Molybdenum, vanadium, titanium and niobium composite oxide negative electrode material and preparation method thereof, and lithium ion battery

By doping titanium niobium oxide with vanadium ions and molybdenum ions, and using a two-step calcination method to prepare molybdenum vanadium titanium niobium composite oxide anode material, the problems of complex preparation process and poor performance of titanium niobium oxide are solved, and lithium ion Improved high rate and cycle performance of batteries.

CN114388772BActive Publication Date: 2024-10-01GREE ALTAIRNANO NEW ENERGY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111499320.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-09
Publication Date
2024-10-01
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

The preparation process of titanium-niobium oxide negative electrode materials in existing lithium batteries is complex, has low conductivity, and poor rate performance and cycle performance.

Method used

By doping titanium niobium oxide with vanadium ions and molybdenum ions, a two-step calcination method is used to prepare the molybdenum vanadium titanium niobium composite oxide negative electrode material, which improves electron mixing and lattice parameters, and improves conductivity and structural stability.

Benefits of technology

It significantly improves the rate performance and cycle performance of lithium-ion batteries, enhances conductivity, simplifies the preparation process, reduces costs, and is suitable for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114388772B_ABST
    Figure CN114388772B_ABST
Patent Text Reader

Abstract

The present invention provides a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material and a preparation method thereof, and a lithium-ion battery. The preparation method comprises step S1, mixing and crushing a first solvent, a niobium source and a titanium source to form a first mixed material, and calcining the first mixed material for the first time to obtain titanium-niobium oxide; step S2, mixing and crushing a second solvent, a vanadium source, a molybdenum source and titanium-niobium oxide to form a second mixed material; and calcining the second mixed material for the second time to obtain a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material. By applying the technical scheme of the present invention, vanadium ions and molybdenum ions can be doped into titanium-niobium oxide to improve electron mixing, increase lattice parameters and unit cell volume, thereby improving the conductivity of the material, and the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material can be directly prepared after two-step calcination, the preparation process is relatively simple, and the rate performance and cycle performance of the battery prepared with the negative electrode material are also significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery materials, and in particular to a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material and a preparation method thereof, and a lithium ion battery. Background Art

[0002] Lithium-ion batteries have the advantages of high specific energy, high operating voltage, and low environmental pollution, and are widely used in energy storage systems and electric vehicles. As one of the most critical links in the lithium-ion battery industry, the production cost of lithium-ion battery negative electrode materials can account for 25-28% of the total battery cost. At present, the negative electrode materials of commercial lithium-ion batteries mainly include carbon materials and lithium titanate materials. Among them, the lithium insertion potential of carbon materials is low, and rapid charging and discharging may form lithium dendrites, which poses certain safety hazards, and has poor kinetic performance under high power; lithium titanate materials have a stable spinel structure. During the charging and discharging process, as lithium ions are inserted and removed, the lithium titanate structure hardly changes. It is known as a "zero strain material" and has a high lithium insertion potential (1.55V), which can effectively avoid the formation of SEI film and safety problems caused by lithium dendrites. However, the theoretical specific capacity of lithium titanate materials is relatively low, only 175mAh / g, which greatly limits the application of lithium titanate.

[0003] In 2011, Goodenough first used titanium niobium oxide TiNb2O7 as the negative electrode material for lithium-ion batteries. The theoretical specific capacity of this material is as high as 385mAh / g, the discharge potential is high, the cycle process is highly reversible, and the high voltage platform can effectively avoid the formation of SEI film. However, there are no unpaired electrons in titanium niobium oxide, which leads to extremely poor conductivity of titanium niobium oxide materials, which are almost insulating. The low electronic conductivity and ionic conductivity lead to a significant reduction in the capacity of titanium niobium oxide materials when they are actually applied to batteries, and the rate performance and cycle performance are poor. In addition, there is a sol-gel preparation method in the prior art, which is to mix the niobium source, titanium source and carbon source solution and centrifuge them to obtain titanium niobium oxide. This method can reduce the calcination temperature and obtain fine particles of titanium niobium oxide. However, the sol-gel method is complicated and difficult to control, and the product has poor cycle characteristics. Carbon coating modification cannot achieve the desired effect. Summary of the invention

[0004] The main purpose of the present invention is to provide a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material and a preparation method thereof, and a lithium-ion battery, so as to solve the problems of complex preparation process, low conductivity, poor rate performance and cycle performance of the titanium-niobium oxide negative electrode material used in lithium batteries in the prior art.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a method for preparing a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material, comprising the following steps: step S1, mixing and crushing a first solvent, a niobium source and a titanium source to form a first mixed material; calcining the first mixed material for the first time to obtain titanium-niobium oxide; step S2, mixing and crushing a second solvent, a vanadium source, a molybdenum source and titanium-niobium oxide to form a second mixed material; calcining the second mixed material for the second time to obtain a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material.

[0006] Further, the niobium source is one or more of niobium pentoxide, niobium ethoxide, niobium pentachloride, and niobium hydroxide; preferably, the niobium source is niobium pentoxide or niobium hydroxide; preferably, the titanium source is one or more of titanium dioxide, metatitanic acid, titanium ethoxide, tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate; more preferably, the titanium source is titanium dioxide or tetrabutyl titanate.

[0007] Further, the vanadium source is one or more of ammonium metavanadate, vanadium pentoxide, sodium metavanadate, and potassium metavanadate; preferably, the vanadium source is ammonium metavanadate or vanadium pentoxide; preferably, the molybdenum source is one or more of molybdenum disulfide, molybdenum dioxide, and ammonium molybdate; more preferably, the molybdenum source is molybdenum disulfide or ammonium molybdate; preferably, the first solvent and the second solvent are independently selected from one or more of ethanol, acetone, isopropanol, and deionized water; more preferably, the first solvent and the second solvent are both ethanol.

[0008] Furthermore, the sum of the molar numbers of niobium in the niobium source, vanadium in the vanadium source and molybdenum in the molybdenum source is denoted as m, and the molar number of titanium in the titanium source is denoted as n, m:n=(2-2.1):1; preferably m:n=(2-2.05):1; preferably, the ratio of the molar number of vanadium in the vanadium source to the molar number of titanium in the titanium source is (0.2-0.6):1, more preferably (0.2-0.5):1; preferably, the ratio of the molar number of molybdenum in the molybdenum source to the molar number of titanium in the titanium source is (0.01-0.05):1, more preferably (0.01-0.03):1.

[0009] Furthermore, the first calcination process includes: heating the first mixed material to 1300-1500°C at a heating rate of 5-7°C / min, and calcining for 12-15h to obtain titanium niobium oxide; preferably, the second calcination process includes: heating the second mixed material to 750-800°C at a heating rate of 8-10°C / min, and calcining for 8-10h to obtain a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material.

[0010] Further, in step S1, the first solvent, niobium source and titanium source are ball-milled for the first time in a high-energy planetary ball mill to obtain a first mixed material; preferably, in step S2, the second solvent, vanadium source, molybdenum source and titanium niobium oxide are ball-milled for the second time in a high-energy planetary ball mill to obtain a second mixed material; more preferably, during the first ball milling process, the revolution speed of the high-energy planetary ball mill is set to 100-150rpm, the rotation speed is set to 550-600rpm, and the ball milling time is 10-12h; further preferably, during the second ball milling process, the revolution speed of the high-energy planetary ball mill is set to 180-200rpm, the rotation speed is set to 750-800rpm, and the ball milling time is 9-10h.

[0011] Furthermore, before the second calcination process is performed, step S2 also includes the process of filtering and drying the second mixed material in sequence.

[0012] According to another aspect of the present invention, a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material is provided, which is prepared by the preparation method of the present invention.

[0013] Furthermore, the general structural formula of the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material is TiNb 2-x-y V x Mo y O7, wherein 0.2≤x≤0.6, 0.01≤y≤0.05; preferably, 0.2≤x≤0.5, 0.01≤y≤0.03.

[0014] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a negative electrode material prepared by the preparation method of the present invention, or the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material of the present invention.

[0015] By applying the technical solution of the present invention, vanadium ions and molybdenum ions can be doped into titanium niobium oxide, and the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material can be directly prepared through two-step calcination, and the preparation process is relatively simple. The present invention can improve electron mixing, increase lattice parameters and unit cell volume by doping vanadium ions and molybdenum ions into titanium niobium oxide at the same time, and the obtained negative electrode material has a small and uniform particle size, maintains better structural stability, and significantly improves conductivity. The negative electrode sheet of a lithium titanate battery made by making a negative electrode slurry with this material and coating it on a current collector is applied to lithium-ion batteries. In addition to the high safety and high capacity of titanium niobium oxide as a negative electrode material, the battery's rate performance and cycle performance are also significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0017] Figure 1 The 10C discharge curves of Example 1 of the present invention and the comparative example are shown;

[0018] Figure 2 The room temperature 2C / 2C cycle curves of Example 1 of the present invention and the comparative example are shown. DETAILED DESCRIPTION

[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0020] As described in the background technology of this application, the prior art has the problems of complex preparation process, low conductivity, poor rate performance and cycle performance of titanium niobium oxide negative electrode materials used in lithium batteries. In view of the above problems, this application provides a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material and its preparation method, and a lithium-ion battery.

[0021] In a typical embodiment of the present application, a method for preparing a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material is provided, comprising step S1, mixing and crushing a first solvent, a niobium source and a titanium source to form a first mixed material; calcining the first mixed material for a first time to obtain titanium-niobium oxide; step S2, mixing and crushing a second solvent, a vanadium source, a molybdenum source and titanium-niobium oxide to form a second mixed material; calcining the second mixed material for a second time to obtain a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material.

[0022] By doping vanadium ions and molybdenum ions in titanium niobium oxide at the same time, the electron mixing in titanium niobium oxide can be improved, the lattice parameters and unit cell volume can be increased, and more defect vacancies appear in the material, which is more conducive to the deintercalation of lithium ions in the negative electrode material. The two-step calcination process can ensure that all niobium and titanium elements can react at the atomic level, and vanadium ions and molybdenum ions can also be uniformly doped, thereby ensuring that the synthesized molybdenum-vanadium-titanium-niobium composite oxide negative electrode material has a complete crystal structure, effectively improving the electronic conductivity and ion diffusion rate of the material, thereby improving the rate performance and cycle performance of the battery. The solid-phase preparation process used in the present invention is simple, and only a small amount of solvent is used in the mixing and crushing stage, so it is more environmentally friendly. In addition, the reaction is easy to control, low cost, and easier to industrialize. The prepared negative electrode material and lithium battery have good crystallization performance, high conductivity, high rate performance and high cycle performance.

[0023] In a preferred embodiment, the niobium source is one or more of niobium pentoxide, niobium ethoxide, niobium pentachloride, and niobium hydroxide. These niobium sources have low steric hindrance during the process of lithium insertion, have the ability to quickly deintercalate lithium, and exhibit good lithium deintercalation performance and good cycle stability. Preferably, the niobium source is niobium pentoxide or niobium hydroxide, and in particular, niobium pentoxide has a three-dimensional porous structure and a quasi-two-dimensional lithium ion storage and migration channel. Its shear surface structure can maintain good structural stability during lithium ion insertion and extraction, and the lithium ion channel formed by the structure is also conducive to the deintercalation and diffusion of lithium ions.

[0024] Preferably, the titanium source is one or more of titanium dioxide, metatitanic acid, titanium ethoxide, tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate; more preferably, the titanium source is titanium dioxide or tetrabutyl titanate. These titanium sources can reduce the charge transfer resistance and shorten the ion diffusion path. In particular, titanium dioxide has the advantages of being non-toxic, low in price, large in reserves, and having a stable chemical structure, which can enable the lithium-ion battery prepared by the negative electrode material to have higher rate performance and cycle performance while greatly reducing the cost.

[0025] The selection of doping materials is crucial to improving the conductivity of titanium niobium oxide. As mentioned above, the present invention selects vanadium ions and molybdenum ions to co-dope titanium niobium oxide to achieve the above-mentioned beneficial effects. In the actual selection process, it is sufficient to use raw materials that can form vanadium oxide and molybdenum oxide during the calcination process. Of course, taking into account the cost of raw materials, environmental protection during the calcination process, etc., in a preferred embodiment, the vanadium source is one or more of ammonium metavanadate, vanadium pentoxide, sodium metavanadate, and potassium metavanadate. In addition to the above advantages, the above-mentioned materials can improve electron mixing, increase lattice parameters and unit cell volume. Preferably, the vanadium source is ammonium metavanadate or vanadium pentoxide. The above-mentioned materials can enable the negative electrode material to maintain better structural stability, and the conductivity is also significantly improved. At the same time, the material structure will also be optimized, which is conducive to further improving the rate performance and cycle stability of the battery.

[0026] Preferably, the molybdenum source is one or more of molybdenum disulfide, molybdenum dioxide or ammonium molybdate; more preferably, the molybdenum source is molybdenum disulfide or ammonium molybdate; these molybdenum sources can achieve the purpose of improving the electronic conductivity and structural stability of the negative electrode material by doping a small amount in the negative electrode material. In particular, the co-doping of molybdenum disulfide with a vanadium source can provide more two-dimensional channels for lithium ion transmission, reduce charge transfer resistance, shorten the ion diffusion path, and provide more active sites for lithium storage, thereby better improving the conductivity and forming a more stable lattice structure, and further improving the conductivity of the titanium niobium oxide after doping, which is conducive to further improving the battery rate performance and cycle performance.

[0027] In the two ball milling processes, the first solvent and the second solvent are independently selected from one or more of ethanol, acetone, isopropanol, and deionized water; more preferably, the first solvent and the second solvent are both ethanol. These solvents have good wetting or dispersibility for each raw material, which is conducive to building a stable mixed system and obtaining a material with a small and uniform particle size. At the same time, they have a low boiling point, are easy to volatilize, have little residue, and have little impact on the subsequent reaction system.

[0028] In a preferred embodiment, the sum of the molar numbers of niobium in the niobium source, vanadium in the vanadium source and molybdenum in the molybdenum source is denoted as m, and the molar number of titanium in the titanium source is denoted as n, m:n=(2-2.1):1, more preferably m:n=(2-2.05):1; preferably, the ratio of the molar number of vanadium in the vanadium source to the molar number of titanium in the titanium source is (0.2-0.6):1, more preferably (0.2-0.5):1; preferably, the ratio of the molar number of molybdenum in the molybdenum source to the molar number of titanium in the titanium source is (0.01-0.05):1, more preferably (0.01-0.03):1. This ratio is conducive to more uniform doping of vanadium ions and molybdenum ions into titanium niobium oxide, thereby better improving the electrical conductivity of titanium niobium oxide and avoiding the situation where the conductivity improvement effect is not obvious, or impurities are generated, which destroys the original crystal structure of titanium niobium oxide, hinders the transmission of lithium ions and electrons, and causes battery performance to decline. The prepared negative electrode material has a better electrochemical capacity and can be applied to lithium-ion batteries to obtain better balanced cycle performance and rate performance.

[0029] In order to make the doping process more stable and further improve the uniformity of doping, in a preferred embodiment, the first calcination process includes: heating the first mixed material to 1300-1500°C at a heating rate of 5-7°C / min, and calcining for 12-15h to obtain titanium niobium oxide; preferably, the second calcination process includes: heating the second mixed material to 750-800°C at a heating rate of 8-10°C / min, and calcining for 8-10h to obtain molybdenum vanadium titanium niobium composite oxide negative electrode material. Controlling the reaction temperature and time within the above range is more conducive to the uniformity of doping, and is conducive to avoiding the generation of impurities that may be caused by excessive temperature, which has a better improvement in the doping effect, thereby being more conducive to the performance improvement of titanium niobium oxide, and further improving the conductivity of the molybdenum vanadium titanium niobium composite oxide negative electrode material after doping, thereby being conducive to better improvement of battery rate performance and cycle performance.

[0030] In a preferred embodiment, in step S1, the first solvent, niobium source and titanium source are subjected to a first ball milling in a high-energy planetary ball mill to obtain a first mixed material; preferably, in step S2, the second solvent, vanadium source, molybdenum source and titanium niobium oxide are subjected to a second ball milling in a high-energy planetary ball mill to obtain a second mixed material. Ball milling the material before calcination can crush the material to the target particle size in a short time and with high efficiency. At the same time, wet ball milling can utilize solvent to assist grinding, reduce the impact force on the grinding balls, and reduce the impact and collision loss of the ball mill.

[0031] Preferably, during the first ball milling process, the revolution speed of the high-energy planetary ball mill is set to 100-150rpm, the rotation speed is set to 550-600rpm, and the ball milling time is 10-12h; preferably, during the second ball milling process, the revolution speed of the high-energy planetary ball mill is set to 180-200rpm, the rotation speed is set to 750-800rpm, and the ball milling time is 9-10h. Under this ball milling condition, the material has a higher degree of pulverization, which is conducive to the improvement of the molding density, and the corresponding sintering density will also be higher, which is more conducive to the uniform mixing of different materials in the subsequent calcination process.

[0032] In addition, in a preferred embodiment, before the second calcination process, step S2 also includes filtering and drying the second mixed material in sequence, which can remove the second solvent, reduce the burden of subsequent calcination, and make the preparation process more environmentally friendly and energy-saving.

[0033] According to another aspect of the present invention, a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material is provided. The negative electrode material is prepared by the preparation method of the present invention. Under the co-doping effect of vanadium ions and molybdenum ions, more defect vacancies appear in the material, which is more conducive to the deintercalation of lithium ions in the negative electrode material. The negative electrode material has a complete crystal structure, and the electronic conductivity and ion diffusion rate are significantly improved, so that the rate performance and cycle performance of the battery are also improved.

[0034] Preferably, the general structural formula is TiNb 2-x-y V x Mo y O7, wherein 0.2≤x≤0.6, 0.01≤y≤0.05; more preferably, 0.2≤x≤0.5, 0.01≤y≤0.03. This ratio is conducive to more uniform doping of vanadium ions and molybdenum ions in titanium niobium oxide, thereby improving the conductivity of titanium niobium oxide, and the prepared negative electrode material can also obtain better high conductivity, and can also obtain high rate performance and high cycle performance when applied to lithium ion batteries. Compared with the sol-gel method, the preparation method used in the present invention has a simpler preparation process, milder reaction conditions, lower cost, and is suitable for large-scale industrial applications.

[0035] According to another aspect of the present invention, a lithium-ion battery is provided, including a negative electrode material, the negative electrode material is prepared by the preparation method of the present invention, or is the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material of the present invention. The negative electrode material used has good lithium insertion and extraction performance and good cycle stability and structural stability, and the conductivity is further improved. The negative electrode slurry made of this material is coated on the current collector to form a negative electrode sheet. The prepared lithium-ion battery has high rate performance and cycle performance, and the electrochemical capacity is also good. It also overcomes the defect of low battery conductivity when the traditional titanium-niobium composite oxide is used as the negative electrode material. In addition to the significant improvement in conductivity, a lithium-ion battery with good rate performance and cycle performance is obtained as a whole.

[0036] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0037] Comparative Example 1

[0038] Add 500 g of anhydrous ethanol, 200 g of niobium pentoxide, and 74.3 g of titanium dioxide into a high-energy planetary ball mill. Set the orbital speed of the ball mill to 150 rpm and the rotation speed to 600 rpm. After ball milling for 12 hours, heat the mixture to 1500°C at a rate of 7°C / min and calcine it in air for 12 hours. Grind the calcined material to obtain titanium niobium oxide TiNb2O7 negative electrode material.

[0039] Example 1

[0040] Step 1 Preparation of titanium niobium oxide: Add 500 g of anhydrous ethanol, 200 g of niobium pentoxide, and 74.3 g of titanium dioxide to a high-energy planetary ball mill. Set the orbital speed of the ball mill to 150 rpm and the rotation speed to 600 rpm. After ball milling in the ball mill for 12 hours, heat it to 1500°C at a rate of 7°C / min and calcine it in air for 12 hours. Grind the calcined material to obtain titanium niobium oxide TiNb2O7 material.

[0041] Step 2 Preparation of molybdenum-vanadium-titanium-niobium composite oxide negative electrode material: Weigh 200g of TiNb2O7 material prepared in step 1 (containing 0.58mol Ti and 1.16mol Nb), 20.358g of ammonium metavanadate (containing 0.174mol V), and 1.856g of molybdenum disulfide (containing 0.0116mol Mo), add them to a high-energy planetary ball mill, and add 500g of anhydrous ethanol. The ball mill revolution speed is set to 200rpm, and the rotation speed is set to 800rpm. Ball milling in the ball mill for 10h. After the end, the ball milling mixture is filtered to remove the solvent, dried in an environment of 100℃, and transferred to a crucible, and then the crucible is placed in a muffle furnace for calcination, and the temperature is increased to 800℃ at a rate of 8℃ / min and calcined for 10h to obtain TiNb 1.68 V 0.3 Mo 0.02 The product O7 is further subjected to mechanical pulverization to obtain a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material.

[0042] Example 2

[0043] The difference between Example 2 and Example 1 is that in step 2, 27.144 g of ammonium metavanadate (containing 0.232 mol of V) and 0.928 g of molybdenum disulfide (containing 0.0058 mol of Mo) are weighed, and the muffle furnace calcination temperature is 850 ° C. Finally, the composite oxide negative electrode material TiNb is obtained. 1.59 V 0.4 Mo 0.01 O7.

[0044] Example 3

[0045] The only difference between Example 3 and Example 1 is that in step 2, 13.572 g of ammonium metavanadate (containing 0.116 mol of V) and 2.784 g of molybdenum disulfide (containing 0.0174 mol of Mo) are weighed, and the muffle furnace calcination temperature is 850 ° C. Finally, the composite oxide negative electrode material TiNb 1.77 V 0.2 Mo 0.03 O7.

[0046] Example 4

[0047] The only difference between Example 4 and Example 1 is that in step 2, 33.930 g of ammonium metavanadate (containing 0.290 mol of V) and 0.928 g of molybdenum dioxide (containing 0.0058 mol of Mo) are weighed, and the muffle furnace calcination temperature is 900 ° C. Finally, the composite oxide negative electrode material TiNb 1.49 V 0.5 Mo 0.01 O7.

[0048] Example 5

[0049] The only difference between Example 5 and Example 1 is that in step 2, 40.716 g of ammonium metavanadate (containing 0.348 mol of V) and 4.640 g of molybdenum dioxide (containing 0.0290 mol of Mo) are weighed, and the muffle furnace calcination temperature is 800 ° C. Finally, the composite oxide negative electrode material TiNb 1.35 V 0.6 Mo 0.05 O7.

[0050] Example 6

[0051] The only difference between Example 6 and Example 1 is that in step 2, 6.786 g of ammonium metavanadate (containing 0.058 mol of V) and 0.464 g of molybdenum dioxide (containing 0.0029 mol of Mo) are weighed, and the muffle furnace calcination temperature is 850°C to finally obtain the composite oxide negative electrode material TiNb 1.895 V 0.1 Mo 0.005 O7.

[0052] Example 7

[0053] The only difference between Example 7 and Example 1 is that in step 2, 54.288 g of ammonium metavanadate (containing 0.464 mol of V) and 6.496 g of molybdenum dioxide (containing 0.0406 mol of Mo) are weighed, and the muffle furnace calcination temperature is 850 ° C. Finally, the composite oxide negative electrode material TiNb 1.13 V 0.8 Mo 0.07 O7.

[0054] The resistance of each material prepared in the comparative example and embodiments 1 to 7 was tested using a resistance tester. The results are shown in Table 1.

[0055] Performance Test:

[0056] The materials, conductive agent and binder prepared in Comparative Example 1 and Examples 1 to 7 were mixed uniformly in a mass ratio of 92:4.5:3.5, wherein the conductive agent used SP: carbon nanotubes = 3:1, and the binder used PVDF (900:5130 = 2:1), and the solvent N-methylpyrrolidone was added and stirred uniformly to obtain a negative electrode slurry with a solid content of 54.5%, and the slurry was evenly coated on the current collector carbon coated aluminum foil, and then dried, and rolled and cut to obtain a negative electrode sheet. NCM111: conductive agent: binder was mixed uniformly in a mass ratio of 94:3:3, wherein the conductive agent used acetylene black: SP = 1:2, and the binder used PVDF (900:5130 = 2:1), and the solvent N-methylpyrrolidone was added and stirred uniformly to obtain a positive electrode slurry with a solid content of 65%, and the slurry was evenly coated on the current collector carbon coated aluminum foil, and then dried, and rolled and cut to obtain a positive electrode sheet. The positive electrode plate, negative electrode plate and polypropylene isolation film are assembled into a 2Ah small soft-pack battery using a stacking process. After liquid injection and standing, they are charged and discharged at a constant current and constant voltage with a current of 1C, and then aged at high temperature for 24 to 48 hours. The battery is then tested for its electrochemical properties, and the charge and discharge cut-off voltage is 1.5 to 2.9V.

[0057] 1) Discharge test

[0058] After the soft pack battery is assembled, perform 1C discharge: ① discharge: 2A constant current discharge to 1.5V; ② charge: 2A constant current charge to 2.9V; the discharge specific capacity is recorded as Q1.

[0059] 10C discharge: ①Discharge: 20A constant current discharge to 1.5V; ②Charge: 20A constant current charge to 2.9V; the discharge specific capacity is recorded as Q10.

[0060] 2) Cycle performance test

[0061] ①Discharge: 4A constant current discharge to 1.5V, interval 10min; ②Charge: 4A constant current charge to 2.9V, interval 10min; ③Repeat "①, ②" 2000 times, calculate the capacity retention rate.

[0062] 3) Rate performance test

[0063] ① Discharge the battery to 1.5V at a constant current of 6A, wait for 10 minutes, and then charge it to 2.9V at a constant current of 6A; ② Repeat ① 10 times; ③ Increase the current density in "①, ②" to 12A and 20A, and calculate the capacity retention rate.

[0064] The performance test results of the comparative examples and embodiments 1 to 7 are shown in Table 1. The 10C discharge curves of the comparative examples and embodiment 1 are shown in Table Figure 1 , normal temperature 2C / 2C cycle curve see Figure 2 .

[0065] Table 1

[0066]

[0067] As can be seen from Table 1, the comparative example directly uses titanium niobium oxide as the negative electrode material, the resistivity is large, the conductivity is low, and the prepared lithium ion battery rate performance and cycle performance are poor. In comparison, the molybdenum vanadium titanium niobium composite oxide negative electrode material prepared by the preparation method provided by the present invention in Examples 1 to 7, especially the negative electrode material doped with vanadium ions and molybdenum ions according to the preferred ratio, has a significantly reduced resistivity and a high conductivity, and the rate performance and cycle performance of the prepared lithium ion battery have been significantly improved, and can better take into account the conductivity, rate performance and cycle performance.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a molybdenum-vanadium-titanium-niobium composite oxide negative electrode material, characterized in that: The following steps are involved: Step S1, mixing and crushing a first solvent, a niobium source and a titanium source to form a first mixed material; calcining the first mixed material for the first time to obtain titanium niobium oxide; Step S2, mixing and grinding the second solvent, the vanadium source, the molybdenum source and the titanium niobium oxide to form a second mixed material; calcining the second mixed material for a second time to obtain the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material; The first calcination process comprises: heating the first mixed material to 1300-1500° C. at a heating rate of 5-7° C. / min, and calcining for 12-15 hours to obtain the titanium niobium oxide; The second calcination process includes: heating the second mixed material to 750-800° C. at a heating rate of 8-10° C. / min, and calcining for 8-10 hours to obtain the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material.

2. The preparation method according to claim 1, characterized in that: The niobium source is one or more of niobium pentoxide, niobium ethoxide, niobium pentachloride and niobium hydroxide.

3. The preparation method according to claim 2, characterized in that: The niobium source is niobium pentoxide or niobium hydroxide.

4. The preparation method according to claim 2, characterized in that: The titanium source is one or more of titanium dioxide, metatitanic acid, titanium ethoxide, tetrabutyl titanate, tetraethyl titanate, and tetraisopropyl titanate.

5. The preparation method according to claim 2, characterized in that: The titanium source is titanium dioxide or tetrabutyl titanate.

6. The preparation method according to claim 1 or 2, characterized in that: The vanadium source is one or more of ammonium metavanadate, vanadium pentoxide, sodium metavanadate, and potassium metavanadate.

7. The preparation method according to claim 6, characterized in that: The vanadium source is ammonium metavanadate or vanadium pentoxide.

8. The preparation method according to claim 6, characterized in that: The molybdenum source is one or more of molybdenum disulfide, molybdenum dioxide, and ammonium molybdate.

9. The preparation method according to claim 6, characterized in that: The molybdenum source is molybdenum disulfide or ammonium molybdate.

10. The preparation method according to claim 6, characterized in that: The first solvent and the second solvent are independently selected from one or more of ethanol, acetone, isopropanol, and deionized water.

11. The preparation method according to claim 6, characterized in that: The first solvent and the second solvent are both ethanol.

12. The preparation method according to claim 1 or 2, characterized in that: The sum of the molar numbers of niobium in the niobium source, vanadium in the vanadium source and molybdenum in the molybdenum source is denoted as m, and the molar number of titanium in the titanium source is denoted as n, m:n=(2-2.1):

1.

13. The preparation method according to claim 12, characterized in that: m:n=(2~2.05):

1.

14. The preparation method according to claim 12, characterized in that: The molar ratio of the vanadium element in the vanadium source to the titanium element in the titanium source is (0.2-0.6):

1.

15. The preparation method according to claim 12, characterized in that: The molar ratio of the vanadium element in the vanadium source to the titanium element in the titanium source is (0.2-0.5):

1.

16. The preparation method according to claim 12, characterized in that: The molar ratio of the molybdenum element in the molybdenum source to the titanium element in the titanium source is (0.01-0.05):

1.

17. The preparation method according to claim 12, characterized in that: The molar ratio of the molybdenum element in the molybdenum source to the titanium element in the titanium source is (0.01-0.03):

1.

18. The preparation method according to claim 1 or 2, characterized in that: In the step S1, the first solvent, the niobium source and the titanium source are subjected to a first ball milling in a high-energy planetary ball mill to obtain the first mixed material.

19. The preparation method according to claim 18, characterized in that: In the step S2, the second solvent, the vanadium source, the molybdenum source and the titanium niobium oxide are subjected to a second ball milling in a high-energy planetary ball mill to obtain the second mixed material.

20. The preparation method according to claim 18, characterized in that: During the first ball milling process, the revolution speed of the high-energy planetary ball mill is set to 100-150 rpm, the rotation speed is set to 550-600 rpm, and the ball milling time is 10-12 hours.

21. The preparation method according to claim 19, characterized in that: During the second ball milling process, the revolution speed of the high-energy planetary ball mill is set to 180-200 rpm, the rotation speed is set to 750-800 rpm, and the ball milling time is 9-10 hours.

22. The preparation method according to claim 1 or 2, characterized in that: Before the second calcination process is performed, the step S2 further includes filtering and drying the second mixed material in sequence.

23. A molybdenum-vanadium-titanium-niobium composite oxide negative electrode material, characterized in that: Prepared by the preparation method described in any one of claims 1 to 22.

24. The molybdenum-vanadium-titanium-niobium composite oxide negative electrode material according to claim 23, characterized in that: The structural formula of the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material is TiNb 2-x-y V x Mo y O7, where 0.2≤x≤0.6, 0.01≤y≤0.

05.

25. The molybdenum-vanadium-titanium-niobium composite oxide negative electrode material according to claim 24, characterized in that: 0.2≤x≤0.5, 0.01≤y≤0.

03.

26. A lithium ion battery comprising a negative electrode material, characterized in that: The negative electrode material is prepared by the preparation method described in any one of claims 1 to 22, or is the molybdenum-vanadium-titanium-niobium composite oxide negative electrode material described in any one of claims 23 to 25.