A lithium metal negative electrode, preparation method and lithium metal battery

By using a combined structure of metallic lithium foil and current collector strips in lithium metal batteries, the problem of uneven thickness of the negative electrodes of lithium metal batteries after lamination is solved, the flatness and high energy density of the battery are achieved, and internal short circuits and Deterioration of cycle performance.

CN114335430BActive Publication Date: 2024-10-25SHANGHAI INST OF SPACE POWER SOURCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111481574.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-10-25
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

Existing lithium metal battery negative electrodes can easily lead to uneven battery thickness after lamination, which increases the risk of internal short circuit and deterioration of cycle performance, making it difficult to meet the demand for high specific energy density.

Method used

It adopts a structure that combines metal lithium foil and current collector lead strips. The current guide part is located outside the main body of the lithium foil and does not participate in the reaction. The current collector lead strip and the current guide part are connected by crimping to ensure the flatness of the lithium metal battery and pass Surface roughening improves bonding strength.

Benefits of technology

It effectively avoids internal short circuit and degradation of cycle performance, improves the mass energy density of the battery, and ensures the flatness and stable diversion of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114335430B_ABST
    Figure CN114335430B_ABST
Patent Text Reader

Abstract

The present invention discloses a negative electrode of a lithium metal battery, a preparation method and a lithium metal battery. The lithium metal negative electrode of the present invention comprises a metal lithium foil and a current collecting lead-out strip, wherein the lithium foil comprises a main body and a current guiding part; the current guiding part is located on one side of the main body and extends outside the main body, is not opposite to the positive electrode main body in the battery, does not participate in the reaction, and ensures the flatness of the main body. The current collecting lead-out strip is connected to the current guiding part of the metal lithium foil, and the position of the crimping current collecting lead-out strip is located outside the negative electrode main body and the positive electrode main body of the lithium foil, which can ensure that the lithium metal battery after lamination becomes more flat. On the one hand, it can easily ensure that when the upper clamp or battery group applies pressure during the test, the battery internal short circuit caused by the uneven negative electrode body is avoided, and on the other hand, the deterioration of the cycle performance caused by the uneven current density of lithium deposition can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of chemical power sources, and in particular relates to a lithium metal battery negative electrode, a preparation method and a lithium metal battery using the negative electrode. Background Art

[0002] With the development of science and technology, new energy vehicles, electric tools, electric drones, electric ships and other fields have higher and higher requirements for battery specific energy. Existing lithium-ion batteries can no longer meet the demand for energy density. Lithium metal batteries with lithium metal as the negative electrode can reach a specific energy of more than 500Wh / kg, which is the development direction of high specific energy batteries in the future.

[0003] The traditional method of preparing lithium metal negative electrodes is mainly to press lithium strips or lithium foils onto current collectors. For example, Chinese invention patent 200820073651.3 folds lithium foil in half, sandwiches stainless steel or nickel metal current collectors in the middle, and presses them tightly together to prepare lithium negative electrodes. Chinese invention patent 201310250752.9 uses copper foil as the lithium negative electrode current collector, and at least one side is tightly provided with metal lithium foil or alloy lithium foil as the negative electrode of the battery. Chinese invention patent 201810993887.7 also has a similar structure of copper foil as the current collector. Although this type of lithium negative electrode current collector with an overall area has the function of preventing the lithium strip from breaking during the lithium cycle and causing the capacity to drop, it will increase the weight of the battery and it is difficult to meet the future demand for high-density lithium metal batteries above 500Wh / kg.

[0004] In order to further reduce weight and improve battery specific energy, some patents have begun to cancel the overall area of ​​lithium negative electrode current collectors and use a crimped lead-out strip design instead. For example, Chinese invention patents 201410705352.7 and 201811611825.1 crimp the current collector nickel foil, copper foil or foamed nickel to one corner of the negative terminal, and the other end is used to weld the pole ear after lamination. Chinese utility model patent 201821341529.X also stacks a non-lithium metal lug extending vertically on the lithium belt, one end of the non-lithium metal lug protrudes from the lithium belt, and the part of the non-lithium metal lug protruding from the lithium belt is used to weld the pole ear. The above-mentioned structure is prone to uneven thickness of the lithium negative electrode body due to the lead-out strip directly crimped on the surface of the lithium belt or lithium foil body, and the crimped current collector part is prone to bulge, resulting in uneven battery thickness after lamination. This thickness bulge can easily cause internal short circuits in the battery when pressure is applied to the upper plate or battery groups during testing. It can also easily cause uneven current density of lithium deposition, leading to deterioration of the cycle.

[0005] Therefore, it is necessary to develop a new negative electrode manufacturing method for lithium metal batteries to ensure that the lithium negative electrode body is flat and avoid short circuits or cycle deterioration in the battery caused by uneven battery thickness after lamination. Summary of the invention

[0006] The purpose of the present invention is to overcome the above defects and provide a negative electrode of a lithium metal battery, a preparation method and a lithium metal battery. The lithium metal negative electrode comprises a metal lithium foil and a current collecting lead-out bar, wherein the lithium foil comprises a main body and a current guiding part; the current guiding part is located on one side of the main body and extends outside the main body, is not opposite to the positive electrode main body in the battery, does not participate in the reaction, and ensures the flatness of the main body. The current collecting lead-out bar is connected to the current guiding part of the metal lithium foil, and the position of the crimping current collecting lead-out bar is located outside the negative electrode main body and the positive electrode main body of the lithium foil, which can ensure that the lithium metal battery after lamination becomes more flat. On the one hand, it is easy to ensure that when the upper clamp or battery group applies pressure during the test, the battery will not be short-circuited due to the uneven negative electrode body. On the other hand, it can reduce the deterioration of the cycle performance caused by the uneven current density of lithium deposition.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] A lithium metal negative electrode comprises a metal lithium foil and a current collecting lead-out strip, wherein the metal lithium foil comprises a main body portion and a current guiding portion extending outward from the main body portion, the width of the current guiding portion is 10% to 100% of the width of the main body portion, and the length is 7 to 15 mm; the current collecting lead-out strip is connected to the current guiding portion.

[0009] Furthermore, the current collecting lead-out strip is connected to the current guiding part by means of crimping, and the total thickness of the crimping part is ≤ 105% of the thickness of the main body part.

[0010] Furthermore, in the metal lithium foil, the main body and the guide part have the same thickness, which is 0.1 to 0.3 mm.

[0011] Furthermore, the thickness of the current collecting lead strip is less than 15% of the thickness of the main body of the metal lithium foil.

[0012] Furthermore, the current collecting lead-out bar is a copper foil or a nickel foil subjected to surface roughening treatment, and the surface roughness of the current collecting lead-out bar after the surface roughening treatment is more than 1.5 times the surface roughness before the treatment;

[0013] Surface roughening methods include sanding or sand blasting.

[0014] Furthermore, the width of the current collecting and leading-out strip is consistent with the width of the current guiding portion, and the length thereof is 150-250% of the length of the current guiding portion.

[0015] Furthermore, when the current collecting and lead-out bar is connected to the current guiding part, the current collecting and lead-out bar covers the entire current guiding part.

[0016] Furthermore, the area of ​​the crimping region between the current collecting lead-out strip and the current guiding portion is more than 80% of the area of ​​the current guiding portion.

[0017] The above-mentioned method for preparing a lithium metal negative electrode comprises the following steps:

[0018] S1. Cover the current collecting lead-out bar on the surface of the current guiding part of the metal lithium foil, and connect the current collecting lead-out bar with the current guiding part;

[0019] S2 leveling collector lead strip;

[0020] S3 uses polyimide tape to bond the connection between the current collecting lead strip and the guide part.

[0021] A lithium metal battery is a multilayer structure formed by stacking lithium metal negative electrode / diaphragm / positive electrode / diaphragm in sequence, wherein the lithium metal negative electrode adopts the above-mentioned lithium metal negative electrode, the main part of the metal lithium foil is opposite to the positive electrode main part, and the guide part is not opposite to the positive electrode main part.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) In a lithium metal negative electrode of the present invention, the lithium foil is extended outward to form a current guide portion. Compared with crimping a lead-out strip on the lithium foil body, the present invention crimps a current collecting lead-out strip on the current guide portion, so that the position of the crimped current collecting lead-out strip is located outside the lithium foil negative electrode body and the positive electrode body, which can ensure that the lithium metal battery after lamination becomes more flat. On the one hand, it can ensure that when the upper clamping plate or the battery group applies pressure during the test, the battery internal short circuit caused by the uneven negative electrode body can be avoided. On the other hand, it can reduce the deterioration of the cycle performance caused by the uneven current density of lithium deposition;

[0024] (2) Compared with the conventional whole-surface lithium negative electrode using metal mesh, foam metal or metal foil as the current collector, the current collector lead-out strip using foil material in the lithium metal negative electrode of the present invention is lighter in weight, which is beneficial to improving the mass energy density of the battery;

[0025] (3) The dimensions of the current guide part and the current collecting lead-out strip as well as the connection method between the current collecting lead-out strip and the current guide part are further optimized in a lithium metal negative electrode of the present invention, thereby avoiding the unevenness of the battery caused by the excessive thickness of the negative electrode current guide part due to the addition of the current collecting lead-out strip, resulting in a decrease in electrical performance. At the same time, the wrinkling and breakage of the current guide part caused by the addition of the current collecting lead-out strip is avoided, thereby forming a stable current guide method. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the method for manufacturing the negative electrode of a lithium metal battery of the present invention, wherein (a) is a schematic diagram of the initial state, (b) is a schematic diagram of the current collecting lead-out bar covering the surface of the current guiding part, and (c) is a schematic diagram of the current collecting lead-out bar and the current guiding part being crimped;

[0027] Figure 2 Schematic diagram of the cutting size of lithium foil in Example 1;

[0028] Figure 3 Schematic diagram of the cutting size of the positive electrode in Example 1;

[0029] Figure 4 is the first discharge curve of the lithium metal battery in Example 1;

[0030] Figure 5 Schematic diagram of the cutting size of lithium foil in Example 2;

[0031] Figure 6 Schematic diagram of the cutting size of the positive electrode in Example 2;

[0032] Figure 7 This is the first discharge curve of the lithium metal battery in Example 2. DETAILED DESCRIPTION

[0033] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0034] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.

[0035] The present invention provides a lithium metal negative electrode, a manufacturing method and a lithium metal battery, so as to solve the problem of short circuit in the battery or deterioration of cycle performance caused by uneven thickness of the battery after lithium negative electrode lamination.

[0036] The present invention discloses a lithium metal negative electrode, comprising a metal lithium foil 1 and a current collecting lead strip 2, wherein the metal lithium foil 1 comprises a main body 11 and a current guiding part 12; the current guiding part 12 is located on one side of the main body 11 and extends outside the main body 11, is not opposite to the positive electrode main body in the battery, does not participate in the reaction, and ensures the flatness of the main body 11. The current collecting lead strip 2 has good conductivity and is connected to the current guiding part 12 of the metal lithium foil 1.

[0037] In order to prevent the negative electrode current conducting portion 12 from being too thick due to the addition of the current collecting lead-out bar 2 , the thickness of the current collecting lead-out bar 2 and the connection method between the current collecting lead-out bar 2 and the current conducting portion 12 are optimized.

[0038] In a preferred embodiment, the lithium foil main body portion 11 and the flow guide portion 12 have the same thickness, which is 0.1-0.3 mm.

[0039] In a preferred embodiment, the thickness of the current collecting lead strip 2 is less than 15% of the thickness of the lithium foil.

[0040] In a preferred embodiment, the current collecting lead-out bar 2 is connected to the lithium foil conducting portion 12 by crimping.

[0041] In a preferred embodiment, the current collecting lead-out bar 2 is a copper foil or a nickel foil, and the surface of the current collecting lead-out bar 2 is roughened by sandpaper grinding or sandblasting to enhance the pressure-bonding strength with lithium.

[0042] In a preferred embodiment, the total thickness of the current collecting lead-out strip 2 and the lithium foil current guiding portion 12 after being crimped is the same as the thickness of the lithium foil main body portion 11 or does not exceed 105% of the thickness of the main body portion.

[0043] In order to avoid wrinkling and breaking of the current-conducting portion 12 after the addition of the current-collecting lead-out bar 2, the shape, position and fixing method of the current-collecting lead-out bar 2 and the lithium foil current-conducting portion 12 are optimized.

[0044] In a preferred embodiment, the width of the lithium foil guide portion 12 is 10% to 100% of the width of the lithium foil main body portion 11, and the length is 7 to 15 mm.

[0045] In a preferred embodiment, the width of the current collecting and drawing strip 2 is consistent with that of the guide portion 12 , and the length thereof is 150-250% of the length of the guide portion 12 . Furthermore, the current collecting and drawing strip 2 covers the entire guide portion 12 .

[0046] In a preferred embodiment, the area of ​​the pressing connection between the current collecting lead-out bar 2 and the lithium foil current guiding portion 12 is more than 80% of the area of ​​the current guiding portion 12 .

[0047] In a preferred embodiment, the current collecting lead-out bar 2 needs to be further leveled after being crimped with the lithium foil current guiding portion 12 .

[0048] In a preferred embodiment, the crimping portion between the current collecting lead-out strip 2 and the lithium foil current guiding portion 12 is insulated and further fixed by using polyimide tape.

[0049] The preparation method of the lithium metal negative electrode of the present invention is as follows Figure 1 As shown, the current collecting lead-out bar 2 is first covered on the surface of the lithium foil current conducting part 12, and then the current collecting lead-out bar 2 and the lithium foil current conducting part 12 are crimped together by crimping to prepare a lithium negative electrode, and the current collecting lead-out bar 2 is leveled, and then the crimping part 3 of the current collecting lead-out bar 2 and the lithium foil current conducting part 12 is insulated and further fixed by using polyimide tape.

[0050] The above-mentioned lithium metal negative electrode can be used with transition metal oxide, sulfur and other positive electrodes and diaphragm stacks to prepare lithium metal batteries. The battery structure is a multilayer structure formed by stacking lithium metal negative electrode / diaphragm / positive electrode / diaphragm in sequence. The lithium metal negative electrode lithium foil main body 11 is opposite to the positive electrode main body and separated by a diaphragm. The lithium foil guide part 12 is located outside the main body 11 after crimping the current collecting lead-out bar 2. The positive and negative current collecting lead-out bars are respectively welded to aluminum pole ears and nickel pole ears by ultrasonic welding, and then heat-sealed with the outer packaging to prepare lithium metal batteries. The diaphragm is one of the microporous polypropylene and polypropylene / polyethylene multilayer composite films with a thickness of 10 to 30 μm; the electrolyte is a commonly used commercial lithium battery liquid organic electrolyte; the outer packaging is an aluminum-plastic film or a metal shell.

[0051] Example 1

[0052] Lithium metal anode preparation:

[0053] according to Figure 2 The lithium foil with a thickness of 0.1 mm was cut according to the size of the main body. The lithium foil guide part was located on the short side of the main body and 6 mm away from the edge of the lithium foil. The width of the lithium foil guide part was 8 mm and the length was 7 mm. The surface of the 10 μm thick copper foil was roughened with sandpaper. The surface roughness R a The copper foil was then cut into 8mm wide and 15mm long copper foil lead-out strips. Figure 1 The surface of the lithium foil guide part is covered by a cold welding machine, and then the copper foil current collecting lead strip and the lithium foil guide part are crimped together. The cold welding crimping area is 50mm 2 Then the crimped part was gently flattened, and the thickness of the guide part after crimping was measured to be 102μm. Then the crimped part was further fixed with a 30μm thick polyimide tape.

[0054] Preparation of transition metal oxide positive electrode:

[0055] The transition metal oxides (lithium nickel cobalt manganese oxide, LiNi) were prepared by double-sided coating on the surface of 13 μm aluminum foil by transfer coating. 0.8 Co 0.1 Mn 0.1 O2) positive electrode. After drying, the electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 O2): conductive agent (SuperP): binder (PVDF) ratio is 95:3:2. The surface density of the electrode single-sided coating is 25mg / cm 2 . The rolled positive electrode is Figure 3 The size of the positive electrode is cut, and a blank aluminum foil protrusion is reserved at one end of the main body of the positive electrode as the positive electrode current collecting lead strip. The thickness of the cut positive electrode is about 143μm.

[0056] Lithium metal battery preparation:

[0057] Under dry air conditions with a dew point of <-40°C, the 13 lithium metal negative electrode sheets and 12 transition metal oxide positive electrode sheets prepared in advance are separated by a Celgard2325 separator with a width of 88mm and assembled into a battery cell by stacking. The position of the lithium foil guide part crimping the copper foil current collector lead-out strip is outside the main part of the lithium foil and the main part of the positive electrode, ensuring the flatness of the battery cell. After the stacking is completed, the 12 positive electrode current collector lead-out strips are ultrasonically welded to the 8mm×0.1mm aluminum pole tabs, and the 13 negative electrode copper foil current collector lead-out strips are ultrasonically welded to the 8mm×0.1mm nickel pole tabs. The battery shell is sealed with a 73μm aluminum-plastic composite film and assembled into a soft-package battery. 45 g of electrolyte consisting of 1 mol / L lithium hexafluorophosphate (LiPF6) / ethylene carbonate (EC) + ethyl methyl carbonate (EMC) (volume ratio of 3:7) was added, the bottle was sealed and left for 48 hours, and then vacuum sealed again to obtain a lithium metal battery.

[0058] Battery discharge test:

[0059] At 25±2℃, the battery charge and discharge performance was tested: the battery charge / discharge current was 450mA, the charge cut-off voltage was 4.3V, and the discharge cut-off voltage was 3V. The battery's first discharge capacity was 4.82Ah. The first discharge curve is as follows: Figure 4 As shown in the figure, the battery capacity is 4.48Ah after 10 cycles.

[0060] Example 2

[0061] Lithium metal anode preparation:

[0062] according to Figure 5 The lithium foil with a thickness of 0.2 mm was cut according to the size of the main body. The lithium foil guide part was located on the short side of the main body and 8 mm away from the edge of the lithium foil. The width of the lithium foil guide part was 10 mm and the length was 8 mm. The surface of the 20 μm thick nickel foil was roughened with sandpaper. The surface roughness R a The nickel foil is then cut into nickel foil current collecting lead strips with a width of 10 mm and a length of 16 mm. Figure 1 The surface of the lithium foil guide part is covered by a cold welding machine, and then the nickel foil current collecting lead strip and the lithium foil guide part are crimped together. The cold welding crimping area is 70mm 2 Then, the crimped part was gently flattened, and the thickness of the guide part after crimping was measured to be 205μm. Then, the crimped part was further fixed with a 30μm thick polyimide tape.

[0063] Sulfur cathode sheet preparation:

[0064] The sulfur-carbon composite material (sulfur content ~87.6%) positive electrode was prepared by double-sided coating on the surface of 13μm aluminum foil by transfer coating. The ratio of active material (sulfur-carbon composite material): conductive agent (Super P): conductive agent (CNT): binder (LA133) in the electrode design is 89:3:2:6. After drying, the sulfur content in the electrode is ~78%. The surface density of the single-sided coating of the electrode is 7.8mg / cm 2 . The rolled positive electrode is Figure 6 The size of the positive electrode is cut, and a blank aluminum foil protrusion is reserved at one end of the positive electrode as the positive electrode ear lead-out strip. The thickness of the cut positive electrode is about 315μm.

[0065] Lithium metal battery preparation:

[0066] Under dry air conditions with a dew point of <-40°C, the 11 lithium metal negative electrode sheets and 10 sulfur positive electrode sheets prepared in advance are separated by a Celgard2320 separator with a width of 108mm and assembled into a battery cell by stacking. The position where the lithium foil guide part is crimped to the nickel foil current collector lead-out strip is outside the main part of the lithium foil and the main part of the positive electrode, ensuring the flatness of the battery cell. After the stacking is completed, the 10 positive electrode current collector lead-out strips are ultrasonically welded to the 8mm×0.1mm aluminum pole tabs, and the 11 negative electrode copper foil current collector lead-out strips are ultrasonically welded to the 8mm×0.1mm nickel pole tabs. The battery shell is sealed with a 73μm aluminum-plastic composite film and assembled into a soft-package battery. 26 g of electrolyte consisting of 1.0 mol / L lithium bistrifluoromethylsulfonyl imide (LiTFSI) / 1,3-dioxolane (DOL) + ethylene glycol dimethyl ether (DME) (volume ratio of 1:1) / 1% lithium nitrate (LiNO3) was added, the battery was sealed and left for 48 hours, and then vacuum sealed for a second time to obtain a lithium metal battery.

[0067] Battery discharge test:

[0068] At 25±2℃, the battery discharge performance was tested: the battery charge / discharge current was 300mA, the discharge cut-off voltage was 1.7V, and the charge cut-off voltage was 2.5V. The battery's first discharge capacity was 10.53Ah. The first discharge curve is as follows: Figure 7 As shown in the figure, the battery capacity is 8.58Ah after 10 cycles.

[0069] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0070] The contents not described in detail in the specification of the present invention belong to the common knowledge of those skilled in the art.

Claims

1. A lithium metal negative electrode, characterized in that The invention comprises a metal lithium foil (1) and a current collecting lead strip (2), wherein the metal lithium foil (1) comprises a main body (11) and a current guiding part (12) extending outward from the main body (11), the width of the current guiding part (12) is 10% to 100% of the width of the main body (11), and the length is 7 to 15 mm; the current collecting lead strip (2) is connected to the current guiding part (12); The current collecting lead-out strip (2) is connected to the current guiding part (12) by means of crimping, and the total thickness of the crimping part is ≤ 105% of the thickness of the main part (11); In the metal lithium foil, the main body part (11) and the flow guide part (12) have the same thickness, which is 0.1 to 0.3 mm; The thickness of the current collecting lead strip (2) is less than 15% of the thickness of the main body (11) in the metal lithium foil; The current collecting lead-out strip (2) is a copper foil or a nickel foil that has been subjected to a surface roughening treatment, and the surface roughness of the current collecting lead-out strip (2) after the surface roughening treatment is more than 1.5 times the surface roughness before the treatment; Surface roughening methods include sandpapering or sandblasting; The width of the current collecting and leading strip (2) is consistent with the width of the current guiding part (12), and the length is 150 to 250% of the length of the current guiding part (12); When the current collecting and leading-out bar (2) is connected to the current guiding part (12), the current collecting and leading-out bar (2) covers the entire current guiding part (12); The area of ​​the crimping region between the current collecting lead strip (2) and the current guiding part (12) is more than 80% of the area of ​​the current guiding part (12) The current-conducting part is not opposite to the main part of the positive electrode in the battery and does not participate in the reaction, thereby ensuring the flatness of the main part.

2. The method for preparing a lithium metal negative electrode according to claim 1, characterized in that: The steps include: S1: Covering the current collecting lead-out bar (2) on the surface of the metal lithium foil current guiding part (12), and connecting the current collecting lead-out bar (2) with the current guiding part (12); S2 leveling collector lead strip (2); S3 uses polyimide tape to bond the connection portion between the current collecting lead-out strip (2) and the current guiding portion (12).

3. A lithium metal battery, characterized in that: The invention relates to a multilayer structure in which a lithium metal negative electrode / diaphragm / positive electrode / diaphragm are stacked in sequence, wherein the lithium metal negative electrode is a lithium metal negative electrode as claimed in claim 1, wherein the main part (11) of the metal lithium foil (1) is opposite to the main part of the positive electrode, and the conducting part (12) is not opposite to the main part of the positive electrode.