A solid electrolyte with mechanical gradient and its preparation method and application
By introducing mechanical gradient and in-situ polymerization process into the solid electrolyte, the problems of lithium dendrite growth and interface mechanical failure are solved, the stability and safety of the battery are improved, and the ionic conductivity is improved.
Patent Information
- Application Number
- CN202111515118.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-12-13
AI Technical Summary
Solid-state lithium metal batteries face problems such as lithium dendrite growth, interface mechanical failure and poor interfacial compatibility, resulting in battery short circuit and low cycle efficiency, and it is difficult for inorganic solid electrolytes to remain stable in long-term cycle tests.
A solid electrolyte with a mechanical gradient is designed. By controlling the lithium salt concentration and initiator concentration, the Young's modulus of the gradient electrolyte gradually increases from the positive electrode to the negative electrode. Combined with the in-situ polymerization process, a close interface is formed to inhibit the growth and mitigation of lithium dendrites. Interfacial mechanical stress caused by volume expansion of the cathode.
It effectively reduces the height of the lithium dendrite tip on the negative electrode side, prevents battery short circuit, improves the cycle stability and safety performance of the battery, and improves ion conductivity.
Smart Images

Figure CN114497716B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of battery technology, and specifically relates to the field of solid electrolyte technology, and specifically relates to a solid electrolyte with a mechanical gradient, and a preparation method and application thereof. Background Art
[0002] At present, the successful commercial application of electrolytes represented by organic solvents such as liquid ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) has made lithium batteries represented by lithium iron phosphate widely recognized and accepted by the market. However, due to the intrinsic characteristics of the liquid organic electrolyte system, it is difficult to meet the requirements of high energy density scenarios and high safety scenarios. Therefore, the development of solid-state batteries is imminent. The energy density of traditional lithium-ion batteries has reached a bottleneck, and liquid organic electrolytes have safety hazards such as easy leakage, easy volatility, and easy combustion. In comparison, the intrinsic characteristics of solid electrolytes that are non-leaking and non-volatile can significantly improve the safety of the battery, while avoiding the problem of short battery life caused by electrolyte drying up. In addition, the higher mechanical strength of solid electrolytes helps to inhibit the growth of lithium dendrites, which can not only further ensure the safety of the battery, but also make it possible to use lithium metal as the negative electrode, which is conducive to greatly improving the energy density of the battery. However, solid-state lithium metal batteries face problems such as lithium dendrite growth, interface mechanical failure, and poor interface compatibility: (1) Lithium dendrites nucleate and grow on the negative electrode side, penetrating the solid electrolyte and causing a short circuit in the solid-state battery; (2) The repeated volume changes of the positive electrode material during the charge and discharge process generate mechanical stress, which destroys the physical contact properties of the electrode / electrolyte interface and causes interface mechanical failure, thereby reducing the battery's cycle efficiency and stability.
[0003] The research on solid electrolytes mainly focuses on inorganic solid electrolytes and polymer solid electrolytes. Inorganic solid electrolytes not only have high ionic conductivity, such as Li10GeP2S12 ionic conductivity can reach 10mS / cm (Journal of the Electrochemical Society, 2015; 163(2): A67-A74.), Li6.5La3Zr1.5Ta0.5O12 ionic conductivity can reach 1mS / cm (Chemistry of Materials, 2016; 28(1): 197-206.), but in long-cycle tests, these inorganic solid electrolytes are difficult to maintain stability, and interface problems gradually accumulate and worsen during the cycle. Polymers as electrolytes have a simple production process and can effectively alleviate interface problems, so they have gradually attracted the attention of researchers. Usually, researchers reduce the crystallinity of polymers and improve ionic conductivity through methods such as cross-linking, grafting, blending and doping. At the same time, the volume expansion of the positive electrode during the cycle may also cause battery failure. Combining the characteristics of polymer solid electrolytes, researchers have designed various types of multilayer heterostructures: Goodenough et al. constructed an organic / inorganic / organic multilayer solid electrolyte. The inorganic layer can limit the transmission of lithium salt anions in the polymer electrolyte and increase the ion migration number; the organic layer with good flexibility can enhance the contact performance with the positive and negative electrode interfaces (Journal of the Americal Chemical Society, 2016; 138(30): 9385-9388.). Guo et al. designed an asymmetric multilayer electrolyte: the middle layer is a dense Li7La3Zr2O12 inorganic solid electrolyte, and the side facing the lithium metal negative electrode is a 7.5nm ultra-thin polymer electrolyte layer. The two work together to enhance the interface contact performance while effectively preventing lithium dendrites from penetrating the electrolyte; the side facing the positive electrode is a thicker polymer solid electrolyte, which helps to maintain the close physical contact between the electrolyte and the positive electrode during the charge and discharge process and ensure stable interfacial ion transmission (Journal of the Americal Chemical Society, 2018; 140(1): 82-85.). The construction of double-layer / multilayer structures such as inorganic solid electrolyte layer / organic solid electrolyte layer, organic solid electrolyte layer / inorganic solid electrolyte layer / organic solid electrolyte layer can, on the one hand, alleviate the problem of mechanical failure of the interface on the positive electrode side, while limiting the growth of lithium dendrites on the negative electrode side, and on the other hand, improve the chemical / electrochemical compatibility of the interface.However, due to the crystal phase mismatch and chemical potential difference on both sides of the heterogeneous interface, the lithium ion transport across the interface needs to overcome a higher diffusion energy barrier, which limits the lithium ion diffusion kinetics in the solid electrolyte, resulting in the currently reported double-layer / multi-layer heterostructure solid electrolytes exhibiting low ionic conductivity (no more than 0.1mS / cm).
[0004] In view of this, the present invention provides a mechanical gradient solid electrolyte designed to address the problem of lithium dendrites on the negative electrode side and the problem of interfacial mechanical failure caused by volume changes of positive electrode materials such as lithium iron phosphate during the cycle. The mechanical properties of the gradient electrolyte are shown as a gradual increase in Young's modulus from the positive electrode to the negative electrode; at the same time, the implementation of the mechanical gradient electrolyte is regulated by the concentration of lithium salts and the concentration of initiators; in addition, a solid electrolyte with a high Young's modulus can reduce the height of the tip of the lithium dendrite on the negative electrode side, inhibit the growth of lithium dendrites, and prevent battery short circuits; and a solid electrolyte with certain elastic strain and bonding properties can alleviate the problem of interfacial mechanical stress caused by volume expansion of the positive electrode during the cycle; in addition, the interface contact layer adopts an in-situ polymerization process, which is conducive to forming a closely bonded interface and avoiding the formation of voids and holes at the interface. In addition, the present invention also discloses a solid electrolyte with this force gradient structure, a preparation method, and an application thereof. Summary of the invention
[0005] In order to solve the problem of lithium dendrites on the negative electrode side and the problem of interface mechanical failure caused by volume change of positive electrode materials such as lithium iron phosphate during the cycle, the present invention designs a solid electrolyte with a mechanical gradient, which satisfies the contradictory requirements of the mechanical properties of the solid electrolyte on the positive and negative electrode sides of the solid-state battery while obtaining high ionic conductivity. Therefore, the present application provides a solid electrolyte with a mechanical gradient, a preparation method thereof, and an application in a battery.
[0006] The present invention provides a solid electrolyte with a mechanical gradient and a preparation method thereof. The mechanical gradient electrolyte comprises: (1) a solid polymer electrolyte precursor solution and an initiator with a high Young's modulus, (2) a gel polymer electrolyte precursor solution and an initiator with certain elasticity and bonding properties, and (3) an electrolyte salt; wherein (1) the gradient electrolyte is characterized in that the Young's modulus gradually increases from the positive electrode to the negative electrode in terms of mechanical properties; (2) the implementation of the mechanical gradient electrolyte is regulated by the concentration of lithium salt and the concentration of initiator; (3) the solid polymer electrolyte with a high Young's modulus can reduce the height of the tip of the lithium dendrite on the negative electrode side, inhibit the growth of lithium dendrites, and prevent the battery from short circuiting; (4) the solid electrolyte with certain elastic strain and bonding properties can alleviate the problem of interfacial mechanical stress caused by volume expansion of the positive electrode during the cycle; (5) in addition, the interfacial contact layer adopts an in-situ polymerization process, which is conducive to forming a closely bonded interface and avoiding the formation of voids and holes at the interface.
[0007] The (1) solid polymer electrolyte precursor solution and initiator having a high Young's modulus, wherein the precursor solution is selected from methyl methacrylate (MMA), methacrylate (VMA), vinylene carbonate (VC), vinylene carbonate (VEC), acrylonitrile (AN), vinyl acetate (VAC), styrene (ST), polyethylene oxide (PEO), polyethylene oxide (PPO), polyoxymethylene (POM), polyvinyl acetate (PVA), polyethylene imine (PEI), polyethylene succinate, polyoxetane, polyβ-propiolactone, polyepichlorohydrin, poly-N-propylaziridine, polyalkylene oxide (PEI), polyisocyanate ... One or more of sulfur, polyvinylidene fluoride (PVDF), methyl acrylate (MA), acrylamide (AM), 2-hydroxymethyl acrylate, trifluoroethyl acrylate (TFMA), polyethylene glycol phenyl ether acrylate (PEGPEA), polyethylene glycol diacrylate (PEGDA), polyethylene glycol diglycidyl ether (PEGDE), ethoxylated trimethyl propane triacrylate (ETPTA), polycyanopolyvinyl alcohol (PVA-CN), 1,3-dioxolane (DOL), 1,3,5-trioxane, 1,4-dioxane, tetrahydrofuran (THF), polyvinyl formal (PVFM), etc.
[0008] Preferably, the solid polymer precursor solution is 1,3-dioxolane (DOL).
[0009] The initiator is selected from commonly used free radical initiators, cationic initiators, anionic initiators and coordination polymerization initiators. Free radical initiators are mainly azo initiators (azobisisobutyronitrile (AIBN), dimethyl azobisisobutyrate initiator, etc.), peroxide initiators (benzamide peroxide (BPO), etc.) and redox initiators, etc.; cationic polymerization initiators mainly include protonic acids and Lewis acids (mainly including BF3, PF5, AlCl3, Al(CF3SO3)3, Sn(CF3SO3)2, etc.); anionic polymerization initiators (mainly alkali metals, organic compounds of alkali metals and alkaline earth metals, bases such as tertiary amines, electron donors or nucleophiles, etc.); coordination polymerization initiators (mainly Ziegler-Natta initiators, metallocene initiators, etc.) are one or more.
[0010] Preferably, the solid polymer precursor solution initiator is a cationic initiator LiPF6 which can decompose to form PF5.
[0011] The (2) gel polymer electrolyte precursor solution and initiator having certain elasticity and adhesion properties, typical but not limiting precursor solutions are selected from methyl methacrylate (MMA), methyl methacrylate (VMA), vinyl carbonate (VC), acrylonitrile (AN), vinyl acetate (VAC), styrene (ST), polyethylene oxide (PEO), polyethylene oxide (PPO), polyoxymethylene (POM), polyvinyl acetate (PVA), polyethylene imine (PEI), polyethylene succinate, polyoxetane, polyβ-propiolactone, polyepichlorohydrin, poly N-propylaziridine, polyalkylene polysulfide, polyvinylidene fluoride (PVDF), methyl acrylate (MA), acrylamide (AM), polyvinyl fluoride (PVDF), polyvinyl acrylate (PVD), polyvinyl fluoride (PVDF ... ), 2-hydroxymethyl acrylate, trifluoroethyl acrylate (TFMA), polyethylene glycol phenyl ether acrylate (PEGPEA), polyethylene glycol diacrylate (PEGDA), polyethylene glycol diglycidyl ether (PEGDE), ethoxylated trimethyl propane triacrylate (ETPTA), polycyanopolyvinyl alcohol (PVA-CN), 1,3-dioxolane (DOL), 1,3,5-trioxane, 1,4-dioxane, tetrahydrofuran (THF), polyvinyl formal (PVFM), propylene carbonate, ethylene carbonate, diethyl carbonate, fluoroethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethyl sulfone, dimethyl ether, etc.
[0012] Preferably, the gel polymer precursor solution is 1,3-dioxolane (DOL).
[0013] The gel polymer precursor solution initiator is selected from commonly used free radical initiators, cationic initiators, anionic initiators and coordination polymerization initiators. Free radical initiators are mainly azo initiators (azobisisobutyronitrile (AIBN), dimethyl azobisisobutyrate initiator, etc.), peroxide initiators (benzamide peroxide (BPO), etc.) and redox initiators, etc.; cationic polymerization initiators mainly include protonic acids and Lewis acids (mainly including BF3, PF5, AlCl3, Al(CF3SO3)3, Sn(CF3SO3)2, etc.); anionic polymerization initiators (mainly alkali metals, organic compounds of alkali metals and alkaline earth metals, bases such as tertiary amines, electron donors or nucleophiles, etc.); coordination polymerization initiators (mainly Ziegler-Natta initiators, metallocene initiators, etc.) are one or more.
[0014] Preferably, the gel polymer precursor solution initiator is a cationic initiator LiPF6, which can be decomposed to form PF5.
[0015] The (3) electrolyte lithium salt is selected from one or more of lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonate)imide [LiN(CF3SO2)2, LiTFSI] and its derivatives, perfluoroalkyl lithium phosphate [LiPF3(C2F5)3, LiFAP], lithium tetrafluorooxalate phosphate [LiPF4(C2O4)], lithium bis(oxalatoborate) (LiBOB), lithium tri(catechol) phosphate (LTBP) and sulfonated polysulfonamide lithium salt, lithium hexafluorophosphate (LiPF6), aluminum perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), etc.
[0016] Preferably, the electrolyte lithium salt is lithium bis(trifluoromethanesulfonic acid)imide LiTFSI, and the concentration range is 0.01-10 mol / L (preferably 0.25-1 mol / L).
[0017] In a second aspect, the present invention provides a method for preparing a continuous mechanical gradient solid electrolyte controlled by lithium salt concentration, the method comprising:
[0018] (1) Preparation of high Young's modulus solid polymer electrolyte precursor solution: First, take a certain amount of solid polymer monomer solvent; then take an appropriate amount of lithium salt and dissolve it in the precursor solution, and stir it thoroughly; remove water from the above solution with a lithiated molecular sieve for 24 hours, and finally take an appropriate amount of initiator and add it to the above solution while stirring, and stir it thoroughly until the solution is completely uniform. The above operations are all carried out in an argon glove box (the water and oxygen content is less than 0.1ppm).
[0019] (2) Preparation of a gel polymer electrolyte precursor solution with certain elasticity and adhesion: weigh a certain amount of gel polymer monomer solvent, add an appropriate amount of lithium salt, and stir thoroughly until dissolved; dehydrate the above solution with a lithiated molecular sieve for 24 hours, and finally take an appropriate amount of initiator and add it to the above solution while stirring, and stir thoroughly until the solution is completely uniform. The above operations are all carried out in an argon glove box (the water and oxygen content is less than 0.1ppm).
[0020] (3) Preparation of button cells: drip a solid polymer electrolyte precursor solution regulated by low lithium salt concentration on the surface of the negative electrode, keep a sample for observation, and when the precursor solution in the glass bottle solidifies, proceed to the next step, which is pre-curing; drip a gel polymer electrolyte precursor solution regulated by high lithium salt concentration on the surface of the solidified gel polymer, stack lithium iron phosphate or ternary positive electrode on top, and assemble the button cell. The above operations are all carried out in an argon glove box (water and oxygen content are all less than 0.1ppm); the reverse order of the above operations is also within the scope of the technical application.
[0021] Or (4) soft pack battery assembly, cut a lithium ribbon of a certain shape, drip a solid polymer electrolyte precursor solution regulated by a low lithium salt concentration on the surface of the negative electrode, keep a sample for observation, and when the precursor solution in the glass bottle solidifies, proceed to the next step, which is pre-curing; wrap the diaphragm between the lithium ribbon and the lithium iron phosphate positive electrode or the ternary positive electrode, inject a gel polymer electrolyte precursor solution regulated by a high lithium salt concentration, vacuum evacuate and package, compact and solidify, and assemble the soft pack battery. The above operations are all carried out in an argon glove box (the water and oxygen content is less than 0.1ppm); the reverse order of the above operations is also within the scope of the technical application.
[0022] In addition, the present invention also provides a secondary battery structure based on the mechanical gradient solid electrolyte, including a positive electrode current collector 1, a positive electrode 2, a negative electrode 4, a solid electrolyte 3 with a mechanical gradient, and a battery shell for packaging.
[0023] The positive electrode current collector 1 is selected from one of aluminum, vanadium, copper, iron, tin, zinc, nickel, titanium, manganese or an alloy thereof or a composite of any one of these metals or an alloy thereof. Preferably, the positive electrode current collector is aluminum foil.
[0024] The positive electrode 2 material of the lithium-ion battery is one or more composite materials of positive electrode compound materials (such as lithium cobalt oxide, lithium iron phosphate, nickel-cobalt-manganese ternary materials, etc.). Preferably, the positive electrode active material is lithium iron phosphate.
[0025] The negative electrode 4 material of the lithium-ion battery includes alloying materials such as lithium, lithium aluminum alloy, lithium magnesium alloy, and other lithium composite materials, etc. Preferably, the negative electrode active material is lithium.
[0026] The negative electrode, the solid electrolyte with a mechanical gradient, the positive electrode, the positive electrode current collector and the battery shell are assembled, and then in-situ polymerization is performed by thermal initiation or other initiation methods to form a solid-state battery.
[0027] The present invention also provides a method for preparing a secondary battery structure based on the mechanical gradient solid electrolyte, comprising the following steps:
[0028] Step 101: Prepare the positive electrode: weigh the positive electrode active material, conductive agent and binder in a certain proportion, add them into an appropriate solvent and mix them thoroughly into a uniform slurry to form a positive electrode active material layer; clean the positive electrode current collector, and then evenly apply the positive electrode active material layer on the surface of the positive electrode current collector, and cut the positive electrode active material layer after it is completely dried to obtain a battery positive electrode of the required size. The positive electrode active material, conductive agent and binder are preferably weighed in a mass ratio of 8:1:1 or 7:2:1.
[0029] Step 102: Prepare the negative electrode: Cut the negative electrode into discs with a diameter of 14 mm and place them in a vacuum drying oven for later use.
[0030] Step 103: Preparation of solid polymer electrolyte precursor solution with high Young's modulus: First, take a certain amount of solid polymer monomer solvent; then take an appropriate amount of lithium salt and dissolve it in the precursor solution, and stir it thoroughly; remove water from the above solution with a lithiated molecular sieve for 24 hours, and finally take an appropriate amount of initiator and add it to the above solution while stirring, and stir it thoroughly until the solution is completely uniform. The above operations are all carried out in an argon glove box (the water and oxygen content is less than 0.1ppm). Set aside.
[0031] Step 104: Preparation of a gel polymer electrolyte precursor solution with certain elasticity and adhesion, weigh a certain amount of gel polymer monomer solvent, add an appropriate amount of lithium salt, and stir thoroughly until dissolved; remove water from the above solution with a lithiated molecular sieve for 24 hours, and finally take an appropriate amount of initiator and add it to the above solution while stirring, and stir thoroughly until the solution is completely uniform. The above operations are all carried out in an argon glove box (water and oxygen content are all less than 0.1ppm). Set aside.
[0032] Step 105: button cell preparation, drip a solid polymer electrolyte precursor solution with high Young's modulus on the negative electrode surface, keep a sample for observation, and when the precursor solution in the glass bottle solidifies, proceed to the next step, which is pre-curing; drip a gel polymer electrolyte precursor solution with certain elasticity and adhesion on the solidified gel polymer surface, stack lithium iron phosphate or ternary positive electrode on top, and assemble the button cell. The above operations are all carried out in an argon glove box (water and oxygen content are all less than 0.1ppm); the above operations in reverse order are also within the scope of the technical application.
[0033] Step 106: Soft pack battery assembly, cut a lithium strip of a certain shape, drip a solid polymer electrolyte precursor solution with a high Young's modulus on the surface of the negative electrode, keep a sample for observation, and when the precursor solution in the glass bottle solidifies, proceed to the next step, which is pre-curing; wrap the diaphragm between the lithium strip and the lithium iron phosphate positive electrode or the ternary positive electrode, inject a gel polymer electrolyte precursor solution with certain elasticity and adhesion, package after vacuum evacuation, compact and solidify, and assemble the soft pack battery. The above operations are all carried out in an argon glove box (the water and oxygen content is less than 0.1ppm); the above operations in reverse order are also within the scope of the technical application.
[0034] The preparation method of the solid-state battery is further described below through specific examples. However, it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form.
[0035] It should be noted that although the above steps 101 to 104 describe the operations of the preparation method of the present invention in a specific order, this does not require or imply that these operations must be performed in this specific order. The preparations of steps 101 to 104 can be performed simultaneously or in any order.
[0036] In the present application, for the gradient monolayer solid electrolyte with targeted modification of the positive and negative electrodes, the formation of the mechanical gradient is regulated by the concentration gradient of the lithium salt / initiator, and the polymer solid electrolyte is constructed in situ inside the battery by an in-situ polymerization process. This design of regulating the lithium salt / initiator concentration gradient at a certain degree of freedom to achieve the mechanical gradient can simultaneously inhibit the growth of lithium dendrites and alleviate the interfacial mechanical stress failure problem caused by volume expansion of the positive electrode without introducing an additional solid phase interface. The in-situ polymerization process effectively improves the interface contact and wettability between the solid electrolyte and the electrolyte, thereby improving the cycle stability, rate performance and safety performance of the battery. Compared with the prior art, the key to the solid electrolyte with mechanical gradient prepared by the present invention lies in the control of the lithium salt concentration gradient and the control of the initiator concentration. (1) The mechanical properties of the gradient electrolyte are manifested as a gradual increase in Young's modulus from the positive electrode to the negative electrode; (2) The implementation of the mechanical gradient electrolyte is regulated by the lithium salt concentration and the initiator concentration; (3) The solid electrolyte with a high Young's modulus can reduce the height of the tip of the lithium dendrite on the negative electrode side, inhibit the growth of lithium dendrites, and prevent battery short circuit; (4) The solid electrolyte with certain elastic strain and bonding properties can alleviate the interfacial mechanical stress problem caused by the volume expansion of the positive electrode during the cycle; (5) In addition, the interface contact layer adopts an in-situ polymerization process, which is conducive to forming a closely bonded interface and avoiding the formation of voids and holes at the interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic diagram of the structure of a secondary battery with a gradient structure solid electrolyte, including a positive electrode current collector 1, a positive electrode 2, a gradient polymer solid electrolyte / solid electrolyte with a mechanical gradient 3, and a negative electrode 4.
[0038] Figure 2 (a) 0.5 mA / cm 2 Time-voltage curves of the Li / GSPE / Li symmetric cell at different areal current densities (GSPE stands for gradient structured solid electrolyte).
[0039] Figure 2 (b) is the capacity-voltage diagram of LFP / GSPE / Li battery at the 1st, 50th, 100th, 150th and 200th cycles.
[0040] Figure 2 (c) is the cycling performance diagram of LFP / GSPE / Li. DETAILED DESCRIPTION
[0041] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The following is a preferred embodiment of the present invention. It should be noted that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the embodiments of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.
[0042] Example 1
[0043] Prepare a solid polymer electrolyte precursor solution with high Young's modulus: dissolve 0.25 mol / L LiTFSI, a lithium salt, and an appropriate amount of initiator LiPF6 in 5 mL 1,3-dioxolane (DOL), stir well to dissolve, and set aside.
[0044] Prepare a gel polymer electrolyte precursor solution with certain elasticity and adhesion: dissolve 1 mol / L LiTFSI of lithium salt and an appropriate amount of initiator LiPF6 in 5 mL of 1,3-dioxolane (DOL), stir thoroughly to dissolve, and set aside.
[0045] Preparation of lithium iron phosphate positive electrode: weigh the positive electrode active material, conductive agent, and binder in a mass ratio of 8:1:1 or 7:2:1, add appropriate amount of N-methylpyrrolidone (NMP), mix and grind them into a uniform slurry; clean the positive electrode collector aluminum foil, and then evenly apply the lithium iron phosphate positive electrode slurry on the surface of the positive electrode collector to form a positive electrode active material layer, place it at room temperature for 8 hours, and then put it into a vacuum drying oven at 60°C and dry it for 24 hours. After the positive electrode active material layer is completely dried, take it out and cut it into 10 mm discs, and place it in a vacuum drying oven for use.
[0046] Preparation of lithium negative electrode: The lithium sheet was cut into discs with a diameter of 14 mm and placed in an argon-filled glove box (the water and oxygen contents were both less than 0.1 ppm) for later use.
[0047] Assembly of button cells with gradient structure polymer solid electrolyte: drip a solid polymer electrolyte precursor solution with high Young's modulus on the surface of the negative electrode, keep a sample for observation, and proceed to the next step when the precursor solution in the glass bottle solidifies; drip a gel polymer electrolyte precursor solution with certain elasticity and adhesion on the surface of the solidified gel polymer, stack lithium iron phosphate or ternary positive electrode on top, and assemble the button cell. The above operations are all carried out in an argon glove box (water and oxygen content are all less than 0.1ppm).
[0048] Specific examples 2 to 6 use the same process steps as example 1, and the specific positive and negative electrode materials, monomers, lithium salts, initiators, etc. used and the corresponding results of the full battery are shown in Table 1 below:
[0049] Table 1. Specific materials used in Examples 2-6 and corresponding results of full batteries
[0050]
[0051]
[0052] The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. Obviously, the above embodiments are only examples for clear explanation, and are not limitations on the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A solid electrolyte having a mechanical gradient, characterized in that: include: A solid polymer electrolyte precursor solution with high Young's modulus and its initiator, a gel polymer electrolyte precursor solution with certain elasticity and bonding properties and its initiator, and an electrolyte lithium salt; the solid electrolyte with mechanical gradient has a mechanical property that the Young's modulus gradually increases from the positive electrode to the negative electrode and is prepared by an in-situ polymerization process; The in-situ polymerization process comprises the following steps: Step S1: First, take the solid polymer electrolyte precursor solution with high Young's modulus; then take the electrolyte lithium salt and dissolve it in the precursor solution, and stir it thoroughly to make it uniform; finally, take the solid polymer electrolyte precursor solution initiator with high Young's modulus and add it to the above solution while stirring, and stir it thoroughly until the solution is completely uniform; Step S2: weighing the gel polymer electrolyte precursor solution with certain elasticity and adhesion properties, adding the electrolyte lithium salt, and stirring thoroughly until dissolved; finally taking the gel polymer electrolyte precursor solution initiator with certain elasticity and adhesion properties and adding it to the above solution while stirring, and stirring thoroughly until the solution is completely uniform; Step S3: drip the solution prepared in step S1 on the surface of the negative electrode, keep a sample for observation, and when the precursor solution in the glass bottle solidifies, proceed to the next step, which is pre-curing; drip or inject the solution prepared in step S2 on the surface of the solidified gel polymer.
2. The solid electrolyte with mechanical gradient according to claim 1, characterized in that: The solid polymer electrolyte precursor solution with high Young's modulus is selected from one or more of methyl methacrylate, methacrylate, vinyl carbonate, acrylonitrile, vinyl acetate, styrene, polyethylene oxide, polyoxymethylene, polyvinyl acetate, polyethylene imine, polyvinyl succinate, polyoxetane, polyβ-propiolactone, polyepichlorohydrin, poly-N-propylaziridine, polyalkylene polysulfide, polyvinylidene fluoride, methyl acrylate, acrylamide, 2-hydroxymethyl acrylate, trifluoroethyl acrylate, polyethylene glycol phenyl ether acrylate, polyethylene glycol diacrylate, polyethylene glycol diglycidyl ether, ethoxylated trimethylpropane triacrylate, polycyanopolyvinyl alcohol, 1,3-dioxolane, tetrazofuran and polyvinyl formal.
3. The solid electrolyte with mechanical gradient according to claim 2, characterized in that: The solid polymer electrolyte precursor solution with high Young's modulus is 1,3-dioxolane.
4. The solid electrolyte with mechanical gradient according to claim 1, characterized in that The solid polymer electrolyte precursor solution initiator with high Young's modulus is selected from commonly used initiators, including one or more of azo initiators, peroxide initiators, redox initiators, cationic polymerization initiators, anionic polymerization initiators, and coordination polymerization initiators.
5. The solid electrolyte with mechanical gradient according to claim 4, characterized in that: The azo initiator is selected from one or more of azobisisobutyronitrile (AIBN) and dimethyl azobisisobutyrate initiators; the peroxide initiator is selected from dibenzamide peroxide (BPO); the cationic polymerization initiator is selected from one or more of BF3, PFS, AlC13, Al(CF3SO3)3, Sn(CF3SO3)2; the anionic polymerization initiator is selected from one or more of alkali metals, organic compounds of alkali metals and alkaline earth metals, bases such as tertiary amines, electron donors or nucleophiles; the coordination polymerization initiator is selected from one or more of Ziegler-Natta initiators and metallocene initiators.
6. The solid electrolyte with mechanical gradient according to claim 5, characterized in that: The initiator of the solid polymer electrolyte precursor solution with high Young's modulus is a cationic initiator LiPF6, which can be decomposed to form PF5.
7. The solid electrolyte with mechanical gradient according to claim 1, characterized in that The gel polymer electrolyte precursor solution with certain elasticity and adhesion is selected from methyl methacrylate, methacrylate, vinyl carbonate, acrylonitrile, vinyl acetate, styrene, polyethylene oxide, polyoxymethylene, polyvinyl acetate, polyethylene imine, polyvinyl succinate, polyoxetane, polyβ-propiolactone, polyepichlorohydrin, poly-N-propylaziridine, polyalkylene polysulfide, polyvinylidene fluoride, methyl acrylate, acrylic amine, 2-hydroxymethyl acrylate, trifluoroethyl acrylate One or more of acrylate, polyethylene glycol phenyl ether acrylate, polyethylene glycol diacrylate, polyethylene glycol diglycidyl ether, ethoxylated trimethyl propane triacrylate, polycyanopolyvinyl alcohol, 1,3-dioxolane, 1,3,5-trioxane, 1,4-dioxane, tetrazofuran, polyvinyl formal, propylene carbonate, ethylene carbonate, diethyl carbonate, fluoroethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethyl sulfone and dimethyl ether.
8. The solid electrolyte with mechanical gradient according to claim 7, characterized in that The gel polymer electrolyte precursor solution with certain elasticity and adhesion is 1,3-dioxolane.
9. The solid electrolyte with mechanical gradient according to claim 1, characterized in that: The gel polymer electrolyte precursor solution initiator having certain elasticity and adhesion is selected from commonly used initiators, including one or more of azo initiators, peroxide initiators, redox initiators, cationic polymerization initiators, and anionic polymerization initiators.
10. The solid electrolyte with mechanical gradient according to claim 9, characterized in that: The azo initiator is selected from one or more of azobisisobutyronitrile (AIBN) and dimethyl azobisisobutyrate initiators; the peroxide initiator is selected from dibenzoyl peroxide (BPO); the cationic polymerization initiator is selected from one or more of BF3, PF5, A1C13, A1(CF3SO3)3, Sn(CF3SO3)2; the anionic polymerization initiator is selected from one or more of alkali metals, organic compounds of alkali metals and alkaline earth metals, bases such as tertiary amines, electron donors or nucleophiles.
11. The solid electrolyte with mechanical gradient according to claim 10, characterized in that: The initiator of the gel polymer electrolyte precursor solution with certain elasticity and adhesion is a cationic initiator L1PF6, which can be decomposed to form PF5.
12. The solid electrolyte with mechanical gradient according to claim 1, characterized in that The electrolyte lithium salt is selected from one or more of lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonate)imide [LiN(CF3SO2)2, LiTFSI] and its derivatives, perfluoroalkyl lithium phosphate [LiPF3(C2F5)3, LiFAP], lithium tetrafluorooxalate phosphate [LiF4(C2O4)], lithium bis(oxalatoborate) (LiBOB), lithium tris(catechol) phosphate (LTBP), sulfonated polysulfonamide lithium salt, lithium hexafluorophosphate (LiPF6), aluminum perchlorate (LiC1O4), lithium tetrafluoroborate (LiBF4) and lithium hexafluoroarsenate (LiAsF6), and the concentration range is 0.01-10 mol / L.
13. The solid electrolyte with mechanical gradient according to claim 1, characterized in that The electrolyte lithium salt is lithium bis(trifluoromethanesulfonic acid)imide LiTFSI, and the concentration range is 0.2 to 5-1 mol / L.
14. A secondary battery based on a solid electrolyte with a mechanical gradient, characterized in that: The invention comprises a positive electrode current collector, a positive electrode, a negative electrode, a solid electrolyte with a mechanical gradient as claimed in any one of claims 1 to 13, and a battery casing for packaging.
15. A method for preparing a secondary battery containing a solid electrolyte having a mechanical gradient according to any one of claims 1 to 13, characterized in that: include: Step 101: preparing a positive electrode: weighing a positive electrode active material, a conductive agent and a binder, adding them to a solvent and fully mixing them into a uniform slurry to form a positive electrode active material layer, cleaning the positive electrode current collector, and then uniformly coating the positive electrode active material layer on the surface of the positive electrode current collector, and cutting the positive electrode active material layer after it is completely dried to obtain a battery positive electrode of a desired size; Step 102: preparing the negative electrode: cutting the negative electrode into a disc with a diameter of 14 mm and placing it in a vacuum drying oven for standby use; Step 103: First, take a solid polymer electrolyte precursor solution with a high Young's modulus; then take an electrolyte lithium salt and dissolve it in the precursor solution, and stir it thoroughly; remove water from the above solution with a lithiated molecular sieve for 24 hours, and finally take a solid polymer electrolyte precursor solution initiator with a high Young's modulus and add it to the above solution while stirring, and stir it thoroughly until the solution is completely uniform. The above operations are all carried out in an argon glove box, and the water and oxygen content is less than 0.1ppm, and it is set aside; Step 104: weigh a gel polymer electrolyte precursor solution with certain elasticity and adhesion properties, add electrolyte lithium salt, and stir thoroughly until dissolved; remove water from the above solution using a lithiated molecular sieve for 24 hours, and finally take a gel polymer electrolyte precursor solution initiator with certain elasticity and adhesion and add it to the above solution while stirring, and stir thoroughly until the solution is completely uniform. The above operations are all carried out in an argon glove box, and the water and oxygen content is less than 0.1ppm; set aside; Step 105: button cell preparation, drip the solution prepared in step S103 on the surface of the negative electrode, keep the sample for observation, and when the precursor solution in the glass bottle is solidified, proceed to the next step, which is pre-curing; drip the solution prepared in step 104 on the surface of the solidified gel polymer, stack lithium iron phosphate or ternary positive electrode on top, and assemble the button cell; the above operations are all carried out in an argon glove box, and the water and oxygen content are all less than 0.1ppm; or soft-pack battery assembly, cut a lithium strip of a certain shape, drip the solution prepared in step S103 on the surface of the negative electrode, keep the sample for observation, and when the precursor solution in the glass bottle is solidified, proceed to the next step, which is pre-curing; wrap the diaphragm between the lithium strip and the lithium iron phosphate positive electrode or ternary positive electrode, inject the solution prepared in step 104, package after vacuum evacuation, compact and solidify, and assemble the soft-pack battery. The above operations are all carried out in an argon glove box, and the water and oxygen content are all less than 0.1ppm.