A two-stage leaching method for hydrometallurgical zinc smelting to improve copper recovery rate

By using boiling roasting and step-by-step two-stage leaching methods in the hydrometallurgical zinc smelting process, the charge adsorption properties of alum are used to solve the problem of low copper recovery rate in the conventional two-stage leaching method, and achieve efficient copper recovery and process Simplify, reduce costs and environmental pollution.

CN114517258BActive Publication Date: 2024-10-18云南云铜锌业股份有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210026096.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-11
Publication Date
2024-10-18
Estimated Expiration
2042-01-11

AI Technical Summary

Technical Problem

The copper recovery rate in the conventional two-stage leaching method of existing hydrometallurgical zinc smelting is low, only 20% to 40%, resulting in waste of copper resources and environmental pollution.

Method used

An improved two-stage leaching method for wet zinc smelting is adopted, including boiling roasting, alumite silicon precipitation and hot acid leaching processes. By controlling the insoluble sulfur content and soluble silicon content in the zinc roasted ore, the charge adsorption of alumite is used. The properties of silicon are fixed, and the leaching operation is divided into two steps to improve the copper recovery rate.

Benefits of technology

The copper recovery rate is increased to 70% to 80%, which is 3 to 4 times that of the original process. The investment cost is reduced, the operation process is simplified, and the problem of iron and silicon recycling enrichment is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114517258B_ABST
    Figure CN114517258B_ABST
Patent Text Reader

Abstract

The invention discloses a two-stage leaching method for wet zinc smelting for improving copper recovery rate, which specifically includes the steps of boiling roasting, one-stage leaching and two-stage leaching, wherein the two-stage leaching includes ferroalloy silicon precipitation and hot acid leaching. The invention controls the amount of insoluble sulfur (Ss) in the zinc roasting ore to between 0.4% and 0.6% by boiling roasting, which not only meets the requirement of improving copper recovery rate, but also reduces the content of soluble silicon in the zinc roasting ore, and reduces the pressure of subsequent ferroalloy silicon precipitation; the two-stage leaching is divided into two steps, and the ferroalloy is insoluble in acid and ferroalloy carries positive charge while silica gel carries negative charge. The ferroalloy can fix silicon in the ferroalloy slag through charge adsorption, thereby improving the copper recovery rate, so that the copper recovery rate reaches 70% to 80%, which is 3 to 4 times that of the original process. In addition, the invention only needs to be modified on the original process flow, and does not need to change the original process flow on a large scale, reduces investment cost and is simple to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of zinc smelting, and in particular to a two-stage leaching method for hydrometallurgical zinc smelting for improving copper recovery rate. Background Art

[0002] Hydrometallurgy of zinc refers to the process of dissolving zinc roasted ore or other zinc sulfide materials and zinc in zinc sulfide ore in sulfuric acid solution to extract metallic zinc or zinc compounds. It is the main method of modern zinc smelting. It consists of three major steps: zinc leaching, zinc sulfide solution purification, and zinc electrolytic deposition.

[0003] Zinc sulfide concentrate generally contains 0.5% to 1.0% copper. After boiling roasting, copper mainly exists in the zinc roasting ore in the form of copper oxide. The recovery of copper from zinc roasting ore can be divided into five types according to the zinc smelting process, namely: conventional two-stage leaching method, yellow potassium ferroalloy method, goethite method, para-goethite method, and hematite method. Among them, the conventional two-stage leaching method has a short process flow and simple operation, and is the mainstream process in China, but the copper recovery rate is low, only 20% to 40%; while the copper recovery rate of the other four processes reaches 70% to 95%, but there are different process disadvantages, such as the difficulty in handling the slag produced by the yellow potassium ferroalloy method; the long process flow of the goethite method and the para-goethite method, and the poor adaptability of raw materials; the hematite method has high investment costs, large steam consumption, and a large amount of gypsum slag.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a two-stage leaching method for wet zinc smelting with improved copper recovery rate, aiming to solve the problem of low recovery rate when copper is recovered by conventional two-stage leaching process in the prior art.

[0006] The technical solution of the present invention is as follows:

[0007] A two-stage leaching method for hydrometallurgical zinc smelting for improving copper recovery rate, specifically comprising the steps of:

[0008] The zinc sulfide concentrate and the returned electric field roasting dust are subjected to fluidized bed roasting in a fluidized bed roasting furnace to obtain zinc roasted ore;

[0009] subjecting the zinc roasted ore to intermediate leaching;

[0010] Then zinc and copper are obtained through the processes of silicon precipitation with iron alum and hot acid leaching.

[0011] The two-stage leaching method for wet zinc smelting with improved copper recovery rate comprises the following steps: the temperature of the fluidized bed roasting is 940-980° C., and the excess air coefficient is between 1.2 and 1.3.

[0012] The two-stage leaching method for wet zinc smelting with improved copper recovery rate, wherein the zinc roasted ore includes roasted sand, boiler roasted dust, and electric field roasted dust.

[0013] In the two-stage leaching method for hydrometallurgical zinc smelting for improving copper recovery rate, the ratio of the roasted sand, boiler roasted dust and electric field roasted dust is 6:3:1.

[0014] The two-stage leaching method for wet zinc smelting with improved copper recovery rate, wherein the amount of insoluble sulfur (Ss) contained in the zinc roasted ore is between 0.4% and 0.6%.

[0015] The two-stage leaching method for wet zinc smelting to improve copper recovery rate, wherein the content of soluble silicon in the zinc roasted ore is less than 2%.

[0016] The two-stage leaching method for hydrometallurgical zinc smelting for improving copper recovery rate, wherein the soluble silicon includes zinc silicate and lead silicate.

[0017] The two-stage leaching method for wet zinc smelting to improve copper recovery rate, wherein the precursor liquid for silicon precipitation by iron alum is the slurry of the intermediate leaching residue and the acid supernatant after hot acid leaching; the precursor liquid for hot acid leaching is the unfiltered silicon precipitation slurry by iron alum.

[0018] The two-stage leaching method for wet zinc smelting to improve copper recovery rate, wherein the reaction temperature of the iron alum precipitation silicon is 85-90°C, the reaction time is 1.5h-2.5h, and the pH is 2.6-3.2.

[0019] The two-stage leaching method for wet zinc smelting with improved copper recovery rate comprises the following steps: the reaction temperature of the hot acid leaching is 80-85°C, the reaction time is 1.5h-2.5h, and the end point acidity is 40-50g / l.

[0020] Beneficial effects: The present invention provides a two-stage leaching method for wet zinc smelting to improve the copper recovery rate, which specifically includes the steps of boiling roasting, one-stage leaching and two-stage leaching, wherein the second-stage leaching includes iron alum precipitation of silicon and hot acid leaching. The present invention controls the amount of insoluble sulfur (Ss) in the zinc roasted ore to between 0.4% and 0.6% through boiling roasting, which not only meets the requirement of improving the copper recovery rate, but also reduces the content of soluble silicon in the zinc roasted ore, and reduces the pressure of subsequent iron alum precipitation of silicon; the two-stage leaching is divided into two steps, and the iron alum is insoluble in acid and the iron alum is positively charged while the silica gel is negatively charged. The iron alum can fix silicon in the iron alum slag through charge adsorption, thereby improving the copper recovery rate, so that the copper recovery rate reaches 70% to 80%, which is 3 to 4 times that of the original process. In addition, the present invention only needs to be modified on the original process flow, and does not need to change the original process flow on a large scale, reducing investment costs and being simple to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1The present invention is a process flow chart of a two-stage leaching method for hydrometallurgical zinc smelting for improving copper recovery rate;

[0022] Figure 2 This is a process flow chart of Example 1 of the present invention. DETAILED DESCRIPTION

[0023] The present invention provides a two-stage leaching method for hydrometallurgical zinc smelting with improved copper recovery rate. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0024] At present, the main method for recovering copper from zinc roasted ore in China is the conventional two-stage leaching method. This method has a short process flow and is relatively simple to operate. However, when using this method to recover copper from zinc roasted ore, the recovery rate of copper is only 20% to 40%, resulting in a large amount of copper being wasted due to ineffective recovery, and also causing serious pollution to the environment.

[0025] Based on this, please refer to the attached Figure 1 The present invention provides a two-stage leaching method for hydrometallurgical zinc smelting for improving copper recovery rate, which specifically comprises the steps of:

[0026] S10, fluidized bed roasting: the zinc sulfide concentrate and the returned electric field roasting dust are subjected to fluidized bed roasting in a fluidized bed roasting furnace to obtain zinc roasted ore;

[0027] S20, primary leaching: subjecting the zinc roasted ore to intermediate leaching;

[0028] S30, two-stage leaching: After the intermediate leaching, zinc and copper are obtained by the processes of silicon precipitation with iron alum and hot acid leaching.

[0029] The present invention utilizes the electric field roasting dust to return to the fluidized bed roasting furnace for re-fluidized bed roasting, thereby ensuring that the amount of insoluble sulfur (Ss) in the zinc roasted ore is controlled between 0.4% and 0.6%, and the fluidized bed roasting is medium-temperature oxidative roasting. The roasting conditions can not only meet the requirement of improving the copper recovery rate, but also reduce the content of soluble silicon in the zinc roasted ore, reduce the pressure of silicon precipitation by iron alum, and ensure the normal liquid-solid separation of each stage; in addition, in order to improve the copper recovery rate, the present invention creates a process of generating iron alum and adsorbing silicon in the existing conventional two-stage leaching process flow - iron alum precipitation silicon, that is, using the properties that iron alum is insoluble in acid and that iron alum carries a positive charge while silica gel carries a negative charge, the iron alum fixes silicon into the iron alum through charge adsorption; that is, the leached iron is converted into iron alum, and the leached silicon is fixed in the iron alum slag at the same time, and finally mixed with the leaching slag and discharged from the leaching system.

[0030] When the zinc sulfide concentrate is fluidized roasted, three types of zinc roasted ores are produced: roasted sand, boiler roasted dust and electric field roasted dust, and the ratio of the roasted sand, boiler roasted dust and electric field roasted dust is 6:3:1. In this embodiment, the electric field roasted dust is returned for re-fluidized roasting because the insoluble sulfur (Ss) in the electric field roasted dust is 2-3 times that of roasted sand and boiler roasted dust; the electric field roasted dust is the smoke produced by the electric dust collector. By returning the electric field roasted dust to the fluidized roasting furnace for re-fluidized roasting, the amount of insoluble sulfur (Ss) in the zinc roasted ore is controlled between 0.4% and 0.6%. While meeting the requirement of improving the copper recovery rate, the content of soluble silicon in the zinc roasted ore is also reduced, thereby reducing the pressure of subsequent iron alum precipitation silicon, which is sufficient to ensure the normal progress of each stage of liquid-solid separation.

[0031] Specifically, the content of soluble silicon in the zinc roasted ore is less than 2%, and the soluble silicon includes but is not limited to zinc silicate, lead silicate and the like.

[0032] In this embodiment, the temperature of the fluidized bed roasting is 940-980°C, and the excess air coefficient is between 1.2 and 1.3. In a preferred embodiment, the temperature of the fluidized bed roasting is 960°C, and the excess air coefficient is 1.25; when the fluidized bed roasting is performed under these parameters, the amount of insoluble sulfur (Ss) in the zinc roasted ore obtained by the fluidized bed roasting can be controlled between 0.4% and 0.6%, and the content of soluble silicon in the zinc roasted ore is less than 2%.

[0033] In the present invention, in order to improve the copper recovery rate, the second stage leaching in the conventional two-stage leaching process is divided into two steps (iron alum precipitation of silicon, hot acid leaching), the purpose of which is to solve the problem of cyclic enrichment of iron and silicon. The original conventional two-stage leaching process cannot improve the acidity of the second stage leaching, and usually controls its end point pH to about 3.0. If the acidity is increased, a large amount of iron and silicon in the zinc roasting ore will be leached and cyclically enriched, which eventually leads to the inability to separate the liquid and solid in each stage; and if the acidity of the second stage leaching is not increased, the leaching rate of copper cannot be increased. Therefore, in order to improve the recovery rate of copper, solving the problem of cyclic enrichment of iron and silicon is the key.

[0034] In this embodiment, the silicon precipitation by iron alum specifically includes the steps of: converting the leached iron into iron alum, controlling the reaction temperature of the silicon precipitation by iron alum to be 85-90°C, the reaction time to be 1.5h-2.5h, and the end point pH to be 2.6-3.2. Preferably, the reaction temperature of the silicon precipitation by iron alum is 85°C, the reaction time is 2h, and the end point pH is 2.6-3.2. Under this condition, the precipitation reaction is easy to occur, and the efficiency of converting iron into iron alum can be improved.

[0035] Specifically, the leached iron is the iron hydroxide or secondary goethite generated by returning to the intermediate leaching process and the iron in the liquid acid supernatant after hot acid leaching; that is, the precursor liquid for the iron alum precipitation of silicon is the slurry of the intermediate leaching residue and the acid supernatant after hot acid leaching.

[0036] In this embodiment, there is no need to add ferrocyanide cations when converting iron into ferrocyanide, and various raw materials in the system will bring in sufficient potassium ions and sodium ions; and ferrocyanide can only occur under acidic conditions. The higher the acidity, the more stringent the ferrocyanide conditions.

[0037] In this embodiment, the hot acid leaching specifically comprises the steps of: increasing the acidity of the slurry of the iron alum precipitated silicon (liquid-solid separation is not required) and continuing leaching, and the reaction temperature of the hot acid leaching is 80-85°C, the reaction time is 1.5h-2.5h, and the end point acidity is 40-50g / l. Preferably, the reaction temperature of the hot acid leaching is 80°C, the reaction time is 2h, and the end point acidity is 40-50g / l.

[0038] Specifically, the precursor solution for hot acid leaching is unfiltered iron alum-precipitated silicon ore slurry.

[0039] In this embodiment, since the iron alum generated in the iron alum silicon precipitation process will not dissolve again in the hot acid leaching process, the acidity is improved while solving the problem of cyclic enrichment of iron and silicon.

[0040] Specifically, when the acidity of the slurry of silicon precipitated by iron alum is increased and leaching is continued, the acidity of the slurry of silicon precipitated by iron alum is increased by adding electrolytic waste liquid.

[0041] In the present invention, the second-stage leaching is divided into two steps. However, since the slurry of iron alum silicon precipitation does not need to be separated into liquid and solid, the slurry enters the hot acid leaching reaction tank through a chute or a pipeline. Therefore, the present invention only needs to modify the original process flow, does not need to change the original process flow on a large scale, saves equipment investment, and the process flow is simple to operate.

[0042] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention.

[0043] Example 1

[0044] like Figure 2As shown, a batch of zinc sulfide concentrate is subjected to fluidized bed roasting according to the fluidized bed roasting process in the two-stage leaching method of wet zinc smelting for improving copper recovery rate described in the present invention to obtain roasted sand, boiler roasted dust and electric field roasted dust; the roasted sand and boiler roasted dust are ball milled to obtain zinc roasted ore, and the components (%) of the output zinc roasted ore are: Zn: 56.54, Fe: 9.13, Cu: 0.7, Pb: 2.12, SiO2: 3.42 (including soluble silicon 1.89%), S: 2.37, Ss: 0.51, Ca: 1.38, Mg: 0.42.

[0045] The temperature of the fluidized bed roasting is 960° C., and the excess air coefficient is 1.25; and a small amount of electric field roasting dust obtained by the fluidized bed roasting is returned to the fluidized bed roasting furnace for re-performing the fluidized bed roasting.

[0046] Preparation of oxidation solution: The acid supernatant after hot acid leaching is mixed with the liquid after other processes and manganese powder to obtain oxidation solution.

[0047] The electrolytic waste liquid (referred to as waste liquid) from the production area was taken, and its composition (g / l) included: Zn: 38.32, H2SO4: 158.26, Na: 6.45.

[0048] The zinc roasted ore is subjected to intermediate leaching (one-stage leaching) by using the oxidizing liquid and the waste liquid, and then the intermediate supernatant obtained after the intermediate leaching is replaced by zinc powder to obtain sponge copper; the intermediate bottom flow obtained after the intermediate leaching is filtered, and the filtrate obtained by filtration is returned to the intermediate leaching process, and the intermediate leaching residue is slurried and treated with the acid supernatant after hot acid leaching through the above-mentioned iron alum silicon precipitation process to obtain iron alum silicon precipitation slurry, and then the unfiltered iron alum silicon precipitation slurry is subjected to hot acid leaching treatment, and finally filtered to obtain the acid supernatant and leaching residue.

[0049] A total of 10 closed-loop leaching tests were carried out according to the two-stage leaching method for wet zinc smelting for improving copper recovery rate of the present invention, and 200g of the above-mentioned zinc roasting ore and 1060ml of the above-mentioned waste liquid (795ml for intermediate leaching and 265ml for hot acid leaching) were put into each cycle.

[0050] The results of the closed-circuit leaching test are:

[0051] Supernatant components (g / l): Zn: 131.67, pH: 4.05 (70°C), Fe: 7.65 mg / l, Cu: 0.89, SiO2: 0.024;

[0052] Acid supernatant composition (g / l): Zn: 101.89, H2SO4: 39.49, Fe: 8.53, Fe 2+ :0.32, Cu: 2.24, SiO2: 0.079;

[0053] Leaching residue composition (%): Zn: 15.81, Fe: 24.15, Cu: 0.43, Pb: 5.61, SiO2: 8.76, S: 7.24, Ca: 3.76, Mg: 0.78;

[0054] Therefore, in Example 1, the slag rate from zinc roasted ore to leached slag is 38.41%, the recovery rates of zinc and copper are 89.26% and 76.41% respectively, the liquid-solid separation in each stage is normal, and there is no phenomenon of cyclic enrichment of iron and silicon.

[0055] In summary, the present invention provides a two-stage leaching method for wet zinc smelting to improve the copper recovery rate, which specifically includes the steps of boiling roasting, one-stage leaching and two-stage leaching, wherein the second-stage leaching includes ferroalloy silicon precipitation and hot acid leaching. The present invention controls the amount of insoluble sulfur (Ss) in the zinc roasted ore to between 0.4% and 0.6% by boiling roasting, which not only meets the requirement of improving the copper recovery rate, but also reduces the content of soluble silicon in the zinc roasted ore, and reduces the pressure of subsequent ferroalloy silicon precipitation; the two-stage leaching is divided into two steps, and the ferroalloy is insoluble in acid and the ferroalloy carries a positive charge while the silica gel carries a negative charge. The ferroalloy can fix silicon in the ferroalloy slag through charge adsorption, thereby improving the copper recovery rate, so that the copper recovery rate reaches 70% to 80%, which is 3 to 4 times that of the original process. In addition, the present invention only needs to be modified on the original process flow, and does not need to change the original process flow on a large scale, reducing investment costs and being simple to operate.

[0056] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A two-stage leaching method for hydrometallurgical zinc smelting to improve copper recovery rate, characterized in that: The specific steps include: The zinc sulfide concentrate and the returned electric field roasting dust are subjected to fluidized bed roasting in a fluidized bed roasting furnace to obtain zinc roasted ore; subjecting the zinc roasted ore to intermediate leaching; Then, zinc and copper are obtained by the processes of silicon precipitation with iron alum and hot acid leaching. The temperature of the fluidized bed roasting is 960°C and the excess air coefficient is 1.25; The zinc roasted ore includes roasted sand, boiler roasted dust, and electric field roasted dust; the ratio of the roasted sand, boiler roasted dust, and electric field roasted dust is 6:3:1; the insoluble sulfur in the electric field roasted dust is 2 to 3 times that of the roasted sand and the boiler roasted dust; The amount of insoluble sulfur (Ss) contained in the zinc roasted ore is between 0.4% and 0.6%; the content of soluble silicon in the zinc roasted ore is less than 2%; the soluble silicon includes zinc silicate and lead silicate; The precursor liquid of the silicon precipitation by iron alum is the acid supernatant after the slurry adjustment of the intermediate leaching residue and the hot acid leaching; the precursor liquid of the hot acid leaching is the unfiltered silicon precipitation by iron alum slurry and the electrolytic waste liquid is added; The reaction temperature of the iron alum precipitation silicon is 85°C, the reaction time is 2h, and the pH is 2.6-3.2; the reaction temperature of the hot acid leaching is 80°C, the reaction time is 2h, and the end point acidity is 40-50g / l.

Citation Information

Patent Citations

  • Method for selectively leaching voluble metal in copper refinery cinder

    CN101619399A