A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer and a preparation method thereof

By using a three-dimensional conductive substrate and an interface modification layer in a lithium metal battery to form a multifunctional interface layer of lithium tin alloy and lithium fluoride, the problems of uneven deposition and volume expansion of lithium metal batteries during the charge and discharge process are solved, and the battery life is extended. longevity and improved stability.

CN114512637BActive Publication Date: 2024-10-11WUHAN INST OF TECH

Patent Information

Application Number
CN202210063418.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-20
Publication Date
2024-10-11
Estimated Expiration
2042-01-20

AI Technical Summary

Technical Problem

Uneven deposition and volume expansion of lithium metal batteries during the charge and discharge process lead to the growth of lithium dendrites, which may cause short circuits and explosions, and have short cycle life. It is difficult to effectively suppress these problems with existing technology.

Method used

A three-dimensional conductive substrate and an interface modification layer with high ion conductivity are used to form a multifunctional interface layer through lithium tin alloy and lithium fluoride to regulate the uniform deposition of lithium, inhibit the growth of lithium dendrites, and buffer volume expansion.

Benefits of technology

It significantly extends the service life of lithium metal anodes, improves electrochemical cycle performance, inhibits lithium dendrite growth and volume expansion, and improves the stability and application potential of lithium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114512637B_ABST
    Figure CN114512637B_ABST
Patent Text Reader

Abstract

The present invention discloses a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer, which includes a three-dimensional conductive substrate, a multifunctional interface layer and loaded metal lithium; the multifunctional interface layer contains lithium-tin alloy and lithium fluoride. The present invention combines a three-dimensional conductive substrate with an interface modification layer having high ionic conductivity and being stable to an electrolyte, firstly loads stannous fluoride on the three-dimensional conductive substrate, and then uses high-temperature molten lithium to prepare the three-dimensional composite lithium metal negative electrode, which can simultaneously realize the construction of lithium-tin alloy and lithium fluoride at the interface between the lithium layer and the three-dimensional conductive substrate, and simultaneously solve the problem of lithium affinity of the three-dimensional substrate and the problem of ion transmission and interface stability of the electrode; and the preparation method involved is relatively simple, easy to operate, and suitable for popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer and a preparation method thereof. Background Art

[0002] With the widespread application of consumer electronics, electric bicycles and electric vehicles in life, people's demand for the mass / volume energy density of energy storage battery devices has gradually increased. However, the energy density of the current commercial lithium-ion battery system has basically reached a bottleneck. Therefore, it is urgent to explore the next generation of new energy storage materials and develop battery systems with high energy density. In recent years, metallic lithium has been used for a long time due to its high theoretical specific capacity (3860mAh g -1 ), low electrode potential (-3.04 V compared to standard hydrogen electrode) and low density (0.534 g cm -3 ) and other characteristics, once again attracted the attention of battery researchers.

[0003] However, there are still some bottlenecks in the application of lithium metal batteries, which limit their commercial application. Specifically, the uneven deposition / stripping of lithium metal during the charge and discharge process will cause the growth of lithium dendrites, which may pierce the diaphragm, causing battery short circuits and even serious explosions; secondly, the high reactivity of lithium metal and the volume expansion problem during cyclic charge and discharge lead to the continuous consumption of active lithium and electrolyte, which in turn leads to low coulomb efficiency and short cycle life, which seriously hinder the practical application of lithium metal batteries. In response to the above challenges, current research can be roughly divided into two categories: surface regulation and substrate modification. Common strategies starting from the surface are: 1) optimizing the electrolyte composition, introducing electrolyte additives and other stable electrode / electrolyte surface layers (SEI layers); 2) artificially coating the surface of metallic lithium with an artificial protective layer, such as an inorganic carbon layer, an organic polymer layer, etc. The main strategies for substrate modification are: 1) using three-dimensional current collectors (porous copper, carbon cloth, etc.) as carriers of metallic lithium to buffer its volume expansion during charging and discharging; 2) constructing vertical nanopores on the surface of two-dimensional current collectors such as copper foil to regulate lithium deposition.

[0004] Lithium metal anode is a host-free electrode. When the electrode undergoes a drastic volume change, the interface film constructed by the surface regulation strategy is not strong and stable enough to inhibit the growth of dendrites. Most of the three-dimensional composite electrodes constructed only by substrate modification are lithium-phobic, and it is difficult to directly use them as carriers of metallic lithium to pre-store lithium. In addition, the electrode surface lacks a stable solid electrolyte film, and the electrode is prone to side reactions with the electrolyte, resulting in battery capacity decay. Therefore, further exploration and optimization of three-dimensional composite anodes that can regulate the deposition of lithium ions and inhibit dendrite growth and buffer electrode volume changes, in order to effectively solve the problems of lithium dendrites and volume expansion caused by uneven lithium deposition, has important research and application significance. Summary of the invention

[0005] The main purpose of the present invention is to address the problems and shortcomings of the prior art and provide a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer. The three-dimensional conductive framework substrate and the interface modification layer with high ionic conductivity and stability to the electrolyte are adopted to regulate the uniform deposition of lithium while suppressing the volume expansion of the metal lithium negative electrode during the charge and discharge process, showing a low lithium deposition overpotential and stable electrochemical cycle performance, and significantly extending the service life.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer comprises a three-dimensional conductive substrate, a multifunctional interface layer (an interface layer between the three-dimensional conductive substrate and metallic lithium), and metallic lithium filled in the gaps of the three-dimensional conductive substrate and / or loaded on the surface of the multifunctional interface layer; the multifunctional interface layer comprises lithium-tin alloy and lithium fluoride.

[0008] In the above scheme, the lithium-tin alloy is Li2Sn5, LiSn, Li7Sn3, Li5Sn2, Li 13 One or more of Sn5, Li7Sn2, etc.

[0009] In the above scheme, the three-dimensional composite lithium metal negative electrode is first prepared by loading stannous fluoride on the surface of a three-dimensional conductive substrate, and then depositing and cooling high-temperature molten lithium; when the three-dimensional conductive substrate is infused with high-temperature molten lithium, the loaded stannous fluoride reacts with the contacted lithium under the action of high temperature to generate lithium-tin alloy and lithium fluoride, thereby forming the multifunctional interface structure and surface lithium layer.

[0010] Preferably, in the high-temperature molten lithium deposition step, part of the lithium fluoride obtained by the reaction further migrates to the lithium surface. The lithium fluoride formed on the surface can effectively reduce the side reaction between lithium and the electrolyte solution, thereby improving the interface stability of lithium / electrolyte and inhibiting the growth of lithium dendrites.

[0011] In the above scheme, the temperature used in the high-temperature molten lithium deposition step is 200-250° C. and the time is 30-90 seconds.

[0012] In the above scheme, the three-dimensional conductive substrate can be selected from carbon fiber cloth, foamed carbon, graphene foam, carbon nanotube film or biomass carbon film.

[0013] Preferably, the three-dimensional conductive substrate may be in the shape of a disc with a diameter of 8 to 12 mm.

[0014] The method for preparing the three-dimensional composite lithium metal negative electrode having a multifunctional interface layer comprises the following steps:

[0015] 1) heating and dissolving stannous fluoride in a polar solvent to prepare a stannous fluoride solution;

[0016] 2) adding the three-dimensional conductive substrate into a stannous fluoride solution for soaking treatment, taking out the soaked three-dimensional conductive substrate after cooling, and drying it to obtain a three-dimensional conductive substrate loaded with stannous fluoride;

[0017] 3) Under a protective atmosphere, high-temperature molten lithium deposition is performed on the three-dimensional conductive substrate loaded with stannous fluoride to fill the three-dimensional conductive substrate with a lithium layer, and then naturally cooled to room temperature to obtain the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0018] In the above scheme, the three-dimensional conductive substrate is first washed (alcohol washed and water washed) and dried (60-80° C., 8-12 h) before use.

[0019] In the above scheme, the protective atmosphere can be nitrogen or argon.

[0020] In the above scheme, the concentration of the stannous fluoride solution is 20 to 80 mmol / L.

[0021] In the above scheme, the heating and dissolving temperature in step 1) is 100-120° C. and the time is 1-2 hours.

[0022] In the above scheme, the polar solvent can be selected from dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF) or tetrahydrofuran (THF) and the like.

[0023] In the above scheme, the soaking treatment step in step 2) adopts a heating soaking process, the temperature used is 100-120° C., and the time is 2-4 hours.

[0024] In the above scheme, the temperature used in the high-temperature molten lithium deposition step is 200-250° C., preferably 210° C., and the time is 30-90 seconds.

[0025] In the above scheme, the high-temperature molten lithium deposition step comprises: adding the three-dimensional conductive substrate loaded with stannous fluoride obtained in step 2) into molten lithium and allowing it to deposit for 30 to 90 seconds.

[0026] In the above scheme, the molten lithium is obtained by heating and melting a single substance of lithium.

[0027] In the above scheme, the drying temperature in step 2) is 40-60° C. and the drying time is 4-6 hours.

[0028] In the above scheme, during the high-temperature molten lithium deposition process in step 3), when molten lithium is used to infuse the three-dimensional conductive substrate, the loaded stannous fluoride reacts with the contacted lithium under the action of high temperature and is converted into a multifunctional interface layer containing lithium-tin alloy and lithium fluoride near the interface, and then naturally cooled to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0029] The three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared according to the above scheme can form a multifunctional interface layer (including lithium-tin alloy and lithium fluoride) on a three-dimensional conductive substrate, which is conducive to the manufacture of rich electrochemical active sites, forming a stable electrolyte / lithium metal interface during the cycle, inducing uniform deposition / stripping of lithium, effectively inhibiting the growth of lithium dendrites, and improving the volume effect, thereby enhancing the cycle stability of the three-dimensional composite material as a lithium metal negative electrode.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1) The present invention selects a commercial low-cost three-dimensional conductive substrate such as carbon fiber cloth as a carrier of the metal lithium negative electrode, which has excellent conductivity and large specific surface area, can effectively buffer the volume change of lithium during the deposition / stripping process, and can reduce the local current density, which is beneficial to inhibit the growth of lithium dendrites;

[0032] 2) The present invention first loads stannous fluoride on a three-dimensional conductive substrate, and then uses high-temperature molten lithium to react with stannous fluoride to generate a multifunctional interface layer containing tin alloy and lithium fluoride, which can effectively improve the molten lithium wettability of the three-dimensional conductive substrate and promote the uniform deposition of molten lithium on the three-dimensional conductive substrate; the formed lithium-tin alloy has a very high ion diffusion coefficient, which can promote the transmission of lithium ions in metallic lithium, reduce the nucleation overpotential of lithium and guide the uniform deposition of lithium; the generated part of lithium fluoride can further migrate to the lithium surface, which has a high ion diffusion coefficient and is an electronic insulator, which can effectively prevent the growth of lithium dendrites in the SEI film, improve the interface stability of lithium to the liquid electrolyte, and play a role in interface protection; the present invention adopts a simple one-step lithium precipitation composite process, which can simultaneously realize the construction of tin alloy and lithium fluoride at the interface between the lithium layer and the three-dimensional conductive substrate, and can simultaneously solve the lithium affinity problem of the three-dimensional substrate and the ion transmission and interface stability problems of the electrode;

[0033] 3) The present invention combines a three-dimensional conductive substrate with an interface modification layer having high ionic conductivity and being stable to the electrolyte, which can effectively improve the dendrite growth and volume expansion problems existing in lithium metal batteries, and will further promote the practical application of lithium metal batteries;

[0034] 4) The preparation method of the present invention is relatively simple, easy to operate, and suitable for popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a scanning electron microscope (SEM) image of the carbon fiber cloth used in Example 1 of the present invention;

[0036] Figure 2 This is a scanning electron microscope (SEM) image of the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared in Example 1 of the present invention;

[0037] Figure 3 This is a comparison chart of X-ray diffraction (XRD) of the carbon fiber cloth loaded with stannous fluoride, the carbon fiber cloth, and commercial stannous fluoride in Example 1 of the present invention;

[0038] Figure 4 This is an X-ray diffraction (XRD) comparison diagram of the three-dimensional composite lithium metal negative electrode (Example 1) obtained in Example 1 of the present invention and the carbon fiber cloth deposited lithium negative electrode (Comparative Example 1);

[0039] Figure 5 The three-dimensional composite lithium metal negative electrode obtained in Example 1 of the present invention and the negative electrode of Comparative Example 1 are used as negative electrodes and assembled with lithium iron phosphate (LiFePO4) positive electrodes to obtain a cycle performance comparison diagram of a full battery;

[0040] Figure 6 The figure is a rate performance diagram of a full battery assembled with the three-dimensional composite lithium metal negative electrode and lithium iron phosphate (LiFePO4) positive electrode obtained in Example 1 of the present invention;

[0041] Figure 7 The three-dimensional composite lithium metal negative electrode obtained in Example 2 of the present invention and the negative electrode of Comparative Example 1 are used as the negative electrode and the positive electrode of lithium iron phosphate (LiFePO4) to assemble the obtained full battery cycle performance comparison diagram;

[0042] Figure 8 The three-dimensional composite lithium metal negative electrode obtained in Example 3 of the present invention and the negative electrode of Comparative Example 1 are respectively used as negative electrodes and assembled with lithium iron phosphate (LiFePO4) positive electrodes to obtain a full battery cycle performance comparison chart;

[0043] Fig. 9 The three-dimensional composite lithium metal negative electrode obtained in Example 4 of the present invention and the negative electrode in Comparative Example 1 are respectively assembled with a lithium iron phosphate (LiFePO4) positive electrode to obtain a full battery cycle performance comparison chart;

[0044] Fig.10 The three-dimensional composite lithium metal negative electrode obtained in Example 5 of the present invention and the negative electrode of Comparative Example 1 are respectively assembled with a lithium iron phosphate (LiFePO4) positive electrode to obtain a full battery cycle performance comparison chart;

[0045] Fig.11This is a comparison chart of the cycle performance of a full battery obtained by assembling the three-dimensional composite lithium metal negative electrode obtained in Example 6 of the present invention and the negative electrode of Comparative Example 1 with a lithium iron phosphate (LiFePO4) positive electrode. DETAILED DESCRIPTION

[0046] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific embodiments, but the content of the present invention is not limited to the following embodiments.

[0047] Example 1

[0048] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer is prepared by a solution heating immersion method and a high-temperature molten lithium deposition method, and specifically comprises the following preparation steps:

[0049] 1) Cut the three-dimensional conductive substrate material carbon fiber cloth into discs with a diameter of 8 mm, put it into an ultrasonic cleaner, and use ethanol and deionized water to ultrasonically clean it three times in sequence, each time for 10 minutes to remove surface impurities, and put it into a vacuum drying oven at 60° C. to dry for 8 to 12 hours for use;

[0050] 2) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), add 39.2mg of stannous fluoride to 5mL of DMSO, place it on an intelligent magnetic stirrer, stir and heat (heating temperature is 120°C) to completely dissolve it to form a solution, prepare a stannous fluoride solution with a concentration of 50mM, and stop stirring; add the cleaned carbon fiber cloth in step 1) to the obtained stannous fluoride solution and soak it at 120°C for two hours, then stop heating, wait for the solution to cool naturally to room temperature, take out the carbon fiber cloth, and dry it on a heating table at 60°C for 6h for use;

[0051] 3) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), weigh the carbon fiber cloth loaded with stannous fluoride that was fully dried in step 2), set the heating table temperature to 210°C, place an appropriate amount of lithium sheets in a crucible to melt, and when the lithium sheets are completely melted, use sharp tweezers to clamp the carbon fiber cloth loaded with stannous fluoride and place it in the molten lithium for deposition for 30 seconds. When it is not completely cooled, use a roller pressing device to flatten the surface, and wait for it to cool naturally to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0052] Comparative Example 1

[0053] A three-dimensional composite lithium metal negative electrode, the preparation method of which comprises the following steps:

[0054] 1) Cut the three-dimensional conductive substrate material carbon fiber cloth into discs with a pore size of 8 mm, clean them according to step 1) in Example 1 to remove surface impurities, and dry them for later use;

[0055] 2) The negative electrode was prepared according to step 3) of Example 1, except that the temperature of the heating stage was set to 320° C. (increasing the temperature increases the wettability of the simple substrate to molten lithium).

[0056] Figure 1 This is a scanning electron microscope (SEM) image of the carbon fiber cloth used in Example 1. Figure 2 This is a scanning electron microscope (SEM) image of the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared in Example 1. Figure 1 and Figure 2 By comparison, it can be seen that after lithium deposition, the carbon fibers of the three-dimensional carbon fiber cloth modified by the above process of the present invention are fully infused with molten lithium, which indicates that the surface modification of the three-dimensional conductive carbon fiber cloth can effectively induce uniform lithium deposition and improve the problem of dendrite growth.

[0057] Figure 3 The X-ray diffraction (XRD) comparison diagram of the carbon fiber cloth loaded with stannous fluoride obtained in step 2) of Example 1 of the present invention, the carbon fiber cloth and the commercial stannous fluoride. Figure 3 It can be seen that characteristic peaks of stannous fluoride appear at 19.761°, 25.049°, 27.857°, etc., proving that stannous fluoride is successfully loaded on the three-dimensional conductive carbon fiber cloth.

[0058] Figure 4 This is an X-ray diffraction (XRD) comparison diagram of the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared in Example 1 of the present invention, the negative electrode prepared in Comparative Example 1, and the carbon fiber cloth. Figure 4 It can be seen that the product obtained in Example 1 has characteristic peaks of lithium tin alloy (Li7Sn2) at 25.818°, 29.198°, 32.039°, 59.878°, etc. and characteristic peaks of lithium fluoride (LiF) at 44.996°, 65.494°, etc. (partial lithium fluoride is formed in the obtained three-dimensional composite lithium metal negative electrode), indicating the formation of a multifunctional interface layer. At the same time, characteristic peaks of lithium (Li) appear at 36.190°, 51.973°, 64.980°, 87.887°, etc., indicating that lithium is uniformly deposited on the carbon fiber cloth, and the stannous fluoride loaded on the three-dimensional conductive carbon fiber cloth will fully react with the contacted lithium to form a multifunctional interface layer containing lithium tin alloy and lithium fluoride.

[0059] Figure 5 The graph is a comparison of the cycle performance of a full battery assembled with a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared in Example 1 of the present invention and a negative electrode obtained in Comparative Example 1 and a lithium iron phosphate (LiFePO4) positive electrode. The graph shows that at 0.5C (1C = 170 mAh g -1) When cycled at low rate, the first discharge capacity of the full battery assembled with the negative electrode prepared in Example 1 was 143.7 mAh g -1 After 100 cycles, the reversible specific capacity can still be maintained at 144.1 mAh g -1 The first discharge capacity of the three-dimensional conductive carbon fiber cloth deposited with lithium as the negative electrode obtained in Comparative Example 1 was 122.1 mAh g -1 After a short cycle, the specific capacity decays significantly. It can be seen that the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared by the present invention not only improves the battery lithium storage performance, but also shows good cycle stability.

[0060] Figure 6 The figure is a rate performance diagram of a full battery assembled with a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer and a lithium iron phosphate (LiFePO4) positive electrode prepared in Example 1 of the present invention. As can be seen from the figure, the discharge specific capacity of the full battery prepared in Example 1 at 0.2C, 0.5C, 1C, 2C, 3C, 4C, and 5C is 156 mAh g -1 , 145mAh g -1 , 131.5mAh g -1 , 120.6mAh g -1 , 107.8mAh g -1 , 98mAh g -1 , 81.7mAh g -1 When the cycle rate returns to 0.2C, the discharge capacity of the full battery prepared in Example 1 can still be maintained at 155 mAh g -1 , indicating that it has excellent cycle rate performance.

[0061] Example 2

[0062] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer is prepared by a solution heating immersion method and a high-temperature molten lithium deposition method, and specifically comprises the following preparation steps:

[0063] 1) Cut the three-dimensional conductive substrate material carbon fiber cloth into discs with a diameter of 8 mm, put it into an ultrasonic cleaner, and use ethanol and deionized water to ultrasonically clean it three times in sequence, each time for 10 minutes to remove surface impurities, and put it into a vacuum drying oven at 60° C. to dry for 8 to 12 hours for use;

[0064] 2) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), add 16mg of stannous fluoride to 5mL of DMSO, place it on an intelligent magnetic stirrer, stir and heat (heating temperature is 120°C) to completely dissolve it to form a solution, prepare a stannous fluoride solution with a concentration of 20mM, and stop stirring; add the cleaned carbon fiber cloth in step 1) to the obtained stannous fluoride solution and soak it at 120°C for two hours, then stop heating, wait for the solution to cool naturally to room temperature, take out the carbon fiber cloth, and dry it on a heating table at 60°C for 6h for use;

[0065] 3) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), weigh the carbon fiber cloth loaded with stannous fluoride that was fully dried in step 2), set the heating table temperature to 210°C, place an appropriate amount of lithium sheets in a crucible to melt, and when the lithium sheets are completely melted, use sharp tweezers to pick up the carbon fiber cloth loaded with stannous fluoride and place it in the molten lithium for deposition for 30 seconds. Take it out, and when it is not completely cooled, use a roller pressing device to flatten the surface, and wait for it to cool naturally to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0066] Example 3

[0067] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer is prepared by a solution heating immersion method and a high-temperature molten lithium deposition method, and specifically comprises the following preparation steps:

[0068] 1) Cut the three-dimensional conductive substrate material carbon fiber cloth into discs with a diameter of 8 mm, put it into an ultrasonic cleaner, and use ethanol and deionized water to ultrasonically clean it three times in sequence, each time for 10 minutes to remove surface impurities, and put it into a vacuum drying oven at 60° C. to dry for 8 to 12 hours for use;

[0069] 2) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), add 62.7mg of stannous fluoride to 5mL of DMSO, place on an intelligent magnetic stirrer, stir and heat (heating temperature is 120°C) to completely dissolve it to form a solution, prepare a stannous fluoride solution with a solution concentration of 80mM, stop stirring, add the cleaned carbon fiber cloth in step 1) to the obtained stannous fluoride solution and soak it at 120°C for two hours, stop heating, wait for the solution to cool naturally to room temperature, take out the carbon fiber cloth, and dry it on a heating table at 60°C for 6h for use;

[0070] 3) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), weigh the fully dried carbon fiber cloth with stannous fluoride attached in step 2), set the heating table temperature to 210°C, and place an appropriate amount of lithium sheets in a crucible to melt. When the lithium sheets are completely melted, use sharp tweezers to pick up the carbon fiber cloth loaded with stannous fluoride and place it in the molten lithium for deposition for 30 seconds. When it is not completely cooled, use a roller pressing device to flatten the surface, and wait for it to cool naturally to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0071] Example 4

[0072] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer is prepared by a solution heating immersion method and a high-temperature molten lithium deposition method, and specifically comprises the following preparation steps:

[0073] 1) Cut the three-dimensional conductive self-supporting graphene paper into discs with a diameter of 8 mm, put them into an ultrasonic cleaner, and alternately ultrasonically clean them with ethanol and deionized water for 3 times, each time for 10 minutes to remove surface impurities, and put them into a vacuum drying oven at 60° C. to dry for 8 to 12 hours for use;

[0074] 2) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), add 39.2mg of stannous fluoride to 5mL of DMSO, place it on an intelligent magnetic stirrer, stir and heat (heating temperature is 120°C) to completely dissolve it to form a solution, prepare a stannous fluoride solution with a concentration of 50mM, stop stirring, add the three-dimensional conductive self-supporting graphene paper cleaned in step 1) to the obtained stannous fluoride solution and soak it at 120°C for two hours, stop heating, wait for the solution to cool naturally to room temperature, take out the three-dimensional conductive self-supporting graphene paper, and dry it on a heating table at 60°C for 6h for use;

[0075] 3) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), weigh the three-dimensional conductive self-supporting graphene paper with stannous fluoride attached that is fully dried in step 2), set the heating table temperature to 210°C, place an appropriate amount of lithium sheets in a crucible to melt, and when the lithium sheets are completely melted, use sharp tweezers to pick up the three-dimensional conductive self-supporting graphene paper loaded with stannous fluoride, put it into the molten lithium for deposition for 30 seconds, take it out, and when it is not completely cooled, use a roller pressing device to flatten the surface, and wait for it to cool naturally to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0076] Example 5

[0077] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer is prepared by a solution heating immersion method and a high-temperature molten lithium deposition method, and specifically comprises the following preparation steps:

[0078] 1) Cut the three-dimensional conductive carbon nanotube film into discs with a diameter of 8 mm, put it into an ultrasonic cleaner, and alternately ultrasonically clean it with ethanol and deionized water for 3 times, each time for 10 minutes to remove surface impurities, and put it into a vacuum drying oven at 60° C. to dry for 8 to 12 hours for use;

[0079] 2) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), add 39.2mg of stannous fluoride to 5mL of DMSO, place on an intelligent magnetic stirrer, stir and heat (heating temperature is 120°C) to completely dissolve it to form a solution, prepare a stannous fluoride solution with a concentration of 50mM, and stop stirring; add the three-dimensional conductive carbon nanotube film cleaned in step 1) to the obtained stannous fluoride solution and soak it at 120°C for two hours, then stop heating, wait for the solution to cool naturally to room temperature, take out the three-dimensional conductive carbon nanotube film, and dry it on a heating table at 60°C for 6 hours for later use;

[0080] 3) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), weigh the three-dimensional conductive carbon nanotube film with stannous fluoride attached that is fully dried in step 2), set the heating table temperature to 210°C, place an appropriate amount of lithium sheets in a crucible to melt, and when the lithium sheets are completely melted, use sharp tweezers to pick up the three-dimensional conductive carbon nanotube film loaded with stannous fluoride and place it in the molten lithium for deposition for 30 seconds. Take it out, and when it is not completely cooled, use a roller pressing device to flatten the surface, and wait for it to cool naturally to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0081] Example 6

[0082] A three-dimensional composite lithium metal negative electrode with a multifunctional interface layer is prepared by a solution heating immersion method and a high-temperature molten lithium deposition method, and specifically comprises the following preparation steps:

[0083] 1) Cut the three-dimensional conductive biomass carbon film into discs with a diameter of 8 mm, put it into an ultrasonic cleaner, and ultrasonically clean it three times with ethanol and deionized water alternately for 10 minutes each time to remove surface impurities, and put it into a vacuum drying oven at 60° C. to dry for 8 to 12 hours for use;

[0084] 2) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), add 39.2mg of stannous fluoride to 5mL of DMSO, place it on an intelligent magnetic stirrer, stir and heat (heating temperature is 120°C) to completely dissolve it to form a solution, prepare a stannous fluoride solution with a concentration of 50mM, stop stirring, add the three-dimensional conductive biomass carbon film cleaned in step 1) to the obtained stannous fluoride solution and soak it at 120°C for two hours, stop heating, wait for the solution to cool naturally to room temperature, take out the three-dimensional conductive biomass carbon film, and dry it on a heating table at 60°C for 6h for use;

[0085] 3) In an argon glove box (water content <0.01ppm, oxygen content <0.01ppm), weigh the three-dimensional conductive biomass carbon film with stannous fluoride attached that is fully dried in step 2), set the heating table temperature to 210°C, place an appropriate amount of lithium sheets in a crucible to melt, and when the lithium sheets are completely melted, use sharp tweezers to pick up the three-dimensional conductive biomass carbon film loaded with stannous fluoride and place it in molten lithium for deposition for 30 seconds. Take it out, and when it is not completely cooled, use a roller pressing device to flatten the surface, and wait for it to cool naturally to room temperature to obtain a three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

[0086] Figures 7 to 11 The three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared in Examples 2 to 6 of the present invention and the negative electrode obtained in Comparative Example 1 are respectively assembled with a lithium iron phosphate (LiFePO4) positive electrode to form a full battery.

[0087] The results show that: at a low rate of 0.5C, the first discharge specific capacity of the full battery assembled using the negative electrodes obtained in Examples 2 to 6 is significantly higher than the first discharge specific capacity of the three-dimensional conductive carbon fiber cloth deposited lithium as the negative electrode obtained in Comparative Example 1, and the cycle stability is also significantly better than that of Comparative Example 1. The specific capacity of Comparative Example 1 decays significantly after a short cycle. It can be seen that the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer prepared by the present invention has excellent electrochemical cycle performance.

[0088] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A three-dimensional composite lithium metal anode with a multifunctional interface layer, It is characterized in that The invention comprises a three-dimensional conductive substrate, a multifunctional interface layer and loaded metallic lithium; the multifunctional interface layer contains lithium-tin alloy and lithium fluoride; the lithium-tin alloy is Li 2 Sn 5 、LiSn、Li 7 Sn 3 , Li 5 Sn 2 , Li 13 Sn 5 , Li 7 Sn 2 One or more of the following; The method for preparing the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer comprises the following steps: 1) Heat and dissolve stannous fluoride in a polar solvent to prepare a stannous fluoride solution; 2) adding the three-dimensional conductive substrate into a stannous fluoride solution for soaking treatment, taking out the soaked three-dimensional conductive substrate after cooling, and drying it to obtain a three-dimensional conductive substrate loaded with stannous fluoride; 3) Under a protective atmosphere, high-temperature molten lithium deposition is performed on the three-dimensional conductive substrate loaded with stannous fluoride, molten lithium is poured into the three-dimensional conductive framework of the three-dimensional conductive substrate, and then naturally cooled to room temperature to obtain the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer; The concentration of the stannous fluoride solution is 20-80 mmol / L; The soaking treatment step in step 2) adopts a heating soaking process, the temperature used is 100-120° C., and the time is 2-4 hours.

2. The three-dimensional composite lithium metal negative electrode according to claim 1, It is characterized in that The temperature used in the high-temperature molten lithium deposition step is 200-250° C. and the time is 30-90 seconds.

3. The three-dimensional composite lithium metal negative electrode according to claim 1, It is characterized in that The three-dimensional conductive substrate is carbon fiber cloth, foamed carbon, graphene foam, carbon nanotube film or biomass carbon film.

4. A method for preparing a three-dimensional composite lithium metal negative electrode having a multifunctional interface layer according to any one of claims 1 to 3, It is characterized in that The steps include: 1) Heat and dissolve stannous fluoride in a polar solvent to prepare a stannous fluoride solution; 2) adding the three-dimensional conductive substrate into the stannous fluoride solution for soaking treatment, taking out the soaked three-dimensional conductive substrate after cooling, and drying it to obtain the three-dimensional conductive substrate loaded with stannous fluoride; 3) Under a protective atmosphere, high-temperature molten lithium deposition is performed on the three-dimensional conductive substrate loaded with stannous fluoride, molten lithium is poured into the three-dimensional conductive framework of the three-dimensional conductive substrate, and then naturally cooled to room temperature to obtain the three-dimensional composite lithium metal negative electrode with a multifunctional interface layer.

5. The preparation method according to claim 4, It is characterized in that The heating and dissolving temperature in step 1) is 100-120° C. and the time is 1-2 hours.

6. The preparation method according to claim 4, It is characterized in that The polar solvent is dimethyl sulfoxide, N,N-dimethylformamide or tetrahydrofuran.

7. The preparation method according to claim 4, It is characterized in that The drying temperature in step 2) is 40-60°C and the drying time is 4-6 hours.

Citation Information

Patent Citations

  • Preparation method of complex lithium negative pole of solid state battery

    CN106784635A

  • Lithium metal surface protection method and equipment, negative electrode plate and lithium battery

    CN109638235A

  • Method for preparing lithium metal battery negative electrode supported by carbon / tin composite substrate

    CN110299512A

  • Composite lithium metal negative pole and preparation method thereof

    CN110660968A

  • Organic lithium-philic composite negative electrode taking three-dimensional conductive carbon material as substrate and preparation method of organic lithium-philic composite negative electrode

    CN111952567A

Cited By

  • Three-dimensional vertical porous lithium tin alloy negative electrode, preparation method and battery

    CN122599368A