Etching liquid and preparation method thereof, and metal film material processing method

By adding specific surfactants and metal corrosion inhibitors to the chemical etching solution to regulate the etching rate and ratio of aluminum and molybdenum, the problems of inconsistent etching rates and side etching of the aluminum and molybdenum layers in the existing technology are solved, and high precision is achieved. , Uniform etching effect.

CN114507859BActive Publication Date: 2024-10-11FUJIAN ZHONGAN HIGH-TECH MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111481164.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-10-11
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

In the existing chemical etching technology, during the etching process of metal films containing aluminum or molybdenum, the etching speed is inconsistent due to the difference in chemical properties of aluminum and molybdenum, resulting in poor etching uniformity, low precision, and serious side etching, making it difficult to control the line width. and angle.

Method used

An etching solution containing phosphoric acid, nitric acid, acetic acid, nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate is used to control the etching rate and ratio through specific surfactants and metal corrosion inhibitors. Ensure consistent etching rates for aluminum and molybdenum and reduce undercutting.

Benefits of technology

It achieves uniform etching of aluminum and molybdenum layers, improves etching accuracy and control capabilities, ensures the verticality and dimensional accuracy of the etched film layer, and reduces the loss of critical dimensions of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114507859B_ABST
    Figure CN114507859B_ABST
Patent Text Reader

Abstract

The present application provides an etching solution and a preparation method thereof, and a method for treating a metal film material. The etching solution contains the following components in parts by weight: 50-80 parts of phosphoric acid, 1-10 parts of nitric acid, 10-30 parts of acetic acid, 0.01-1 parts of metal corrosion inhibitors, 0.01-1 parts of surfactants, and the balance is water; the surfactants include nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate; the metal corrosion inhibitors include potassium acetate, sulfonated lignin, phosphine carboxylic acid, and at least one of mercaptobenzothiazole. The etching solution has strong controllability, good etching uniformity, smooth etching angle, and high precision. It can complete the etching of materials in a short time. After etching, the critical size loss of the metal film material is less than 0.5μm, the etching angle is less than 60°, and there is no residue on the surface of the glass panel. And it can simultaneously meet the etching requirements of aluminum film, aluminum alloy film, molybdenum film, molybdenum alloy film, and molybdenum-aluminum laminated film, aluminum-molybdenum-aluminum laminated film and molybdenum-aluminum-molybdenum laminated film with different thicknesses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of chemical etching, and in particular to an etching solution and a preparation method thereof, and a metal film material processing method. Background Art

[0002] At present, the industry often uses chemical etching to etch aluminum or molybdenum-containing metal film layers to obtain gates, sources, drains, etc. of thin displays with certain patterns. Among them, due to the different chemical properties of aluminum and molybdenum, there are differences in their respective etching speeds during the chemical etching process, resulting in poor etching uniformity, which in turn leads to certain differences between the actual pattern obtained and the pre-designed pattern. In addition, chemical etching is isotropic, and the etched film layer is very prone to side etching, which makes it difficult to control the etching line width and angle, and the poor etching accuracy will also affect. Summary of the invention

[0003] The industry often uses a mixture of phosphoric acid, nitric acid and acetic acid to etch metal film materials such as aluminum-containing, molybdenum-containing or molybdenum-aluminum laminated films. During the etching process, nitric acid oxidizes metal molybdenum and metal aluminum into multivalent molybdenum oxides and Al2O3, respectively, and the phosphoric acid in the system can form complexes with the above oxides to dissolve the oxides, so as to achieve the purpose of etching the molybdenum layer and / or aluminum layer. However, molybdenum is more susceptible to oxidation, and the etching rate of molybdenum is much greater than that of aluminum, which ultimately leads to poor etching uniformity. On the other hand, the above-mentioned etching solution has poor controllability, and the strip width loss of the molybdenum-aluminum laminated film after etching is large and the precision is poor. In order to solve the above-mentioned technical problems, the present application provides an etching solution and a preparation method thereof, and a method for processing metal film materials.

[0004] In the first aspect, specifically, the present application provides an etching solution, which contains the following components in parts by weight: 50-80 parts of phosphoric acid, 1-10 parts of nitric acid, 10-30 parts of acetic acid, 0.01-1 parts of metal corrosion inhibitors, 0.01-1 parts of surfactants, and the balance is water; the surfactants include nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfates; the metal corrosion inhibitors include at least one of potassium acetate, sulfonated lignin, phosphinocarboxylic acid, and mercaptobenzothiazole.

[0005] In the etching solution provided by the present application, nitric acid can oxidize metal molybdenum and metal aluminum into multivalent molybdenum oxide and Al2O3 respectively. In the presence of acetic acid, phosphoric acid can react with the above oxides to form a complex to dissolve the oxides, so as to achieve the purpose of etching the molybdenum layer and / or the aluminum layer. On the basis of phosphoric acid, nitric acid and acetic acid, the present application adds specific surfactants - nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate, as well as specific metal corrosion inhibitors (at least one of potassium acetate, sulfonated lignin, phosphine carboxylic acid and mercaptobenzothiazole), so that the etching rate of the etching solution for the molybdenum layer and the aluminum layer can be basically consistent, and the etching accuracy can be guaranteed. Among them, nonylphenol polyoxyethylene ether has good penetration and dispersion ability, is not easy to foam, and also has good antioxidant and reduction ability. It can exist stably in the etching solution and will not have side reactions with the nitric acid in the etching solution; nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate are used together as surfactants, and can effectively improve the infiltration speed of the above-mentioned etching solution on the surface of the aluminum film, as well as the penetration ability of the aluminum film, and can improve the etching rate of the aluminum film by the etching solution to a certain extent, so that the etching rates of aluminum and molybdenum tend to be consistent. In addition, the above-mentioned surfactant can increase the dispersion of the complex generated by aluminum oxide and phosphoric acid in the etching solution, thereby effectively avoiding the problem that the complex generated by aluminum oxide and phosphoric acid in the etching process reaches a certain concentration and gathers on the surface of the metal film to reduce the aluminum etching rate, thereby improving the uniformity of etching and alleviating the side etching problem of the aluminum layer.

[0006] On the other hand, the above-mentioned surfactant can be matched with the metal corrosion inhibitor to regulate the etching ratio of molybdenum and aluminum. Potassium acetate, sulfonated lignin, phosphine carboxylic acid, and mercaptobenzothiazole can effectively regulate the etching rate of the etching solution to molybdenum and aluminum without affecting the effectiveness of the etching solution. Among them, potassium acetate can simultaneously achieve corrosion inhibition of aluminum and molybdenum, but its corrosion inhibition effect on metal molybdenum is better. The affinity of organic metal corrosion inhibitors such as sulfonated lignin, phosphine carboxylic acid, and mercaptobenzothiazole to molybdenum is better than that of aluminum. After compounding with surfactants, they can preferentially infiltrate and adhere to the surface of metal molybdenum, hindering the etching of metal molybdenum by acid, thereby reducing the etching rate of metal molybdenum. When the etching solution is used to process aluminum-molybdenum, molybdenum-aluminum-molybdenum or aluminum-molybdenum-aluminum laminated films, the difference in the corrosion inhibition effect of the metal corrosion inhibitor on aluminum and molybdenum can make the overall etching solution The etching rate of aluminum and molybdenum tends to be consistent, thereby achieving uniform etching of molybdenum-aluminum laminated films. In particular, under the action of the metal corrosion inhibitor, the etching solution can also effectively alleviate the side etching effect of the metal film material, and reduce the etching selectivity on the side wall of the laminated film (that is, improve the verticality of the side wall of the laminated film after etching), thereby improving the etching accuracy. In particular, the laminated film will not be stratified after etching, that is, the etching solution will not affect the interfacial bonding force of the metal film layer. In summary, the above-mentioned surfactant is compounded with the metal corrosion inhibitor, which can further improve the metal corrosion inhibitor's ability to regulate the speed and angle of etching, so that the etching solution can effectively regulate the etching ratio of metal molybdenum and aluminum, reduce the occurrence of film side etching, reduce the strip width loss of the film, and improve etching accuracy.

[0007] In the present application, the etching solution contains 50-80 parts of phosphoric acid. For example, the weight parts of phosphoric acid can be 50 parts, 55 parts, 60 parts, 62 parts, 65 parts, 68 parts, 70 parts, 75 parts, 78 parts, or 80 parts.

[0008] In the present application, the etching solution contains 1-10 parts of nitric acid. Exemplarily, the weight parts of nitric acid can be 1 part, 2 parts, 2.5 parts, 3 parts, 5 parts, 7.5 parts, 8 parts, and 10 parts.

[0009] In the present application, the etching solution contains 10-30 parts of acetic acid. Exemplarily, the weight parts of acetic acid can be 10 parts, 15 parts, 17.5 parts, 19 parts, 20 parts, 25 parts, and 30 parts.

[0010] In the present application, the etching solution contains 0.01-1 parts of metal corrosion inhibitor. Exemplarily, the weight parts of the metal corrosion inhibitor can be 0.01 parts, 0.02 parts, 0.05 parts, 0.08 parts, 0.1 parts, 0.5 parts, 0.75 parts, and 1.0 parts.

[0011] In the present application, the etching solution contains 0.01-1 parts of a surfactant. For example, the weight parts of the surfactant can be 0.01 parts, 0.02 parts, 0.05 parts, 0.08 parts, 0.1 parts, 0.5 parts, 0.75 parts, and 1.0 parts.

[0012] In the embodiment of the present application, the phosphoric acid, nitric acid and acetic acid are all commercially available reagents. The phosphinocarboxylic acid can be aminotrimethylenephosphonic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 2-hydroxyphosphonoacetic acid, etc.

[0013] In the embodiment of the present application, the etching solution contains the following components in parts by weight: 72-78 parts of phosphoric acid, 2.5-4.5 parts of nitric acid, 16-19 parts of acetic acid, and the balance is water. The preferred contents of phosphoric acid, nitric acid and acetic acid are more conducive to ensuring the overall etching rate of the etching solution, and are conducive to regulating the etching selectivity and etching accuracy of molybdenum and aluminum.

[0014] In the embodiment of the present application, the etching solution contains 0.005-0.75 parts of nonylphenol polyoxyethylene ether, and illustratively, the weight parts of nonylphenol polyoxyethylene ether can be 0.005 parts, 0.01 parts, 0.02 parts, 0.03 parts, 0.05 parts, 0.1 parts, 0.15 parts, 0.2 parts, and 0.25 parts. The etching solution contains 0.005-0.25 parts of fatty alcohol polyoxyethylene ether sulfate, and illustratively, the weight parts of fatty alcohol polyoxyethylene ether sulfate can be 0.005 parts, 0.01 parts, 0.025 parts, 0.03 parts, 0.05 parts, 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, and 0.75 parts. In some embodiments, the fatty alcohol polyoxyethylene ether sulfate is fatty alcohol polyoxyethylene ether sodium sulfate and / or fatty alcohol polyoxyethylene ether ammonium sulfate. Fatty alcohol polyoxyethylene ether sulfate is an ionic surfactant, and nonylphenol polyoxyethylene ether is a nonionic surfactant. After the two are compounded in an appropriate ratio, the cloud point of nonylphenol polyoxyethylene ether can be increased and its dispersibility in the system can be improved, so that the above etching solution has better temperature resistance and can remain stable at a higher temperature.

[0015] In the embodiment of the present application, the metal corrosion inhibitor further comprises a phosphonate, and the phosphonate may be 2,4-di-tert-butylphenoxy sodium phosphate for example. The phosphonate and the metal corrosion inhibitor can produce a certain synergistic effect, especially in the presence of phosphine carboxylic acid compounds, the presence of a small amount of phosphonate can effectively improve the corrosion inhibition effect of the metal corrosion inhibitor.

[0016] In some embodiments of the present application, the metal corrosion inhibitor is a mixture of any one or more of sulfonated lignin, phosphinocarboxylic acid and mercaptobenzothiazole and potassium acetate. The presence of potassium acetate can increase the corrosion inhibition rate of these organic corrosion inhibitors such as sulfonated lignin on metal molybdenum, making the etching rates of aluminum and molybdenum more consistent. Furthermore, in the case of containing phosphinocarboxylic acid, it is preferred to add a small amount of phosphonate. This can greatly improve the corrosion inhibition effect of phosphinocarboxylic acid. In other embodiments, the metal corrosion inhibitor is potassium acetate.

[0017] In the embodiment of the present application, the mass ratio of the surfactant to the metal corrosion inhibitor is 1:(0.5-2). The appropriate mass ratio between the surfactant and the metal corrosion inhibitor can effectively improve their compounding effect, thereby ensuring the etching selectivity of the etching solution to molybdenum and aluminum.

[0018] In the embodiment of the present application, the pH value of the etching solution is 1.5-2.5. A suitable pH value can ensure good stability and etching effect of the etching solution.

[0019] In a second aspect, the present application provides a method for preparing an etching solution, comprising the following steps:

[0020] Phosphoric acid, nitric acid, acetic acid, a surfactant, a metal corrosion inhibitor and water are mixed in proportion to obtain an etching solution; the etching solution contains the following components in parts by weight: 50-80 parts of phosphoric acid, 1-10 parts of nitric acid, 10-30 parts of acetic acid, 0.01-1 parts of metal corrosion inhibitor, 0.01-1 parts of surfactant, and the balance is water; wherein the surfactant includes nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate; the metal corrosion inhibitor includes at least one of potassium acetate, sulfonated lignin, phosphine carboxylic acid, and mercaptobenzothiazole.

[0021] The preparation method can obtain the etching solution only by mixing the raw materials. The preparation method has simple process and high production efficiency and is suitable for large-scale industrial production.

[0022] In a third aspect, the present application provides a method for processing a metal film material, comprising contacting the etching solution provided in the first aspect of the present application or the etching solution prepared according to the preparation method described in the second aspect with the metal film material to perform etching; wherein the metal film material comprises an aluminum film, an aluminum alloy film, a molybdenum film, a molybdenum alloy film, a molybdenum-aluminum laminated film, an aluminum-molybdenum-aluminum laminated film, and a molybdenum-aluminum-molybdenum laminated film. The processing method is simple to operate and is suitable for large-scale industrial production.

[0023] In the embodiment of the present application, the contacting includes immersing the metal film material in an etching solution, or spraying / rinsing the etching solution on the metal film material, which can be selected according to actual production conditions.

[0024] In the embodiment of the present application, the etching time is 90s-110s. The appropriate time can ensure that there is no residue after etching.

[0025] In the embodiment of the present application, the etching temperature is 40° C.-70° C. A suitable temperature can ensure the etching accuracy and etching speed.

[0026] The etching solution provided in the present application has strong controllability, good etching uniformity, smooth etching angle, high precision, can complete the etching of materials in a short time, no residue on the surface of the glass panel after etching, the key size loss of the material is less than 0.5μm, and the etching angle is less than 60°, which ensures the coverage of the film on the substrate in the subsequent process. And it can also meet the etching requirements of aluminum film, aluminum alloy film, molybdenum film, molybdenum alloy film, and molybdenum-aluminum laminated film, aluminum-molybdenum-aluminum laminated film and molybdenum-aluminum-molybdenum laminated film with different thicknesses. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a scanning electron microscopy (SEM) photograph of sample S6 obtained by etching a molybdenum-aluminum-molybdenum laminated film with the etching solution of Example 6;

[0028] Figure 2 is a SEM photograph of sample S8 obtained after the molybdenum-aluminum-molybdenum laminated film was etched by the etching solution of Example 8;

[0029] Figure 3 is a SEM photograph of sample S9 obtained by etching a molybdenum-aluminum-molybdenum laminated film with the etching solution of Example 9;

[0030] Figure 4 This is a SEM photograph of sample S10 obtained by etching the molybdenum-aluminum laminated film with the etching solution of Example 10. DETAILED DESCRIPTION

[0031] The technical solution of the present application is described in detail below in multiple embodiments.

[0032] Example 1

[0033] Phosphoric acid, nitric acid, acetic acid, metal corrosion inhibitor and water are mixed uniformly in a certain proportion, and then filtered to obtain an etching solution. The etching solution includes the following components in parts by weight: 65 parts of phosphoric acid, 3 parts of nitric acid, 17.5 parts of acetic acid, 0.05 parts of metal corrosion inhibitor, specifically a mixture of potassium acetate, sulfonated lignin, 2-phosphonic acid butane-1,2,4-tricarboxylic acid, and mercaptobenzothiazole, 0.5 parts of nonylphenol polyoxyethylene ether, 0.05 parts of fatty alcohol polyoxyethylene ether sodium sulfate, and the balance is water.

[0034] The glass panel covered with the molybdenum-aluminum-molybdenum laminated film was immersed in the above etching solution at 40° C. for 100 seconds, wherein the thickness of each metal film along the thickness direction was 200 nm, 3800 nm, and 500 nm, respectively. The sample after etching was recorded as S1.

[0035] Example 2

[0036] The difference between Example 2 and Example 1 is that the etching solution includes the following components in parts by weight: 50 parts of phosphoric acid, 1 part of nitric acid, 10 parts of acetic acid, 0.01 parts of potassium acetate, sulfonated lignin, 2-phosphonobutane-1,2,4-tricarboxylic acid, and a mixture of mercaptobenzothiazole, 0.01 parts of nonylphenol polyoxyethylene ether, 0.05 parts of fatty alcohol polyoxyethylene ether sodium sulfate, and the balance is water. The sample after etching is recorded as S2.

[0037] Example 3

[0038] The difference between Example 3 and Example 1 is that the etching solution includes the following components in parts by weight: 80 parts of phosphoric acid, 10 parts of nitric acid, 30 parts of acetic acid, 0.05 parts of potassium acetate, sulfonated lignin, 2-phosphonobutane-1,2,4-tricarboxylic acid, and a mixture of mercaptobenzothiazole, 0.25 parts of nonylphenol polyoxyethylene ether, 0.75 parts of fatty alcohol polyoxyethylene ether sodium sulfate, and the balance is water. The sample after etching is recorded as S3.

[0039] Example 4

[0040] The difference between Example 4 and Example 1 is that the etching solution contains 62 parts of phosphoric acid, 2.5 parts of nitric acid, and 16 parts of acetic acid. The sample after etching is recorded as S4.

[0041] Example 5

[0042] The difference between Example 5 and Example 1 is that the etching solution contains 68 parts of phosphoric acid, 4.5 parts of nitric acid, and 19 parts of acetic acid. The sample after etching is recorded as S5.

[0043] Example 6

[0044] The difference between Example 6 and Example 1 is that the metal corrosion inhibitor is a mixture of potassium acetate, sulfonated lignin, 2-phosphonobutane-1,2,4-tricarboxylic acid, phosphonate and mercaptobenzothiazole. The etched sample is recorded as S6.

[0045] Example 7

[0046] The difference between Example 7 and Example 1 is that the metal corrosion inhibitor is potassium acetate. The sample after etching is recorded as S7.

[0047] Example 8

[0048] The difference between Example 8 and Example 1 is that the thickness of each metal film in the Mo-Aluminum-Mo stacked film along the thickness direction is 200 nm, 3300 nm, and 500 nm respectively. The sample after etching is recorded as S8.

[0049] Example 9

[0050] The difference between Example 9 and Example 1 is that the thickness of each metal film in the Mo-Aluminum-Mo stacked film along the thickness direction is 200 nm, 2500 nm, and 500 nm respectively. The sample after etching is recorded as S9.

[0051] Example 10

[0052] The difference between Example 10 and Example 1 is that the object to be etched is a molybdenum-aluminum laminated film, the thickness of the molybdenum layer is 800 nm, and the thickness of the aluminum layer is 2000 nm. The sample after etching is recorded as S10.

[0053] Embodiment 11

[0054] The difference between Example 11 and Example 1 is that the object of etching is a molybdenum film, and the thickness of the molybdenum film is 2000 nm. The sample after etching is recorded as S11.

[0055] Example 12

[0056] The difference between Example 12 and Example 1 is that the etching object is an aluminum film, and the thickness of the aluminum film is 2000 nm. The sample after etching is recorded as S12.

[0057] In order to highlight the beneficial effects brought about by the technical solutions of the embodiments of the present application, the following comparative examples are set.

[0058] Comparative Example 1

[0059] The difference between Comparative Example 1 and Example 1 is that the sample does not contain surfactant and metal corrosion inhibitor. The sample after etching is recorded as DS1.

[0060] Comparative Example 2

[0061] The difference between Comparative Example 2 and Example 1 is that the sample does not contain a metal corrosion inhibitor. The sample after etching is recorded as DS2.

[0062] Comparative Example 3

[0063] The difference between Comparative Example 3 and Example 1 is that the surfactant is only sodium fatty alcohol polyoxyethylene ether sulfate. The etched sample is recorded as DS3.

[0064] The samples prepared in the above embodiments and comparative examples were subjected to SEM test. The SEM photos of the samples prepared in some embodiments can be found in Figure 1-Figure 4The critical dimension loss and etching angle of the sample film layer after etching can be directly measured from the SEM photos. The test results of each embodiment and comparative example are summarized in Table 1.

[0065] Table 1 Test results of metal film materials prepared in various embodiments and comparative examples

[0066]

[0067]

[0068] From the data in Table 1, it can be seen that the samples S1-S11 prepared in the examples of the present application have smaller critical loss dimensions and etching angles (critical dimension loss is less than 0.5 μm, etching angle is less than 60°) than the samples DS1-DS3 prepared in the comparative examples, and the etching cleanliness is high with no material residue. In addition, phosphonate is also added to the etching solution of Example 6, and the results show that the performance of the etching solution is more significantly improved.

[0069] It can be seen that the etching liquid provided in the present application has strong controllability, good etching uniformity, smooth etching angle and high precision. The key dimension loss of the material after etching is less than 0.5μm, the etching angle is less than 60°, and there is no residue on the surface of the glass panel.

[0070] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.

Claims

1. An etching solution for metal film material, characterized in that: The etching solution contains the following components in parts by weight: 50-80 parts of phosphoric acid, 1-10 parts of nitric acid, 10-30 parts of acetic acid, 0.01-1 parts of metal corrosion inhibitor, 0.01-1 parts of surfactant, and the balance is water; the surfactant includes nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate, and the weight portion of the nonylphenol polyoxyethylene ether is 0.005-0.75 parts, and the weight portion of the fatty alcohol polyoxyethylene ether sulfate is 0.005-0.25 parts; The metal corrosion inhibitor includes at least one of potassium acetate, sulfonated lignin, phosphine carboxylic acid, and mercaptobenzothiazole; The mass ratio of the surfactant to the metal corrosion inhibitor is 1:(0.5-2); the pH value of the etching solution is 1.5-2.

5.

2. The etching solution according to claim 1, characterized in that The metal corrosion inhibitor also includes phosphonates.

3. The etching solution according to claim 1, characterized in that The etching solution contains the following components in parts by weight: 72-78 parts of phosphoric acid, 2.5-4.5 parts of nitric acid, 16-19 parts of acetic acid, and the balance is water.

4. A method for preparing an etching solution for a metal film material, characterized in that: The following steps are involved: Phosphoric acid, nitric acid, acetic acid, a surfactant, a metal corrosion inhibitor and water are mixed in proportion to obtain an etching solution; the etching solution contains the following components in parts by weight: 50-80 parts of phosphoric acid, 1-10 parts of nitric acid, 10-30 parts of acetic acid, 0.01-1 parts of metal corrosion inhibitor, 0.01-1 parts of surfactant, and the balance is water; wherein the surfactant comprises nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether sulfate, and the weight portion of the nonylphenol polyoxyethylene ether is 0.005-0.75 parts, and the weight portion of the fatty alcohol polyoxyethylene ether sulfate is 0.005-0.25 parts; the metal corrosion inhibitor comprises at least one of potassium acetate, sulfonated lignin, phosphine carboxylic acid, and mercaptobenzothiazole; The mass ratio of the surfactant to the metal corrosion inhibitor is 1:(0.5-2); the pH value of the etching solution is 1.5-2.

5.

5. A method for processing a metal film material, characterized in that: The following steps are involved: The etching solution according to any one of claims 1 to 3 or the etching solution prepared by the preparation method according to claim 4 is brought into contact with a metal film material to etch the metal film material; wherein the metal film material includes an aluminum film, an aluminum alloy film, a molybdenum film, a molybdenum alloy film, a molybdenum-aluminum laminated film, an aluminum-molybdenum-aluminum laminated film, and a molybdenum-aluminum-molybdenum laminated film.

6. The processing method according to claim 5, characterized in that: The etching time is 90s-110s.

7. The processing method according to claim 5, characterized in that: The etching temperature is 40°C-70°C.