A low-VOC, high-environmental-friendly glass fiber reinforced polypropylene material and preparation method thereof
By optimizing the formulation and production process, combined with the screw combination adjustment of the twin-screw extruder, the problem of failure to control the odor and VOC of glass fiber reinforced polypropylene material from the source in the prior art is solved, and the preparation of low VOC and high environmentally friendly materials is realized. , meet strict air quality requirements for automobile interiors.
Patent Information
- Application Number
- CN202111651325.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-27
AI Technical Summary
The prior art is difficult to control the odor and VOC content of glass fiber reinforced polypropylene materials from the source, mainly because the influence of all raw materials and additives in the formula is not fully considered, resulting in the material still slowly releasing odor and VOC during use.
By optimizing the formulation and production process, select raw materials and additives that meet the Volkswagen PV3900 odor testing standards, and adjust the screw combination in the twin-screw extruder to reduce the generation of melt degradation small molecules and increase the vacuum degree to remove residual small molecules. Prepare low VOC high-environmental glass fiber reinforced polypropylene materials.
The material odor and VOC content are controlled from the source, and the odor and VOC content of low VOC and high environmentally friendly glass fiber reinforced polypropylene materials are reduced, which meets strict air quality requirements for automobile interiors and significantly reduces the detection results of harmful substances.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer material processing and modification, and in particular to a low-VOC and highly environmentally friendly glass fiber reinforced polypropylene material and a preparation method thereof. Background Art
[0002] With the development and progress of social economy, the public's awareness of environmental protection is constantly improving, and the country has continuously issued relevant standards such as automotive interior air quality requirements that require mandatory implementation. Based on user feedback, major manufacturers have put forward higher low-VOC and high environmental performance requirements for modified raw materials. This requires technicians to strictly optimize the selection of formula materials and production processes. However, there are no relevant national standards for the selection of raw materials, and it is difficult to uniformly achieve the purpose of controlling odor and VOC from the source.
[0003] In response to the problem of high VOC content in glass fiber reinforced polypropylene composite materials, the existing technologies basically target the small molecules generated during the production process, using various deodorants including physical adsorbents such as activated carbon and zeolites for adsorption, or using chemical deodorants for targeted decomposition and elimination, or just adjusting a certain auxiliary agent such as a compatibilizer that has a greater impact on the odor. However, few people consider screening out all the raw materials and auxiliary agents in the source formula that may produce small molecules that affect the odor, and reducing the generation of small molecules from the source. This is because the small molecules that affect the odor and VOC content of the final material include not only small molecules generated by melt degradation during the production process, but also the volatilization of small molecules such as monomers, catalysts, solvents, etc. that remain in the production or storage of the raw materials and auxiliary agents in the formula.
[0004] Chinese patent publication number CN102030945A, named a low-odor glass fiber reinforced polypropylene composite material and its preparation method, uses the addition of physical odor inhibitors in the formula as a means of improving odor and VOC. Although the odor of the material is prevented to a certain extent, the odor is actually still inside the material and will be slowly released during use in the future, which cannot fundamentally solve the odor and VOC problems. Chinese patent publication number CN 103342859 A, named a low-odor, low-VOC glass fiber reinforced polypropylene composite material and its preparation method, changes the odor inhibitor into a deodorant, that is, it uses a combination of physical and chemical adsorption to decompose some odor source small molecules to a certain extent, and improves the odor and VOC problems by improving the production process such as increasing the vacuum degree. Chinese patent publication number CN105037941 A, named a low-VOC, low-odor wood fiber reinforced polypropylene composite material and its preparation method, only replaces the ordinary fiber in the formula with more environmentally friendly wood fiber, without considering the influence of other raw materials in the formula, and then adds an appropriate amount of odor absorbent and odor small molecules to react chemically and consume them. Chinese patent publication number CN 112552599 A, a low-fog, low-odor, low-VOC glass fiber and mineral raw material mixed reinforced polypropylene composite material and its preparation method, mainly uses short-cut flat high-strength and high-modulus glass fiber obtained by treating with a homemade low-odor, low-VOC impregnating agent to replace the ordinary cylindrical glass fiber in the formula, and uses low-odor, high-activity maleic anhydride grafted PP as a compatibilizer, and adds appropriate odor absorbents to achieve the purpose of improving VOC, and does not fully consider the influence of the remaining additives in the formula. Chinese patent publication number CN 113603964A, named a low-VOC glass fiber reinforced polypropylene composite material for automotive interior and its preparation method, also only achieves the purpose of reducing VOC by making a homemade low-VOC composite compatibilizer instead of the ordinary maleic anhydride grafted polypropylene compatibilizer, and then combining it with a compound odor absorbent. Summary of the invention
[0005] Technical problem to be solved: In view of the shortcomings of the prior art, the present invention provides a low-VOC, high-environmental-friendly glass fiber reinforced polypropylene material and a preparation method thereof. The low-VOC, high-environmental-friendly glass fiber reinforced polypropylene material controls the odor and VOC content of the material from the source. All its formulas comply with the Volkswagen PV3900 odor test standard, and the odor level does not exceed level 3. The production process is optimized, and the shear stress is improved by adjusting the screw combination of the twin-screw extruder to further reduce the generation of melt degradation small molecules, and the vacuum degree is increased to remove residual small molecules, thereby obtaining a low-VOC, high-environmental-friendly glass fiber reinforced polypropylene composite material.
[0006] Technical solution: A low-VOC, highly environmentally friendly glass fiber reinforced polypropylene material, containing the following components by mass: polypropylene: 60-80 parts, short glass fiber: 20-40 parts, compatibilizer: 3-5 parts, antioxidant: 0.4-1 part, deodorant: 0.5-1 part, masterbatch: 0.5-2 parts, lubricant: 0.1-0.5 part; the polypropylene, short glass fiber, compatibilizer, antioxidant, deodorant, masterbatch and lubricant are all tested according to the Volkswagen PV3900 odor test standard, and the odor level does not exceed level 3.
[0007] The above-mentioned detection method is as follows: 20-40g of samples are respectively placed in a 1L German Volkswagen PV3900 standard odor test bottle, and then the test bottle is placed in an 80°C oven, taken out after 2 hours, and judged by professional odor testers to select polypropylene, chopped glass fiber, compatibilizer, antioxidant, deodorant, masterbatch and lubricant with an odor level not exceeding level 3.
[0008] The polypropylene mentioned above is homopolymer polypropylene or copolymer polypropylene; the homopolymer polypropylene is S2040 or V30G; the copolymer polypropylene is BX3800.
[0009] The chopped glass fibers mentioned above are alkali-free chopped glass fibers with a diameter of 10-15 μm and a length of 3-5 mm; the alkali-free chopped glass fibers are T438H, 508A or 305K.
[0010] The compatibilizer mentioned above is maleic anhydride grafted polypropylene, and the maleic anhydride grafted polypropylene is solid phase grafted maleic anhydride grafted polypropylene, and the solid phase grafted maleic anhydride grafted polypropylene is FT-102, CMG5701 or FH118B.
[0011] The antioxidant described above is composed of a primary antioxidant and an auxiliary antioxidant in a weight ratio of (1-3):1, and the melting points of the primary antioxidant and the auxiliary antioxidant are both higher than 100°C; the primary antioxidant is a hindered phenol or a semi-hindered phenol, such as 3144 or S80, and the auxiliary antioxidant is a phosphite or a phosphite ester, such as 168 or 608.
[0012] The deodorant described above is a chemical deodorant containing functional groups such as carboxyl, amino, and hydroxyl, and is GRE-602, JH-200, or XC01.
[0013] The masterbatch described above is a homopolymer PP carrier masterbatch or a PE carrier masterbatch, which is PE2718, PE2705 or PE5861.
[0014] The lubricant described above is silicone, which is silicone powder with a siloxane content not exceeding 40%; the silicone powder is LYSI-100A.
[0015] The preparation steps of the low-VOC and highly environmentally friendly glass fiber reinforced polypropylene material described above are as follows:
[0016] (1) Pre-mixing polypropylene, compatibilizer, antioxidant, deodorant, masterbatch, and lubricant in a low-speed mixer for 5-10 minutes to obtain a premix;
[0017] (2) The premix obtained in step (1) is poured into the feeding hopper of a twin-screw extruder weight loss scale, and the chopped glass fibers are added from the side feeding port of the twin-screw extruder. After melt extrusion through the twin-screw extruder, the premix is granulated and dried to obtain a low-VOC and highly environmentally friendly glass fiber reinforced polypropylene material.
[0018] The screw diameter of the twin-screw extruder described above is 65 mm, and the aspect ratio is 45:1; the extruder temperature is 180° C.-210° C., the extrusion speed is 300-500 r / min, and the vacuum degree is not less than 0.06 MPa.
[0019] Beneficial effects: The low-VOC, highly environmentally friendly glass fiber reinforced polypropylene material and its preparation method provided by the present invention have the following beneficial effects:
[0020] 1. All the formulas of the present invention are in accordance with the Volkswagen PV3900 odor test standard, and the odor level does not exceed level 3. The odor and VOC content are controlled from the source, and the odor and VOC content of the low-VOC and high-environmental-friendly glass fiber reinforced polypropylene material are effectively and stably reduced;
[0021] 2. The preparation method of the present invention further reduces the generation of small molecules degraded by the melt by adjusting the screw combination of the twin-screw extruder to improve the shear stress, and increases the vacuum degree to remove the residual small molecules, thereby obtaining a low-VOC and highly environmentally friendly glass fiber reinforced polypropylene material. DETAILED DESCRIPTION
[0022] All the formulations and materials of the following Examples 1, 2, and 3 were tested according to the Volkswagen PV3900 odor test standard, i.e., 20 g of the sample was placed in a 1L German Volkswagen PV3900 standard odor test bottle, and then placed in an 80° C. oven for 2 hours before being taken out and judged by professional odor testers, and materials with an odor level not exceeding level 3 were preferentially selected.
[0023] Example 1
[0024] This embodiment provides a low-VOC, highly environmentally friendly glass fiber reinforced polypropylene material, which contains the following ingredients: homopolypropylene S2040: 63 parts, short glass fiber T438H: 30 parts; maleic anhydride solid phase grafted polypropylene FT-102: 4 parts; compound antioxidant 3114 / 168 (2:1): 1 part; chemical deodorant GRE-602: 0.5 parts; masterbatch PE2718: 1 part; silicone powder lubricant LYSI-100A: 0.5 parts.
[0025] The preparation steps of the low VOC and highly environmentally friendly glass fiber reinforced polypropylene material are as follows:
[0026] (1) homopolypropylene S2040, maleic anhydride solid phase grafted polypropylene FT-102, compound antioxidant 3114 / 168 (2:1), chemical deodorant GRE-602, masterbatch PE2718, and silicone powder lubricant LYSI-100A were pre-mixed uniformly in a low-speed mixer for 10 minutes to obtain a premix;
[0027] (2) Pour the premix obtained in step (1) into the hopper of a twin-screw extruder weight loss scale, feed the short chopped glass fiber T438H into the extruder from the second to last section of the die head, and extrusion, cooling, and granulation. The screw diameter of the twin-screw extruder is 65 mm, the aspect ratio is 45:1, the extrusion processing temperature is set to 190°C, 200°C, 210°C, 210°C, 210°C, 210°C, 210°C, 205°C, the die head temperature is 205°C, the extrusion speed is 300-500r / min, the vacuum degree is controlled at more than 0.06MPa, and then the formed pellets are placed in an oven with circulating exhaust for dehumidification treatment, the treatment condition is 80°C for 2-4h, and then injection molding standard specimens are tested, and the odor test is tested by professional odor testers according to the PV3900 standard. The specific performance test results are shown in Table 1 below. VOC samples were sent to a third-party specialized testing agency for testing. The specific results are shown in Table 2 below.
[0028] Example 2
[0029] This embodiment provides a low-VOC, highly environmentally friendly glass fiber reinforced polypropylene material, which contains the following ingredients: homopolypropylene V30G: 63 parts, short glass fiber 508A: 30 parts; maleic anhydride solid phase grafted polypropylene CMG5071: 3 parts; compound antioxidant 3114 / 168 (2:1): 1 part; chemical deodorant JH-200: 0.5 parts; masterbatch PE5861: 1 part; silicone powder lubricant LYSI-100A: 0.5 parts.
[0030] The preparation steps of the low VOC and highly environmentally friendly glass fiber reinforced polypropylene material are as follows:
[0031] (1) homopolypropylene V30G, maleic anhydride solid phase grafted polypropylene CMG5071, compound antioxidant 3114 / 168 (2:1), chemical deodorant JH-200, masterbatch PE5861, and silicone powder lubricant LYSI-100A were pre-mixed uniformly in a low-speed mixer for 10 minutes to obtain a premix;
[0032] (2) Pour the premix obtained in step (1) into the hopper of the twin-screw extruder weight loss scale, feed the chopped glass fiber 508A into the extruder from the second-to-last section of the die head, and extrusion, cooling, and granulation. The screw diameter of the twin-screw extruder is 65 mm, the aspect ratio is 45:1, the extrusion processing temperature is set to 190°C, 200°C, 210°C, 210°C, 210°C, 210°C, 210°C, 205°C, the die head temperature is 205°C, the extrusion speed is 300-500r / min, the vacuum degree is controlled at more than 0.06MPa, and then the molded granules are placed in an oven with circulating exhaust for dehumidification treatment, the treatment condition is 80°C for 2-4h, and then injection molding standard specimens are tested, and the odor test is tested by professional odor testers according to the PV3900 standard. The specific performance test results are shown in Table 1 below. VOC samples were sent to a third-party specialized testing agency for testing. The specific results are shown in Table 2 below.
[0033] Example 3
[0034] This embodiment provides a low-VOC, highly environmentally friendly glass fiber reinforced polypropylene material, which contains the following ingredients: copolymer polypropylene BX3800: 63 parts, short glass fiber 305K: 30 parts; maleic anhydride solid phase grafted polypropylene FH118B: 3 parts; compound antioxidant 3114 / 168 (2:1): 1 part; chemical deodorant XC01: 0.5 parts; masterbatch PE2705: 1 part; silicone powder lubricant LYSI-100A: 0.5 parts.
[0035] The preparation steps of the low VOC and highly environmentally friendly glass fiber reinforced polypropylene material are as follows:
[0036] (1) Pre-mixing copolymerized polypropylene BX3800, maleic anhydride solid phase grafted polypropylene FH118B, compound antioxidant 3114 / 168 (2:1), chemical deodorant XC01, masterbatch PE2705, and silicone powder lubricant LYSI-100A in a low-speed mixer for 10 minutes to obtain a premix;
[0037] (2) Pour the premix obtained in step (1) into the hopper of the twin-screw extruder weight loss scale, feed the chopped glass fiber 305K into the extruder from the second-to-last section of the die head, and extrusion, cooling, and granulation. The screw diameter of the twin-screw extruder is 65 mm, the aspect ratio is 45:1, the extrusion processing temperature is set to 190°C, 200°C, 210°C, 210°C, 210°C, 210°C, 210°C, 205°C, the die head temperature is 205°C, the extrusion speed is 300-500r / min, the vacuum degree is controlled at more than 0.06MPa, and then the molded granules are placed in an oven with circulating exhaust for dehumidification treatment, the treatment condition is 80°C for 2-4h, and then injection molding standard specimens are tested, and the odor test is tested by professional odor testers according to the PV3900 standard. The specific performance test results are shown in Table 1 below. VOC samples were sent to a third-party specialized testing agency for testing. The specific results are shown in Table 2 below.
[0038] Comparative Example 1
[0039] The polypropylene material is prepared by selecting the formula components of the existing low-VOC technology, and its ingredients are as follows: copolymer polypropylene K7726H: 63 parts, short glass fiber T438H: 30 parts; maleic anhydride grafted polypropylene KT-1: 4 parts; compound antioxidant 1010 / 168 (1:2): 1 part; chemical deodorant GRE-602: 0.5 parts; masterbatch PE2718: 1 part; lubricant P-130: 0.5 parts.
[0040] The preparation steps of the polypropylene material are as follows:
[0041] (1) Copolymerized polypropylene K7726H, maleic anhydride grafted polypropylene KT-1, compound antioxidant 1010 / 168 (1:2), chemical deodorant GRE-602, masterbatch PE2718, and lubricant P-130 were pre-mixed uniformly in a low-speed mixer for 10 minutes to obtain a premix;
[0042] (2) Pour the premix obtained in step (1) into the hopper of a twin-screw extruder weight loss scale, feed the short chopped glass fiber T438H into the extruder from the second to last section of the die head, and extrusion, cooling, and granulation. The screw diameter of the twin-screw extruder is 65 mm, the aspect ratio is 45:1, the extrusion processing temperature is set to 190°C, 200°C, 210°C, 210°C, 210°C, 210°C, 210°C, 205°C, the die head temperature is 205°C, the extrusion speed is 300-500r / min, the vacuum degree is controlled at more than 0.06MPa, and then the formed pellets are placed in an oven with circulating exhaust for dehumidification treatment, the treatment condition is 80°C for 2-4h, and then injection molding standard specimens are tested, and the odor test is tested by professional odor testers according to the PV3900 standard. The specific performance test results are shown in Table 1 below. VOC samples were sent to a third-party specialized testing agency for testing. The specific results are shown in Table 2 below.
[0043] Table 1
[0044] project Example 1 Example 2 Example 3 Comparative Example 1 Melt index (g / 10min) 9.5 8.4 9.2 8.9 Tensile strength(MPa) 102 96 93 68 Notched impact (KJ / m2) 11 12 19 24 Unnotched impact (KJ / m2) 55 50 64 70 Heat deformation temperature (℃, 1.8MPa) 147 145 140 132 Odor level (PV3900) 2 2 2 4
[0045] Table 2
[0046] Analyze Project Example 1 Example 2 Example 3 Comparative Example 1 Limits benzene ND ND ND ND 50 Toluene ND ND ND 18.5 100 Ethylbenzene ND ND ND ND 100 Xylene ND ND ND 63 100 Styrene ND ND ND ND 100 TVOC 1879 1932 2129 5845 5000 formaldehyde ND ND ND 33 100 Acetaldehyde ND ND ND ND 130 Acrolein ND ND ND ND ND
[0047] Table 2 Notes: The unit is μg / m 3 ND means that the sample is below the detection limit of the instrument and cannot be detected.
[0048] It can be seen from the test results in Table 1 and Table 2 that the odor levels of Examples 1, 2, and 3 composed of raw materials and additives that have been screened are significantly lower than those of the existing conventional low-VOC formula comparison examples that have not been screened, and the TVOC content in their VOC test results is also greatly reduced, and other harmful substances such as formaldehyde, toluene, xylene, etc. are also basically far below environmental protection requirements, indicating that the low-VOC and high-environmental glass fiber reinforced composite materials obtained by this patent can basically be used for automotive interior parts with strict requirements on VOC, as well as parts such as household appliances and electronic appliances with environmental protection requirements.
[0049] The embodiments of the present invention are described in detail above. For those skilled in the art, according to the ideas of the embodiments of the present invention, there may be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A low VOC and highly environmentally friendly glass fiber reinforced polypropylene material, characterized in that The invention contains the following ingredients in parts by mass: polypropylene: 60-80 parts, short glass fiber: 20-40 parts, compatibilizer: 3-5 parts, antioxidant: 0.4-1 parts, deodorant: 0.5-1 parts, masterbatch: 0.5-2 parts, lubricant: 0.1-0.5 parts; the polypropylene, short glass fiber, compatibilizer, antioxidant, deodorant, masterbatch and lubricant are all tested according to the Volkswagen PV3900 odor test standard, and the odor level does not exceed level 3. The detection method is as follows: 20-40g of samples are respectively placed in a 1L German Volkswagen PV3900 standard odor test bottle, and then the test bottle is placed in an oven at 80°C, taken out after 2 hours, and judged by professional odor testers to select polypropylene, short glass fiber, compatibilizer, antioxidant, deodorant, masterbatch and lubricant with an odor level not exceeding level 3; The polypropylene is a homopolymer polypropylene or a copolymer polypropylene, the homopolymer polypropylene is S2040 or V30G, and the copolymer polypropylene is BX3800; The deodorant is GRE-602, JH-200 or XC01, and the masterbatch is PE2718 or PE2705; the chopped glass fiber is an alkali-free chopped glass fiber with a diameter of 10-15 μm and a length of 3-5 mm, and the alkali-free chopped glass fiber is T438H, 508A or 305K; the compatibilizer is maleic anhydride grafted polypropylene, and the maleic anhydride grafted polypropylene is CMG5701; the antioxidant is composed of a main antioxidant and an auxiliary antioxidant in a weight ratio of (1-3):1, and the main antioxidant is 3144 or S80; the auxiliary antioxidant is 168 or 608; the lubricant is silicone powder with a siloxane content not exceeding 40%; the silicone powder is LYSI-100A.
2. A low VOC, highly environmentally friendly glass fiber reinforced polypropylene material as claimed in claim 1, characterized in that The preparation steps of this method are as follows: (1) Premix polypropylene, compatibilizer, antioxidant, deodorant, masterbatch and lubricant in a low-speed mixer for 5-10 minutes to obtain a premix; (2) The premix obtained in step (1) is poured into the feeding hopper of a twin-screw extruder loss-in-weight scale, and short-cut glass fibers are added from the side feeding port of the twin-screw extruder. After melt extrusion through the twin-screw extruder, the premix is pelletized and dried to obtain a low-VOC and highly environmentally friendly glass fiber reinforced polypropylene material.
3. The low VOC and highly environmentally friendly glass fiber reinforced polypropylene material according to claim 2, characterized in that: The screw diameter of the twin-screw extruder is 65 mm, and the aspect ratio is 45:1; the extruder temperature is 180° C.-210° C., the extrusion speed is 300-500 r / min, and the vacuum degree is not less than 0.06 MPa.