). 32 The divalent hydrocarbon group is preferably a divalent saturated aliphatic hydrocarbon group (especially an alkylene group). 32 As for the divalent saturated aliphatic hydrocarbon group (especially alkylene group), for example, -(CH2) q - (wherein q is an integer of 1 to 10, more preferably an integer of 1 to 5). All R 32 can be independently selected from the R 32 , or may be the same groups as each other.
[0168] Specific examples of the compound (2F) represented by the general formula are shown in the following table.
[0169]
Table 2F
[0170] Specific examples of compound (2F)
[0171] Compound <![CDATA[Three Rs 212 > <![CDATA[Three Rs 213 > <![CDATA[Three Rs 214 > <![CDATA[Three Rs 32 > 2F-1 methyl methyl methyl <![CDATA[-CH2CH2CH2-]]> 2F-2 Ethyl Ethyl Ethyl <![CDATA[-CH2CH2CH2-]]>
[0172] Compound (2A) represented by general formula (2A), compound (2B) represented by general formula (2B), compound (2C) represented by general formula (2C), compound (2D) represented by general formula (2D), compound (2E) represented by general formula (2E) and compound (2F) represented by general formula (2F) can be obtained as commercial products or can also be produced by a known method.
[0173] For example, compound (2A) can be obtained as commercially available products such as 1,2-bis(trimethoxysilyl)ethane (manufactured by Tokyo Chemical Industry Co., Ltd.) and 1,6-bis(trimethoxysilyl)hexane (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0174] For another example, compound (2C) can be obtained as a commercial product X-12-5263HP (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0175] For another example, compound (2D) can be obtained as a commercial product, dimethyldimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0176] For another example, compound (2F) can be obtained as a commercial product, tris[3-(trimethoxysilyl)-propyl]isocyanurate (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0177] The second metal alkoxide may be, for example, a compound represented by the general formula (2A), (2B), (2C), (2D), (2E) or (2F) or a mixture thereof. From the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, the second metal alkoxide is preferably a compound represented by the general formula (2A), (2B), (2C) or (2D) or a mixture thereof, and more preferably a compound represented by the general formula (2A) or (2D) or a mixture thereof.
[0178] The content of the second metal alkoxide in the coating 2 (i.e., the reactant constituting the coating) is usually 1% by weight or more and 85% by weight or less relative to its total weight (e.g., the total weight of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide). From the perspective of further improving the cycle characteristics, filling properties, and load characteristics of the positive electrode active material, it is preferably 1% by weight or more and 80% by weight or less, more preferably 1% by weight or more and 60% by weight or less, further preferably 1% by weight or more and 50% by weight or less, and particularly preferably 7% by weight or more and 36% by weight or less. The coating may also include two or more second metal alkoxides, in which case their total amount is as long as it is within the above range. The content of the second metal alkoxide in the coating 2 can be the ratio of the amount of the second metal alkoxide to the total weight of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide.
[0179] The third metal alkoxide is a metal alkoxide containing only one metal atom-carbon atom bond in one molecule, for example, one of the bonds possessed by the metal is connected to a monovalent hydrocarbon group (-R 12 ) bond, and all remaining bonds are connected to alkoxy (-OR 11 ) bonded alkoxide compound. In the third metal alkoxide, the metal atom-carbon atom bond refers to a direct covalent bond between a metal atom and a carbon atom. In the third metal alkoxide, the carbon atom constituting the metal atom-carbon atom bond is a carbon atom constituting a monovalent hydrocarbon group (for example, an alkyl group and an alkenyl group). The third metal alkoxide contains only one such metal atom-carbon atom bond in one molecule. The metal atom of the third metal alkoxide is silicon. The third metal alkoxide reduces the surface free energy of the coating 2 and gives the surface of the coating 2 more sufficient lubricity. Figure 4 As shown, such sufficient lubricity is believed to be based on the monovalent hydrocarbon group 20 of the third metal alkoxide. Therefore, the positive electrode active material of the present invention has more sufficiently excellent filling properties, and the ion conductivity of ions (especially lithium ions) responsible for electron transfer when passing through the film is sufficiently improved. Figure 4 This is a schematic conceptual diagram showing the main surface state of the organic-inorganic hybrid film in the positive electrode active material of the present invention.
[0180] Specifically, the third metal alkoxide is a compound represented by the following general formula (3).
[0181]
Chemical formula 3
[0182] R 12 -Si(OR 11 )3 (3)
[0183] In formula (3), R 11 Each independently represents an alkyl group having 1 to 10 carbon atoms. From the viewpoint of further improving the filling property and loading characteristics of the positive electrode active material, an alkyl group having 1 to 5 carbon atoms is preferred, and an alkyl group having 1 to 3 carbon atoms is more preferred. Examples of such alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl. All R 11 can be independently selected from the above alkyl groups, or all R 11 The alkyl groups may be the same as each other and are selected from the above-mentioned alkyl groups.
[0184] R 12 It is a monovalent hydrocarbon group having 8 to 30 carbon atoms, preferably a monovalent hydrocarbon group having 12 to 24 carbon atoms, and more preferably a monovalent hydrocarbon group having 14 to 20 carbon atoms, from the viewpoint of further improving the packing property and loading characteristics of the positive electrode active material. 12 The monovalent hydrocarbon group of R may be a saturated aliphatic hydrocarbon group (e.g., an alkyl group) or an unsaturated aliphatic hydrocarbon group (e.g., an alkenyl group). 12 The monovalent hydrocarbon group is preferably a saturated aliphatic hydrocarbon group (particularly an alkyl group). 12 As for the monovalent saturated aliphatic hydrocarbon group (particularly alkyl), for example, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl and the like are mentioned.
[0185] Specific examples of the compound (3) represented by the general formula are shown in the following table.
[0186]
Table 3
[0187] Specific examples of compound (3)
[0188] Compound <![CDATA[R 12 ]]> <![CDATA[R 11 ]]> <![CDATA[R 11 ]]> <![CDATA[R 11 ]]> 3A-1 Octadecyl methyl methyl methyl 3A-2 Hexadecyl methyl methyl methyl 3A-3 Decyl methyl methyl methyl 3A-4 Octadecyl Ethyl Ethyl Ethyl 3A-5 Hexadecyl Ethyl Ethyl Ethyl 3A-6 Decyl Ethyl Ethyl Ethyl
[0189] The compound (3) represented by the general formula (3) can be obtained as a commercial product or can be produced by a known method.
[0190] For example, compound (3) can be obtained as commercially available products such as octadecyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.), hexadecyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.), and decyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0191] The content of the third metal alkoxide in the coating 2 (i.e., the reactant constituting the coating) is usually 0% by weight or more and 90% by weight or less relative to its total weight (e.g., the total weight of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide), and is preferably 5% by weight or more and 90% by weight or less from the viewpoint of improving the filling and load characteristics of the positive electrode active material. From the viewpoint of further improving the cycle characteristics, filling and load characteristics of the positive electrode active material, the content of the third metal alkoxide is preferably 20% by weight or more and 90% by weight or less relative to its total weight, more preferably 25% by weight or more and 90% by weight or less, further preferably 28% by weight or more and 90% by weight or less, and particularly preferably 28% by weight or more and 80% by weight or less. The coating may also include two or more third metal alkoxides, in which case their total amount is within the above range. The content of the third metal alkoxide may also be 0% by weight. This means that the present invention (especially the present invention A) may or may not include a third metal alkoxide. The content of the third metal alkoxide in the coating 2 may be a ratio of the amount of the third metal alkoxide blended to the total amount of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide blended.
[0192] The content of the coating 2 on the positive electrode active material 10 is usually 0.010 wt % or more and 2.000 wt % or less relative to the total weight of the positive electrode active material 10 (i.e., the total amount of the positive electrode active material core material and the coating). From the perspective of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, it is preferably 0.020 wt % or more and 1.500 wt % or less, more preferably 0.080 wt % or more and 1.000 wt % or less, further preferably 0.050 wt % or more and 0.400 wt % or less, and particularly preferably 0.070 wt % or more and 0.400 wt % or less. It should be pointed out that when calculating the content, it can be calculated as a substance in which all the alkoxides contained in the metal alkoxide undergo a dehydration condensation reaction, and the reactant with no other structure change. For example, the weight of the reactant obtained by dehydration condensation reaction of all the alkoxides contained in 1 g of 1,2-bis(trimethoxysilyl)ethane is 0.49 g. The content of the coating 2 may be the ratio of the total amount of the first metal alkoxide, the second metal alkoxide, and the third metal alkoxide constituting the coating 2 to the total weight of the positive electrode active material (ie, the total amount of the positive electrode active material core material weight and the total amount).
[0193] The positive electrode active material of the present invention can be manufactured by a method including stirring the positive electrode active material core material with a specified metal alkoxide in an alkaline solvent. The specified metal alkoxide refers to a metal alkoxide mixture containing at least a first metal alkoxide and a second metal alkoxide in the present invention A, and a metal alkoxide mixture containing at least a first metal alkoxide, a second metal alkoxide and a third metal alkoxide in the present invention B. After stirring, the positive electrode active material core material is carefully filtered and cleaned, and heated and dried, thereby obtaining a positive electrode active material formed by a film with a mesh structure formed on the surface of the positive electrode active material core material. It should be pointed out that as a covering method, as long as it can cover the active material core material, it is not limited to the above method, and can also be carried out by coating methods such as spraying and dry mixing.
[0194] The mixing ratio (ie, usage ratio) of the first metal alkoxide, the third metal alkoxide, and the second metal alkoxide is usually directly used as the content ratio of each metal alkoxide in the film, and therefore, a mixing ratio corresponding to the desired content ratio may be adopted.
[0195] The amount of the first metal alkoxide added is usually 0.001 parts by weight or more and 8 parts by weight or less relative to 100 parts by weight of the positive electrode active material core material. From the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, it is preferably 0.005 parts by weight or more and 5 parts by weight or less, more preferably 0.015 parts by weight or more and 0.80 parts by weight or less, and further preferably 0.015 parts by weight or more and 0.50 parts by weight or less.
[0196] The amount of the second metal alkoxide added is usually not less than 0.001 parts by weight and not more than 5 parts by weight relative to 100 parts by weight of the positive electrode active material core material. From the viewpoint of further improving the cycle characteristics, filling properties and loading characteristics of the positive electrode active material, it is preferably not less than 0.005 parts by weight and not more than 3 parts by weight, more preferably not less than 0.015 parts by weight and not more than 1.00 parts by weight, and further preferably not less than 0.015 parts by weight and not more than 0.50 parts by weight.
[0197] The amount of the third metal alkoxide is usually 0 parts by weight or more and 10 parts by weight or less relative to 100 parts by weight of the positive electrode active material core material. From the viewpoint of improving the filling and loading characteristics of the positive electrode active material, it is preferably 0.001 parts by weight or more and 10 parts by weight or less. From the viewpoint of further improving the cycle characteristics, filling and loading characteristics of the positive electrode active material, it is preferably 0.01 parts by weight or more and 10 parts by weight or less, more preferably 0.015 parts by weight or more and 5 parts by weight or less, further preferably 0.05 parts by weight or more and 1.00 parts by weight or less, and further preferably 0.05 parts by weight or more and 0.50 parts by weight or less. The amount of the third metal alkoxide may also be 0 parts by weight. This means that the present invention (especially the present invention A) may or may not contain a third metal alkoxide.
[0198] As long as a coating is formed on the surface of the positive electrode active material core material, the total amount of the first metal alkoxide, the second metal alkoxide and the third metal alkoxide is not particularly limited. For example, it is 0.02 parts by weight or more and 15 parts by weight or less relative to 100 parts by weight of the positive electrode active material core material. From the perspective of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, it is preferably 0.02 parts by weight or more and 5 parts by weight or less, and more preferably 0.05 parts by weight or more and 2 parts by weight or less. By adjusting the total amount, the coating amount of the coating 2 on the positive electrode active material 10 can be controlled. The more the total amount, the more the coating amount.
[0199] As a solvent, as long as it does not hinder the reaction of each metal alkoxide such as the first metal alkoxide, the second metal alkoxide and the third metal alkoxide, it is not particularly limited, and preferably, for example, monoalcohols, ethers, glycols or glycol ethers. In a preferred embodiment, the solvent can be: monoalcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, 1-pentanol, 2-pentanol, 2-methyl-2-pentanol; ethers such as 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol; glycol ethers such as dipropylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, or diethylene glycol monohexyl ether. The preferred solvent is a monoalcohol. In addition, water may be included as needed. The above solvents may be used only one, or two or more may be used. The solvent may contain various additives, such as catalysts, pH adjusters, stabilizers, thickeners, etc. As the above-mentioned additives, for example, acid compounds such as boric acid compounds, alkaline compounds such as ammonia compounds, etc. can be listed. As the amount of the solvent, as long as each metal alkoxide can be uniformly present on the surface of the positive electrode active material core material, it is not particularly limited. For example, it can be more than 20 parts by weight and less than 200 parts by weight, especially more than 30 parts by weight and less than 150 parts by weight, relative to 100 parts by weight of the positive electrode active material core material.
[0200] The temperature of the mixture during stirring is not particularly limited as long as each metal alkoxide can be uniformly present on the surface of the positive electrode active material core, and is, for example, 10° C. to 70° C., preferably 15° C. to 35° C.
[0201] The stirring time is not particularly limited as long as each metal alkoxide can be uniformly present on the surface of the positive electrode active material core material, and is, for example, 10 minutes to 5 hours, preferably 30 minutes to 3 hours.
[0202] Washing is performed to remove the remaining catalyst. For example, it is performed by contacting the filtration residue with a washing solvent. The washing solvent is not particularly limited and may be, for example, acetone.
[0203] The solvent used in the cleaning is removed by heating and drying. The heating temperature is usually 15° C. or more (especially 15° C. or more and 250° C. or less), preferably 15° C. or more and 200° C. or less from the viewpoint of removing the solvent. The heating time is usually 30 minutes or more (especially 30 minutes or more and 24 hours or less), preferably 60 minutes or more and 12 hours or less from the viewpoint of removing the solvent.
[0204] [positive electrode]
[0205] The positive electrode of the present invention is composed of at least a positive electrode layer and a positive electrode collector (foil), and the positive electrode layer contains the above-mentioned covered positive electrode active material. The above-mentioned covered positive electrode active material of the positive electrode layer is composed of, for example, granules, and in order for the particles to fully contact each other and maintain their shape, it is preferred that the positive electrode layer contains a binder. In order to facilitate the smooth transfer of electrons that promote the battery reaction, it is preferred that the positive electrode layer contains a conductive aid. In this way, since it is in a form containing multiple components, the positive electrode layer can also be called a "positive electrode composite layer" or the like.
[0206] The content of the positive electrode active material in the positive electrode layer is usually 50% by weight or more and 95% by weight or less relative to the total weight of the positive electrode layer. From the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, it is preferably 70% by weight or more and 95% by weight or less, more preferably 85% by weight or more and 98% by weight or less, and further preferably 85% by weight or more and 95% by weight or less.
[0207] The positive electrode layer may include the positive electrode active material of the prior art together with the above-mentioned covered positive electrode active material. In the case where the positive electrode layer includes the positive electrode active material of the prior art together with the above-mentioned covered positive electrode active material, the content of the above-mentioned positive electrode active material is the content of all positive electrode active materials. In this case, the covered positive electrode active material generally contains more than 50% by weight, preferably more than 70% by weight, and more preferably more than 90% by weight relative to all positive electrode active materials. The positive electrode active material of the prior art is, for example, a substance that contributes to the adsorption and release of lithium ions. From this point of view, the positive electrode active material of the prior art is preferably, for example, a lithium-containing composite oxide. More specifically, the positive electrode active material of the prior art is preferably a lithium transition metal composite oxide containing lithium and at least one transition metal selected from the group consisting of cobalt, nickel, manganese and iron. For example, the positive electrode active material of the prior art may be a substance in which a portion of lithium cobaltate, lithium nickelate, lithium manganate, lithium iron phosphate or a portion of their transition metals are replaced by other metals.
[0208] The binder that can be included in the positive electrode layer is not particularly limited, and can include at least one selected from the group consisting of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, polytetrafluoroethylene, etc. In a more preferred embodiment, the binder of the positive electrode layer is polyvinylidene fluoride.
[0209] The content of the binder in the positive electrode layer is usually more than 1 weight % and less than 20 weight % relative to the total weight of the positive electrode layer. From the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, it is preferably more than 1 weight % and less than 10 weight %, more preferably more than 1 weight % and less than 8 weight %, and further preferably more than 2 weight % and less than 8 weight %.
[0210] There is no particular limitation on the conductive aid that can be included in the positive electrode layer, and examples thereof include carbon black such as thermal cracking black, furnace black, channel black, Ketjen black and acetylene black, carbon fibers such as graphite, carbon nanotubes and vapor-deposited carbon fibers, metal powders such as copper, nickel, aluminum and silver, and polyphenylene derivatives, etc. In a more preferred embodiment, the conductive aid of the positive electrode layer is carbon black (particularly Ketjen black).
[0211] In a further preferred embodiment, the binder and the conductive aid of the positive electrode layer are a combination of polyvinylidene fluoride and carbon black (particularly Ketjen black).
[0212] The content of the conductive aid in the positive electrode layer is usually 1% by weight or more and 20% by weight or less relative to the total weight of the positive electrode layer. From the viewpoint of further improving the cycle characteristics, filling properties and load characteristics of the positive electrode active material, it is preferably 1% by weight or more and 10% by weight or less, more preferably 1% by weight or more and 8% by weight or less, and further preferably 2% by weight or more and 8% by weight or less.
[0213] The thickness of the positive electrode layer is not particularly limited, and may be, for example, 1 μm to 300 μm, particularly 5 μm to 200 μm. The thickness of the positive electrode layer is the thickness inside the battery (particularly a secondary battery), and the average value of the measured values at any 50 locations is used.
[0214] The positive electrode current collector is a component that helps collect and provide electrons generated in the active material due to the battery reaction. Such a current collector can be a sheet-like metal component, or it can have a porous or perforated form. For example, the current collector can be a metal foil, a stamped metal, a mesh or a mesh iron, etc. The positive electrode current collector for the positive electrode is preferably composed of a metal foil containing at least one selected from the group consisting of aluminum, stainless steel and nickel, etc., for example, it can be aluminum foil.
[0215] In the positive electrode, a positive electrode layer may be provided on at least one side of the positive electrode collector. For example, the positive electrode may be provided with a positive electrode layer on both sides of the positive electrode collector, or may be provided with a positive electrode layer on one side of the positive electrode collector. From the viewpoint of further improving the capacity of the battery (particularly a secondary battery), a preferred positive electrode is provided with a positive electrode layer on both sides of the positive electrode collector.
[0216] For example, the positive electrode active material and the binder are mixed in a dispersion medium to prepare a positive electrode layer slurry, the positive electrode layer slurry is applied to a positive electrode current collector and dried, and then the coating is rolled and dried by a roll press or the like to obtain a positive electrode.
[0217] In the present invention, even if the rolling is carried out at a relatively low pressure, the positive electrode active material can be filled with a higher volume density in the positive electrode layer. The linear pressure during rolling can be, for example, 0.1 t / cm or more and 1.0 t / cm or less. From the viewpoint of further improving the cycle characteristics and filling properties of the positive electrode active material, and preventing the generation of cracks in the positive electrode active material, the unevenness on the positive electrode collector, the damage, and the peeling of the positive electrode layer from the collector, it is preferably 0.5 t / cm or more and 1.0 t / cm or less. The roller temperature is usually 100°C or more and 200°C or less. From the viewpoint of further improving the cycle characteristics and filling properties of the positive electrode active material, and preventing the generation of cracks in the positive electrode active material, the unevenness on the positive electrode collector, the damage, and the peeling of the positive electrode layer from the collector, it is preferably 110°C or more and 150°C or less. The pressing speed is usually above 1 m / min and below 20 m / min. From the perspective of further improving the cycle characteristics and filling properties of the positive electrode active material, and preventing the formation of cracks in the positive electrode active material, bumps and breakages on the positive electrode collector, and peeling of the positive electrode layer from the collector, it is preferably above 5 m / min and below 15 m / min.
[0218] [Battery]
[0219] The present invention provides batteries such as secondary batteries and primary batteries. In this specification, the term "secondary battery" refers to a battery that can be repeatedly charged and discharged. "Secondary battery" is not overly restricted to its name, and may also include "electrochemical devices" such as "power storage devices". The term "primary battery" refers to a battery that can only be discharged. The battery of the present invention is preferably a secondary battery.
[0220] The secondary battery of the present invention includes the above-mentioned positive electrode. The secondary battery of the present invention generally includes the above-mentioned positive electrode and negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte enclosed in an outer casing.
[0221] In the secondary battery of the present invention, the positive electrode, the negative electrode, and the separator disposed between the positive electrode and the negative electrode constitute an electrode assembly. In the secondary battery of the present invention, as long as the above-mentioned positive electrode (especially the above-mentioned positive electrode active material) is included, the electrode assembly can have any structure. Because no matter what structure the electrode assembly has, the effect of filling and load characteristics can be improved by the positive electrode active material. As the structure that the electrode assembly can have, for example: a stacked structure (planar stacked structure), a winding structure (Jelly Roll structure), or a stack-folded structure can be cited. In detail, for example, the electrode assembly can have a planar stacked structure in which one or more positive electrodes and one or more negative electrodes are stacked in a planar shape through a separator. For another example, the electrode assembly can have a winding structure (JellyRoll type) in which the positive electrode, the negative electrode, and the separator disposed between the positive electrode and the negative electrode are wound into a roll shape. For another example, the electrode assembly can have a so-called stack-folded structure in which the positive electrode, the separator, and the negative electrode are stacked on a longer film and then bent.
[0222] The negative electrode is composed of at least a negative electrode layer and a negative electrode collector (foil), and the negative electrode layer is provided on at least one side of the negative electrode collector. For example, the negative electrode may be provided with a negative electrode layer on both sides of the negative electrode collector, or may be provided with a negative electrode layer on one side of the negative electrode collector. From the viewpoint of further improving the capacity of the secondary battery, the preferred negative electrode is provided with a negative electrode layer on both sides of the negative electrode collector.
[0223] The negative electrode layer contains a negative electrode active material. The positive electrode active material contained in the above-mentioned positive electrode layer and the negative electrode active material contained in the negative electrode layer are substances that directly participate in electron transfer in the secondary battery, and are the main substances of the positive and negative electrodes responsible for charging and discharging, that is, battery reactions. More specifically, ions are provided to the electrolyte by the "positive electrode active material contained in the positive electrode layer" and the "negative electrode active material contained in the negative electrode layer", and the ions move between the positive electrode and the negative electrode to transfer electrons, thereby performing charging and discharging. The positive electrode and the negative electrode are preferably electrodes that can adsorb and release lithium ions, that is, the positive electrode layer and the negative electrode layer are preferably layers that can adsorb and release lithium ions. That is, a secondary battery is preferably one in which lithium ions move between the positive electrode and the negative electrode via the electrolyte to perform battery charging and discharging. When lithium ions participate in charging and discharging, the secondary battery of this embodiment is equivalent to a so-called "lithium ion battery".
[0224] The negative electrode active material of the negative electrode layer is composed of, for example, granules. In order to allow the particles to fully contact each other and maintain their shape, a binder is preferably included. In order to facilitate the smooth transfer of electrons that promote the battery reaction, a conductive additive may be included in the negative electrode layer. In this way, since it contains multiple components, the negative electrode layer can also be called a "negative electrode composite layer" or the like.
[0225] The negative electrode active material is preferably a material that contributes to the adsorption and release of lithium ions. From this viewpoint, the negative electrode active material is preferably, for example, various carbon materials, oxides, or lithium alloys.
[0226] As various carbon materials for negative electrode active materials, graphite (natural graphite, artificial graphite), hard carbon, soft carbon, diamond-like carbon, etc. can be listed. In particular, graphite has high electronic conductivity and excellent adhesion to the negative electrode collector, and is preferred in these aspects. As oxides for negative electrode active materials, at least one selected from the group consisting of silicon oxide, tin oxide, indium oxide, zinc oxide, and lithium oxide can be listed. The lithium alloy of the negative electrode active material can be any metal that can form an alloy with lithium, and can be, for example, a binary or ternary alloy of metals such as Al, Si, Pb, Sn, In, Bi, Ag, Ba, Ca, Hg, Pd, Pt, Te, Zn, La, and lithium. Such oxides are preferably formed in an amorphous structure. Therefore, degradation caused by inhomogeneities such as grain boundaries or defects will not occur. In a more preferred embodiment, the negative electrode active material of the negative electrode layer is artificial graphite.
[0227] As the binder that can be included in the negative electrode layer, there is no particular restriction, and at least one selected from the group consisting of styrene-butadiene rubber, polyacrylic acid, polyvinylidene fluoride, polyimide resin and polyamide-imide resin can be listed. In a more preferred embodiment, the binder contained in the negative electrode layer is styrene-butadiene rubber. As the conductive aid that can be included in the negative electrode layer, there is no particular restriction, and at least one selected from carbon black such as thermal cracking black, furnace black, channel black, ketjen black and acetylene black, carbon fibers such as graphite, carbon nanotubes and vapor-deposited carbon fibers, metal powders such as copper, nickel, aluminum and silver, and polyphenylene derivatives can be listed. It should be noted that the negative electrode layer may contain components brought by the thickener component (such as carboxymethyl cellulose) used in the manufacture of the battery.
[0228] In a further preferred embodiment, the negative electrode active material and the binder in the negative electrode layer are a combination of graphite and polyimide.
[0229] The thickness of the negative electrode layer is not particularly limited, and may be, for example, 1 μm to 300 μm, particularly 5 μm to 200 μm. The thickness of the negative electrode layer is the thickness inside the secondary battery, and the average value of the measured values at 50 arbitrary locations is used.
[0230] The negative electrode current collector for the negative electrode is a component that helps collect or provide electrons generated by the active material due to the battery reaction. Like the positive electrode current collector, the negative electrode current collector can be a sheet-like metal component, or it can have a porous or perforated form. For example, the negative electrode current collector can be a metal foil, a stamped metal, a mesh or a mesh iron, etc. The negative electrode current collector for the negative electrode is preferably composed of a metal foil selected from the group consisting of copper, stainless steel, nickel, etc., for example, it can be a copper foil.
[0231] The diaphragm is a component provided from the viewpoint of preventing the positive and negative electrodes from contacting each other and causing a short circuit and maintaining the electrolyte. In other words, the diaphragm can be considered as a component that prevents electronic contact between the positive electrode and the negative electrode while allowing ions to pass through. Preferably, the diaphragm is a porous or microporous insulating component that has a film form due to its small thickness. A microporous membrane made of polyolefin can be used as a diaphragm, but this is only an example. In this regard, the microporous membrane used as a diaphragm may, for example, only contain polyethylene (PE) or polypropylene (PP) as a polyolefin. In addition, the diaphragm may also be a laminate consisting of a "microporous membrane made of PE" and a "microporous membrane made of PP". The surface of the diaphragm may be covered with an inorganic particle coating layer and / or an adhesive layer. The surface of the diaphragm may have adhesiveness.
[0232] The thickness of the separator is not particularly limited and can be, for example, 1 μm to 100 μm, particularly 5 μm to 20 μm. The thickness of the separator is the thickness inside the secondary battery (particularly the thickness between the positive electrode and the negative electrode), and the average value of the measured values at any 50 locations is used.
[0233] The electrolyte helps the metal ions released from the electrodes (positive and negative electrodes) to move. The electrolyte can be a "non-aqueous" electrolyte such as an organic electrolyte and an organic solvent, or it can also be an "aqueous" electrolyte containing water. The secondary battery of the present invention is preferably a non-aqueous electrolyte secondary battery using an electrolyte containing a "non-aqueous" solvent and a solute as an electrolyte. The electrolyte can have a liquid or gel form (it should be noted that in this specification, a "liquid" non-aqueous electrolyte is also referred to as a "non-aqueous electrolyte solution").
[0234] As a specific non-aqueous electrolyte solvent, it is preferred that the solvent at least contains carbonate. The carbonate can be cyclic carbonate and / or chain carbonate. As cyclic carbonate, there is no particular limitation, and at least one of the group consisting of propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC) and vinylene carbonate (VC) can be cited. As chain carbonate, at least one of the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and dipropyl carbonate (DPC) can be cited. In a preferred embodiment of the present invention, a combination of cyclic carbonate and chain carbonate is used as a non-aqueous electrolyte, such as a mixture of ethylene carbonate and ethyl methyl carbonate.
[0235] As a specific solute of the non-aqueous electrolyte, it is preferable to use a Li salt such as LiPF6 and LiBF4.
[0236] The outer casing is not particularly limited, and may be, for example, a soft bag (soft bag body) or a hard case (hard outer casing).
[0237] In the case where the outer body is a soft bag, the soft bag is usually formed by a laminated film, and the sealing is achieved by heat-sealing the peripheral edge. The laminated film is usually a film formed by laminating a metal foil and a polymer film. Specifically, a three-layer structure film consisting of an outer polymer film / metal foil / inner polymer film is exemplified. The outer polymer film is used to prevent damage to the metal foil due to penetration and contact of moisture, etc., and polymers such as polyamide and polyester can be appropriately used. The metal foil is used to prevent the penetration of moisture and gas, and foils of copper, aluminum, stainless steel, etc. can be appropriately used. The inner polymer film is used to protect the metal foil from the influence of the electrolyte contained inside, and melt sealing is performed during heat sealing, and polyolefins (such as polypropylene) or acid-modified polyolefins can be appropriately used. The thickness of the laminated film is not particularly limited, and is preferably, for example, more than 1 μm and less than 1 mm.
[0238] When the outer body is a hard shell, the hard shell is usually formed of a metal plate, and the peripheral portion is laser irradiated to achieve sealing. As the metal plate, a metal material composed of aluminum, nickel, iron, copper, stainless steel, etc. is usually used. The thickness of the metal plate is not particularly limited, and is preferably, for example, 1 μm or more and 1 mm or less.
[0239] Example
[0240] <Positive electrode active material core material>
[0241] As a positive electrode active material core material, lithium cobalt oxide (LiCoO2) was prepared.
[0242] <First Metal Alkoxide>
[0243] As the first metal alkoxide, the following compound was prepared.
[0244] ■Tetraethoxysilane (corresponding to the compound (1A-1))
[0245] ■Tetrabutoxytitanium (corresponding to the compound (1B-1))
[0246] ■Aluminum triisopropoxide (corresponding to the compound (1C-1))
[0247] ■ Zirconium (IV) tetrabutoxide (corresponding to the compound (1D-2))
[0248] <Second Metal Alkoxide>
[0249] As the second metal alkoxide, the following compound was prepared.
[0250] ■The compound (2A-1)
[0251] ■The compound (2A-2)
[0252] ■The compound (2B-1)
[0253] ■The compound (2C-1)
[0254] ■The compound (2D-1)
[0255] <Third Metal Alkoxide>
[0256] As the third metal alkoxide, the following compound was prepared.
[0257] ■Octadecyltrimethoxysilane (corresponding to the compound (3A-1))
[0258] ■ Hexadecyltrimethoxysilane (corresponding to the compound (3A-2))
[0259] ■Decyltrimethoxysilane (corresponding to the compound (3A-3))
[0260] ■Hexyltrimethoxysilane (Comparative Example)
[0261] <Manufacturing of positive electrode active material>
[0262] (Example 1A)
[0263] Prepare 25g of ethanol dissolved with 6g of 28 wt% ammonia water. Add 35g of lithium cobalt oxide (average primary particle size 20μm) to the solution. Next, add the first metal alkoxide, the second metal alkoxide and the third metal alkoxide so that their usage reaches the ratio shown in Table 4 relative to 100 parts by weight of the added lithium cobalt oxide. Then, stir at room temperature (20°C) for 120 minutes. Filter the reaction solution, wash it with acetone, and dry the covered powder at 80°C for 120 minutes to form a coating (thickness 10nm) on the surface of the lithium cobalt oxide. This completes the preparation of lithium cobalt oxide (positive electrode active material) covered with an organic-inorganic hybrid film.
[0264] (Examples 2A to 5A, Examples 1B to 16B and Comparative Examples 1 to 5)
[0265] When manufacturing the positive electrode active material, the positive electrode active material was manufactured by the method similar to Example 1A except that the types and blending amounts of the first metal alkoxide, the second metal alkoxide and the third metal alkoxide were changed as shown in Table 4.
[0266] <Battery Manufacturing>
[0267] ■Positive electrode production process
[0268] The positive electrode is made as follows. First, 90% by weight of the positive electrode active material, 5% by weight of amorphous carbon powder (Ketjen black), and 5% by weight of polyvinylidene fluoride (PVdF) are mixed to prepare a positive electrode mixture. The positive electrode mixture is dispersed in N-methyl-2-pyrrolidone (NMP) to make a positive electrode layer slurry, and then the positive electrode layer slurry is evenly coated on both sides of a 15 μm thick strip of aluminum foil (positive electrode collector) to form a coating. Next, after the coating is dried with warm air, it is compression-molded by a roller press (roller temperature 130°C, linear pressure 0.7t / cm, pressing speed 10m / min) to form a positive electrode sheet having a positive electrode layer. Next, the positive electrode sheet is cut into a strip of 48mm×300mm to make a positive electrode. Next, the positive electrode lead is installed on the exposed portion of the positive electrode collector of the positive electrode.
[0269] ■ Negative electrode production process
[0270] The negative electrode is made as follows. First, graphite particles (average primary particle size 20 μm) as the negative electrode active material are mixed with an NMP solution containing 20 wt% of a polyimide binder so that the weight ratio (graphite particles: NMP solution) is 9:1 to make a negative electrode layer slurry. Next, the negative electrode layer slurry is applied to both sides of a 15 μm thick copper foil (negative electrode collector) using a rod coater with a gap of 35 μm to form a coating film, which is dried at 80°C. Next, the coating film is compression-molded by a roller press and then heated at 700°C for 3 hours to form a negative electrode sheet having a negative electrode layer. The negative electrode sheet is cut into a strip of 50 mm × 310 mm to make a negative electrode. Next, a negative electrode lead is installed on the exposed portion of the negative electrode collector of the negative electrode.
[0271] ■Production process of stacked batteries
[0272] The prepared positive electrode and negative electrode are closely attached to each other through a separator composed of a microporous polyethylene film with a thickness of 25 μm, and are wound in the length direction. A protective tape is attached to the outermost periphery and compressed to produce a flat wound electrode body. Next, the wound electrode body is loaded between the outer packaging components, and three sides of the outer packaging components are heat-fused, while one side is not heat-fused to have an opening. As an outer packaging component, a moisture-proof aluminum laminated film is used, which is formed by stacking a 25 μm thick nylon film, a 40 μm thick aluminum foil, and a 30 μm thick polypropylene film in sequence from the outermost layer.
[0273] ■Electrolyte preparation and injection process
[0274] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed to a mass ratio of EC:EMC=5:5 to prepare a mixed solvent. Then, lithium hexafluorophosphate (LiPF6) as an electrolyte salt is dissolved in the mixed solvent to a concentration of 1 mol / l to prepare an electrolyte. The electrolyte is injected from the opening of the outer casing, and the remaining side of the outer casing is thermally fused under reduced pressure to seal. Thus, the target non-aqueous electrolyte secondary battery is obtained.
[0275] <Evaluation of Battery Characteristics>
[0276] ■Cycling characteristics
[0277] The charge and discharge were performed from the 1st to the 105th cycle under the following conditions, and the capacity retention rate was calculated and evaluated as the ratio of the “discharge capacity after the 101st cycle” to the “discharge capacity after the 1st cycle”.
[0278] ◎: 79% or more (best);
[0279] ○: 70% or more and less than 79% (good);
[0280] ×: Less than 70% (problematic).
[0281] Cycle 1
[0282] Charging conditions: After constant current charging to 4.50 V at 45°C / 0.5C, constant voltage charging to 0.025 C at 45°C / 4.50 V. Then, a 10-minute break.
[0283] Discharge conditions: Discharge at a constant current of 45°C / 0.1C to 3.00 V. Then, interrupt for 10 minutes.
[0284] Cycle 2
[0285] Charging conditions: After constant current charging to 4.50 V at 45°C / 0.5C, constant voltage charging to 0.025 C at 45°C / 4.50 V. Then, a 10-minute break.
[0286] Discharge conditions: Discharge at a constant current of 45°C / 0.2C to 3.00 V. Then, interrupt for 10 minutes.
[0287] Cycle 3
[0288] Charging conditions: After constant current charging to 4.50 V at 45°C / 0.5C, constant voltage charging to 0.025 C at 45°C / 4.50 V. Then, a 10-minute break.
[0289] Discharge conditions: Discharge at a constant current of 45°C / 0.5C to 3.00 V. Then, interrupt for 10 minutes.
[0290] Cycle 4
[0291] Charging conditions: After constant current charging to 4.50 V at 45°C / 0.5C, constant voltage charging to 0.025 C at 45°C / 4.50 V. Then, a 10-minute break.
[0292] Discharge conditions: Discharge at a constant current of 45°C / 1.0C to 3.00 V. Then, interrupt for 10 minutes.
[0293] Cycle 5
[0294] Charging conditions: After constant current charging to 4.50 V at 45°C / 0.5C, constant voltage charging to 0.025 C at 45°C / 4.50 V. Then, a 10-minute break.
[0295] Discharge conditions: Discharge at a constant current of 45°C / 2.0C to 3.00 V. Then, interrupt for 10 minutes.
[0296] Cycle 6 to 50
[0297] Charging conditions: Charging and interruption were performed under the same conditions as those in the first to fifth cycles.
[0298] Discharge conditions: Discharge at a constant current of 45°C / 0.5C to 3.00 V. Then, interrupt for 10 minutes.
[0299] Cycle 51 to 55
[0300] Charging conditions: Charging and discharging were performed under the same conditions as those in the first to fifth cycles.
[0301] Cycle 56 to 100
[0302] Charging and discharging conditions: Charging, discharging, and interruption were performed under the same conditions as those in the 6th to 50th cycles.
[0303] Cycle 101 to 105
[0304] Charging conditions: Charging and discharging were performed under the same conditions as those in the first to fifth cycles.
[0305] ■Filling capacity (bulk density)
[0306] The volume density of the electrode was calculated as follows.
[0307] The thickness of the positive electrode after roll pressing was measured using a height gauge, and the thickness of the positive electrode layer was calculated by subtracting the thickness of the collector foil therefrom, thereby calculating the volume density (g / cc) of the positive electrode layer.
[0308] ◎: 4.01g / cc or more (best);
[0309] ○: 3.96 g / cc or more and less than 4.01 g / cc (good);
[0310] ×: Less than 3.96 g / cc (problematic).
[0311] ■Load characteristics
[0312] The load characteristics were evaluated as follows.
[0313] First, perform constant current charging with a charging current of 0.5A, and then perform constant voltage charging until the current value is reduced to 1 / 10. Then, measure the discharge capacity at a discharge current of 0.2A. Take the discharge capacity obtained here as 1C, then, charge under the above-mentioned charging conditions, and then discharge under the conditions of a discharge current of 0.1C and an end voltage of 3.0V to obtain the discharge capacity. Next, charge under the above-mentioned charging conditions, and then discharge under the conditions of a discharge current of 2.0C and an end voltage of 3.0V. Next, substitute the measured discharge capacity at a discharge current of 0.1C and the discharge capacity at a discharge current value of 2.0C into the following formula to obtain the load characteristics.
[0314] ◎: 79% or more (best);
[0315] ○: 77% or more and less than 79% (good);
[0316] ×: Less than 77% (problematic).
[0317]
Mathematical formula 1
[0318] Load characteristic [%] = (discharge capacity at discharge current value 2.0C) / (discharge capacity at discharge current 0.1C) × 100
[0319]
[0320] (1) Value relative to 100 parts by weight of the positive electrode active material core; (2) Ratio (weight %) when x+y+z=100; (3) Ratio relative to the positive electrode active material to be coated
[0321] “-” means “not matched” or “not evaluated”.
[0322] The positive electrodes manufactured in each of Examples 1A to 5A were disassembled and observed under a microscope. It was found that the coating film had not peeled off from the positive electrode active material core material at all.
[0323] The positive electrodes manufactured in each of Examples 1B to 16B were disassembled and observed under a microscope. It was found that there were no cracks along the grain boundaries of the positive electrode active material, no unevenness or damage on the current collector, and no separation of the positive electrode layer from the current collector.
[0324] The secondary battery of the present invention can be used in various fields that require electricity storage. The secondary battery of the present invention, especially the non-aqueous electrolyte secondary battery, can be used in the electrical, information and communication fields using mobile devices (for example, mobile devices such as mobile phones, smart phones, smart watches, laptops, digital cameras, activity meters, wrist computers, electronic paper, etc.), household and small industrial uses (for example, power tools, golf carts, household, nursing and industrial robots), large industrial uses (for example, forklifts, elevators, gantry cranes), transportation systems (for example, hybrid vehicles, electric vehicles, buses, electric trains, electric bicycles, electric motorcycles, etc.), power system uses (for example, various power generation, load regulators, smart grids, ordinary household power storage systems, etc.), medical uses (medical equipment such as in-ear hearing aids), medical uses (dose management systems, etc.), and IoT fields, space and deep-sea uses (for example, space probes, diving research vessels, etc.), etc., but these are only examples. Symbol Explanation
[0325] 1: Positive electrode active material core material
[0326] 2: Organic and inorganic mixed coating
[0327] 10: Positive electrode active material.
Claims
1. A positive electrode active material, which is a positive electrode active material for a battery, wherein the positive electrode active material has: Positive electrode active material core material; and A coating formed on the surface of the positive electrode active material core material, The coating is an organic-inorganic hybrid coating composed of reactants, and the reactants at least include: a first alkoxide that does not contain any metal atom-carbon atom bonds in one molecule; and A second alkoxide containing two or more Si atom-carbon atom bonds in one molecule, The first alkoxide is a compound represented by the following general formula (1): The second alkoxide is a compound represented by the following general formula (2A), (2B), (2C), (2D), (2E) or (2F), or a mixture thereof, M 1 (OR 1 ) x (1) In formula (1), M 1 Si, Ti, Al or Zr; x is M 1 The valence of is an integer of 3 or 4; R 1 are independently an alkyl group having 1 to 10 carbon atoms or -C(R 2 )=CH-CO-R 3 , where R 2 is an alkyl group having 1 to 10 carbon atoms, R 3 is an alkyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, or an alkenyloxy group having 1 to 30 carbon atoms; R 1 In the example, two adjacent R 1 When the alkyl group is present, it can bond to each other and to the two R 1 The oxygen atom to which it is bonded and the M to which the oxygen atom is bonded 1 The atoms form a ring, (R 211 O)3Si-R 31 -Si(OR 212 )3 (2A) In formula (2A), R 211 and R 212 are each independently an alkyl group having 1 to 10 carbon atoms; R 31 is a divalent hydrocarbon group having 1 to 20 carbon atoms, In formula (2B), R 211 , R 212 , R 213 and R 214 are each independently an alkyl group having 1 to 10 carbon atoms; R 32 are each independently a divalent hydrocarbon group having 1 to 20 carbon atoms; R 33 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms, (R 211 O)3Si-R 34 -NH-R 35 -NH-R 36 -Si(OR 212 )3 (2C) In formula (2C), R 211 and R 212 are independently an alkyl group having 1 to 10 carbon atoms; 34 , R 35 , and R 36 are each independently a divalent hydrocarbon group having 1 to 10 carbon atoms, (R 211 2-Si(OR 212 )2 (2D) In formula (2D), R 211 and R 212 are each independently an alkyl group having 1 to 10 carbon atoms, In formula (2E), R 212 and R 213 are each independently an alkyl group having 1 to 10 carbon atoms; R 32 are each independently a divalent hydrocarbon group having 1 to 20 carbon atoms; R 33 Each independently is a monovalent hydrocarbon group having 1 to 10 carbon atoms; R 34 are each independently a monovalent hydrocarbon group having 8 to 30 carbon atoms, In formula (2F), R 212 , R 213 and R 214 are each independently an alkyl group having 1 to 10 carbon atoms; R 32 Each independently is a divalent hydrocarbon group having 1 to 20 carbon atoms.
2. The positive electrode active material according to claim 1, wherein The coating includes 5% by weight or more and 85% by weight or less of the first alkoxide and 1% by weight or more and 85% by weight or less of the second alkoxide relative to the total weight of the coating.
3. The positive electrode active material according to claim 1, wherein The coating is an organic-inorganic hybrid coating composed of reactants, and the reactants further include a third alkoxide including one Si atom-carbon atom bond in one molecule.
4. The positive electrode active material according to claim 3, wherein The third alkoxide is a compound represented by the following general formula (3): R 12 -Si(OR 11 )3 (3) In formula (3), R 11 are each independently an alkyl group having 1 to 10 carbon atoms; R 12 It is a monovalent hydrocarbon group having 8 to 30 carbon atoms.
5. The positive electrode active material according to claim 3, wherein The coating includes 5 wt % to 85 wt % of the first alkoxide, 1 wt % to 85 wt % of the second alkoxide, and 5 wt % to 90 wt % of the third alkoxide relative to the total weight of the coating.
6. The positive electrode active material according to claim 1, wherein The content of the coating is 0.010 wt % or more and 2.000 wt % or less relative to the total weight of the positive electrode active material.
7. The positive electrode active material according to claim 1, wherein The positive electrode active material core material contains at least Li.
8. The positive electrode active material according to claim 1, wherein The positive electrode active material core material is a lithium transition metal composite oxide.
9. The positive electrode active material according to claim 1, wherein The battery is a lithium ion secondary battery.
10. A positive electrode, comprising: A positive electrode layer comprising the positive electrode active material according to any one of claims 1 to 9; and Positive electrode collector.
11. A secondary battery, The secondary battery includes the positive electrode according to claim 10, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte sealed in an outer casing.
12. The secondary battery according to claim 11, wherein The electrolyte is a non-aqueous electrolyte.
13. The secondary battery according to claim 11 or 12, wherein: The positive electrode and the negative electrode are electrodes capable of absorbing and releasing lithium ions.
14. A method for producing a positive electrode active material according to any one of claims 1 to 2 and 6 to 9, comprising: The positive electrode active material core material is stirred together with the first alkoxide and the second alkoxide in an alkaline solvent.
15. The method for producing a positive electrode active material according to claim 14, further comprising: A third alkoxide containing one Si atom-carbon atom bond in one molecule is used together with the first alkoxide and the second alkoxide.