Composite ternary positive electrode material, preparation method thereof and lithium ion battery containing composite ternary positive electrode material

By coating the surface of the ternary cathode material with a cobalt compound and a solid electrolyte, a composite ternary cathode material is formed, which solves the stability and cycle performance problems of the cathode material in the existing technology and significantly improves the electrochemical performance and energy of lithium-ion batteries. density.

CN118800892APending Publication Date: 2024-10-18ZHEJIANG ZEEKR INTELLIGENT TECH CO LTD +2
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202410945027.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing high-nickel secondary ball ternary cathode materials in lithium-ion batteries have problems such as high residual alkali, poor processing performance, poor thermal stability, and rapid DCR growth during cycling, which affects the cycle performance and energy density of the battery.

Method used

Composite ternary cathode material is used, and a cobalt compound and solid electrolyte are coated on the surface of the ternary cathode active material to form a uniform coating layer, which improves ionic conductivity, inhibits side reactions between the cathode material and the electrolyte, and enhances high temperature stability and Cycle performance.

Benefits of technology

A more uniform coating layer is achieved, which reduces the initial and cyclic DC impedance of the battery, improves the battery's fast charging performance and cycle performance, and enhances high-temperature stability and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a composite ternary positive electrode material, a preparation method thereof and a lithium ion battery containing the composite ternary positive electrode material, and belongs to the technical field of secondary batteries. The composite ternary positive electrode material comprises a ternary positive electrode active material and a coating layer coating the surface of the ternary positive electrode active material, and the coating layer comprises a cobalt compound and a solid electrolyte. The composite ternary positive electrode material is obtained by wet mixing of a ternary positive electrode active material, a cobalt source and a solid electrolyte and sintering. The composite ternary positive electrode material provided by the invention is uniform in coating, relatively low in surface residual alkali amount, relatively high in ionic conductivity and gram volume, capable of effectively improving the fast charge performance, the cycle performance and the energy density of the lithium ion battery, simple in preparation process, low in cost and beneficial to industrial mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a composite ternary positive electrode material, a preparation method thereof and a lithium ion battery containing the composite ternary positive electrode material. Background Art

[0002] At present, the main pain point of the development of new energy vehicles is to solve the range anxiety: the first method is to increase the energy density of the battery pack; the second method is to improve the fast charging capability. In recent years, as the heart of new energy vehicles, lithium-ion batteries have been installed year by year due to their high specific energy, long life and high safety. Among them, as the key material for providing energy for lithium-ion batteries, the optimization and improvement of positive electrode materials are urgent.

[0003] Ternary cathode materials (LiNi x Co y Mn 1-x-y O2, 0<x, y<1) has become the main development direction of positive electrode materials for power batteries due to its high energy density and long cycle life. However, the high-nickel secondary sphere ternary positive electrode materials currently used in power batteries on the market have problems such as high residual alkali, poor processing performance, strict requirements on the trial production environment, poor thermal stability, fast DCR growth in long-term cycles, and severe gas production.

[0004] Based on this background, researchers have proposed a multi-element doping scheme to improve the material's compressive resistance, reduce the degree of particle cracking, and improve the dynamic stability during the cycle, thereby improving the capacity retention rate of the material during the cycle. There is also a multi-element coating scheme that optimizes the material interface by modifying and optimizing the interface, reducing the damage of the electrolyte to the interface, and improving the capacity and capacity retention rate. However, this material modification process mostly uses solid-phase sintering, and the coating effect still has shortcomings. For example, solid-phase coating of Al2O3, although it can achieve the effect of protecting the interface, the coating effect is uneven. The places where the coating is concentrated are not conducive to lithium ion transmission, which in turn affects the capacity; and the places where the coating is insufficient do not play a role in protecting the interface. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a composite ternary positive electrode material, a preparation method thereof and a lithium ion battery comprising the same.

[0006] In a first aspect, the present invention provides a composite ternary positive electrode material, which comprises a ternary positive electrode active material and a coating layer coated on the surface of the ternary positive electrode active material, wherein the coating layer comprises a cobalt compound and a solid electrolyte.

[0007] In some embodiments of the present invention, the chemical formula of the ternary positive electrode active material is LiNi x Co y Mn 1-x-yO2, where 0.8≤x≤0.95, 0.01≤y≤0.05, and 1-xy>0.

[0008] In some embodiments of the present invention, the cobalt compound includes LiCoO2.

[0009] In some embodiments of the present invention, the solid electrolyte includes any one or a combination of oxide solid electrolyte, sulfide solid electrolyte, polymer solid electrolyte and borate solid electrolyte.

[0010] In some embodiments of the present invention, the solid electrolyte includes any one or a combination of lithium aluminum titanium phosphate (LATP), lithium lanthanum zirconium oxide (LLZO) and lithium lanthanum titanate (LLTO).

[0011] In some embodiments of the present invention, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt compound is 100:(0.5-5).

[0012] In some embodiments of the present invention, the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:(0.1-1).

[0013] In some embodiments of the present invention, the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:(0.1-0.5).

[0014] In a second aspect, the present invention provides a method for preparing the composite ternary cathode material according to the first aspect, the preparation method comprising the following steps:

[0015] (1) mixing a ternary hydroxide precursor, a lithium source and a flux, and sintering the mixture to obtain a ternary positive electrode active material;

[0016] (2) Mixing the ternary positive electrode active material with a cobalt source, a solid electrolyte, a surfactant and water, so that the cobalt source and the solid electrolyte adhere to the surface of the ternary positive electrode active material, and sintering to obtain a composite ternary positive electrode material.

[0017] In some embodiments of the present invention, the chemical formula of the ternary hydroxide precursor is Ni x Co y Mn 1-x-y (OH)2, wherein 0.8≤x≤0.95, 0.01≤y≤0.05, and 1-xy>0.

[0018] In some embodiments of the present invention, the lithium source includes any one or a combination of lithium carbonate, lithium hydroxide and lithium nitrate.

[0019] In some embodiments of the present invention, the flux includes any one or a combination of NaCl, NaF, Na2O, NaBO2, Na2BO3, SrO, Na2SO4, K2SO4, KCl, KF and B2O3.

[0020] In some embodiments of the present invention, the cobalt source includes any one or a combination of Co(OH)2, CoOOH, Co3O4, cobalt chloride, cobalt carbonate and cobalt oxalate.

[0021] In some embodiments of the present invention, the particle size of the cobalt source is 20-200 nm.

[0022] In some embodiments of the present invention, the surfactant is polyethylene glycol.

[0023] In some embodiments of the present invention, the molecular weight of the polyethylene glycol is 200-6000.

[0024] In some embodiments of the present invention, the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:(1.03-1.1).

[0025] In some embodiments of the present invention, the mass of the flux accounts for 200-600 ppm of the total mass of the ternary hydroxide precursor, the lithium source and the flux.

[0026] In some embodiments of the present invention, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:(0.5-5).

[0027] In some embodiments of the present invention, the mass ratio of the ternary positive electrode active material to the surfactant is 100:(0.1-0.3).

[0028] In some embodiments of the present invention, the sintering in step (1) and step (2) are each independently performed in an oxygen-containing atmosphere.

[0029] In some embodiments of the present invention, the oxygen concentration in the oxygen-containing atmosphere is greater than 80%.

[0030] In some embodiments of the present invention, the heating rates of the sintering in step (1) and step (2) are independently 2 to 10° C. / min.

[0031] In some embodiments of the present invention, the sintering in step (1) and step (2) each independently includes a first stage sintering and a second stage sintering.

[0032] In some embodiments of the present invention, the temperature of the first sintering stage in step (1) is 400-600°C.

[0033] In some embodiments of the present invention, the first sintering time in step (1) is 8 to 24 hours.

[0034] In some embodiments of the present invention, the temperature of the second sintering stage in step (1) is 600-900°C.

[0035] In some embodiments of the present invention, the second sintering time in step (1) is 8 to 24 hours.

[0036] In some embodiments of the present invention, the temperature of the first sintering stage in step (2) is 300-500°C.

[0037] In some embodiments of the present invention, the first sintering time in step (2) is 8 to 24 hours.

[0038] In some embodiments of the present invention, the temperature of the second sintering in step (2) is 500-700°C.

[0039] In some embodiments of the present invention, the second sintering time in step (2) is 8 to 24 hours.

[0040] In some embodiments of the present invention, the mixing in step (2) is performed under stirring conditions.

[0041] In some embodiments of the present invention, the stirring time is 10-60 min.

[0042] In some embodiments of the present invention, the stirring rate is 10 to 2000 r / min.

[0043] In some embodiments of the present invention, the preparation method further comprises: aging after the mixing in step (2).

[0044] In some embodiments of the present invention, the aging time is 1 to 5 hours.

[0045] In a third aspect, the present invention provides a lithium-ion battery, which includes the composite ternary positive electrode material described in the first aspect, or the composite ternary positive electrode material prepared by the preparation method described in the second aspect.

[0046] In a fourth aspect, the present invention provides a vehicle, comprising the lithium-ion battery as described in the third aspect.

[0047] The technical solution provided by the embodiment of the present invention has the following advantages compared with the prior art:

[0048] (1) The composite ternary positive electrode material provided by the present invention has a more uniform surface coating and a lower surface residual alkali content. The cobalt compound in the coating layer cooperates with the solid electrolyte to improve the ionic conductivity of the composite ternary positive electrode material, inhibit the side reaction between the positive electrode material and the electrolyte, and increase the specific capacity of the positive electrode material, thereby reducing the initial DCR and cycle DCR of the battery, and improving the high temperature stability, cycle performance and energy density.

[0049] (2) The preparation method provided by the present invention can improve the coating uniformity of the composite ternary positive electrode material and reduce the amount of residual alkali on the surface. The process operation is simple and the cost is low, which is conducive to industrial mass production. DETAILED DESCRIPTION

[0050] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0051] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0053] In a first aspect, an embodiment of the present invention provides a composite ternary positive electrode material, which includes a ternary positive electrode active material and a coating layer coated on the surface of the ternary positive electrode active material, wherein the coating layer includes a cobalt compound and a solid electrolyte.

[0054] It should be noted that the cobalt compound in the coating layer is a substance generated during the sintering process of the cobalt source in the preparation method, including cobalt-lithium compounds generated by the reaction of the cobalt source with residual alkali on the surface of the ternary positive electrode active material, such as LiCoO2.

[0055] The composite ternary positive electrode material provided in the embodiment of the present invention has a more uniform coating layer, and the cobalt compound and the solid electrolyte in the coating layer have good ionic conductivity, which is beneficial to the transmission of lithium ions and helps to reduce the initial DCR (direct current resistance) and cycle DCR of the battery, thereby improving the fast charging performance of the battery; a part of the residual alkali on the surface of the ternary positive electrode active material is converted into cobalt compounds, so the surface residual alkali amount of the composite ternary positive electrode material is small, which helps to reduce side reactions during the battery cycle and improve the cycle performance of the battery; the cobalt compound (such as LiCoO2) in the coating layer can reduce the damage of the electrolyte to the interface of the ternary positive electrode active material, but it itself has high activity and is easy to react with the electrolyte, and the solid electrolyte in the coating layer can protect the cobalt compound and reduce the reaction of the cobalt compound with the electrolyte, thereby further improving the high temperature stability and cycle performance of the battery; in addition, the cobalt in the coating layer can also provide electrons, which can increase the specific capacity of the composite ternary positive electrode material and the energy density of the battery compared with the ordinary coating layer.

[0056] In some embodiments of the present invention, the chemical formula of the ternary positive electrode active material is LiNi x Co y Mn 1-x-y O2;

[0057] Wherein 0.8≤x≤0.95, for example, it can be 0.8, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.9, 0.91, 0.92, 0.93, 0.94 or 0.95, etc.; however, the present invention is not limited to the listed values, and other values ​​not listed in the range are also applicable;

[0058] 0.01≤y≤0.05, for example, it can be 0.01, 0.02, 0.03, 0.04, etc.; however, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable;

[0059] And 1-xy>0.

[0060] In some embodiments of the present invention, the cobalt compound includes LiCoO2.

[0061] The LiCoO2 in the coating layer has a higher ionic conductivity, which is beneficial to the Li + The diffusion and transfer of Co can reduce the initial DCR and cycle DCR of the battery; at the same time, Co can provide electrons, which can effectively improve the specific capacity of the positive electrode material.

[0062] In some embodiments of the present invention, the solid electrolyte includes any one or a combination of oxide solid electrolyte, sulfide solid electrolyte, polymer solid electrolyte and borate solid electrolyte.

[0063] In some embodiments of the present invention, the solid electrolyte includes any one or a combination of lithium aluminum titanium phosphate (LATP), lithium lanthanum zirconium oxide (LLZO) and lithium lanthanum titanate (LLTO).

[0064] In the embodiment of the present invention, the solid electrolyte has a good protective effect on the cobalt compound in the coating layer. On the one hand, it can reduce the reaction between the cobalt compound and the electrolyte. The combination of the two is beneficial to improving the high temperature stability and cycle performance of the battery; on the other hand, the solid electrolyte itself also has good ionic conductivity, which helps to reduce the initial DCR and cycle DCR of the battery.

[0065] In some embodiments of the present invention, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt compound is 100:(0.5-5), for example, it can be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9, 100:1, 100:1.2, 100:1.5, 100:1.8, 100:2, 100:2.2, 100:2.5, 100:2.8, 100:3, 100:3.2, 100:3.5, 100:3.8, 100:4, 100:4.2, 100:4.5, 100:4.8 or 100:5, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0066] In some embodiments of the present invention, the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:(0.1-1), for example, it can be 100:0.1, 100:0.2, 100:0.3, 100:0.4, 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9, 100:1, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0067] In some embodiments of the present invention, the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:(0.1-0.5).

[0068] In an embodiment of the present invention, if the coating amount of the cobalt compound (such as LiCoO2) is too small, its corresponding effect is difficult to play; but LiCoO2 has a high activity. If the coating amount is too much, it is easy to react with the electrolyte, resulting in a decrease in the high temperature stability and cycle performance of the battery. The solid electrolyte can protect the cobalt compound and reduce the reaction between the cobalt compound and the electrolyte, but the solid electrolyte will also reduce the specific capacity of the positive electrode material, so it is not advisable to add too much. In an embodiment of the present invention, by controlling the content of the cobalt compound and the solid electrolyte within the above range, the performance of the composite ternary positive electrode material can be better balanced, while significantly improving the electrochemical performance of the composite ternary positive electrode material, the impact of the specific capacity is minimized.

[0069] In a second aspect, the present invention provides a method for preparing the composite ternary cathode material as described in the first aspect, the preparation method comprising the following steps:

[0070] (1) mixing a ternary hydroxide precursor, a lithium source and a flux, and sintering the mixture to obtain a ternary positive electrode active material;

[0071] (2) Mixing the ternary positive electrode active material with a cobalt source, a solid electrolyte, a surfactant and water, so that the cobalt source and the solid electrolyte adhere to the surface of the ternary positive electrode active material, and sintering to obtain a composite ternary positive electrode material.

[0072] The preparation method provided in the embodiment of the present invention adopts a wet process to coat the ternary positive electrode active material, which can make the coating more evenly coated on the surface of the ternary positive electrode active material, avoiding the situation that the places where the coating is concentrated are not conducive to lithium ion transmission due to uneven coating, thereby affecting the capacity, and the places where the coating is insufficient cannot play the role of protecting the interface. In addition, during the sintering process of step (2), the cobalt source can react with the residual alkali on the surface of the ternary positive electrode active material to generate a cobalt-lithium compound, effectively reducing the amount of residual alkali on the surface of the positive electrode material, increasing the specific capacity of the positive electrode material, and thus improving the cycle performance and energy density of the battery. And the preparation process provided in the embodiment of the present invention is simple, which can reduce production costs.

[0073] In some embodiments of the present invention, the chemical formula of the ternary hydroxide precursor is Ni x Co y Mn 1-x-y (OH)2;

[0074] Wherein 0.8≤x≤0.95, for example, it can be 0.8, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.9, 0.91, 0.92, 0.93, 0.94 or 0.95, etc.; however, the present invention is not limited to the listed values, and other values ​​not listed in the range are also applicable;

[0075] 0.01≤y≤0.05, for example, it can be 0.01, 0.02, 0.03, 0.04, etc.; however, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable;

[0076] And 1-xy>0.

[0077] In some embodiments of the present invention, the lithium source includes any one or a combination of lithium carbonate, lithium hydroxide and lithium nitrate.

[0078] In some embodiments of the present invention, the flux includes any one or a combination of NaCl, NaF, Na2O, NaBO2, Na2BO3, SrO, Na2SO4, K2SO4, KCl, KF and B2O3.

[0079] Flux helps to lower the temperature required for sintering of materials and produce crystals with uniform, complete and well-dispersed particle sizes.

[0080] In some embodiments of the present invention, the cobalt source includes any one or a combination of Co(OH)2, CoOOH, Co3O4, cobalt chloride, cobalt carbonate and cobalt oxalate.

[0081] In some embodiments of the present invention, the particle size of the cobalt source is 20-200 nm, for example, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, 120 nm, 130 nm, 150 nm, 160 nm, 180 nm or 200 nm, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0082] In the embodiment of the present invention, the use of a nano-scale cobalt source helps to make it adhere more evenly to the surface of the ternary positive electrode active material, thereby making the formed coating layer more uniform.

[0083] In the embodiment of the present invention, the solid electrolyte in the preparation method described in the second aspect and the solid electrolyte in the composite ternary positive electrode material described in the first aspect are of the same type and proportion, and will not be repeated here.

[0084] In some embodiments of the present invention, the surfactant is polyethylene glycol.

[0085] The addition of surfactants can improve the particle dispersion, allowing the cobalt source and solid electrolyte particles to adhere more evenly to the surface of the ternary positive electrode active material, thereby making the formed coating more uniform.

[0086] In some embodiments of the present invention, the molecular weight of the polyethylene glycol is 200-6000, for example, 200, 400, 500, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0087] In some embodiments of the present invention, the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:(1.03-1.1), for example, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1.1, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0088] In the embodiment of the present invention, the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is controlled within the above range, which can ensure that the nickel, cobalt and manganese elements in the ternary hydroxide precursor are fully reacted and converted into the ternary positive electrode active material, and the excess lithium can react with the cobalt source to form a cobalt-lithium compound coating layer. If the amount of lithium source used is too much, there will be a lot of residual lithium after sintering in step (1), which cannot be fully converted into the cobalt-lithium compound coating layer in step (2), resulting in a large amount of residual alkali on the surface of the composite ternary positive electrode material, affecting the cycle performance of the battery.

[0089] In some embodiments of the present invention, the mass of the flux accounts for 200-600 ppm of the total mass of the ternary hydroxide precursor, the lithium source and the flux, for example, 200 ppm, 250 ppm, 300 ppm, 350 ppm, 400 ppm, 450 ppm, 500 ppm, 550 ppm or 600 ppm. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0090] In the embodiment of the present invention, the amount of flux is controlled within the above range, which can exert a good fluxing effect and make the particle size of the generated ternary positive electrode active material uniform and complete. If the amount of flux is too much, the content of the ternary positive electrode active material is low, which in turn affects the performance of the gram capacity of the ternary positive electrode active material.

[0091] In some embodiments of the present invention, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:(0.5-5), for example, it can be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9, 100:1, 100:1.2, 100:1.5, 100:1.8, 100:2, 100:2.2, 100:2.5, 100:2.8, 100:3, 100:3.2, 100:3.5, 100:3.8, 100:4, 100:4.2, 100:4.5, 100:4.8 or 100:5, etc. However, the present invention is not limited to the listed values, and other values ​​not listed in the range are also applicable. .

[0092] In some embodiments of the present invention, the mass ratio of the ternary positive electrode active material to the surfactant is 100:(0.1-0.3), for example, it can be 100:0.1, 100:0.12, 100:0.14, 100:0.16, 100:0.18, 100:0.2, 100:0.22, 100:0.24, 100:0.26, 100:0.28, 100:0.3, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0093] In the embodiment of the present invention, the amount of the surfactant is controlled within the above range, which helps to evenly disperse the raw material particles and improve the uniformity of the coating layer in the composite ternary positive electrode material. If the amount of the surfactant is too small, its effect is difficult to play; if the amount of the surfactant is too large, it is easy to aggregate, which is also not conducive to the uniformity of particle dispersion.

[0094] In some embodiments of the present invention, the sintering in step (1) and step (2) are each independently performed in an oxygen-containing atmosphere.

[0095] In some embodiments of the present invention, the oxygen concentration in the oxygen-containing atmosphere is greater than 80%, for example, it may be 81%, 83%, 85%, 88%, 90%, 92%, 95%, 98%, 100%, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0096] For high-nickel ternary positive electrode active materials, due to the high Ni content, Ni 3+ It is easy to reduce to Ni 2+ , and Ni 2+ and Li +The radius of the positive electrode material is equivalent, and Li / Ni mixing is easily formed in the positive electrode material, thereby affecting the crystallinity of the material. In the embodiment of the present invention, the oxygen concentration is controlled within the above range, which can significantly inhibit the Li / Ni mixing, improve the crystallinity of the ternary positive electrode active material, and enable the composite ternary positive electrode material to obtain good electrochemical performance.

[0097] In some embodiments of the present invention, the heating rates of the sintering in step (1) and step (2) are independently 2 to 10°C / min, for example, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0098] In some embodiments of the present invention, the sintering in step (1) and step (2) each independently includes a first stage sintering and a second stage sintering.

[0099] In some embodiments of the present invention, the temperature of the first sintering stage in step (1) is 400-600°C, for example, 425°C, 450°C, 475°C, 500°C, 525°C, 550°C, 575°C, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0100] In some embodiments of the present invention, the first sintering time in step (1) is 8 to 24 hours, for example, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0101] In some embodiments of the present invention, the temperature of the second sintering stage in step (1) is 600-900° C., for example, 650° C., 700° C., 750° C., 800° C., 850° C., etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0102] In some embodiments of the present invention, the second sintering time in step (1) is 8 to 24 hours, for example, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0103] In some embodiments of the present invention, the temperature of the first sintering stage in step (2) is 300-500° C., for example, 325° C., 350° C., 400° C., 425° C., 450° C., 475° C., etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0104] In some embodiments of the present invention, the first sintering time in step (2) is 8 to 24 hours, for example, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0105] In some embodiments of the present invention, the temperature of the second sintering in step (2) is 500-700° C., for example, 525° C., 550° C., 600° C., 625° C., 650° C., 675° C., etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0106] In some embodiments of the present invention, the second sintering time in step (2) is 8 to 24 hours, for example, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0107] In some embodiments of the present invention, the mixing in step (2) is performed under stirring conditions.

[0108] In some embodiments of the present invention, the stirring time is 2-8 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, etc. However, the present invention is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0109] In some embodiments of the present invention, the stirring rate is 10-2000 r / min, such as 50 r / min, 100 r / min, 500 r / min, 1000 r / min, 1500 r / min, etc. However, the present invention is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0110] In some embodiments of the present invention, the preparation method further comprises: aging after the mixing in step (2).

[0111] In the embodiment of the present invention, the aging method is standing still, the purpose of which is to allow the crystal particles to grow to prevent leakage; on the other hand, it can speed up the filtration speed and reduce washing losses.

[0112] In some embodiments of the present invention, the aging time is 1 to 5 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, etc. However, the present invention is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0113] In some embodiments of the present invention, the method for preparing the composite ternary cathode material comprises the following steps:

[0114] (1) fully physically mixing a ternary hydroxide precursor, a lithium source and a flux, and after mixing evenly, placing the mixed material in a box furnace, sintering in an oxygen-containing atmosphere, controlling the oxygen concentration to be greater than 80%, first heating to 400-600° C. at a heating rate of 2-10° C. / min, sintering for 8-24 h, then heating to 600-900° C. at a heating rate of 2-10° C. / min, sintering for 8-24 h, cooling naturally, and successively undergoing jaw crushing, roller crushing, air flow milling, and classification to obtain a ternary positive electrode active material;

[0115] Wherein, the chemical formula of the ternary hydroxide precursor is Ni x Co y Mn 1-x-y (OH)2, wherein 0.8≤x≤0.95, 0.01≤y≤0.05, and 1-xy>0; the lithium source comprises any one or a combination of lithium carbonate, lithium hydroxide and lithium nitrate; the flux comprises any one or a combination of NaCl, NaF, Na2O, NaBO2, Na2BO3, SrO, Na2SO4, K2SO4, KCl, KF and B2O3; the molar ratio of the lithium element in the ternary hydroxide precursor to the lithium source is 1:(1.03-1.1); the mass of the flux accounts for 200-600ppm of the total mass of the ternary hydroxide precursor, the lithium source and the flux;

[0116] (2) The ternary positive electrode active material is mixed with a cobalt source, a solid electrolyte, a surfactant and water at a stirring rate of 10 to 60 minutes, and then allowed to stand for aging for 1 to 5 hours. After filtering and washing the solid product, it is placed in a box furnace and sintered in an oxygen-containing atmosphere, and the oxygen concentration is controlled to be greater than 80%. The temperature is first increased to 300 to 500° C. at a heating rate of 2 to 10° C. / min, and sintered for 8 to 24 hours. The temperature is then increased to 500 to 700° C. at a heating rate of 2 to 10° C. / min, and sintered for 8 to 24 hours. The product is naturally cooled, crushed by jaw crushing, roller crushing, air flow milling, and classified to obtain a composite ternary positive electrode material.

[0117] Wherein, the cobalt source includes any one or a combination of Co(OH)2, CoOOH and Co3O4; the particle size of the cobalt source is 20-200nm; the solid electrolyte includes any one or a combination of LATP, LLZO and LLTO; the surfactant is polyethylene glycol; the molecular weight of the polyethylene glycol is 200-6000; the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:(0.5~5); the mass ratio of the ternary positive electrode active material, the solid electrolyte, the surfactant and water is 100:(0.1~0.5):(0.1~0.3):(300-1000).

[0118] In a third aspect, an embodiment of the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the composite ternary positive electrode material described in the first aspect, or the composite ternary positive electrode material prepared by the preparation method described in the second aspect.

[0119] In a fourth aspect, an embodiment of the present invention provides a vehicle, comprising the lithium-ion battery as described in the third aspect.

[0120] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention will be further described in detail in conjunction with the embodiments below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its applications. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0121] If no specific techniques or conditions are specified in the examples, the conventional techniques or conditions in the art, or the techniques or conditions described in the literature, or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0122] Example 1

[0123] This embodiment provides a composite ternary positive electrode material, including a ternary positive electrode active material LiNi 0.9 Co 0.03 Mn 0.07 O2 and a coating layer coated on the surface of the ternary positive electrode active material;

[0124] The coating layer includes a cobalt compound and a solid electrolyte, and the cobalt compound includes LiCoO2.

[0125] This embodiment also provides a method for preparing the composite ternary positive electrode material, the steps are as follows:

[0126] (1) The ternary hydroxide precursor Ni 0.9 Co 0.03 Mn 0.07 (OH)2, lithium source LiOH and flux SrO are physically mixed, and after being mixed evenly, the mixed material is placed in a box furnace, sintered in an oxygen-containing atmosphere, and the oxygen concentration is controlled to be 85%. The temperature is first increased to 550°C at a heating rate of 5°C / min, sintered for 10 hours, and then increased to 870°C at a heating rate of 5°C / min, sintered for 12 hours, cooled naturally, and then subjected to jaw crushing, roller crushing, air flow milling, and classification to obtain a ternary positive electrode active material;

[0127] Among them, the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:1.05; the mass ratio of the ternary positive electrode active material to the flux is 1:0.5.

[0128] (2) The ternary positive electrode active material obtained in step (1), the cobalt source Co(OH)2(D 50 The solid electrolyte LATP, the surfactant PEG400 and the deionized water are stirred and mixed at a speed of 500r / min for 30min, and then aged for 3h. After filtering and washing, the solid product is placed in a box furnace and sintered in an oxygen-containing atmosphere. The oxygen concentration is controlled to be 85%. The temperature is first increased to 450°C at a heating rate of 5°C / min, sintered for 10h, and then increased to 700°C at a heating rate of 5°C / min. The sintering time is 12h, and the composite ternary positive electrode material is obtained after natural cooling, jaw crushing, roller crushing, air flow crushing and classification.

[0129] Among them, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:1.05; the mass ratio of the ternary positive electrode active material, the solid electrolyte, the surfactant and deionized water is 100:0.1:0.2:500.

[0130] Example 2

[0131] This embodiment provides a composite ternary positive electrode material and a preparation method thereof, which is different from Example 1 only in that the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:1.08, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:2.1, and the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:0.3.

[0132] Example 3

[0133] This embodiment provides a composite ternary positive electrode material and a preparation method thereof, which is different from Example 1 only in that the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:1.1, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:3.15, and the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:0.5.

[0134] Example 4

[0135] This embodiment provides a composite ternary positive electrode material, including a ternary positive electrode active material LiNi 0.85 Co 0.01 Mn 0.14 O2 and a coating layer coated on the surface of the ternary positive electrode active material;

[0136] The coating layer includes a cobalt compound and a solid electrolyte, and the cobalt compound includes LiCoO2.

[0137] This embodiment also provides a method for preparing the composite ternary positive electrode material, the steps are as follows:

[0138] (1) The ternary hydroxide precursor Ni 0.85 Co 0.01 Mn 0.14 (OH)2, lithium source Li2CO3 and flux SrO are physically mixed, and after being mixed evenly, the mixed material is placed in a box furnace, sintered in an oxygen-containing atmosphere, and the oxygen concentration is controlled to be 85%. The temperature is first increased to 400°C at a heating rate of 2°C / min, sintered for 24h, and then increased to 600°C at a heating rate of 2°C / min, sintered for 24h, naturally cooled, and successively subjected to jaw crushing, roller crushing, air flow milling, and classification to obtain a ternary positive electrode active material;

[0139] Among them, the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:1.03; the mass ratio of the ternary positive electrode active material to the flux is 1:1.

[0140] (2) The ternary positive electrode active material obtained in step (1), the cobalt source CoOOH (D 50 The solid electrolyte LLZO, the surfactant PEG400 and the deionized water are stirred and mixed at a speed of 500r / min for 8h, and then aged for 1h. After filtering and washing, the solid product is placed in a box furnace and sintered in an oxygen-containing atmosphere. The oxygen concentration is controlled to be 85%. The temperature is first increased to 300°C at a heating rate of 2°C / min, sintered for 24h, and then increased to 500°C at a heating rate of 2°C / min. The sintering time is 24h, and the composite ternary positive electrode material is obtained after natural cooling, jaw crushing, roller crushing, air flow crushing and classification.

[0141] Among them, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:1.26; the mass ratio of the ternary positive electrode active material, the solid electrolyte, the surfactant and the deionized water is 100:0.8:0.2:500.

[0142] Example 5

[0143] This embodiment provides a composite ternary positive electrode material, including a ternary positive electrode active material LiNi 0.8 Co 0.05 Mn 0.25 O2 and a coating layer coated on the surface of the ternary positive electrode active material;

[0144] The coating layer includes a cobalt compound and a solid electrolyte, and the cobalt compound includes LiCoO2.

[0145] This embodiment also provides a method for preparing the composite ternary positive electrode material, the steps are as follows:

[0146] (1) The ternary hydroxide precursor Ni 0.8 Co 0.05 Mn 0.25 (OH)2, lithium source LiNO3 and flux SrO are physically mixed, and after being mixed evenly, the mixed material is placed in a box furnace and sintered in an oxygen-containing atmosphere, and the oxygen concentration is controlled to be 85%. The temperature is first increased to 600°C at a heating rate of 10°C / min, sintered for 8h, and then increased to 900°C at a heating rate of 10°C / min, sintered for 8h, and naturally cooled. After jaw crushing, roller crushing, air flow milling, and classification, a ternary positive electrode active material is obtained;

[0147] Among them, the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:1.06; the mass ratio of the ternary positive electrode active material to the flux is 1:0.2.

[0148] (2) The ternary positive electrode active material obtained in step (1), the cobalt source Co3O4 (D 50 The solid electrolyte LLTO, the surfactant PEG400 and the deionized water are stirred and mixed at a speed of 500r / min for 2h, and then aged for 5h. After filtering and washing, the solid product is placed in a box furnace and sintered in an oxygen-containing atmosphere. The oxygen concentration is controlled to be 85%. The temperature is first increased to 500°C at a heating rate of 10°C / min, sintered for 8h, and then increased to 600°C at a heating rate of 10°C / min. The sintering time is 8h, and the composite ternary positive electrode material is obtained after natural cooling, jaw crushing, roller crushing, air flow crushing, and classification.

[0149] Among them, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:0.43; the mass ratio of the ternary positive electrode active material, the solid electrolyte, the surfactant and deionized water is 100:1:0.2:500.

[0150] Example 6

[0151] This embodiment provides a composite ternary positive electrode material and a preparation method thereof, which is different from Embodiment 1 in that the molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:1.15.

[0152] Example 7

[0153] This embodiment provides a composite ternary positive electrode material and a preparation method thereof, which is different from Embodiment 1 in that the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:6.

[0154] Example 8

[0155] This embodiment provides a composite ternary positive electrode material and a preparation method thereof, which is different from Embodiment 1 in that the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:2.

[0156] Comparative Example 1

[0157] This comparative example provides a ternary positive electrode active material, and the preparation method is the same as step (1) of Example 1.

[0158] Comparative Example 2

[0159] This comparative example provides a ternary positive electrode active material, and the preparation method is the same as step (1) of Example 2.

[0160] Comparative Example 3

[0161] This comparative example provides a ternary positive electrode active material, and the preparation method is the same as step (1) of Example 3.

[0162] Comparative Example 4

[0163] This comparative example provides a composite ternary positive electrode material and a preparation method thereof, which is different from Example 3 only in that no solid electrolyte is added.

[0164] Comparative Example 5

[0165] This comparative example provides a composite ternary positive electrode material, and its preparation method is as follows:

[0166] (1) The same as step (1) of Example 3;

[0167] (2) Physically mixing the ternary positive electrode active material obtained in step (1) with the cobalt source Co(OH)2, and then placing it in a box furnace for sintering in an oxygen-containing atmosphere, controlling the oxygen concentration to 85%, first heating to 450°C at a heating rate of 5°C / min, sintering for 10 h, then heating to 700°C at a heating rate of 5°C / min, sintering for 12 h, naturally cooling, and crushing by jaw crushing, roller crushing, air flow milling, and grading to obtain a composite ternary positive electrode material.

[0168] Performance Testing

[0169] 1. Preparation of a lithium-ion battery for testing

[0170] (1) The composite ternary positive electrode material prepared in the embodiment and the comparative example, the conductive agent (SP), and the binder polyvinylidene fluoride (PVDF) were added to N-methylpyrrolidone (NMP) in a weight ratio of 95:2:3 and fully mixed, and stirred to form a uniform slurry with a solid content of 65%. The slurry was coated on an aluminum foil current collector, dried and pressed into a positive electrode sheet. The compaction density of the positive electrode active layer was 3.5 g / cm 3 , surface density is 240g / m 2 ;

[0171] (2) Artificial graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and adhesive (SBR) were added to sufficient pure water in a weight ratio of 96:0.8:1.2:2, and stirred to form a uniform slurry. The slurry was coated on a copper foil current collector, dried, and pressed into a negative electrode sheet. The compaction density of the negative electrode active layer was 1.6 g / cm 3 , surface density is 165g / m 2 ;

[0172] (3) The separator is made of PP / PE composite film material, and the positive electrode and the negative electrode are spot welded to the upper pole ears. After the separator is inserted, it is wound on a winder and loaded into a soft package fixture, and the top and side are sealed. Then, it is placed in an oven for baking, and then the electrolyte is injected in an environment with a relative humidity of less than 1.5% (the electrolyte is 1 mol / L lithium hexafluorophosphate, and the solvent is a mixed solvent with a volume ratio of EC:DEC:DMC = 1:1:1). After 24 hours of formation, the vacuum is evacuated and sealed to obtain a lithium-ion battery for testing.

[0173] It should be noted that the above-mentioned test lithium-ion battery is only an example listed for testing the performance of the composite ternary positive electrode material. The present invention is not limited to this type of battery. The raw materials (except the composite ternary positive electrode material), proportions, parameters and processes can all be replaced with other conventional raw materials, proportions, parameters and processes in the art to form a battery different from the test lithium-ion battery.

[0174] 2. Charge and discharge performance test

[0175] The above-mentioned lithium-ion battery is subjected to charge and discharge test according to the test method of GB / T18287-2000:

[0176] In a constant temperature room at 25℃±5℃, charge at a constant current of 0.33C to an upper limit voltage of 4.25V, then change to constant voltage charging. Stop charging when the charging current is less than or equal to 0.05C. The longest charging time is no more than 8h. After charging, place it at 25℃±5℃ for 0.5h, discharge at 0.33C current to a termination voltage of 2.8V, record the discharge capacity, and calculate the gram capacity of the composite ternary positive electrode material.

[0177] 3. Residual alkali test

[0178] The ternary positive electrode active materials and composite ternary positive electrode materials prepared in the above examples and comparative examples were tested for residual alkali. The test method is as follows:

[0179] Weigh 5.0g of sample to an accuracy of 0.0001g, and record the mass as m1. Place the sample in a 100mL glass beaker, add 50g of CO2-free pure water, the water temperature is 25℃±2℃, and the water mass is recorded as m2. Add a magnet, seal it with plastic wrap, place it on a magnetic stirrer, and stir and mix at a rate of 800r / min for 30min. Within 1min after stirring, separate the sample from the water using a vacuum filtration device and a 45μm filter membrane, collect the filtrate in the lower layer, and seal it. Take 20g of the filtrate, place the filtrate in a potentiometric titrator, and titrate it with a 0.1mol / L hydrochloric acid standard titration solution. Record the equivalence point at different pH values.

[0180] When it is judged that pH≈8.5 (the corresponding equivalence point volumes are added), the volume of hydrochloric acid consumed is recorded as V1; when it is judged that pH≈4.5 (the corresponding equivalence point volumes are added), the volume of hydrochloric acid consumed is recorded as V2.

[0181] The lithium carbonate content in the sample is expressed as mass fraction W Li2CO3 According to formula (1):

[0182]

[0183] The lithium hydroxide content in the sample is expressed as mass fraction W LiOH According to formula (2):

[0184]

[0185] The residual alkali content in the sample is expressed as mass fraction Wr a According to formula (3):

[0186] Wra=1.54×W:oH+WLi2cO3(3).

[0187] 4. Initial DCR and 500-cycle ΔDCR test

[0188] The above-mentioned lithium-ion battery for testing is subjected to initial DCR and 500-cycle ΔDCR (%) tests. The test method is as follows:

[0189] Initial DCR (referring to DCR without cycling): charge and discharge the fresh battery at 0.33C in the voltage range of 2.8-4.25V to a fixed capacity, then discharge it at 0.33C current to 50% capacity, record the voltage as V1, discharge it at 4C for 10s, record the current as I, record the voltage at this time as V2, calculate the initial DCR value, initial DCR = (V2-V1) / I;

[0190] The battery is charged and discharged for 500 cycles at a voltage range of 2.8-4.25V and a current of 1C, and then the DCR value at this time is tested in the same way as the initial DCR, recorded as DCR2; then 500 cycles ΔDCR (%) = (DCR2-initial DCR) / initial DCR×100%.

[0191] The results of the above performance tests are shown in Table 1.

[0192] Table 1 Performance test results

[0193]

[0194]

[0195] By comparing Comparative Examples 1-3 and Examples 1-3, it can be seen that the surface residual alkali content of the composite ternary positive electrode material provided by the embodiments of the present invention is significantly reduced, the gram capacity of the composite ternary positive electrode material is improved, the initial DCR and the DCR after 500 cycles of the battery are significantly reduced, the cycle performance is significantly improved, and the overall electrochemical performance of the battery is significantly improved.

[0196] Compared with Example 3, Comparative Example 4 does not add a solid electrolyte. Although the gram capacity of the composite ternary positive electrode material is slightly improved, the LiCoO2 in the coating layer easily reacts with the electrolyte, so the cycle performance of the battery is reduced.

[0197] Compared with Example 3, the surface residual alkali content of the composite ternary positive electrode material obtained in Comparative Example 5 increases, the gram capacity decreases, the initial DCR and cycle DCR of the battery increase, and the cycle performance deteriorates. This is because Comparative Example 5 adopts a solid-phase sintering method to prepare the composite ternary positive electrode material, resulting in uneven coating. The places where the coating is concentrated are not conducive to lithium ion transmission and affect the capacity. The places where the coating is insufficient do not play a role in protecting the interface, resulting in an increase in side reactions and a decrease in battery cycle performance.

[0198] Compared with Example 1, the amount of lithium source added in Example 6 is too large. During the sintering process, the excess lithium cannot enter the crystal lattice and remains on the surface of the material. It also cannot be fully converted into cobalt-lithium compounds. As a result, the residual alkali content of the composite ternary positive electrode material is relatively high, and the cycle performance of the battery is reduced.

[0199] Compared with Example 1, the amount of cobalt source added in Example 7 is relatively large, and more LiCoO2 is generated in the coating layer, resulting in more side reactions between LiCoO2 and the electrolyte, so the cycle performance of the battery is reduced.

[0200] Compared with Example 1, the amount of solid electrolyte added in Example 8 is relatively large, resulting in a lower gram capacity of the composite ternary positive electrode material.

[0201] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0202] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments described herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A composite ternary cathode material, It is characterized in that The composite ternary positive electrode material comprises a ternary positive electrode active material and a coating layer coated on the surface of the ternary positive electrode active material, wherein the coating layer comprises a cobalt compound and a solid electrolyte.

2. The composite ternary cathode material according to claim 1, It is characterized in that The chemical formula of the ternary positive electrode active material is LiNi x Co y Mn 1-x-y O 2 , where 0.8≤x≤0.95, 0.01≤y≤0.05, and 1-xy>0; And / or, the cobalt compound comprises LiCoO 2 ; And / or, the solid electrolyte comprises any one or a combination of oxide solid electrolyte, sulfide solid electrolyte, polymer solid electrolyte and borate solid electrolyte; further preferably comprises any one or a combination of lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide and lithium lanthanum titanate; and / or, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt compound is 100:(0.5-5); And / or, the mass ratio of the ternary positive electrode active material to the solid electrolyte is 100:(0.1-1).

3. A method for preparing the composite ternary positive electrode material as claimed in claim 1 or 2, It is characterized in that The preparation method comprises the following steps: (1) mixing a ternary hydroxide precursor, a lithium source and a flux, and sintering the mixture to obtain a ternary positive electrode active material; (2) Mixing the ternary positive electrode active material with a cobalt source, a solid electrolyte, a surfactant and water, so that the cobalt source and the solid electrolyte adhere to the surface of the ternary positive electrode active material, and sintering to obtain a composite ternary positive electrode material.

4. The preparation method according to claim 3, It is characterized in that The chemical formula of the ternary hydroxide precursor is Ni x Co y Mn 1-x-y (OH) 2 , where 0.8≤x≤0.95, 0.01≤y≤0.05, and 1-xy>0; And / or, the lithium source includes any one or a combination of lithium carbonate, lithium hydroxide and lithium nitrate; And / or, the flux includes NaCl, NaF, Na 2 O、NaBO 2 、Na 2 BO 3 、SrO、Na 2 SO 4 , K 2 SO 4 , KCl, KF and B 2 O 3 Any one or a combination of the following: And / or, the cobalt source comprises Co(OH) 2 、CoOOH、Co 3 O 4 , cobalt chloride, cobalt carbonate and cobalt oxalate, or any combination thereof; And / or, the particle size of the cobalt source is 20-200 nm; And / or, the surfactant is polyethylene glycol; And / or, the molecular weight of the polyethylene glycol is 200-6000.

5. The preparation method according to claim 3 or 4, It is characterized in that The molar ratio of the ternary hydroxide precursor to the lithium element in the lithium source is 1:(1.03-1.1); And / or, the mass of the flux accounts for 200-600 ppm of the total mass of the ternary hydroxide precursor, the lithium source and the flux; and / or, the molar ratio of the ternary positive electrode active material to the cobalt element in the cobalt source is 100:(0.5-5); And / or, the mass ratio of the ternary positive electrode active material to the surfactant is 100:(0.1-0.3).

6. The preparation method according to any one of claims 3 to 5, It is characterized in that The sintering in step (1) and step (2) is independently carried out in an oxygen-containing atmosphere; And / or, the heating rates of the sintering in step (1) and step (2) are each independently 2 to 10°C / min; And / or, the sintering in step (1) and step (2) each independently comprises a first stage sintering and a second stage sintering; And / or, the mixing in step (2) is carried out under stirring conditions; And / or, the preparation method further comprises: aging after the mixing in step (2).

7. The preparation method according to claim 6, It is characterized in that The temperature of the first sintering stage in step (1) is 400-600°C; And / or, the first sintering time in step (1) is 8 to 24 hours; and / or, the temperature of the second sintering stage in step (1) is 600-900° C.; And / or, the second sintering time in step (1) is 8 to 24 hours; and / or, the temperature of the first sintering stage in step (2) is 300-500° C.; And / or, the first sintering time in step (2) is 8 to 24 hours; and / or, the temperature of the second sintering stage in step (2) is 500-700° C.; And / or, the second sintering time in step (2) is 8 to 24 hours.

8. The preparation method according to claim 6, It is characterized in that The oxygen concentration in the oxygen-containing atmosphere is greater than 80%; And / or, the stirring time is 10-60min; And / or, the stirring rate is 10 to 2000 r / min; And / or, the aging time is 1 to 5 hours.

9. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the composite ternary positive electrode material according to claim 1 or 2, or the composite ternary positive electrode material prepared by the preparation method according to any one of claims 3 to 8.

10. A vehicle, It is characterized in that The vehicle includes the lithium-ion battery of claim 9.

Citation Information

Cited By

  • Solid electrolyte coated ternary positive electrode material as well as preparation method and application thereof

    CN119461511A

  • A solid-state electrolyte-coated ternary positive electrode material, a preparation method therefor, and use thereof

    CN119461511B

  • Composite positive electrode material and preparation method thereof, positive plate and secondary battery

    CN119833596A

  • Battery monomer, battery device, power utilization device and energy storage device

    CN120600796A

  • Fast ion conductor-electron conductor positive electrode material precursor and preparation method thereof

    CN122426794A