Grafted polyvinyl alcohol polymers, formulations containing the same, and creping methods
The polyvinyl alcohol polymer formed by graft polymerization solves the problems of high cost and unstable operation in paper towel manufacturing, provides low viscosity and stable aqueous solutions, suitable for high concentrations of adhesives present in water, and improves the Wrinkle performance and ease of operation.
Patent Information
- Application Number
- CN202080063922.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-11
- Filing Date
- 2020-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-09-03
AI Technical Summary
The existing unmodified polyvinyl alcohol (PVOH) is used in paper towel manufacturing for wrinkling, which has high cost, unstable operation and large viscosity changes, resulting in uneven wrinkling and other operational problems, and its water properties are The solution is easily turned into an irreversible gel, affecting factory operations.
Grafted polyvinyl alcohol polymer is formed by graft polymerization, and monomers such as aliphatic carboxylic acid, aliphatic amide, hydroxylated alkyl acrylate, etc. are added to form an aqueous solution with low viscosity and stability, suitable for high concentrations The binder present in water and maintains dispersibility at high pH.
Cost-effective and highly stable wrinkle adhesive is realized, reducing gel formation, improving wrinkle performance and operational ease, and reducing transportation and storage costs.
Smart Images

Figure BDA0003542641070000111 
Figure BDA0003542641070000201 
Figure BDA0003542641070000211
Abstract
Description
[0001] This application claims the benefit of prior U.S. Provisional Patent Application No. 62 / 898,719, filed on September 11, 2019, under 35 U.S.C. §119(e), the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to grafted polyvinyl alcohol polymers and formulations comprising the polymers, such as creping adhesive formulations or Yankee dryer coating compositions. The present invention further relates to methods for creping and methods for imparting tack and release characteristics and / or properties to creped products comprising such formulations. For purposes of the present invention, by Yankee dryer, it includes a rotary dryer commonly used for creping. By Yankee coating, Yankee surface, and the like, it includes rotary dryer coatings and surfaces. Background Art
[0003] To form a thin paper web from a slurry of water and fibers, the wet web is dewatered and the dewatered web is then at least partially dried. In the manufacture of tissue and similar paper products, creping is often used on such dewatered webs to impart desired properties, such as softness and bulk. Typically, creping is accomplished by transferring or conveying the web on a fabric to a heated rotating drum, sometimes called a Yankee dryer. Before the web reaches the disengagement zone of the web from the drum, the web is typically transferred to the adhesive dryer surface of the dryer and conveyed around the main circumference of the dryer. The disengagement zone is equipped with a creping blade against which the web abuts so as to be pushed or compacted back in the machine direction of the web and obtain the well-known tissue crepe paper structure, at which point the resulting creped web is removed from the dryer and collected (usually in roll form).
[0004] Prior to transferring the web to the Yankee dryer, an adhesive composition (sometimes referred to in the industry as a "coating package") is typically applied directly to the dryer surface of the dryer to form an adhesive dryer surface. The creping action typically requires that the web have some adhesion to the outer surface of the dryer to achieve a consistent and uniform creping action. For drying and creping purposes, creping adhesives (alone or in combination with release agents or other adjuvants) have been applied to the web or dryer surface in an effort to provide some balance of adhesion and release between the web and the dryer surface.
[0005] Various properties of the creping adhesive can be factors in achieving creping performance. The degree of adhesion of the creping adhesive to the dryer surface of the drum can be another factor that affects creping performance and results. Inadequate adhesion can result in poor creping, sheet floating, poor sheet handling, or other problems, whereas excessive adhesion can result in creping blade picking, web jamming behind the creping blade, web breaks due to excessive tension, or other problems.
[0006] Various types of creping adhesives have been used to adhere fiber webs to rotary dryers such as Yankee dryers. Unmodified polyvinyl alcohol ("PVOH") is known and has been used as an adhesive in the creping process. Although widely available and cost effective, it tends to coat the dryer with a hard and uneven film that builds up as drying and creping proceeds, causing uneven creping or other problems. Another disadvantage of unmodified PVOH is found in the handling of PVOH at the mill, where PVOH is often obtained off-site and must be shipped to the mill. Due to its molecular weight and its ability to gel in aqueous solution, the total amount of PVOH in water is often low, such as 8% by weight. Therefore, a "concentrated" or bulk amount of PVOH is actually a very low concentration of PVOH, which significantly increases the cost of shipping the PVOH to the paper mill.
[0007] Another disadvantage of aqueous solutions of PVOH is the tendency of these aqueous solutions to increase in viscosity over time. Based on solid content, degree of hydrolysis, and molecular weight, aqueous solutions of PVOH can reach viscosities as high as 2,000-100,000 cP·s, making it difficult to handle PVOH at the factory. In addition, at a certain point (e.g., a few days to a few months, depending on the molecular weight and degree of hydrolysis of the PVOH), aqueous solutions of PVOH can irreversibly turn into a gel, making PVOH essentially unusable as an adhesive composition in the corrugation process.
[0008] Existing graft polymerizations using PVOH have primarily involved graft polymerizations of vinyl monomers such as vinyl acetate, vinyl pyrrolidone, ethylene, and vinyl esters. Some acrylic monomers have been included in the monomer mixture, but past graft polymerizations have found problems with graft polymerizations of acrylic monomers because, in the presence of PVOH, the polymerization rate is too high, resulting in very large particles and agglomeration.
[0009] In view of the foregoing, there is a need for improved PVOH compositions that address the disadvantages discussed above. In particular, it would be desirable to provide formulations that address the disadvantages presented by unmodified PVOH in terms of cost and handling. In addition, it would be desirable to have a PVOH that is more storage stable over time, thereby reducing the waste associated with PVOH compositions that gel over time and irreversibly form highly viscous gels. The present invention provides these solutions, including providing methods and formulations that better address these problems. In addition, it would be desirable to graft polymerize acrylic monomers in the presence of PVOH polymers to form new grafted polyvinyl alcohol polymers. Summary of the invention
[0010] One feature of the present invention is to provide an improved PVOH formulation that can be used in a paper mill in a cost-effective manner.
[0011] Another feature of the present invention is to provide PVOH-based adhesives that can be present in high concentrations in water-based liquids.
[0012] It is a further feature of the present invention to provide improved PVOH formulations that are storage stable over extended periods of time.
[0013] Another feature of the present invention is to provide PVOH-based formulations that can become more dispersible at high pH (eg, pH 8, where unmodified PVOH can form irreversible gels).
[0014] It is a further feature of the present invention to provide PVOH-based formulations having low viscosities at a variety of concentrations.
[0015] Other features and advantages of the present invention will be described in part in the following description, and, in part, will be clear from this description, or can be known through the practice of the present invention. The purpose and other advantages of the present invention will be realized and obtained through the elements and combinations particularly pointed out in this description and the appended claims.
[0016] According to the present invention, one or more of the aforementioned features have been achieved by providing a grafted polyvinyl alcohol polymer of the present invention. The grafted polyvinyl alcohol polymer has or includes a polyvinyl alcohol backbone and a plurality of side chains grafted to the polyvinyl alcohol backbone. One or more side chains from the plurality of side chains have one or more units selected from the group consisting of aliphatic carboxylic acids, aliphatic amides, hydroxylated alkyl (meth) acrylates, and / or alkylamino (meth) acrylates, and / or any combination thereof.
[0017] The present invention further relates to such a formulation, which comprises an aqueous phase and the grafted polyvinyl alcohol polymer of the present invention. For example, the formulation may consist of 100 parts by weight of an aqueous phase and 10 to 40 parts by weight of a grafted polyvinyl alcohol polymer. The grafted polyvinyl alcohol polymer is dispersed in the aqueous phase.
[0018] The present invention further relates to a method for producing an aqueous solution of a grafted polyvinyl alcohol polymer according to the present invention. The method may comprise the steps of adding a base to the dispersion, thereby raising the pH of the dispersion to 4 to 8 or from 5 to 8, and forming an aqueous solution of the grafted polyvinyl alcohol polymer. In the method, the dispersion comprises an aqueous phase and a grafted polyvinyl alcohol polymer dispersed in the aqueous phase. Prior to the adding step, the dispersion may have a pH of 2 to 5 or 2 to 3.
[0019] The present invention further relates to a process for creping a fiber web. The process may include the steps of providing a rotating cylindrical dryer including a dryer surface, and applying a formulation comprising a grafted polyvinyl alcohol polymer of the present invention to the dryer surface. In the process, a fiber web may be conveyed to the dryer surface. Furthermore, the fiber web may be dried on the dryer surface to form a dried fiber web, and the dried fiber web may then be creped from the dryer surface.
[0020] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are intended to provide further explanation of the invention as claimed. DETAILED DESCRIPTION
[0021] The present invention relates to grafted polyvinyl alcohol polymers and formulations comprising the grafted polyvinyl alcohol polymers of the present invention. The formulation can be a creping adhesive formulation or a Yankee dryer coating composition. The adhesive formulation can provide tack and release properties to the fiber web when the fiber web is located on a Yankee dryer or dryer surface. Unless otherwise specified, for "polymer" or "the polymer" herein, it refers to the grafted polyvinyl alcohol polymer of the present invention.
[0022] As used herein, "monomer" (e.g., aliphatic carboxylic acid, aliphatic amide, aminoalkyl (meth)acrylate, hydroxylated alkyl (meth)acrylate, or any combination thereof) refers to a molecule that is capable of reacting to form a polymer by chemically bonding with a monomer, such as itself or other monomers or monomeric units or backbones.
[0023] As used herein, a "monomeric unit" or "unit" (eg, a unit of an aliphatic carboxylic acid, etc.) refers to a chemically bonded unit in a polymer derived from a monomer.
[0024] It should be understood that although monomers or monomer units are described or mentioned herein, the grafted polymer itself has the radical form of each monomer and is therefore referred to as a monomeric unit or monomeric unit (e.g., aliphatic carboxylic acid, aliphatic amide, aminoalkyl (meth) acrylate, hydroxylated alkyl (meth) acrylate, or any combination thereof). Therefore, the reactive functional group (or multiple reactive functional groups) in each monomer described herein is opened or reacted during the polymerization reaction (e.g., such as vinyl or hydroxyl or carbonyl). In such a reaction, the terminal groups of the polymer formed are retained. Therefore, the polymer of the present invention has the structural repeating unit of the monomeric unit described herein. The polymer or grafted polymer can be considered to be a polymer derived from the monomer described herein and the polyvinyl alcohol part as the main chain.
[0025] The grafted polyvinyl alcohol polymer of the present invention comprises, consists essentially of, consists of, includes, or is a polyvinyl alcohol backbone and a plurality of side chains grafted to the polyvinyl alcohol backbone. One or more side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include one or more units selected from aliphatic carboxylic acids, aliphatic amides, hydroxylated alkyl (meth) acrylates, and / or alkylamino (meth) acrylates, or any combination thereof.
[0026] As an explanation for the phrase "one or more side chains ...", the phrase refers to the fact that the grafted polyvinyl alcohol polymer of the present invention has side chains and all or some or one of the side chains may include or be aliphatic carboxylic acids, aliphatic amides, alkylamino (meth) acrylates, and / or hydroxylated alkyl (meth) acrylates. Typically, the total percentage of side chains (which include or are aliphatic carboxylic acids, aliphatic amides, alkylamino (meth) acrylates, and / or hydroxylated alkyl (meth) acrylates) is at least 10% (by number), or at least 25% (by number), or at least 50% (by number), or at least 75% (by number), or at least 85% (by number), or at least 95% (by number), for example, 10% to 100%, 30% to 100%, 30% to 90%, 30% to 80%, or 40% to 100% (all percentages are by number). When the side chain is not, or does not include, an aliphatic carboxylic acid, an aliphatic amide, an alkylamino(meth)acrylate, and / or a hydroxylated alkyl(meth)acrylate, the side chain may be an acetate moiety or an alcohol moiety.
[0027] When the side chain includes or is an aliphatic carboxylic acid, an aliphatic amide, an alkylamino (meth) acrylate, and / or a hydroxylated alkyl (meth) acrylate, it is understood that one, two, three or all four of these side chains may be present in a single side chain. Moreover, each side chain (which includes or is an aliphatic carboxylic acid, an aliphatic amide, an alkylamino (meth) acrylate, and / or a hydroxylated alkyl (meth) acrylate) may be the same or different from the other side chains. When the side chain includes an aliphatic carboxylic acid, an aliphatic amide, an alkylamino (meth) acrylate, and / or a hydroxylated alkyl (meth) acrylate, the side chain may optionally include one or more of the following substituents: hydroxypropyl methacrylate, vinyl acetate, N-vinyl pyrrolidone, 4-hydroxybutyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl caprolactone acrylate, ethylene glycol acrylate, stearyl polyethylene glycol methacrylate, N-(3-aminopropyl)-2-acrylamide, N-(3-aminopropyl) methacrylamide hydrochloride.
[0028] As an option, one or more side chains from the plurality of side chains comprise, consist essentially of, consist of, or include: aliphatic carboxylic acid units, aliphatic amide units, and hydroxylated alkyl (meth) acrylate units. As a further option, one or more side chains from the plurality of side chains comprise, consist essentially of, consist of, or include: aliphatic carboxylic acid units, aliphatic amide units, alkylamino (meth) acrylate units, and hydroxylated alkyl (meth) acrylate units. In these examples of grafted polyvinyl alcohol polymers of the present invention, at least one side chain has units of all three of aliphatic carboxylic acid, aliphatic amide, and hydroxylated alkyl (meth) acrylate. The side chain itself can be considered a copolymer or terpolymer of these monomers.
[0029] As another option, one or more side chains from the plurality of side chains comprise, consist essentially of, consist of, or include: aliphatic carboxylic acid units; aliphatic amide units; hydroxylated alkyl (meth) acrylate units; or alkylamino (meth) acrylate units. In these examples of grafted polyvinyl alcohol polymers of the present invention, at least one side chain has only aliphatic carboxylic acid units, or only aliphatic amide units, or only hydroxylated alkyl (meth) acrylate units, or only alkylamino (meth) acrylate units. The side chain itself can be considered a homopolymer of the monomer used to make the side chain.
[0030] As another option, one or more side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include both aliphatic carboxylic acid units and aliphatic amide units. Alternatively, or in addition to the previous options, one or more of the side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include both aliphatic carboxylic acid units and hydroxylated alkyl (meth) acrylate units. Alternatively, or in addition to the previous options, one or more of the side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include both aliphatic amide units and hydroxylated alkyl (meth) acrylate units. Alternatively, or in addition to the previous options, one or more of the side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include both aliphatic amide units and alkylamino (meth) acrylate units. Alternatively, or in addition to the previous options, one or more of the side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include both alkylamino(meth)acrylate units and hydroxylated alkyl(meth)acrylate units. Alternatively, or in addition to the previous options, one or more of the side chains from the plurality of side chains may comprise, consist essentially of, consist of, or include both alkylamino(meth)acrylate units and aliphatic carboxylic acid units. In each of these examples of the grafted polyvinyl alcohol polymer of the present invention, at least one side chain has units of two of aliphatic carboxylic acid, aliphatic amide, alkylamino(meth)acrylate, and hydroxylated alkyl(meth)acrylate. The side chain itself may be considered a copolymer of the two monomers used to make the side chain.
[0031] When present in an aqueous solution having a pH of 3 to 5 (e.g., 3) at a concentration of 22.5 to 25% by weight at 25° C. and 1 atmosphere, the grafted polyvinyl alcohol polymer of the present invention may have a viscosity of less than 500 cP·s. The viscosity may be less than 300 cP·s, less than 250 cP·s, less than 200 cP·s, less than 150 cP·s, or less than 100 cP·s. Viscosity is generally considered to be an intrinsic property, and therefore, if not in a superfluid state, an aqueous solution of a polymer has a positive, non-zero viscosity value. Therefore, the minimum values of these ranges may be 0.001 cP·s, or 0.005 cP·s, or 0.01 cP·s, or 0.1 cP·s.
[0032] Any viscometer (or viscometer) suitable for measuring the viscosity of a fluid can be used to measure the viscosity of the grafted polyvinyl alcohol polymer in aqueous solution.
[0033] The grafted polyvinyl alcohol polymer of the present invention can be dispersed in an aqueous solution at a concentration of 0.1% to 40% by weight or more (e.g., 1% to 40% by weight, or 5% to 40% by weight, or 10% to 40% by weight). All values between 10% and 40% by weight are included in the range, including the endpoints. For example, the concentration of the polymer can be 12% to 38% by weight, or 15% to 35% by weight, or 20% to 30% by weight, or 25% to 28% by weight. As used herein, weight percentage is defined as the weight of the solute divided by the weight of the solution, wherein the quotient is multiplied by 100%. For example, the solute is the grafted polyvinyl alcohol polymer, and the solution is the combined weight of the solute and the aqueous solvent.
[0034] The grafted polyvinyl alcohol polymer of the present invention is capable of being dispersed in an aqueous solution and forming a stable aqueous dispersion which, when stored at 25° C. and 1 atmosphere, does not exhibit coagulation or precipitation of the grafted polyvinyl alcohol polymer over a period of at least 6 months. Preferably, the stable aqueous dispersion does not exhibit coagulation or precipitation of the grafted polyvinyl alcohol polymer over a period of at least 1 year at 25° C. and 1 atmosphere, more preferably at least 2 years under these same conditions. As used herein, the term “coagulation” may mean the irreversible combination or aggregation of individual grafted polyvinyl alcohol polymers in an aqueous dispersion to form agglomerates or clumps of several or more grafted polyvinyl alcohol polymers. As used herein, the term “precipitation” may mean the sedimentation of the grafted polyvinyl alcohol polymer from an aqueous solution under the action of gravity. The grafted polyvinyl alcohol polymer can be precipitated in the form of polymer particle coagulates.
[0035] The grafted polyvinyl alcohol polymer of the present invention can be in a condensed form when present in an aqueous solution with a pH of about 2 to about 5 or 2 to about 3 (e.g., 1.5 to 3.5, or 2 to 3.5, or 2.2 to 3, or 2.2 to 2.8, or 3 to 5, or 2 to 5, or 4 to 5, or 4, or 4.5, or 5), and can be in a semi-condensed form when present in an aqueous solution with a pH of about 4 to about 5.5 (e.g., 3.8 to 5.8, or 4.0 to 5.5, or 4.2 to 5.2), and can be in an amorphous form when present in an aqueous solution with a pH of about 5.5 to about 8 (e.g., 5.3 to 8.5, or 5.5 to 8.3, or 5.5 to 7.5, or 5.8 to 8, or 6.0 to 7.5). All values between about 2 to about 5, about 2 to about 3, about 4 to about 5.5, and about 5.5 to about 8 are included in these ranges, including the endpoints of each range.
[0036] When the grafted polyvinyl alcohol polymer is in a condensed form, the individual polymers fold on themselves, resulting in tangled groupings of individual polymers clustering together to form polymer particles. The folding of the individual grafted polyvinyl alcohol polymers occurs through intramolecular interactions between the parts of the individual polymers. These intramolecular interactions can be covalent or electrostatic interactions, with the most common interactions being electrostatic interactions between the parts of the individual polymers. For example, without wishing to be bound by a particular theory, the amide units of the grafted polyvinyl alcohol polymer can interact with the vinyl alcohol units along the polymer backbone via electrostatic interactions. In this example, the -NH2 groups of the amide units along the polymer backbone are protonated in a low pH environment. An example of electrostatic interactions is a van der Waals interaction.
[0037] When the grafted polyvinyl alcohol polymer is in a coagulated form, polymer particles can be formed in an aqueous suspension. As an example, when the polymer is an aqueous dispersion with a pH of 2, the average particle size can be 100nm to 1,000nm, 100nm to 200nm, 50nm to 150nm, and / or 150nm to 300nm, including all values within the range, as well as decimals of these values and fractions of these values. For example, the average particle size can be about 170nm. The particle size distribution can be multimodal, wherein, as an example, the overall average particle size is 170nm, wherein about 65% (by number) of the polymer particles have an average diameter of 470nm and about 25% of the polymer particles have an average diameter of 50 microns. The particle size of the polymer can be determined via a dynamic light scattering experiment.
[0038] When the grafted polyvinyl alcohol polymer is in a semi-condensed form, the intramolecular interaction forces are weakened relative to those in the condensed form, and the individual grafted polyvinyl alcohol polymers begin to unfold. However, in this form, the intramolecular interaction forces are high enough to avoid complete unfolding of the individual grafted polyvinyl alcohol polymers, and therefore, the polymer particles in the condensed form swell, causing the polymer particles in the condensed form to transform into a larger size and a semi-condensed form. Although most of the individual polymers swell in size, it is also possible that some polymers remain in the condensed form.
[0039] When the grafted polyvinyl alcohol polymer is in a semi-condensed form, larger, swollen polymer particles can be formed in the solution. As an example, when the polymer is an aqueous solution with a pH value of 4.5, the average particle size can be 175nm to 375nm, including all values within this range, as well as decimals of these values and fractions of these values. For example, the average particle size can be about 300nm. The particle size can be multimodal, where, as an example, the overall average particle size is 300nm, wherein about 95% (by number) of the polymer particles have an average diameter of 38nm. The particle size of the polymer can be determined via dynamic light scattering experiments.
[0040] When the grafted polyvinyl alcohol polymer is in an amorphous form, the intramolecular interaction force is sufficiently weakened so that the individual polymers unfold and take a linear or substantially linear form. Although most of the individual polymers unfold, it is possible that some polymers remain in a condensed or semi-condensed form.
[0041] Compared to all three forms, the coagulated form is the least soluble form of the polymer in aqueous solution, and the amorphous form is the most soluble form of the polymer in aqueous solution. The amorphous form may exist, and / or, have a higher population, and / or, at a higher pH (pH alkaline conditions), and / or, when the concentration of the grafted polyvinyl alcohol polymer of the present invention in aqueous solution is sufficiently low (e.g., 0.1 wt % to 5 wt %).
[0042] When in aqueous solution, the grafted polyvinyl alcohol polymer of the present invention can exhibit reversible dispersibility or reversible solubility in aqueous solution. The ability to become more dispersible or more soluble and the ability to become less dispersible or less soluble can be achieved by changing the pH of the solution having the grafted polyvinyl alcohol polymer of the present invention. For example, an aqueous solution having the grafted polyvinyl alcohol polymer of the present invention in a coagulated form can have a pH of about 2 to about 5 or about 2 to about 3, and, at this pH, the grafted polyvinyl alcohol polymer of the present invention can exhibit low dispersibility or low solubility in aqueous solution. When the pH of the aqueous solution is raised to a pH of about 5.5 to about 8 by adding a base to the aqueous solution, the grafted polyvinyl alcohol polymer of the present invention can be converted to an amorphous dissolved form and exhibit increased dispersibility or solubility in aqueous solution. Thereafter, the pH of the aqueous solution can be reversibly reduced to, for example, about 2 to about 5 or about 2 to about 3, and the grafted polyvinyl alcohol polymer of the present invention can be restored to the coagulated form. When restored to the coagulated form, the grafted polyvinyl alcohol polymer of the present invention may again exhibit low dispersibility or solubility in aqueous solution.The pH is lowered by adding an acid to the aqueous solution having the grafted polyvinyl alcohol polymer of the present invention amorphously dissolved or amorphously dispersed therein.
[0043] The pH of the aqueous solution can be raised and lowered stepwise or with a gradient change by progressively adding an allotment of alkali or an allotment of acid, respectively. The allotment of alkali or acid can be added by a dropper containing an allotment of alkali or acid. The alkali or acid is preferably an aqueous solution of an allotment of alkali or acid. The alkali can be any alkali described herein, and the acid can be, for example, acetic acid, hydrochloric acid, hydrobromic acid, nitric acid, and sulfuric acid. The concentration of the alkali or acid is not particularly limited, as long as the alkali or acid can change the pH of the aqueous solution. For example, the concentration can be 0.01 mole to 5 moles, or 0.05 mole to 3 moles, or 0.1 to 1 mole, including any subvalue therebetween.
[0044] In the present invention, the aliphatic carboxylic acid may comprise acrylic acid and / or methacrylic acid, may consist essentially of acrylic acid and / or methacrylic acid, may consist of acrylic acid and / or methacrylic acid, may include acrylic acid and / or methacrylic acid, or may be acrylic acid and / or methacrylic acid. The aliphatic amide may be an unsaturated aliphatic amide. The aliphatic amide may be a saturated aliphatic amide. The aliphatic amide may comprise, consist essentially of, consist of, may include, or be at least one of acrylamide, methacrylamide, dimethylacrylamide, diethylacrylamide, dipropylacrylamide, and / or N-tert-butylacrylamide. The hydroxylated alkyl (meth) acrylate may comprise, consist essentially of, consist of, may include, or be 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl caprolactone acrylate, ethylene glycol acrylate, and / or hydroxypropyl methacrylate. Additional monomers in any or all of the side chains may include vinyl acetate, N-vinyl pyrrolidone, N-(3-aminopropyl)-2-acrylamide, N-3 (aminopropyl)methacrylamide hydrochloride, and stearyl polyethylene glycol methacrylate.
[0045] In a more specific example, the aliphatic carboxylic acid is methacrylic acid; the aliphatic amide is acrylamide; and the hydroxylated alkyl (meth)acrylate is 2-hydroxyethyl methacrylate.
[0046] In the grafted polyvinyl alcohol polymer of the present invention, the grafted polyvinyl alcohol polymer may comprise structure (I), consist essentially of structure (I), consist of structure (I), or include structure (I):
[0047] -[CH2-CH(OH)] a -[CH2-CH(R])] b -(I).
[0048] In this structure, the total weight percentage of (a) units can be 74% to 95% by weight, based on the total weight of the grafted polyvinyl alcohol polymer. All values between 74% and 95% by weight are included in the range, including the endpoints, and therefore, the range can be 74% to 90%, 77% to 92%, 80% to 95%, 80% to 92%, 80% to 90%, 82% to 95%, 82% to 92%, or 82% to 90%. The total weight percentage of (b) units is 5% to 26% by weight, based on the total weight of the grafted polyvinyl alcohol polymer. All values between 5 wt % and 26 wt % are included in the range, including the endpoints, and thus, the range may be 5 wt % to 23 wt %, 5 wt % to 20 wt %, 8 wt % to 26 wt %, 8 wt % to 23 wt %, 8 wt % to 20 wt %, 10 wt % to 26 wt %, 10 wt % to 23 wt %, 10 wt % to 20 wt %, 12 wt % to 26 wt %, 12 wt % to 23 wt %, or 12 wt % to 20 wt %. The total weight percentage of (a) and (b) units is equal to 100%. In structure (I), R is acetate or a side chain from a plurality of side chains. The plurality of units represented by structure (I) may be included in or as part of all grafted polyvinyl alcohol polymers of the present invention. When more than one unit of structure (I) is present, a, b, and / or R may be the same or different for each structure (I) present.
[0049] In the grafted polyvinyl alcohol polymer of the present invention, the grafted polyvinyl alcohol polymer may comprise structure (II), consist essentially of structure (II), consist of structure (II), include structure (II), or be structure (II):
[0050]
[0051] In the polymer, as relative amounts, a may be 1 to 10; b may be 35 to 55; and c may be 35 to 55, based on a+b+c=100. All values within these ranges are included; therefore, a may be any one of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10; b may be any one of 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, and 55; and c may be any one of 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, and 55, based on a+b+c=100. A plurality of units represented by structure (II) may be included in or as part of the grafted polyvinyl alcohol polymer of the present invention. When there is more than one unit of structure (II), a, b, and / or c may be the same or different for each structure (II) present.
[0052] The grafted polyvinyl alcohol polymer of the present invention may be a polymer that exhibits or has one or more of the following properties: a) the grafted polyvinyl alcohol polymer is a latex; b) the grafted polyvinyl alcohol polymer is capable of being completely dispersed in water in an amount of 1 wt % to 25 wt % at a pH of 2-5 or 2-3; c) the grafted polyvinyl alcohol polymer is not an irreversible gel at any pH; and / or d) the grafted polyvinyl alcohol polymer is gel-free at a pH of 8.
[0053] The grafted polyvinyl alcohol polymer of the present invention may exhibit one or more glass transition temperatures. For example, the grafted polyvinyl alcohol polymer has a first glass transition temperature of -40°C to 60°C or 40°C to 60°C, and a second glass transition temperature of 70°C to 90°C. The glass transition temperature may be any value within these ranges. For example, the first glass transition temperature may be -40°C to 50°C, or -40°C to 40°C, or -40°C to 30°C, or -40°C to 20°C, or -40°C to 20°C, or -30°C to 60°C, or -20°C to 60°C, or -10°C to 60°C, or 0°C to 60°C, or 10°C to 60°C, or 20°C to 60°C, or 30°C to 60°C, or 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, or 60°C. The second glass transition temperature may be 70° C., 71° C., 72° C., 73° C., 74° C., 75° C., 76° C., 77° C., 78° C., 79° C., 80° C., 81° C., 82° C., 83° C., 84° C., 85° C., 86° C., 87° C., 88° C., 89° C., or 90° C. These numbers may be the minimum or maximum of a sub-range with a broader range.
[0054] Without wishing to be bound by a particular theory, the first glass transition temperature is the glass transition temperature of one or more side chains grafted to the polyvinyl alcohol backbone, and the second glass transition temperature is the glass transition temperature of the polyvinyl alcohol backbone. Any method and / or technique suitable for measuring glass transition temperatures can be used to measure the glass transition temperature of the grafted polyvinyl alcohol polymer of the present invention. As an example, the glass transition temperature can be measured using a dynamic mechanical thermal analysis rheometer.
[0055] Other properties of the grafted polyvinyl alcohol polymer of the present invention include the weight average molecular weight and number average molecular weight of the grafted polyvinyl alcohol polymer. For example, the grafted polyvinyl alcohol polymer of the present invention can have a weight average molecular weight of about 50,000 Daltons to about 1,500,000 Daltons (e.g., 100,000 Daltons to 1,000,000 Daltons, or 250,000 Daltons to 750,000 Daltons). The grafted polyvinyl alcohol polymer of the present invention can have a number average molecular weight of 2,000 Daltons to about 50,000 Daltons. The weight average molecular weight and number average molecular weight of the grafted polyvinyl alcohol polymer can be measured by gel permeation chromatography.
[0056] The polydispersity of a polymer is generally defined as the weight average molecular weight of the polymer divided by the number average molecular weight of the polymer (PD=Mw / Mn). The grafted polyvinyl alcohol polymer of the present invention may have a polydispersity Mw / Mn of at least 1.5.
[0057] As shown by two glass transition temperatures in an exemplary grafted polyvinyl alcohol of the present invention, the main chain of the polymer can have the properties of the main chain itself when in free, unreacted form. For example, before the monomer is grafted onto the main chain, the polyvinyl alcohol main chain in unreacted form can have a molecular weight distribution of about 5,000 daltons to about 1,000,000 daltons. In this example, the molecular weight distribution of the polyvinyl alcohol main chain in free, unreacted form is a unimodal, bimodal, or multimodal molecular weight distribution. The polyvinyl alcohol main chain in free, unreacted form can have a weight average molecular weight of 2,000 daltons to 500,000 daltons, and / or, can have a number average molecular weight of about 1,000 daltons to about 50,000 daltons. Therefore, the polyvinyl alcohol main chain in free, unreacted form can have a polydispersity Mw / Mn of 2 to 7.
[0058] In addition, the free, unreacted polyvinyl alcohol backbone can have a degree of hydrolysis of about 74 mol % to about 98 mol %, or other amounts below or above this range. All values between 74 mol % and 98 wt % are included in the range, including the endpoints, and therefore, the range can be 74 mol % to 95 mol %, 74 mol % to 90 mol %, 74 mol % to 88 mol %, 76 mol % to 95 mol %, 76 mol % to 90 mol %, and 76 mol % to 88 mol %. Since all values between 74 mol% and 98 wt% are included in this range, the degree of hydrolysis can be 74 mol%, 75 mol%, 76 mol%, 77 mol%, 78 mol%, 79 mol%, 80 mol%, 81 mol%, 82 mol%, 83 mol%, 84 mol%, 85 mol%, 86 mol%, 87 mol%, 88 mol%, 89 mol%, 90 mol%, 91 mol%, 92 mol%, 93 mol%, 94 mol%, 95 mol%, 96 mol%, 97 mol%, and 98 mol%, including decimals and fractions thereof.
[0059] The degree of hydrolysis can be an indicator of how many free alcohol moieties (-OH) are present on the backbone of the polyvinyl alcohol backbone. The synthesis of polyvinyl alcohol first involves the polymerization of vinyl acetate, which forms polyvinyl acetate. Thereafter, the acetate moieties (-O-(CO)-CH3) are replaced by alcohol moieties via a hydrolysis reaction. Thus, as used herein, "degree of hydrolysis" can refer to the mole % of acetate moieties that are replaced by alcohol moieties when polyvinyl acetate undergoes transesterification. Thus, as an example, for a polyvinyl alcohol backbone characterized by a degree of hydrolysis of 74 mole %, 74 mole % of the acetate moieties are replaced by alcohol moieties.
[0060] The unreacted form of polyvinyl alcohol main chain can be: POVAL TM (Kurary Co., Ltd.) 5 / 88, 3 / 80, 3 / 82, 3 / 85, 4 / 85, 4 / 88, 5 / 82, 6 / 88, 13 / 88, 3 / 88, 5 / 74, 5 / 88, 8 / 88, and one or more of RS2117; Selvol TM (Sekisui Specialty Chemicals America, LLC) one or more of 5002, 513, 518, 418, 425, 443, 203, 523, 205, and 540; and any combination thereof.
[0061] Another aspect and feature of the invention relates to a formulation that may comprise, consist of, consist essentially of, may include, or is: an aqueous phase and a grafted polyvinyl alcohol polymer of the invention. In one aspect, the formulation may comprise, consist of, consist essentially of, or may include: 100 parts by weight of an aqueous phase and 1 part by weight to 40 parts by weight or more (e.g., 10 parts by weight to 40 parts by weight) of a grafted polyvinyl alcohol polymer of the invention, wherein in the formulation, the grafted polyvinyl alcohol polymer is dispersed in the aqueous phase. All values between 1 part by weight and 40 parts by weight are included in the range, including the endpoints, and thus, the range can be 5 parts by weight to 35 parts by weight, 10 parts by weight to 35 parts by weight, 10 parts by weight to 30 parts by weight, 12 parts by weight to 40 parts by weight, 12 parts by weight to 38 parts by weight, 12 parts by weight to 35 parts by weight, 14 parts by weight to 40 parts by weight, 14 parts by weight to 35 parts by weight, 15 parts by weight to 40 parts by weight, 15 parts by weight to 38 parts by weight, and 15 parts by weight to 35 parts by weight. Since all values between 1 part by weight and 40 parts by weight are included in the range, the parts by weight can be, for example, 2 parts by weight, 5 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, and 40 parts by weight, including decimals and fractions thereof.
[0062] The formulation of the present invention may be a stable aqueous dispersion that exhibits no coagulation or precipitation of the grafted polyvinyl alcohol polymer over a period of at least 6 months when stored at 25° C. and 1 atmosphere. Alternatively, the aqueous dispersion is stable over a period of at least 1 year, or over a period of at least 2 years, when stored at 25° C. and 1 atmosphere. The terms “coagulation” and “precipitation” herein have the same definitions as given above.
[0063] The formulation of the present invention may have a pH of about 2 to about 5 or about 2 to about 3, and, when the formulation has this pH, the grafted polyvinyl alcohol polymer may be in a coagulated form as discussed above. As another option, the formulation of the present invention may have a pH of about 4 to about 5.5, and, when the formulation has this pH, the grafted polyvinyl alcohol polymer is in a semi-coagulated form as discussed above. As a further option, the formulation of the present invention may have a pH of about 5.5 to about 8, and, when the formulation has this pH, the grafted polyvinyl alcohol polymer is in an amorphous dissolved form as discussed above.
[0064] In the formulation of the present invention, the grafted polyvinyl alcohol polymer can be dissolved in the aqueous phase of the formulation in an amount of at least 10 g / 100 g of water. As an option, the maximum amount of grafted polyvinyl alcohol polymer in the formulation of the present invention can be about 50 g / 100 g of water or more. Other ranges within these extremes are also possible, for example: 10 g / 100 g water-45 g / 100 g water; 12 g / 100 g water-45 g / 100 g water; 15 g / 100 g water-45 g / 100 g water; 15 g / 100 g water-40 g / 100 g water; 18 g / 100 g water-45 g / 100 g water; 18 g / 100 g water-40 g / 100 g water; 20 g / 100 g water-45 g / 100 g water; 20 g / 100 g water-40 g / 100 g water. All values within these ranges are available, for example: 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, and 50, or decimals or fractions thereof.
[0065] At these concentrations of polymer in water, the formulations of the present invention can be highly concentrated products, which reduces the volume for shipping and storage. Since the grafted polyvinyl alcohol polymer can be dispersed or dissolved in aqueous solutions without gelling or other viscosity problems, formulations with higher concentrations of grafted polyvinyl alcohol polymer can exist, especially compared to conventional polyvinyl alcohol. The end user of the concentrated product (e.g., a paper company or other user) can dilute the concentrate to the solids content required for the application, or it can be directly pumped or otherwise transferred to a Yankee or drum spray boom coating solution.
[0066] In addition to the aqueous phase and the grafted polyvinyl alcohol polymer, the formulation of the present invention may also include at least one plasticizer. The plasticizer may be at least one of glycerol, propylene glycol, 2-oxydipropyl dibenzoate, 3-dipropylene glycol dibenzoate, and 4-diethylene glycol dibenzoate. If present, the amount of the plasticizer may be 1 to 15 weight %, relative to 100 weight % of the dispersion. For example, if glycerol is present, the amount of the plasticizer may be 1 to 15 weight %, relative to 100 weight % of the dispersion. If 2-oxydipropyl dibenzoate is present, the amount of the plasticizer may be 1 to 5 weight %, relative to 100 weight % of the dispersion. If 3-dipropylene glycol dibenzoate is present, the amount of the plasticizer may be 1 to 5 weight %, relative to 100 weight % of the dispersion. If 4-diethylene glycol dibenzoate is present, the amount of the plasticizer may be 1 to 5 weight %, relative to 100 weight % of the dispersion. If present, propylene glycol may be present in an amount of 1 to 5% by weight relative to 100% by weight of the dispersion.
[0067] In addition to the aqueous phase and the grafted polyvinyl alcohol polymer, the formulation of the present invention may also include one or more surfactants or may not include a surfactant. Although no surfactant is needed in the formulation of the present invention, it can be present in any conventional amount. Since a surfactant is not necessary, the amount of the surfactant may be less than 1% by weight of a surfactant (e.g., 0% by weight-0.9% by weight, 0.001% by weight-0.5% by weight, 0.001% by weight-0.1% by weight). The formulation of the present invention may be surfactant-free, or surfactant-free. If present, the surfactant may be at least one of a cationic surfactant, an anionic surfactant, and / or a nonionic surfactant.
[0068] Examples of surfactants include, but are not limited to, hexadecyltrimethylammonium bromide, sodium lauryl sulfate, and / or condensation products of alkylene oxides (e.g., ethylene oxide (EO)) and hydrophobic molecules. Examples of hydrophobic molecules include fatty alcohols, fatty acids, fatty acid esters, triglycerides, fatty amines, fatty amides, alkylphenols, polyols, and some of their fatty acid esters. Other examples include polyalkylene oxide block copolymers, polyalkylene oxide tetrablock copolymers, and alkyl polyglycosides. Examples include nonionic surfactants that are fatty alcohol ethoxylates, wherein the alcohol is about C. 10 -C 18Branched or linear, for example, SURFONIC L (Huntsman Corporation, Houston, Tex.) or TDA series, NEODOL (Shell Chemical Company, Houston, Tex.) series and TERGITOL series (Union Carbide Corporation, Danbury Conn.). Other examples of nonionic surfactants include alkylphenol ethoxylates, polyethylene glycol esters of long chain fatty acids, ethoxylated fatty amines, polymers including ethylene oxide and propylene oxide blocks, and alkyl polyglycosides.
[0069] Surfactants (e.g., polymeric surfactants) can have an average molecular weight (in Daltons) of 1,000 to about 20,000, for example, about 2,000 to about 15,000, about 3,000 to about 12,000, about 5,000 to about 20,000, about 10,000 to about 20,000, about 12,000 to about 17,000, about 13,500 to about 16,000, at least about 20,000, at least about 50,000, at least about 100,000, or at least about 500,000.
[0070] Another aspect of the invention is a method of making a grafted polyvinyl alcohol polymer according to the invention. The method may comprise, consist essentially of, consist of, include, or be the following steps: polymerizing at least one of an aliphatic carboxylic acid, an aliphatic amide, and / or a hydroxylated alkyl (meth)acrylate via free radical polymerization in the presence of free polyvinyl alcohol.
[0071] The method may comprise, consist essentially of, consist of, include, or have the following steps: adding or mixing at least one of an aliphatic carboxylic acid, an aliphatic amide, an alkylamino (meth) acrylate, and a hydroxylated alkyl (meth) acrylate in an aqueous solution (the aqueous solution comprises, consists essentially of, consists of, or includes water and a polyvinyl alcohol polymer) to obtain an aqueous solution of monomer and free PVOH. The adding or mixing step may be performed for at least 15 minutes or longer, for example, 15 minutes to 2 hours or longer. The polymerization step is initiated by adding an initiator (e.g., ammonium persulfate, sodium bisulfite, hydrogen peroxide, and tert-butyl hydroperoxide) to the aqueous solution of monomer and free PVOH.
[0072] Alternatively, the process may comprise, consist essentially of, consist of, include, or have the step of adding monomers to a reactor stepwise or semi-continuously at a temperature of 35° C. to 80° C. The reactor may contain the polyvinyl alcohol backbone in unreacted form prior to the stepwise or semi-continuous addition of monomers to the reactor. The temperature range may be, for example, 40° C. to 70° C., and preferably 65° C. The process may also comprise, consist essentially of, consist of, include, or have the step of polymerizing by adding an initiator such as ammonium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide to an aqueous solution of a mixture of monomers and free PVOH. Sodium bisulfite may be included as part of the initiator, and, without wishing to be bound by a particular theory, it is believed that sodium bisulfite may reduce the dissociation temperature of any peroxide present in the initiator, thereby reducing the energy cost associated with initiating polymerization.
[0073] The initiator can be added all at once at the start of the polymerization, or can be added over time (e.g., dropwise and over a period of time). If added dropwise, the time period for dropwise semi-continuous addition of the monomer can be 15 minutes to 5 hours or more, 30 minutes to 3 hours, or 45 minutes to 2 hours.
[0074] When the initiator is added in whole or in part, the aqueous solution of the monomer and free PVOH can be regarded as a reaction solution, and the graft polymerization of the monomer can be carried out in the reaction solution. The temperature of the reaction solution during polymerization can be 30° C. to 100° C., for example 30° C. to 85° C., and all numbers and values therein are included in this range.
[0075] The method may further comprise, consist essentially of, consist of, include, or have a step of terminating the polymerization step. Polymerization termination may occur by adding hydroquinone to the reaction solution.
[0076] An interesting aspect of the present invention is that the graft polymerization of the monomers in the present invention can be carried out entirely using acrylic monomers. In other words, the graft polymerization can be carried out in the substantial absence or complete absence of vinyl monomers. Using the present invention, the percentage of acrylic monomers used in the graft polymerization can be, for example, 50% (by number) or higher, for example, 50% (by number) to 100% (by number), or 75% (by number) to 99% (by number), or 85% (by number) to 98% (by number), based on the total number of grafting sites on the polyvinyl alcohol backbone. The vinyl monomer present can be 0, or less than 5%, or less than 3%, or less than 1%, or less than 0.5%, or less than 0.1% (by number), based on the total number of grafting sites on the polyvinyl alcohol backbone.
[0077] Another aspect of the invention is a method of making an aqueous solution of a grafted polyvinyl alcohol polymer according to the invention. The method may comprise, consist essentially of, consist of, include, or be the following steps: adding a base to the dispersion to raise the pH of the dispersion to 4 to 8 (e.g., from 5 or more to 8) and forming an aqueous solution of the grafted polyvinyl alcohol polymer. In the method, the dispersion may comprise, consist essentially of, consist of, include, or be: an aqueous phase and a grafted polyvinyl alcohol polymer dispersed in the aqueous phase. Prior to the step of adding a base to the dispersion, the dispersion may have a pH of 2 to 5 or 2 to 3.
[0078] The alkali can be any compound or composition with alkaline pH and capable of raising the pH of the dispersion. Examples of alkali include, but are not limited to, caustic substances, alkaline substances (e.g., alkali metal substances, alkaline earth metal substances), and alkaline buffer substances, or any combination thereof. The alkali can be inorganic or organic, or a combination or mixture of these different types of alkaline substances. The alkali can be, for example, alkali hydroxides, alkali oxides, alkali phosphates, alkali carbonates, alkali bicarbonates, alkaline earth hydroxides, alkaline earth oxides, alkaline earth phosphates, alkaline earth carbonates, ammonium zirconium carbonate, organic titanates, organic zirconates, ammonium hydroxide, ammonium carbonate, ammonium bicarbonate, alkali metal silicates, urea, substituted urea, cyanates, alkylamines, alkanolamines, quaternary ammonium salts, salts of weak acids and strong bases, alkaline buffer solutions, polyalkali metal pyrophosphates, or any combination thereof. The example of an alkali hydroxide that can be used is NaOH. Alkali salts (alkali salts) can be used as salt water or in the form of water-soluble salts. As an option, an alkaline buffering agent can be used in the adhesive base formulation to establish alkalinity and resist pH changes. Examples of alkaline buffers that can be used include, for example, magnesium oxide, and aqueous solutions of disodium phosphate and monosodium phosphate. Examples of alkanolamines include triethanolamine, diethanolamine, or monoethanolamine. The base can be, for example, an Arrhenius base (i.e., a substance that ionizes in water to produce hydroxide ions), a Bronsted-Lowry base (i.e., a substance that can receive protons or hydrogen cations (H + ) substances), or Lewis bases (ie, species that donate electron pairs), as long as their introduction is able to affect an increase in the pH of the adhesive base formulation.
[0079] The dosage rate of the base depends on the following factors: the level of pH increase sought, the base strength of the specific material, and the addition rate. As a non-limiting example, to increase the pH of the dispersion by about 0.5 units, a 10 wt. % NaOH solution can be added in a weight:weight ratio (based on solids only) to a dispersion having an original pH of about 4.0 to about 6.0 in water in an amount ranging from about 1 / 30 to about 30 / 1 (e.g., 1 / 10, or 10 / 1, or other range values). The magnitude of the further increase in pH obtained by further increasing the amount of base added can be approximately proportional, or, at least, can trend together.
[0080] As an alternative to adding a base, the aqueous dispersion can be diluted with water to increase the pH. The transition of the grafted polyvinyl alcohol polymer in the aqueous dispersion from a coagulated form to a semi-coagulated form to an amorphous dissolved form can be performed while adding water to the low pH aqueous dispersion.
[0081] The present invention further relates to a creping process comprising using the formulation of the present invention as a creping adhesive. For example, a process for creping a fiber web may comprise providing a rotating cylindrical dryer or similar roll comprising a dryer surface. Applying an adhesive formulation comprising the formulation of the present invention to the dryer surface, and conveying a fiber web to the dryer surface. On the dryer surface, the fiber web is dried to form a dried fiber web, and the dried fiber web is creped from the dryer surface. As an option, the fiber web to be creped may be through-air dried and thereafter transferred to a Yankee dryer surface that has been pre-coated with the improved creping adhesive formulation.
[0082] As an option, the adhesive formulation is a dispersion as described herein. During the creping process of the present invention, the formulation can have a pH of about 4.5 to about 6, and the grafted polyvinyl alcohol polymer can be amorphously dissolved in the dispersion. The formulation can have the grafted polyvinyl alcohol polymer present in a concentration of 0.1 wt % to 5 wt % (e.g., about 0.5 wt % to 3 wt %, or other amounts), all based on the total weight of the adhesive formulation.
[0083] The wrinkling process may further comprise, consist of, consist essentially of, or include substantially removing the formulation from the wrinkled dryer surface. Prior to the substantial removal of the formulation from the dryer surface, the pH of the formulation on the dryer surface may be raised to a pH above 6, which may facilitate removal of the formulation from the dryer surface.
[0084] The formulation may be applied to a Yankee dryer or other cylindrical dryer used in such a creping process. The formulation can be applied to the cylindrical dryer surface on a continuous basis, a semi-continuous basis, an intermittent basis, or a one-time basis before rotation, during rotation, or before and during rotation. The formulation of the present invention may be applied as follows: to the surface of the cylindrical dryer (e.g., after the creping blade and before the web transfer position); before applying the fiber web to the cylindrical dryer surface, or, during the process of applying the fiber web to the cylindrical dryer surface, and / or, after applying the fiber web to the cylindrical dryer surface, to the fiber web. The formulation may be applied by using one or more nozzles of a spray bar, a roller coater, an immersion bath for the fiber web, or other coating device. The application rate or use rate of the adhesive formulation may be 0.1 mg / m 2 Dryer surface up to 40mg / m 2 Dryer surface, e.g. 0.1 mg / m 2Dryer surface up to 20mg / m 2 Dryer surface, or 0.1mg / m 2 Dryer surface up to 10mg / m 2 Dryer surface, or 1mg / m 2 Dryer surface up to 10mg / m 2 Dryer surface, or 5mg / m 2 Dryer surface up to 10mg / m 2 Dryer surface, or other quantity.
[0085] Creping systems, methods, and adhesives are described in the following U.S. Patents (the entire contents of which are incorporated herein by reference): 3,640,841; 4,304,625; 4,440,898; 4,788,243; 4,994,146; 5,025,046; 5,187,219; 5,326,434; 5,246,544; 5,370,773; 5,487,813; 5,490,903; 5,633,309; 5,660,687; 5,846,380; 4 ,300,981; 4,063,995; 4,501,640; 4,528,316; 4,886,579; 5,179,150; 5,234,547; 5,374,334; 5,382,323; 5,468,796; 5,902,862; 5,942,085; 5,944,954; 3,301,746; 3,879,257; 4,684,439; 3,926,716; 4,883,564; and 5,437,766.
[0086] The adhesive formulations of the present invention may be used in other applications in the papermaking industry or other industries. The adhesive formulations of the present invention may be considered biodegradable, and / or, non-toxic, and / or, contain one or more food grade ingredients.
[0087] The present invention will be further illustrated by the following examples, which are intended as illustrations of the present invention.
[0088] Example
[0089] Example 1 - Synthesis of Polymer 1
[0090] The resin is prepared by dissolving polyvinyl alcohol polymer in water. Methacrylic acid, acrylamide, and 2-hydroxyethyl methacrylate are mixed in the PVOH aqueous solution for at least 30 minutes to form a precursor solution.
[0091] Batch polymerization was initiated by adding a solution of ammonium persulfate initiator to the precursor solution at 60°C, and the polymerization was carried out at 80°C for 2 hours. The ammonium persulfate was maintained at 80°C at a constant feed rate for 120 minutes. The residual monomer was suppressed by tert-butyl hydroperoxide and hydrogen peroxide at 40°C for 30 minutes. Table 1 shows the reactants and relative amounts in the polymerization.
[0092] Table 1. Graft copolymerization formula of polymer 1
[0093]
[0094]
[0095] Polymer 1 was analyzed using gel permeation chromatography ("GPC"). A GPC trace was obtained, and, from the GPC trace, the weight average and number average molecular weights of Polymer 1 were obtained. The weight average molecular weight of Polymer 1 was 194,831 Daltons, and the number average molecular weight of Polymer 1 was 25,790 Daltons. The polydispersity index value Mw / Mn of Polymer 1 was 7.74.
[0096] Polymer 1 was dispersed in the aqueous phase of the aqueous formulation and the pH of the formulation was adjusted to 2. The pH adjustment was performed by adding 10% aqueous sodium hydroxide solution to the formulation. The formulation was analyzed using dynamic light scattering to determine the polymer particle size distribution at this pH. It was found that the average particle size of the polymer was 170 nm, of which 66.1% by volume of the particles had an average diameter of 470 nm and 24% by volume of the particles had an average diameter of 50 microns.
[0097] The pH of the formulation was raised to 4.5 by adding a base to the pH 2 formulation, and the pH 4.5 formulation was analyzed using dynamic light scattering to determine the polymer particle size distribution at this pH. The average particle size of the polymer was found to be 300 nm, with 95% by volume of the particles having an average diameter of 380 nm.
[0098] Example 2 - Testing using polymer 1
[0099] A test method was developed in which, after heating at 100°C for 15 seconds, the nonwoven was laminated with a polymer solution and then the nonwoven was dried at different time intervals of 15, 30 and 60 seconds. For each time interval, the peeling force (debonding force) was measured separately and independently. The 15 second measurement result was defined as the pick-up adhesion value when the polymer film was still wet, the 30 second measurement result was the holding capacity of the semi-dry film on a semi-dry tissue substrate, and finally, the 60 second measurement result was the adhesion between the dry tissue and the dry film when they hit the creping blade; the assumption was based on the drying curve of 0.8 ml of a 2.5% polymer solution over a hot stainless steel plate at 100°C.
[0100] Table 2: Adhesion ability of polymer 1 compared to other polymer compositions
[0101]
[0102]
[0103] Example 3 - Particle size analysis of polymer 1 in aqueous media at different pH
[0104] At pH 2, an aqueous dispersion of polymer 1 was obtained. As the pH increased from 2 to 4.5, the average particle size increased from 170 nm to 300 nm, as shown in Table 3 below. This increase may be due to water swelling of the particles caused by the carboxyl, hydroxyl and amide groups of the polymer. At pH 4.5, 95% of the particle population had an average diameter of 380 nm, and the polydispersity index decreased from 0.61 at pH 2 to 0.39 at pH 4.5 due to water swelling.
[0105] The pH was further increased to 6, which significantly reduced the average particle diameter to 80 nm due to the transition from the colloidal particle state to an expanded free-flowing amorphous polymer. The polydispersity index at pH 6 increased to 0.8; this broad polydispersity is attributed to the complete decomposition of the coagulated particles into an expanded fully hydrated polymer. At pH 2, the particles as well as the free PVOH particles were forced to shrink due to the increased level of intramolecular attraction, and therefore, 72% of the volume-weighted particles had an average diameter of 29 nm. At pH 4.5, the level of physical attraction within the molecules and between the particles was reduced, which supports the finding that 88% of the particles had an increased average diameter of 500 nm. When the particles were converted into solution or expanded at pH 6, 99.8% of the particles had an average diameter of only 6 nm, a result indicating that the polymer dispersion undergoes a transition between particles and free hydrocolloidal molecules.
[0106] Table 3: Particle size of polymer 1 at different pH
[0107]
[0108] The present invention includes the following aspects / embodiments / features in any order and / or in any combination:
[0109] 1. A grafted polyvinyl alcohol polymer comprising a polyvinyl alcohol main chain and a plurality of side chains grafted to the polyvinyl alcohol main chain,
[0110] One or more of the side chains from the plurality of side chains comprises one or more units selected from the group consisting of aliphatic carboxylic acids, aliphatic amides, hydroxylated alkyl (meth) acrylates, alkylamino (meth) acrylates, or any combination thereof.
[0111] 2. The grafted polyvinyl alcohol polymer of any preceding or subsequent embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises: an aliphatic carboxylic acid unit, an aliphatic amide unit, and a hydroxylated alkyl (meth)acrylate unit.
[0112] 3. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises an aliphatic carboxylic acid unit.
[0113] 4. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises an aliphatic amide unit.
[0114] 5. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises a hydroxylated alkyl (meth)acrylate unit.
[0115] 6. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises an alkylamino(meth)acrylate unit.
[0116] 7. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises: an aliphatic carboxylic acid unit and an aliphatic amide unit.
[0117] 8. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises: an aliphatic carboxylic acid unit and a hydroxylated alkyl (meth)acrylate unit.
[0118] 9. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises: an aliphatic amide unit and a hydroxylated alkyl (meth)acrylate unit.
[0119] 10. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein one or more of the side chains from the plurality of side chains comprises: an aliphatic amide unit and an alkylamino(meth)acrylate unit.
[0120] 11. The grafted polyvinyl alcohol polymer of any preceding or subsequent embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has a viscosity of less than 500 cP·s when present in an aqueous dispersion at a pH of 3 at a concentration of 22.5-25 wt% at 25° C. and 1 atmosphere.
[0121] 12. The grafted polyvinyl alcohol polymer of any preceding or subsequent embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has a viscosity of less than 100 cP·s when present in an aqueous solution at a concentration of 2.5-10 wt. % at 25° C. and 1 atmosphere of pH 3.
[0122] 13. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer is dispersible in an aqueous solution at a concentration of 10 wt% to 40 wt%.
[0123] 14. The grafted polyvinyl alcohol polymer of any preceding or subsequent embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer is capable of being dispersed in an aqueous solution and forming a stable aqueous dispersion that does not exhibit coagulation or precipitation of the grafted polyvinyl alcohol polymer at 25°C and 1 atmosphere for a period of at least 6 months.
[0124] 15. The grafted polyvinyl alcohol polymer of any preceding or subsequent embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer is capable of being in a coagulated form when present in an aqueous solution with a pH of about 2 to about 5 or about 2 to about 3, and is capable of being in a semi-coagulated form when present in an aqueous solution with a pH of about 4 to about 5.5, and is capable of being in an amorphous form when present in an aqueous solution with a pH of about 5.5 to about 8.
[0125] 16. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has one or more of the following properties:
[0126] a) the grafted polyvinyl alcohol polymer is a latex;
[0127] b) the grafted polyvinyl alcohol polymer is fully dispersible in water at a pH of 2-3 or a pH of 2-5 in an amount of 1 wt % to 25 wt %;
[0128] c) the grafted polyvinyl alcohol polymer is not an irreversible gel at any pH; and
[0129] d) The grafted polyvinyl alcohol polymer is gel-free at a pH of 8.
[0130] 17. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has a first glass transition temperature of -40°C to 60°C, and a second glass transition temperature of 70°C to 90°C.
[0131] 18. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has a weight average molecular weight of 5,000 Daltons to about 1,500,000 Daltons.
[0132] 19. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has a number average molecular weight of 1,000 Daltons to about 50,000 Daltons.
[0133] 20. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer has a polydispersity Mw / Mn of at least 1.5.
[0134] 21. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the polyvinyl alcohol backbone in unreacted form has a weight average molecular weight of about 5,000 Daltons to about 1,500,000 Daltons.
[0135] 22. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the molecular weight distribution is unimodal, bimodal, or multimodal.
[0136] 23. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the polyvinyl alcohol backbone in unreacted form has a number average molecular weight of about 1,000 Daltons to about 50,000 Daltons.
[0137] 24. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the polyvinyl alcohol backbone in unreacted form has a polydispersity Mw / Mn of 2 to 7.
[0138] 25. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the polyvinyl alcohol backbone has a degree of hydrolysis of about 74 mol % to about 95 mol %.
[0139] 26. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect,
[0140] wherein the aliphatic carboxylic acid is present and comprises at least one of acrylic acid and methacrylic acid,
[0141] wherein the aliphatic amide is present and comprises at least one of acrylamide, methacrylamide, dimethylacrylamide, diethylacrylamide, dipropylacrylamide and N-tert-butylacrylamide, and
[0142] The hydroxylated alkyl (meth)acrylate is present and includes at least one of 2-hydroxyethyl methacrylate and hydroxypropyl methacrylate.
[0143] 27. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect,
[0144] Wherein, the alkylamino (meth)acrylate is present and is or comprises N-(3-aminopropyl)-2-acrylamide and / or N-(3-aminopropyl)methacrylamide hydrochloride.
[0145] 28. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect,
[0146] wherein an aliphatic carboxylic acid is present and is methacrylic acid,
[0147] wherein the aliphatic amide is present and is acrylamide, and
[0148] Among them, the hydroxylated alkyl (meth)acrylate is present and is 2-hydroxyethyl methacrylate.
[0149] 29. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, comprising structure (I):
[0150] -[CH2-CH(OH)] a -[CH2-CH(R])] b -(I)
[0151] Wherein, based on the total weight of the grafted polyvinyl alcohol polymer, the total weight percentage of (a) units is 74% to 95%,
[0152] Wherein, based on the total weight of the grafted polyvinyl alcohol polymer, the total weight percentage of (b) units is 5% to 26%,
[0153] wherein each R is acetate or a side chain from the plurality of side chains.
[0154] 30. The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, comprising structure (II):
[0155]
[0156] wherein a is 1 to 10; b is 35 to 55; and c is 35 to 55, provided that a+b+c=100.
[0157] 31. A preparation comprising:
[0158] aqueous phase; and
[0159] The grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect.
[0160] 32. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation comprises:
[0161] 100 parts by weight of an aqueous phase; and
[0162] 10 to 40 parts by weight of a grafted polyvinyl alcohol polymer, wherein
[0163] The grafted polyvinyl alcohol polymer is dispersed in the water phase.
[0164] 33. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation is a stable aqueous dispersion that does not exhibit coagulation or precipitation of the grafted polyvinyl alcohol polymer over a period of at least 6 months.
[0165] 34. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation has a pH of about 2 to about 3, and
[0166] Therein, the grafted polyvinyl alcohol polymer is in a coagulated form.
[0167] 35. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation has a pH of about 4 to about 5.5, and
[0168] The grafted polyvinyl alcohol polymer is in a semi-condensed form.
[0169] 36. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation has a pH of about 5.5 to about 8, and
[0170] Among them, the grafted polyvinyl alcohol polymer is in an amorphous dissolved form.
[0171] 37. The formulation of any preceding or following embodiment / feature / aspect, wherein the grafted polyvinyl alcohol polymer is soluble in the aqueous phase in an amount of at least 10 g / 100 g water.
[0172] 38. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation contains less than 1 wt% surfactant.
[0173] 39. The formulation of any preceding or following embodiment / feature / aspect, wherein the formulation is free of surfactant.
[0174] 40. A method for making the grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, the method comprising:
[0175] At least one of an aliphatic carboxylic acid, an aliphatic amide, an aminoalkyl(meth)acrylate, and a hydroxylated alkyl(meth)acrylate is polymerized via free radical polymerization in the presence of free polyvinyl alcohol.
[0176] 41. A method for producing an aqueous solution of a grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, the method comprising:
[0177] A base is added to the dispersion, thereby raising the pH of the dispersion to 4 to 8 and forming an aqueous solution of the grafted polyvinyl alcohol polymer, wherein
[0178] The dispersion contains:
[0179] aqueous phase; and
[0180] A grafted polyvinyl alcohol polymer dispersed in an aqueous phase, wherein the dispersion has a pH of 2 to 3 or 2 to 5 before said adding.
[0181] 42. A process for creping a fiber web, comprising:
[0182] providing a rotating cylindrical dryer comprising a dryer surface,
[0183] applying a formulation comprising the grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect to a dryer surface,
[0184] conveying the fiber web onto the dryer surface,
[0185] drying the fibrous web on the dryer surface to form a dried fibrous web, and
[0186] The dried fiber web is creped from the dryer surface.
[0187] 43. The process of any preceding or following embodiment / feature / aspect, wherein the formulation is a dispersion.
[0188] 44. The process of any preceding or following embodiment / feature / aspect, wherein the formulation has a pH of about 4.5 to about 6.
[0189] 45. The process of any preceding or subsequent embodiment / feature / aspect, further comprising:
[0190] The formulation is substantially removed from the creped dryer surface.
[0191] 46. The process of any preceding or subsequent embodiment / feature / aspect, further comprising:
[0192] Prior to said substantially removing, the pH of said formulation located on said dryer surface is raised to a pH above 6.
[0193] 47. Any product or process of the grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the plurality of side chains do not contain vinyl-based monomers.
[0194] 48. Any product or process of the grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the plurality of side chains are substantially free of vinyl-based monomers.
[0195] 49. Any product or process of the grafted polyvinyl alcohol polymer of any preceding or following embodiment / feature / aspect, wherein the plurality of side chains are exclusively acrylic monomers.
[0196] The present invention may include any combination of these different aspects, features, or embodiments set forth above and / or below in sentences and / or paragraphs. Any combination of features disclosed herein is considered part of the present invention and there is no limitation on the combinable features.
[0197] The applicant specifically incorporates the full content of all cited references into the present disclosure. In addition, when the list of equivalent, concentration or other value or parameter is given as scope, preferred range or upper preferred value and lower preferred value, it should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, no matter whether scope is disclosed individually. In the numerical range listed herein, unless otherwise indicated, the scope is intended to include all integers and fractions in its endpoints and the scope. It is not intended that the scope of the present invention is limited to the specific values listed when defining the scope.
[0198] For those skilled in the art, it is clear that various modifications and variations can be made to the embodiments of the present invention without departing from the spirit or scope of the present invention. Therefore, the present invention is intended to cover other modifications and variations of the present invention as long as they are within the scope of the appended claims and their equivalents.
Claims
1. A grafted polyvinyl alcohol polymer comprising a polyvinyl alcohol main chain and a plurality of side chains grafted to the polyvinyl alcohol main chain, in, One or more of the side chains from the plurality of side chains comprises i) an aliphatic carboxylic acid unit or an aliphatic amide unit or both, and ii) an aminoalkyl(meth)acrylate unit or a hydroxylated alkyl(meth)acrylate unit or both, and Wherein, the grafted polyvinyl alcohol polymer has each of the following properties: a) the grafted polyvinyl alcohol polymer is a latex; b) the grafted polyvinyl alcohol polymer is fully dispersible in water at a pH of 2-5 in an amount of 1 wt % to 25 wt %; c) the grafted polyvinyl alcohol polymer is not an irreversible gel at any pH; d) the grafted polyvinyl alcohol polymer is gel-free at a pH of 8; and e) The grafted polyvinyl alcohol polymer has a first glass transition temperature of -40°C to 60°C, and a second glass transition temperature of 70°C to 90°C.
2. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains include: an aliphatic carboxylic acid unit, an aliphatic amide unit, an aminoalkyl(meth)acrylate unit, and a hydroxylated alkyl(meth)acrylate unit.
3. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains comprises an aliphatic carboxylic acid unit.
4. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains comprises an aliphatic amide unit.
5. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains comprises a hydroxylated alkyl (meth)acrylate unit.
6. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains comprises: an aliphatic carboxylic acid unit and an aliphatic amide unit.
7. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains comprises: an aliphatic carboxylic acid unit and a hydroxylated alkyl (meth)acrylate unit.
8. The grafted polyvinyl alcohol polymer of claim 1, wherein One or more of the side chains from the plurality of side chains comprises: an aliphatic amide unit and a hydroxylated alkyl (meth)acrylate unit.
9. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer has a viscosity of less than 500 cP·s when present in an aqueous dispersion having a pH of 3 at a concentration of 22.5-25 wt % at 25° C. and 1 atmosphere.
10. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer has a viscosity of less than 100 cP·s when present in an aqueous solution with a pH of 3 at a concentration of 2.5-10 wt % at 25° C. and 1 atmosphere.
11. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer can be dispersed in an aqueous solution at a concentration of 10 wt % to 40 wt %.
12. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer is capable of being dispersed in an aqueous solution and forms a stable aqueous dispersion that exhibits no coagulation or precipitation of the grafted polyvinyl alcohol polymer over a period of at least 6 months at 25°C and 1 atmosphere.
13. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer can be in a coagulated form when present in an aqueous solution with a pH of 2 to 5, can be in a semi-coagulated form when present in an aqueous solution with a pH of 4 to 5.5, and can be in an amorphous form when present in an aqueous solution with a pH of 5.5 to 8.
14. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer has a weight average molecular weight of 5,000 Daltons to 1,500,000 Daltons.
15. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer has a number average molecular weight of 1,000 to 50,000 Daltons.
16. The grafted polyvinyl alcohol polymer of claim 1, wherein The grafted polyvinyl alcohol polymer has a polydispersity Mw / Mn of at least 1.
5.
17. The grafted polyvinyl alcohol polymer of claim 1, wherein The polyvinyl alcohol backbone in its unreacted form has a weight average molecular weight of 5,000 to 1,500,000 Daltons.
18. The grafted polyvinyl alcohol polymer of claim 17, wherein The molecular weight distribution can be unimodal, bimodal, or multimodal.
19. The grafted polyvinyl alcohol polymer of claim 1, wherein The polyvinyl alcohol backbone in its unreacted form has a number average molecular weight of 1,000 to 50,000 Daltons.
20. The grafted polyvinyl alcohol polymer of claim 1, wherein The polyvinyl alcohol backbone has a polydispersity Mw / Mn of 2 to 7 in unreacted form.
21. The grafted polyvinyl alcohol polymer of claim 1, wherein The polyvinyl alcohol backbone has a degree of hydrolysis of 74 mol % to 95 mol %.
22. The grafted polyvinyl alcohol polymer of claim 1, in, an aliphatic carboxylic acid is present and comprises at least one of acrylic acid and methacrylic acid, wherein the aliphatic amide is present and comprises at least one of acrylamide, methacrylamide, dimethylacrylamide, diethylacrylamide, dipropylacrylamide and N-tert-butylacrylamide, and The hydroxylated alkyl (meth)acrylate is present and includes at least one of 2-hydroxyethyl methacrylate and hydroxypropyl methacrylate.
23. The grafted polyvinyl alcohol polymer of claim 1, in, An aliphatic carboxylic acid is present and is methacrylic acid, wherein the aliphatic amide is present and is acrylamide, and Among them, the hydroxylated alkyl (meth)acrylate is present and is 2-hydroxyethyl methacrylate.
24. The grafted polyvinyl alcohol polymer of claim 1 comprising structure (I): -[CH2-CH(OH)] a -[CH2-CH(R])] b -(I) in, Based on the total weight of the grafted polyvinyl alcohol polymer, the total weight percentage of (a) units is 74% to 95%, Wherein, based on the total weight of the grafted polyvinyl alcohol polymer, the total weight percentage of (b) units is 5% to 26%, wherein each R is acetate or a side chain from the plurality of side chains.
25. The grafted polyvinyl alcohol polymer of claim 1 comprising structure (II): in, a is 1 to 10; b is 35 to 55; c is 35 to 55, provided that a+b+c=100.
26. The grafted polyvinyl alcohol polymer of claim 1, wherein The plurality of side chains do not contain a vinyl monomer, and the vinyl monomer is selected from vinyl acetate, vinyl pyrrolidone, ethylene and vinyl ester.
27. The grafted polyvinyl alcohol polymer of claim 1, wherein The plurality of side chains are only acrylic monomers.
28. A preparation comprising: aqueous phase; and The grafted polyvinyl alcohol polymer of claim 1.
29. The formulation of claim 28, wherein The formulation comprises: 100 parts by weight of an aqueous phase; and 10 to 40 parts by weight of a grafted polyvinyl alcohol polymer, wherein The grafted polyvinyl alcohol polymer is dispersed in the water phase.
30. The formulation of claim 28, wherein The formulation is a stable aqueous dispersion that exhibits no coagulation or precipitation of the grafted polyvinyl alcohol polymer over a period of at least 6 months.
31. The formulation of claim 28, wherein The formulation has a pH of 2 to 5, and Therein, the grafted polyvinyl alcohol polymer is in a coagulated form.
32. The formulation of claim 28, wherein The formulation has a pH of 4 to 5.5, and The grafted polyvinyl alcohol polymer is in a semi-condensed form.
33. The formulation of claim 28, wherein The formulation has a pH of 5.5 to 8, and Among them, the grafted polyvinyl alcohol polymer is in an amorphous dissolved form.
34. The formulation of claim 28, wherein The grafted polyvinyl alcohol polymer is soluble in the aqueous phase in an amount of at least 10 g / 100 g water.
35. The formulation of claim 28, wherein The formulation contains less than 1 wt% surfactant.
36. The formulation of claim 28, wherein The formulation contains no surfactant.
37. A method of making the grafted polyvinyl alcohol polymer of claim 1, the method comprising: At least one of an aliphatic carboxylic acid, an aliphatic amide, an aminoalkyl(meth)acrylate, and a hydroxylated alkyl(meth)acrylate is polymerized via free radical polymerization in the presence of free polyvinyl alcohol.
38. A method of making an aqueous solution of the grafted polyvinyl alcohol polymer of claim 1, the method comprising: A base is added to the dispersion, thereby raising the pH of the dispersion to 4 to 8 and forming an aqueous solution of the grafted polyvinyl alcohol polymer, wherein The dispersion contains: Water phase; and The grafted polyvinyl alcohol polymer is dispersed in an aqueous phase, wherein the dispersion has a pH of 2 to 5 prior to said adding.
39. A process for creping a fiber web, comprising: providing a rotating cylindrical dryer comprising a dryer surface, applying a formulation comprising the grafted polyvinyl alcohol polymer of claim 1 to a dryer surface, conveying the fiber web onto the dryer surface, drying the fibrous web on the dryer surface to form a dried fibrous web, and The dried fiber web is creped from the dryer surface.
40. The process of claim 39, wherein The formulation is a dispersion.
41. The process of claim 40, wherein The formulation had a pH of 4.5 to 6.
42. The process of claim 40, further comprising: The formulation is substantially removed from the creped dryer surface.