Resist underlayer film material, pattern forming method, and resist underlayer film forming method
By using specific resist underlying film materials and treatment methods in semiconductor manufacturing, the problems of substrate planarization and etch resistance are solved, and high-precision fine pattern processing is achieved, which improves etch selectivity and resolution.
Patent Information
- Application Number
- CN202111402884.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-25
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-11-24
AI Technical Summary
In the manufacturing process of semiconductor devices, especially when pattern size is refined and substrate structure is complicated, it is difficult for existing resist materials to achieve planarization and landfill characteristics, resulting in poor etch selectivity, low resolution, and etch resistance Inadequate, affects processing accuracy and efficiency.
A specific resist underlayer film material is used, which consists of compounds containing specific terminal structures and organic solvents, and forms a hardened film through heat treatment, combining acid generators, surfactants, crosslinking agents and pigments to optimize the Etching characteristics and optical characteristics are suitable for pattern formation in multilayer resist method.
It realizes the formation of a resist lower film with excellent flatness and film formation on wide trenches and high-low difference substrates, improves etch selectivity and resolution, enhances etch resistance and optical performance, and is suitable for high-precision micro pattern processing. .
Smart Images

Figure CN114545733B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resist underlayer film material used for fine patterning by a multilayer resist method in a semiconductor device manufacturing process, a pattern forming method using the material, and a resist underlayer film forming method. Prior art
[0002] With the high integration and high speed of LSI, the miniaturization of pattern size is progressing rapidly. With this miniaturization, photolithography technology has achieved the formation of fine patterns by shortening the wavelength of the light source and appropriately selecting the corresponding resist composition. The center of this is the positive photoresist composition used in a single layer. The single-layer positive photoresist composition forms a pattern by making the resist resin have a skeleton that is etch-resistant to dry etching using chlorine or fluorine gas plasma, and has a switching mechanism such as the exposure part dissolving, so that the exposure part dissolves, and the remaining resist pattern is used as an etching mask to perform dry etching processing on the processed substrate.
[0003] However, when the photoresist film used is miniaturized while maintaining its film thickness, that is, when the pattern width is further reduced, the resolution of the photoresist film is reduced, and when the photoresist film is patterned with a developer, the so-called aspect ratio becomes too large, resulting in pattern collapse. Therefore, as the pattern is miniaturized, the photoresist film is gradually thinned.
[0004] On the other hand, the processing of the processed substrate usually uses a method of processing the substrate by using a photoresist film formed with a pattern as an etching mask and using dry etching, but in reality there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the processed substrate. Therefore, there will be a problem that the resist film is also damaged and collapsed during the processing of the substrate, and the resist pattern cannot be correctly transferred to the processed substrate. Therefore, with the miniaturization of the pattern, the resist composition is gradually seeking higher dry etching resistance. However, on the other hand, in order to improve the resolution, the resin used in the photoresist composition has gradually sought a resin with small light absorption at the exposure wavelength. Therefore, as the exposure light is shortened to i-rays, KrF, and ArF, the resin is gradually changed to a novolac resin, a resin with a polyhydroxystyrene, and an aliphatic polycyclic skeleton, but in reality, the etching speed under the dry etching conditions during substrate processing gradually becomes faster, and the recent photoresist composition with high resolution tends to weaken the etching resistance.
[0005] In view of this situation, it becomes necessary to perform dry etching processing on the substrate to be processed using a thin photoresist film with poor etching resistance, and it is important to ensure the materials and processing in this processing step.
[0006] As one of the methods for solving such a problem, there is a multilayer resist method. In this method, an intermediate film having an etching selectivity different from that of a photoresist film (i.e., a resist upper film) is inserted between the resist upper film and a substrate to be processed, and after the resist upper film has a pattern, the resist upper film pattern is used as a dry etching mask to transfer the pattern to the intermediate film by dry etching, and further, the intermediate film is used as a dry etching mask to transfer the pattern to the substrate to be processed by dry etching.
[0007] As one of the multilayer resist methods, there is a three-layer resist method that can be implemented using a general resist composition used in the single-layer resist method. In the three-layer resist method, for example, an organic film composed of a novolac resin or the like is formed on a processed substrate as a resist lower film, a silicon-containing film is formed thereon as a resist intermediate film, and then a normal organic photoresist film is formed thereon as a resist upper film. When dry etching using fluorine-based gas plasma is performed, the organic resist upper film can achieve a good etching selectivity ratio relative to the silicon-containing resist intermediate film, so the resist upper film pattern can be transferred to the silicon-containing resist intermediate film using dry etching using fluorine-based gas plasma. According to this method, even if a resist composition that is difficult to form a pattern having a sufficient film thickness required for directly processing a substrate to be processed or a resist composition that does not have sufficient dry etching resistance required for processing a substrate is used, the pattern can be transferred to a silicon-containing film (resist intermediate film), and then the pattern transfer is performed by dry etching using oxygen or hydrogen gas plasma, so that a pattern of an organic film (resist underlayer film) composed of a novolac resin or the like having sufficient dry etching resistance required for processing a substrate can be obtained. As for the above-mentioned resist underlayer film, many are already known, such as those described in Patent Document 1.
[0008] On the other hand, in recent years, the manufacture of semiconductor devices with new structures such as multi-gate structures has been actively studied. In response to this, the resist lower film is increasingly required to have better flattening and filling properties than before. For example, when the base substrate to be processed has micro-pattern structures such as holes, trenches, fins, etc., it is necessary to utilize the characteristics of the resist lower film to fill the pattern with a film without gaps. In addition, when the base substrate to be processed has a height difference, when the pattern-dense part and the area without pattern exist on the same wafer, it is necessary to use the resist lower film to flatten the film surface (planarization). By flattening the surface of the lower film, the film thickness variation of the resist intermediate film and the resist upper film formed thereon can be suppressed, and the focal length tolerance of the lithography and the tolerance reduction in the subsequent processing steps of the processed substrate can be suppressed.
[0009] Furthermore, organic film materials with excellent filling / planarization characteristics are not limited to being used as underlayer films for multilayer resists, but can also be widely used as planarization materials for semiconductor device manufacturing, such as substrate planarization before patterning by nanoimprinting. In addition, overall planarization in the semiconductor device manufacturing process is currently generally performed by CMP processing, but CMP is a high-cost process, and materials are expected to be used as an alternative to the overall planarization method.
[0010] In order to form a planarization film for planarizing a semiconductor substrate having uneven surfaces, a resist underlayer film material comprising a compound having a specific structure containing an aromatic portion having a triple bond at the end and a chain ether portion has been proposed (Patent Document 2). However, this material is not sufficient to meet the requirements of the most advanced devices such as planarization performance of wide trench portions in substrates, and a resist underlayer film material having excellent planarity on a wider substrate structure is sought.
[0011] In addition, as the structure of the processed substrate becomes more complicated, some people have studied the surface of the processed substrate and used novel materials with high electron mobility such as strained silicon, gallium arsenide, and ultra-thin film polysilicon controlled in angstroms, etc., and it is expected that films can be formed for a variety of surface shapes and materials of the processed substrate. Therefore, in order to ensure the process tolerance, not only excellent filling and flattening characteristics are important characteristics, but also the ability to form films independently of the material and shape of the processed substrate is also an important characteristic.
[0012] Prior art literature
[0013] Patent Literature
[0014] [Patent Document 1] Japanese Patent Application Publication No. 2004-205685
[0015] [Patent Document 2] Japanese Patent Application Publication No. 2017-119670 Summary of the invention
[0016] Problem that the invention aims to solve
[0017] The present invention is made in view of the above facts, and aims to provide a resist underlayer film material that can form a resist underlayer film with excellent flatness and film-forming properties, and has appropriate etching characteristics and optical characteristics, even on a processed substrate having a portion that is particularly difficult to flatten, such as a wide trench structure, in a fine patterning process using a multilayer resist method in the semiconductor device manufacturing step; and aims to provide a pattern forming method and a resist underlayer film forming method using the material.
[0018] Solutions for solving problems
[0019] In order to solve the above-mentioned problems, the present invention provides a resist underlayer film material, which is a resist underlayer film material used in a multilayer resist method, comprising:
[0020] (A) one or more compounds represented by the following general formula (1); and
[0021] (B) Organic solvent.
[0022] [Chemistry 1]
[0023]
[0024] In the formula, W is an n-valent organic group having 2 to 50 carbon atoms, X is any one of the terminal group structures represented by the following general formula (2) and the following general formula (3), and when the ratios of the structures of the following general formula (2) and the following general formula (3) constituting the aforementioned X are a and b, respectively, the relationship of a+b=1.0, 0.70≤a≤0.99, and 0.01≤b≤0.30 is satisfied. n is an integer of 1 to 10.
[0025] [Chemistry 2]
[0026]
[0027] In the formula, the dotted line represents an atomic bond. Z represents a (k+1)-valent aromatic group having 6 to 20 carbon atoms. A is a single bond or -O-(CH2) p -. k is an integer of 1 to 5. p is an integer of 1 to 10.
[0028] [Chemistry 3]
[0029]
[0030] In the formula, the dotted line represents an atomic bond. L is a single bond or -(CH2) r -. l is 2 or 3, and r is an integer from 1 to 5.
[0031] If such a resist underlayer film material is used, a resist underlayer film having excellent flatness and film-forming properties can be formed even on a substrate having a portion that is particularly difficult to flatten, such as a wide trench structure. Furthermore, if a and b satisfy the above-mentioned relationship, a resist underlayer film having both flatness and film-forming properties can be formed.
[0032] Furthermore, A in the above general formula (2) is preferably -OCH2-.
[0033] According to such a resist underlayer film material, film shrinkage due to thermal curing is suppressed, and a resist underlayer film having excellent flatness can be formed.
[0034] In addition, the general formula (2) is preferably any one of the following formulas (4), (5) and (6).
[0035] [Chemistry 4]
[0036]
[0037] In the formula, the dotted lines represent atomic bonds.
[0038] Such a resist underlayer film material can impart not only the planarization improvement effect due to the suppression of shrinkage but also various properties such as heat resistance and etching resistance, thereby enabling the formation of a resist underlayer film having an excellent process margin.
[0039] In addition, the general formula (3) is preferably any one of the following formulas (7) or (8).
[0040] [Chemistry 5]
[0041]
[0042] In the formula, the dotted lines represent atomic bonds.
[0043] By introducing such a terminal group structure into the resist underlayer film material, not only adhesion to the substrate can be imparted but also film-forming properties can be improved.
[0044] Furthermore, W in the above general formula (1) is preferably represented by the following general formula (9).
[0045] [Chemistry 6]
[0046]
[0047] In the formula, the dotted lines represent atomic bonds. 1 W is a hydrogen atom, or an alkyl group or acyl group having 1 to 20 carbon atoms which may contain an oxygen atom or a nitrogen atom. 1 is an n-valent organic group having 1 to 47 carbon atoms. Y is a single bond or a carbonyl group. n is an integer of 1 to 10.
[0048] Such a resist underlayer film material can form a resist underlayer film regardless of the shape and structure of the substrate, and can form a resist underlayer film having excellent flatness.
[0049] Furthermore, W in the above general formula (9) 1 It is preferably a structure represented by any of the following formulae.
[0050] [Chemistry 7]
[0051]
[0052] [Chemistry 8]
[0053]
[0054] In the formula, the dotted lines represent atomic bonds.
[0055] Such a resist underlayer film material can form a resist underlayer film having excellent film-forming properties and flatness, and can be manufactured particularly easily.
[0056] Furthermore, the organic solvent (B) is preferably a mixture of one or more organic solvents having a boiling point of less than 180 degrees and one or more organic solvents having a boiling point of 180 degrees or more.
[0057] With such a resist underlayer film material, the flatness of the formed resist underlayer film can be improved regardless of the design of the substrate to be processed, such as the density of the pattern.
[0058] Furthermore, the resist underlayer film material of the present invention may further contain one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, (F) a plasticizer, and (G) a dye.
[0059] Thus, the resist underlayer film material of the present invention may also include (C) an acid generator for accelerating hardening, (D) a surfactant for improving coating properties during spin coating, (E) a crosslinking agent for further accelerating crosslinking hardening reaction, (F) a plasticizer for further improving the embedding / planarization properties, and (G) a pigment for adjusting the light absorption properties. The presence or absence / selection of such various additives allows fine adjustment of the required performances such as film-forming properties, hardening properties, embedding properties, and optical properties, which is practically preferable.
[0060] Furthermore, the present invention provides a pattern forming method, which is a method for forming a pattern on a processed substrate, comprising the following steps:
[0061] (I-1) coating the above-mentioned resist underlayer film material on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film;
[0062] (I-2) forming a resist upper film on the resist lower film using a photoresist material;
[0063] (I-3) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film;
[0064] (I-4) using the resist upper layer film having the pattern formed thereon as a mask, and transferring the pattern to the resist lower layer film by dry etching; and
[0065] (I-5) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
[0066] Furthermore, the present invention provides a pattern forming method, which is a method for forming a pattern on a processed substrate, comprising the following steps:
[0067] (II-1) coating the above-mentioned resist underlayer film material on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film;
[0068] (II-2) forming a resist intermediate film on the resist underlayer film;
[0069] (II-3) forming a resist upper film on the resist intermediate film using a photoresist material;
[0070] (II-4) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film;
[0071] (II-5) using the patterned resist upper film as a mask, and transferring the pattern to the resist intermediate film by dry etching;
[0072] (II-6) using the resist intermediate film having the transferred pattern as a mask, transferring the pattern to the resist underlayer film by dry etching; and
[0073] (II-7) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
[0074] Furthermore, the present invention provides a pattern forming method, which is a method for forming a pattern on a processed substrate, comprising the following steps:
[0075] (III-1) coating the above-mentioned resist underlayer film material on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film;
[0076] (III-2) forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film on the resist underlayer film;
[0077] (III-3) forming an organic thin film on the aforementioned inorganic hard mask intermediate film;
[0078] (III-4) forming a resist upper layer film on the aforementioned organic thin film using a photoresist material;
[0079] (III-5) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film;
[0080] (III-6) using the patterned resist upper layer film as a mask, transferring the pattern to the organic thin film and the inorganic hard mask intermediate film by dry etching;
[0081] (III-7) using the inorganic hard mask intermediate film having the transferred pattern as a mask, transferring the pattern to the resist underlayer film by dry etching; and
[0082] (III-8) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
[0083] Thus, the resist lower film material of the present invention can be ideally used in various pattern forming methods such as two-layer resist processing, three-layer resist processing using a resist intermediate film, and four-layer resist processing using an organic thin film. If it is such a pattern forming method, the unevenness and height difference of the processed substrate can be effectively alleviated by forming a resist lower film, which is suitable for optical lithography of the resist upper film.
[0084] Furthermore, in the pattern forming method of the present invention, the substrate to be processed may be a substrate having a structure or a height difference of 30 nm or more.
[0085] The pattern forming method of the present invention uses the resist underlayer film material of the present invention which can form a resist underlayer film having high filling / planarization properties, and is therefore particularly useful for microfabrication of such a substrate having a structure or a step.
[0086] The present invention also provides a method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in the manufacturing steps of a semiconductor device, wherein the resist underlayer film material is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated at a temperature in the range of 100° C. to 600° C. for 10 to 600 seconds to form a cured film.
[0087] The present invention also provides a method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in the manufacturing steps of a semiconductor device, wherein the resist underlayer film material is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated in an environment with an oxygen concentration of not less than 1% and not more than 21%, thereby forming a hardened film.
[0088] By using such a method, the crosslinking reaction during the formation of the resist lower film can be promoted, and the mixing with the upper film can be suppressed to a higher degree. In addition, by appropriately adjusting the heat treatment temperature, time and oxygen concentration within the above range, the filling / planarization characteristics and hardening characteristics of the resist lower film suitable for the application can be obtained.
[0089] The present invention also provides a method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in the manufacturing steps of a semiconductor device, wherein the resist underlayer film material is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated in an environment with an oxygen concentration of less than 1%, thereby forming a hardened film.
[0090] Such a method is useful because it can promote the crosslinking reaction during formation of the resist lower film and suppress mixing with the upper film to a higher degree without causing degradation of the processed substrate even when the processed substrate contains a material that is unstable to heating in an oxygen environment.
[0091] At this time, the substrate to be processed may have a structure with a height of 30 nm or more or a height difference.
[0092] The resist underlayer film forming method of the present invention uses the resist underlayer film material of the present invention which can form a resist underlayer film having high filling / planarization properties, and is therefore particularly suitable for forming a resist underlayer film on such a substrate having a structure or level differences.
[0093] Effects of the Invention
[0094] As described above, the resist underlayer film material, pattern forming method, and resist underlayer film forming method of the present invention can be particularly preferably used in multilayer resist processing including planarization of a processed substrate having height differences and projections and depressions, and are extremely useful in fine patterning for semiconductor device manufacturing. In particular, a resist underlayer film material can be provided, which can form a resist underlayer film having excellent flatness and being able to be formed without substrate dependence, and having appropriate etching characteristics and optical characteristics, even on a processed substrate having a portion that is particularly difficult to planarize, such as a wide trench structure, in a fine patterning process using a multilayer resist method in a semiconductor device manufacturing step; and a pattern forming method and a resist underlayer film forming method using the material can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0095] [ Figure 1 ](A) to (F) are explanatory diagrams of an example of a pattern forming method utilizing a three-layer resist process according to the present invention.
[0096] [ Figure 2 ](G) to (I) are explanatory diagrams of the landfill characteristic evaluation method in the example.
[0097] [ Figure 3 ](J) and (K) are explanatory diagrams of the flattening characteristic evaluation method in the embodiment. DETAILED DESCRIPTION
[0098] As mentioned above, a resist underlayer film material is sought which can form a resist underlayer film having excellent film-forming properties and flatness, and has excellent filling properties, appropriate etching properties, and optical properties, even on a processed substrate having a portion which is particularly difficult to flatten, such as a wide trench structure, in a fine patterning process using a multilayer resist method in the steps of manufacturing a semiconductor device; and a pattern forming method and a resist underlayer film forming method using the material are sought.
[0099] The inventors of the present application have explored various resist underlayer film materials and pattern forming methods in order to achieve high-level embedding / planarization and excellent film-forming properties obtained by underlayer film formation in multilayer lithography using a resist underlayer film. As a result, they have found that a resist underlayer film material having a compound combined with a specific terminal structure as a main component, a pattern forming method using the material, and a resist underlayer film forming method are very effective, and have completed the present invention.
[0100] That is, the present invention is a resist underlayer film material, which is a resist underlayer film material used in a multilayer resist method, comprising:
[0101] (A) one or more compounds represented by the following general formula (1); and
[0102] (B) Organic solvent.
[0103] [Chemistry 9]
[0104]
[0105] In the formula, W is an n-valent organic group having 2 to 50 carbon atoms, X is any one of the terminal group structures represented by the following general formula (2) and the following general formula (3), and when the ratios of the structures of the following general formula (2) and the following general formula (3) constituting the aforementioned X are a and b, respectively, the relationship of a+b=1.0, 0.70≤a≤0.99, and 0.01≤b≤0.30 is satisfied. n is an integer of 1 to 10.
[0106] [Chemistry 10]
[0107]
[0108] In the formula, the dotted line represents an atomic bond. Z represents a (k+1)-valent aromatic group having 6 to 20 carbon atoms. A is a single bond or -O-(CH2) p -. k is an integer of 1 to 5. p is an integer of 1 to 10.
[0109] [Chemistry 11]
[0110]
[0111] In the formula, the dotted line represents an atomic bond. L is a single bond or -(CH2) r -. l is 2 or 3, and r is an integer from 1 to 5.
[0112] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0113] <Resist Underlayer Film Materials>
[0114] The resist underlayer film material of the present invention is a resist underlayer film material used in the multilayer resist method as described above, comprising:
[0115] (A) one or more compounds represented by the following general formula (1); and
[0116] (B) Organic solvent.
[0117] [Chemistry 12]
[0118]
[0119] In the formula, W is an n-valent organic group having 2 to 50 carbon atoms, X is any one of the terminal group structures represented by the following general formula (2) and the following general formula (3), and when the ratios of the structures of the following general formula (2) and the following general formula (3) constituting the aforementioned X are a and b, respectively, the relationship of a+b=1.0, 0.70≤a≤0.99, and 0.01≤b≤0.30 is satisfied. n is an integer of 1 to 10.
[0120] [Chemistry 13]
[0121]
[0122] In the formula, the dotted line represents an atomic bond. Z represents a (k+1)-valent aromatic group having 6 to 20 carbon atoms. A is a single bond or -O-(CH2) p -. k is an integer of 1 to 5. p is an integer of 1 to 10.
[0123] [Chemistry 14]
[0124]
[0125] In the formula, the dotted line represents an atomic bond. L is a single bond or -(CH2) r -. l is 2 or 3, and r is an integer from 1 to 5.
[0126] [(A) one or more compounds represented by the general formula (1)]
[0127] It is believed that the resist underlayer film material of the present invention has excellent fluidity and substrate affinity due to the compound represented by the above-mentioned general formula (1). Therefore, even on a processed substrate having a portion that is particularly difficult to flatten, such as a wide trench structure, a resist underlayer film with excellent flatness can be formed, and the resist underlayer film also has excellent film-forming properties on a processed substrate having a complex fine structure and various surface materials.
[0128] In the above general formula (2), the dotted line represents an atomic bond. Z represents a (k+1)-valent aromatic group having 6 to 20 carbon atoms. Z is a (k+1)-valent group having a structure obtained by removing (k+1) hydrogen atoms from an aromatic compound having 6 to 20 carbon atoms. Examples of the aromatic compound having 6 to 20 carbon atoms in this case include benzene, naphthalene, phenanthrene, anthracene, pyrene, biphenyl, toluene, xylene, methylnaphthalene, fluorene, etc., and benzene and naphthalene are preferably used from the viewpoint of imparting thermal fluidity and ease of obtaining raw materials. k is an integer of 1 to 5, and in order to obtain good flatness, k is preferably 1 to 3. A is a single bond, or -O-(CH2) p -, p is an integer from 1 to 10, and in order to obtain good flatness, -OCH2- where p=1 is preferred.
[0129] Preferred structures of the general formula (2) are as follows.
[0130] [Chemistry 15]
[0131]
[0132] Particularly preferred structures of the general formula (2) include the following formulas (4) to (6).
[0133] [Chemistry 16]
[0134]
[0135] In the resist underlayer film material of the present invention, the terminal group structure of the general formula (2) functions as a heat curing group. When the substituent A satisfies the relationship of p=1 and is located at the β position of naphthalene, as in the formulas (4) to (6) exemplified as particularly preferred structures, it is presumed that the mechanism of heat curing is carried out via the ring structure shown in the following reaction formula. In this case, it functions as a substituent that imparts thermal fluidity before curing, and a curing reaction occurs via the rigid ring structure during curing, so that the opposite characteristics of thermal fluidity and heat resistance can be taken into account.
[0136] [Chemistry 17]
[0137]
[0138] In the above general formula (3), the dotted line represents an atomic bond. L represents a single bond or -(CH2) r- is preferably a single bond or r = 1. l is 2 or 3, and l is preferably 2 from the viewpoint of imparting close adhesion.
[0139] Preferred structures of the general formula (3) are as follows.
[0140] [Chemistry 18]
[0141]
[0142] Particularly preferred structures of the general formula (3) are shown by the following formulas (7) and (8).
[0143] [Chemistry 19]
[0144]
[0145] In the resist underlayer film material of the present invention, the terminal group structure of the general formula (3) functions as an adhesion group and a film-forming auxiliary group. When the terminal structure of the catechol type of the formula (7) and (8) is present as particularly preferred structures, the affinity with the substrate is improved, thereby exhibiting good flatness, and the adhesion to the substrate is improved, thereby preventing the film from being unevenly coated and peeling off from the substrate during film formation.
[0146] In addition, when the ratios of the terminal group structures of the above general formulas (2) and (3) constituting the terminal group X in the above general formula (1) are a and b, respectively, the relationship a+b=1.0, 0.70≤a≤0.99, 0.01≤b≤0.30 (when a+b=100, 70≤a≤99, 1≤b≤30) must be satisfied. More preferably, 0.75≤a≤0.97, 0.03≤b≤0.25, and particularly preferably, 0.80≤a≤0.95, 0.05≤b≤0.20. If the terminal ratio is not adjusted to the above range, it is impossible to achieve both flatness and film-forming properties while maintaining thermal curability. The terminal group ratio can be calculated using 1H NMR as a triple bond-containing terminal group / a phenolic hydroxyl-containing terminal group.
[0147] In the above general formula (1), W is an n-valent organic group having 2 to 50 carbon atoms, and W is a monovalent to decavalent organic group having a structure obtained by removing 1 to 10 hydrogen atoms from an organic compound having 2 to 50 carbon atoms. The compound having an organic group W having 2 to 50 carbon atoms having a structure obtained by adding 1 to 10 hydrogen atoms to W has at least one of the terminal structures represented by the above general formulas (2) and (3), and the organic group represented by W may also contain a linear, branched or cyclic saturated or unsaturated hydrocarbon group, an aromatic group, a heteroaromatic group, an ether group, a hydroxyl group, an ester group, a ketone group, an amino group, a halogen group, a thioether group, a carboxyl group, a sulfonic acid group, an imide group, a cyano group, an aldehyde group, an imino group, a urea group, a carbamate group, a carbonate group, a nitro group, a sulfone group, etc. In consideration of both good flatness and sufficient heat curability, n is preferably 2 to 4.
[0148] By appropriately selecting W, X and n in the compound of the general formula (1) according to the application, the etching resistance, heat resistance, optical properties, polarity, flexibility and other properties of the resist underlayer film material can be adjusted. Among them, in terms of optical properties, when the resist underlayer film material has appropriate optical properties at a wavelength of 193nm, it is possible to suppress reflected light during exposure in multilayer ArF lithography and to produce a material with excellent resolution. In addition, in order to suppress reflected light, the optical constants of the resist underlayer film material are preferably in the range of a refractive index n of about 1.4 to 1.9 and an attenuation coefficient k of about 0.1 to 0.5.
[0149] In addition, W in the above general formula (1) is preferably a structure represented by the following general formula (9).
[0150] [Chemistry 20]
[0151]
[0152] In the formula, the dotted lines represent atomic bonds. 1 W is a hydrogen atom, or an alkyl group or acyl group having 1 to 20 carbon atoms which may contain an oxygen atom or a nitrogen atom. 1 is an n-valent organic group having 1 to 47 carbon atoms. Y is a single bond or a carbonyl group. n is an integer of 1 to 10.
[0153] Since W in the above general formula has the partial structure represented by the above general formula (9), the resist underlayer film material of the present invention has improved affinity with a substrate to be processed and can be provided with thermal fluidity, thereby providing good flatness.
[0154] In the above general formula (9), R 1Examples include a hydrogen atom, a methyl group, a methoxymethyl group, a 1-ethoxyethyl group, a 1-(2-ethylhexyloxy)ethyl group, a 2-tetrahydropyranyl group, an allyl group, a benzyl group, a propargyl group, a formyl group, an acetyl group, a propionyl group, a butyryl group, a hexanoyl group, an eicosanoyl group, an acryloyl group, a methacryloyl group, a propioloyl group, a methoxyacetyl group, a benzoyl group, a 4-acetamidobenzoyl group, a carbamoyl group, an N-methylcarbamoyl group, an N,N-dimethylcarbamoyl group, and the like. Among them, a hydrogen atom, an acetyl group, and an acryloyl group are preferred, and a hydrogen atom is particularly preferred.
[0155] In the above general formula (9), Y represents a single bond or a carbonyl group, and Y is more preferably a carbonyl group.
[0156] W in the above general formula (9) 1 W is an n-valent organic group having 1 to 47 carbon atoms. 1 The organic group having 1 to 47 carbon atoms may also contain a linear, branched or cyclic saturated or unsaturated hydrocarbon group, an aromatic group, a heteroaromatic group, an ether group, a hydroxyl group, an ester group, a ketone group, an amino group, a halogen group, a thioether group, a carboxyl group, a sulfonic acid group, an imide group, a cyano group, an aldehyde group, an imino group, a urea group, a carbamate group, a carbonate group, a nitro group, or a sulfone group. n is an integer of 1 to 10, and in consideration of both good flatness and sufficient thermal curability, n is preferably 2 to 4.
[0157] W in the above general formula (9) 1 The structure of the following formula and the like can be preferably exemplified.
[0158] [Chemistry 21]
[0159]
[0160] [Chemistry 22]
[0161]
[0162] In the formula, the dotted lines represent atomic bonds.
[0163] R is appropriately selected according to the required performance and application of the present invention. 1 , W 1 , Y, n, can adjust the etching resistance, heat resistance, optical constants, polarity, flexibility, hardenability and other properties.
[0164] In the present invention, the compound of the general formula (1) may be used alone or in combination of two or more. In addition, the compound may be used in the form of a mixture containing the compound represented by the general formula (1). When used in the form of a mixture, the compound represented by the general formula (1) preferably accounts for 10% by mass or more, and more preferably 20% by mass or more, of the total solid content of the resist underlayer film material excluding the solvent. When it is 10% by mass or more, a sufficient blending effect can be obtained. The formula weight of the compound of the general formula (1) is preferably 300 to 3,000, and particularly preferably 500 to 2,500. When the molecular weight is 300 or more, the film-forming property is excellent, and there is no contamination of the device due to the increase of sublimates during curing. When the molecular weight is 3,000 or less, the flattening / filling characteristics are excellent. In addition, in the present invention, the molecular weight may be a weight average molecular weight (Mw) calculated as polystyrene obtained by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent.
[0165] Such a resist underlayer film material can form a resist underlayer film having excellent flatness and can be manufactured particularly easily.
[0166] In the resist underlayer film material of the present invention, in addition to the compound represented by the above general formula (1), other substances may also be blended. The blending substance is mixed with the compound represented by the above general formula (1) to improve the film-forming property of spin coating and the filling property of substrates with height differences. There is no particular limitation on the substance that can be mixed at this time, and known substances can be used. Specifically, acrylic resins, styrene resins, phenolic resins, polyether resins, epoxy resins, and compounds having phenolic hydroxyl groups are preferred. The blending amount of the above blending substance is preferably 1 to 100 parts by mass, and more preferably 2 to 50 parts by mass, relative to 100 parts by mass of the compound represented by the above general formula (1).
[0167] [(B) Organic solvent]
[0168] The (B) organic solvent that can be used in the resist underlayer film material of the present invention is not particularly limited as long as it can dissolve (A) one or more of the compounds represented by the above-mentioned general formula (1), and is preferably one that can also dissolve the (C) acid generator, (D) surfactant, (E) crosslinking agent, (F) plasticizer, and (G) pigment described later.
[0169] Specifically, the solvents described in paragraphs
[0091] to
[0092] of Japanese Patent Application Laid-Open No. 2007-199653 may be added. More specifically, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, cyclopentanone, cyclohexanone and γ-butyrolactone, or a mixture containing one or more of these may be preferably used.
[0170] The amount of the organic solvent blended is appropriately adjusted according to the desired film thickness of the resist underlayer film, and is usually in the range of 100 to 50,000 parts by mass based on 100 parts by mass of the compound of the general formula (1).
[0171] In the resist underlayer film material of the present invention, the organic solvent (B) is preferably a mixture of one or more organic solvents having a boiling point of less than 180 degrees and one or more organic solvents having a boiling point of 180 degrees or more (hereinafter also referred to as "high boiling point solvents").
[0172] Specific examples of the organic solvent having a boiling point of less than 180 degrees include propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, cyclopentanone, and cyclohexanone.
[0173] The organic solvent with a boiling point of 180 degrees or more is not limited to hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc. as long as it can dissolve the components of the resist underlayer film material of the present invention. Specific examples include: 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, 2-ethyl-1, 3-Hexanediol, Diethylene Glycol, Dipropylene Glycol, Triethylene Glycol, Tripropylene Glycol, Glycerol, Nonyl Acetate, Monohexyl Ether, Ethylene Glycol Mono-2-ethylhexyl Ether, Ethylene Glycol Monophenyl Ether, Ethylene Glycol Monobenzyl Ether, Diethylene Glycol Monoethyl Ether, Diethylene Glycol Monoisopropyl Ether, Diethylene Glycol Mono-n-butyl Ether, Diethylene Glycol Monoisobutyl Ether, Diethylene Glycol Monohexyl Ether, Diethylene Glycol Monophenyl Ether, Diethylene Glycol Monobenzyl Ether, Diethylene Glycol Diethyl Ether, Diethylene Glycol Dibutyl Ether, Diethylene Glycol Butyl Methyl Ether, Triethylene Glycol Dimethyl Ether, Triethylene Glycol Monomethyl ether, triethylene glycol-n-butyl ether, triethylene glycol butyl methyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol diacetate, dipropylene glycol Diol methyl-n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, 1,6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, dibutyl adipate, etc., which can be used alone or in combination.
[0174] The organic solvent with a boiling point of more than 180 degrees can be appropriately selected from, for example, the above-mentioned ones according to the temperature at which the resist lower film material of the present invention is heat-treated. The boiling point of the organic solvent with a boiling point of more than 180 degrees is preferably 180°C to 300°C, and is more preferably 200°C to 300°C. It is believed that if it is such a boiling point, there will be no risk of volatilization too fast during baking (heat treatment) due to too low a boiling point, so sufficient thermal fluidity can be obtained during film formation, and a resist lower film with excellent filling / planarization characteristics can be formed. In addition, if it is such a boiling point, there will be no situation where it does not volatilize after baking due to too high a boiling point and remains in the film, so there will be no risk of adversely affecting the film properties such as etching resistance.
[0175] In addition, the blending amount when using an organic solvent having a boiling point of 180 degrees or more is preferably 1 to 30 parts by mass relative to 100 parts by mass of the organic solvent having a boiling point of less than 180 degrees. If it is such a blending amount, there will be no risk of not being able to impart sufficient thermal fluidity during baking due to too little blending amount, or of remaining in the film due to too much blending amount, resulting in the risk of deterioration of film properties such as etching resistance, which is preferred.
[0176] [(C) Acid generator]
[0177] The resist underlayer film material of the present invention may further promote the curing reaction by adding (C) an acid generator. Acid generators may generate acid by thermal decomposition or by light irradiation, and may be added. Specifically, materials described in paragraphs
[0061] to
[0085] of Japanese Patent Application Publication No. 2007-199653 may be added, but the invention is not limited thereto.
[0178] The acid generator may be used alone or in combination of two or more. The amount of the acid generator added is preferably 0.05 to 50 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the compound represented by the general formula (1).
[0179] [(D) Surfactant]
[0180] In the resist underlayer film material of the present invention, a surfactant (D) may be added to improve the coating properties during spin coating. As the surfactant, for example, those described in
[0142] to
[0147] in Japanese Patent Publication No. 2009-269953 may be used. The amount of the surfactant added is preferably 0.001 to 20 parts by mass, more preferably 0.01 to 10 parts by mass, relative to 100 parts by mass of the compound represented by the general formula (1).
[0181] [(E) Cross-linking agent]
[0182] In addition, in the resist lower film material of the present invention, in order to improve the curability and further inhibit the cross-mixing with the upper film, a (E) crosslinking agent may also be added. The crosslinking agent is not particularly limited, and various known systems of crosslinking agents can be widely used. As an example, melamine-based crosslinking agents, glycoluril-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, epoxy-based crosslinking agents, and phenol-based crosslinking agents (such as hydroxymethyl or alkoxymethyl-type crosslinking agents of polynuclear phenols) can be exemplified. The amount of the crosslinking agent added is preferably 1 to 50 parts by mass, and more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the compound represented by the general formula (1).
[0183] As melamine-based crosslinking agents, specifically, hexamethoxymethylated melamine, hexabutoxymethylated melamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. As glycoluril-based crosslinking agents, specifically, tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. As benzoguanamine-based crosslinking agents, specifically, tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. As urea-based crosslinking agents, specifically, dimethoxymethylated dimethoxyethylene urea, its alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. As β-hydroxyalkylamide-based crosslinking agents, specifically, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide can be exemplified. Specific examples of isocyanurate crosslinking agents include triglycidyl isocyanurate and triallyl isocyanurate. Specific examples of aziridine crosslinking agents include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of the oxazoline crosslinking agent include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers. Specific examples of the epoxy crosslinking agent include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0184] Specific examples of the polynuclear phenol crosslinking agent include compounds represented by the following general formula (10).
[0185] [Chemistry 23]
[0186]
[0187] In the formula, Q is a single bond or a q-valent hydrocarbon group having 1 to 20 carbon atoms. 2 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. q is an integer of 1 to 5.
[0188] Q is a single bond or a q-valent hydrocarbon group having 1 to 20 carbon atoms. q is an integer of 1 to 5, preferably 2 or 3. Specific examples of Q include groups obtained by removing q hydrogen atoms from methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, and eicosane. R 2 It is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, isopentyl, hexyl, octyl, ethylhexyl, decyl, and eicosyl, and it is preferably a hydrogen atom or a methyl group.
[0189] As examples of the compound represented by the general formula (10), specifically, the following compounds can be exemplified. Among them, from the viewpoint of improving the hardening property and film thickness uniformity of the resist underlayer film, hexamethoxymethylated products of trisphenolmethane, trisphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred.
[0190] [Chemistry 24]
[0191]
[0192] [Chemistry 25]
[0193]
[0194] In the formula, R 2 Same as above.
[0195] [(F) Plasticizer]
[0196] In addition, in the resist underlayer film material of the present invention, a plasticizer (F) may be added to further improve the planarization / burying characteristics. The plasticizer is not particularly limited, and plasticizers of various known systems can be widely used. As an example, low molecular weight compounds such as phthalates, adipic acid esters, phosphates, trimellitic acid esters, and citrates, and polymers such as polyethers, polyesters, and polyacetal polymers described in Japanese Patent Application Laid-Open No. 2013-253227 can be illustrated. The amount of the plasticizer added is preferably 5 to 500 parts by mass, and more preferably 10 to 200 parts by mass, relative to 100 parts by mass of the compound represented by the general formula (1).
[0197] [(G) Pigment]
[0198] In addition, in the resist lower film material of the present invention, a pigment (G) may be added in order to further improve the resolution during patterning of multilayer lithography. The pigment is not particularly limited as long as it is a compound having moderate absorption at the exposure wavelength, and various known compounds can be widely used. As an example, benzene, naphthalene, anthracene, phenanthrene, pyrene, isocyanuric acid, and triazine can be illustrated. The amount of the pigment added is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the compound represented by the general formula (1).
[0199] <Pattern Formation Method>
[0200] Furthermore, the present invention provides a pattern forming method (two-layer resist processing), which is a method for forming a pattern on a processed substrate, comprising the following steps:
[0201] (I-1) coating the above-mentioned resist underlayer film material on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film;
[0202] (I-2) forming a resist upper film on the resist lower film using a photoresist material;
[0203] (I-3) exposing the resist upper layer film to a pattern, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film;
[0204] (I-4) using the patterned resist upper film as a mask, transferring the pattern to the resist lower film by dry etching; and
[0205] (I-5) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
[0206] In addition, the present invention provides a pattern forming method (three-layer resist processing), which is a method for forming a pattern on a processed substrate, comprising the following steps:
[0207] (II-1) coating the above-mentioned resist underlayer film material on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film;
[0208] (II-2) forming a resist intermediate film on the resist underlayer film;
[0209] (II-3) forming a resist upper film on the resist intermediate film using a photoresist material;
[0210] (II-4) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film;
[0211] (II-5) using the patterned resist upper film as a mask, and transferring the pattern to the resist intermediate film by dry etching;
[0212] (II-6) using the resist intermediate film having the transferred pattern as a mask, transferring the pattern to the resist underlayer film by dry etching; and
[0213] (II-7) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
[0214] In addition, a pattern forming method (four-layer resist processing) is provided, which is a method for forming a pattern on a processed substrate, comprising the following steps:
[0215] (III-1) coating the above-mentioned resist underlayer film material on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film;
[0216] (III-2) forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film on the above-mentioned resist underlayer film;
[0217] (III-3) forming an organic thin film on the inorganic hard mask intermediate film;
[0218] (III-4) forming a resist upper film on the organic thin film using a photoresist material;
[0219] (III-5) exposing the resist upper layer film to a pattern, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film;
[0220] (III-6) using the patterned resist upper layer film as a mask, and transferring the pattern to the organic thin film and the inorganic hard mask intermediate film by dry etching;
[0221] (III-7) using the inorganic hard mask intermediate film having the transferred pattern as a mask, transferring the pattern to the resist underlayer film by dry etching; and
[0222] (III-8) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
[0223] The thickness of the resist lower film used in the present invention can be appropriately selected, and is preferably 2 to 20,000 nm, and particularly preferably 50 to 15,000 nm. In the case of a three-layer resist lower film, a silicon-containing resist intermediate film and a silicon-free resist upper film can be formed thereon. In the case of a two-layer resist lower film, a silicon-containing resist upper film or a silicon-free resist upper film can be formed thereon.
[0224] The pattern forming method of the present invention can be ideally used for multilayer resist processing such as a two-layer resist processing containing silicon, a three-layer resist processing using a silicon-containing intermediate layer film, a four-layer resist processing using a silicon-containing intermediate layer film and an organic film, and a two-layer resist processing not containing silicon.
[0225] [3-layer resist processing]
[0226] The pattern forming method of the present invention is described below by taking a three-layer resist process as an example, but is not limited to this process. In this case, the resist lower film can be formed on the substrate using the above-mentioned resist lower film material, the resist middle film material containing silicon atoms can be used on the resist lower film to form a resist middle film, and the resist upper film material of the photoresist composition can be used on the resist middle film to form a resist upper film, thereby forming a multilayer resist film, exposing the pattern circuit area of the above-mentioned resist upper film, and then developing it with a developer to form a resist pattern on the resist upper film, using the resist upper film with the pattern as a mask to etch the resist middle film, using the resist middle film with the pattern as a mask to etch the resist lower film, and further, using the resist lower film with the pattern as a mask, processing the substrate to form a pattern on the substrate.
[0227] The resist interlayer film containing silicon atoms exhibits etching resistance to oxygen or hydrogen gas. Therefore, as described above, etching of the resist underlayer film using the resist interlayer film as a mask is preferably performed using an etching gas mainly containing oxygen or hydrogen gas.
[0228] Furthermore, in the pattern forming method of the present invention, the above-mentioned resist underlayer film material can be used at least on a substrate to form a resist underlayer film, an inorganic hard mask intermediate film selected from silicon oxide film, silicon nitride film and silicon oxide nitride film is formed on the resist underlayer film, and a resist upper layer film material composed of a photoresist composition is used on the inorganic hard mask intermediate film to form a resist upper layer film, after exposing the pattern circuit area of the above-mentioned resist upper layer film, it is developed with a developer to form a resist pattern on the above-mentioned resist upper layer film, the obtained resist pattern is used as an etching mask, the above-mentioned inorganic hard mask intermediate film is etched, the obtained inorganic hard mask intermediate film pattern is used as an etching mask, the above-mentioned resist underlayer film is etched, the obtained resist underlayer film pattern is used as a mask, and the substrate is processed to form a pattern on the substrate.
[0229] As described above, when an inorganic hard mask intermediate layer film is formed on the resist lower layer film, a silicon oxide film, a silicon nitride film, or a silicon oxide nitride film (SiON film) is formed by a CVD method, an ALD method, or the like. The method for forming a nitride film is described in Japanese Patent Application Publication No. 2002-334869 and WO2004 / 066377. The film thickness of the inorganic hard mask is 5 to 200 nm, preferably 10 to 100 nm. Among them, a SiON film having a high effect as an antireflection film is most preferably used for ArF exposure.
[0230] For the silicon-containing resist intermediate film in the three-layer resist treatment, a polysilsesquioxane-based intermediate film can be preferably used. The polysilsesquioxane-based intermediate film is easy to have an anti-reflection effect in excimer exposure, thereby suppressing the reflected light when the pattern of the resist upper film is exposed, and has the advantage of excellent resolution. In particular, if a material containing many aromatic groups is used as a resist lower film for 193nm exposure, the k value will become higher and the substrate reflection will increase, but the reflection can be suppressed by the resist intermediate film, and the substrate reflection can be reduced to less than 0.5%. As a resist intermediate film with an anti-reflection effect, for 248nm and 157nm exposure, it is preferable to use a polysilsesquioxane with anthracene pendant and cross-linked by acid or heat, and for 193nm exposure, it is preferable to use a polysilsesquioxane with phenyl pendant or light-absorbing groups with silicon-silicon bonds and cross-linked by acid or heat.
[0231] In this case, forming the resist intermediate layer film containing silicon by spin coating is simpler and has a cost advantage than by CVD.
[0232] The resist upper film in the three-layer resist film can be positive or negative, and can use the same photoresist composition as commonly used. When the resist upper film is formed using the above-mentioned photoresist composition, it is preferable to use a spin coating method, as in the case of forming the above-mentioned resist lower film. After spin coating the photoresist composition, pre-bake it, preferably at 60 to 180°C for 10 to 300 seconds. Afterwards, expose it according to the usual method, and perform post-exposure baking (PEB) and development to obtain a resist pattern. In addition, the thickness of the resist upper film is not particularly limited, and is preferably 30 to 500 nm, and particularly preferably 50 to 400 nm.
[0233] Examples of the exposure light include high energy rays having a wavelength of 300 nm or less, and specifically, excimer lasers of 248 nm, 193 nm, and 157 nm, and soft X-rays, electron beams, and X-rays of 3 to 20 nm.
[0234] Then, the obtained resist pattern is used as a mask for etching. The etching of the resist intermediate layer film in the three-layer process is performed using a fluorine-based gas and the resist pattern as a mask. Then, the resist lower layer film is etched using oxygen or hydrogen gas using the resist intermediate layer film pattern as a mask.
[0235] The subsequent etching of the processed substrate can also be carried out according to the conventional method. For example, if the substrate is SiO2, SiN, or a silicon dioxide-based low dielectric insulating film, etching is performed mainly using a fluorine-based gas. If it is p-Si, Al, or W, etching is performed mainly using a chlorine-based or bromine-based gas. When the substrate is processed by etching using a fluorine-based gas, the silicon-containing intermediate layer of the three-layer processing will be stripped off at the same time as the substrate is processed. When etching the substrate using a chlorine-based or bromine-based gas, the stripping of the silicon-containing intermediate layer needs to be performed separately after the substrate is processed by dry etching stripping using a fluorine-based gas.
[0236] In addition, as for the processed substrate, a processed layer is formed on the substrate. The substrate is not particularly limited, and a material different from the processed layer can be used, such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, etc. The processed layer can be various Low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, TiN, W-Si, Al, Cu, Al-Si, and barrier films thereof, and is usually formed to a thickness of 50 to 10,000 nm, especially 100 to 5,000 nm.
[0237] The pattern forming method of the present invention is also suitable for processing a structure having a height of 30 nm or more or a height difference substrate such as a height difference. By forming the resist lower layer film of the present invention on the height difference substrate, and performing filling and flattening, the film thickness of the resist intermediate film and the resist upper layer film formed later can be made uniform, so it is easy to ensure the exposure depth tolerance (DOF) during optical lithography, which is very ideal.
[0238] For an example of 3-layer resist processing, using Figure 1 The details are as follows. When the 3-layer resist is processed, Figure 1 As shown in (A), after a resist lower layer film 3 is formed on a processing layer 2 stacked on a substrate 1, a resist intermediate layer film 4 is formed, and a resist upper layer film 5 is formed thereon.
[0239] Then, if Figure 1 As shown in (B), the used portion 6 of the resist upper film is exposed, and PEB (post-exposure baking) and development are performed to form a resist upper film pattern 5a ( Figure 1 (C)). The obtained resist upper film pattern 5a is used as a mask, and the resist intermediate film 4 is etched using CF-based gas to form a resist intermediate film pattern 4a ( Figure 1 (D)). After removing the resist upper film pattern 5a, the obtained resist intermediate film pattern 4a is used as a mask to perform oxygen or hydrogen plasma etching on the resist lower film 3 to form a resist lower film pattern 3a ( Figure 1 (E)). After removing the resist intermediate film pattern 4a, the resist lower film pattern 3a is used as a mask to etch the processed layer 2 to form a pattern 2a ( Figure 1 (F)).
[0240] When an inorganic hard mask interlayer film is used, the resist interlayer film 4 is an inorganic hard mask interlayer film, and when an organic thin film is applied, an organic thin film layer is provided between the resist interlayer film 4 and the resist upper film 5. The etching of the organic thin film may be performed continuously before the etching of the resist interlayer film 4, or the etching of the resist interlayer film 4 may be performed after only the etching of the organic thin film is performed, and then the etching device is changed or the like.
[0241] [4-layer resist processing]
[0242] Furthermore, the present invention is also ideally applicable to a four-layer resist process using an organic thin film, in which case, at least the resist underlayer film material is used on a substrate to form a resist underlayer film, an inorganic hard mask intermediate film selected from silicon oxide film, silicon nitride film and silicon oxide nitride film is formed on the resist underlayer film, an organic thin film is formed on the inorganic hard mask intermediate film, a resist upper film is formed on the organic thin film using a resist upper film material composed of a photoresist composition, the pattern circuit area of the resist upper film is exposed, and then developed using a developer to form a resist pattern on the resist upper film, the obtained resist pattern is used as an etching mask, the organic thin film and the inorganic hard mask intermediate film are etched, the obtained inorganic hard mask intermediate film pattern is used as an etching mask, the resist underlayer film is etched, the obtained resist underlayer film pattern is used as a mask, and the substrate is processed to form a pattern on the substrate.
[0243] A photoresist film can be formed on the resist intermediate film as a resist upper film, or an organic thin film can be formed on the resist intermediate film by spin coating as described above, and a photoresist film can be formed thereon. When a SiON film is used as the resist intermediate film and an organic antireflection film (BARC) having a light-absorbing group at the exposure wavelength is used as the organic thin film, the two layers of antireflection films of the SiON film and the organic thin film can suppress reflection in the immersion exposure with a high NA exceeding 1.0 during the excimer exposure. Other advantages of forming an organic thin film include the effect of reducing the tailing of the photoresist pattern directly above the SiON film. In addition, when a close contact film (ADL) having excellent affinity with the upper photoresist is used as the organic thin film, it also has the advantage of suppressing the pattern collapse of the photoresist.
[0244] <Resist Underlayer Film Formation Method>
[0245] The present invention provides a method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in the manufacturing steps of a semiconductor device, wherein the resist underlayer film material is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated at a temperature in the range of 100° C. to 600° C. for 10 to 600 seconds to form a cured film.
[0246] In addition, a method for forming a resist underlayer film is provided, which is a method for forming a resist underlayer film that functions as an organic flat film used in the manufacturing steps of a semiconductor device, wherein the resist underlayer film material is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated in an environment with an oxygen concentration of not less than 1% and not more than 21%, thereby forming a hardened film.
[0247] Or a method for forming a resist underlayer film is provided, which is a method for forming a resist underlayer film that functions as an organic flat film used in the manufacturing steps of a semiconductor device, wherein the resist underlayer film material is spin-coated on a processed substrate, and the substrate coated with the resist underlayer film material is heat-treated in an environment with an oxygen concentration of less than 1%, thereby forming a hardened film.
[0248] In the resist lower film forming method of the present invention, the resist lower film material is applied to the processed substrate by spin coating or the like. By using the spin coating method or the like, good embedding characteristics can be obtained. After spin coating, baking is performed to evaporate the solvent, prevent mixing with the resist upper film and the resist intermediate film, and promote the crosslinking reaction. Baking is performed in a temperature range of 100°C to 600°C, preferably 100°C to 300°C, and more preferably 150°C to 280°C, and for 10 seconds to 600 seconds, preferably 10 to 300 seconds. By appropriately adjusting the baking temperature and time within the above range, flattening, embedding characteristics, and curing characteristics suitable for the application can be obtained. If the baking temperature is above 100°C, the curing will be fully carried out and mixing with the upper film or the intermediate film will not occur. If the baking temperature is below 600°C, the thermal decomposition of the base resin can be suppressed, the film thickness will not be reduced, and the film surface becomes uniform.
[0249] The baking environment can also be selected from an oxygen-containing environment such as air (oxygen concentration 1% to 21%) or a non-oxygen environment such as nitrogen. For example, when the substrate to be processed is easily oxidized by air, the substrate can be damaged by performing heat treatment in an environment with an oxygen concentration of less than 1% and forming a hardened film.
[0250] Furthermore, the resist underlayer film forming method of the present invention is preferably used as a substrate to be processed, which has a structure with a height of 30 nm or more or a height difference. The resist underlayer film forming method of the present invention is particularly useful for forming a planarized organic film without gaps on a structure with a height of 30 nm or more or a height difference substrate.
[0251] [Example]
[0252] The present invention is specifically described below with reference to Examples and Comparative Examples, but the present invention is not limited to these descriptions. In addition, the molecular weight and dispersity are measured using the following method. The weight average molecular weight (Mw) and dispersity (Mw / Mn) calculated based on polystyrene obtained by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent are obtained. In addition, the introduction ratio of the terminal groups is calculated using 1H NMR.
[0253] [Synthesis Example: Synthesis of Compound for Resist Underlayer Film Material]
[0254] The synthesis of compounds (D1) to (D16) for resist underlayer film materials, compounds (R1) to (R4) for comparative examples, and polymers (R5) for comparative examples uses the following triple-bond-containing carboxylic acid compounds: compound group A (A1) to (A5), phenolic hydroxyl-containing carboxylic acids: compound group B (B1) to (B6), and epoxy compounds: compound group C: (C1) to (C7).
[0255] [Chemistry 26]
[0256]
[0257] [Chemistry 27]
[0258]
[0259] [Chemistry 28]
[0260]
[0261] [Synthesis Example 1] Synthesis of Compound (D1)
[0262] [Chemistry 29]
[0263]
[0264] Under nitrogen atmosphere, 12.44 g of a carboxylic acid compound (A1) containing a triple bond, 1.46 g of a carboxylic acid compound (B1) containing a phenolic hydroxyl group, 16.10 g of an epoxy compound (C1) and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C to prepare a uniform solution, and then 1.00 g of benzyltriethylammonium chloride was added and stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added, and the mixture was washed with 100 g of a 1 wt% ammonia solution twice, 100 g of a 3% nitric acid solution twice, and 100 g of ultrapure water five times. The organic layer was dried under reduced pressure to obtain compound (D1).
[0265] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC. As a result, Mw=980 and Mw / Mn=1.03.
[0266] The terminal group ratio calculated by 1H NMR was triple bond-containing terminal group / phenolic hydroxyl group-containing terminal group=90.8 / 9.2.
[0267] [Synthesis Examples 2 to 20] Synthesis of Compounds (D2) to (D16) and Comparative Example Compounds (R1) to (R4)
[0268] Compounds (D2) to (D16) and (R1) to (R4) shown in Tables 2 to 6 were obtained as products under the same conditions as in Synthesis Example 1 except that compound group A, compound group B and compound group C shown in Table 1 were used. The weight average molecular weight (Mw), dispersity (Mw / Mn) and terminal group ratio (triple bond-containing group / phenolic hydroxyl group-containing group) of these compounds were determined and shown in Table 7.
[0269] [Table 1]
[0270] Synthesis example Compound Group A Compound Group B Compound Group C product 1 A1: 12.44g B1: 1.46g C1: 16.10g D1 2 A2: 15.69g B2: 1.19g C1: 13.12g D2 3 A2: 14.32g B3: 1.18g C2: 14.50g D3 4 A3: 13.38g B2: 1.16g C2: 15.46g D4 5 A2: 13.56g B2: 1.03g C3: 15.41g D5 6 A4: 13.74g B4: 2.09g C3: 14.17g D6 7 A3: 16.00g B2: 1.38g C4: 12.62g D7 8 A4: 17.67g B4: 1.89g C4: 10.43g D8 9 A2: 17.02g B2: 3.37g C5: 9.62g D9 10 A2: 19.48g B2: 1.21g C5: 9.31g D10 11 A2: 17.92g B3: 2.66g C5: 9.42g D11 12 A5: 16.22g B2: 2.84g C5: 10.95g D12 13 A1: 15.70g B2: 2.92g C6: 11.38g D13 14 A2: 18.75g B3: 2.46g C6: 8.79g D14 15 A2: 16.27g B2: 1.96g C7: 11.77g D15 16 A4: 17.75g B3: 1.88g C7: 10.37g D16 17 A2: 19.80g - C5: 10.20g R1 18 A2: 14.12g B2: 5.90g C5: 9.98g R2 19 A2: 19.78g B5: 0.91g C5: 9.31g R3 20 A2: 18.10g B6: 2.57g C5: 9.33g R4
[0271] [Table 2]
[0272]
[0273] [Table 3]
[0274]
[0275] [Table 4]
[0276]
[0277] [Table 5]
[0278]
[0279] [Table 6]
[0280]
[0281] [Table 7]
[0282]
[0283] [Synthesis Example 21] Synthesis of Comparative Polymer (R5)
[0284] [Chemistry 30]
[0285]
[0286] After dissolving 4.11 g of a carboxylic acid compound (B4) containing a phenolic hydroxyl group, 12.69 g of 3,3'-dithiopropionic acid, 20.00 g of an epoxy compound (C4) and 1.00 g of tetrabutylphosphonium in 60 g of 2-methoxy-1-propanol, the mixture was stirred at an internal temperature of 105°C for 24 hours under a nitrogen atmosphere. After dissolving at room temperature, the mixture was dried under reduced pressure to obtain a polymer (R5) having a phenolic hydroxyl group at the terminal structure. The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the results were Mw=3300 and Mw / Mn=1.78.
[0287] [Preparation of Resist Underlayer Film Materials (UDL-1 to 18, Comparative UDL-1 to 5)]
[0288] The above-mentioned compounds (D1) to (D16), (R1) to (R5), and (S1) tripropylene glycol monomethyl ether as a high boiling point solvent: boiling point 242°C, (S2) 1,6-diacetoxyhexane: boiling point 260°C, (TAG) pyridine trifluoromethanesulfonate as a thermal acid generator, and propylene glycol monomethyl ether acetate (PGMEA) or 2-methoxy-1-propanol (PGME) containing 0.1% by mass of PF6320 (manufactured by OMNOVA) were used. After dissolving in the proportions shown in Table 8, filtering was performed using a 0.1μm fluororesin filter to prepare resist underlayer film materials (UDL-1 to 18, comparative UDL-1 to 5).
[0289] [Table 8]
[0290]
[0291] [Example 1 Evaluation of Solvent Resistance (Examples 1-1 to 1-18, Comparative Examples 1-1 to 1-5)]
[0292] The resist underlayer film materials (UDL-1 to 18, comparative UDL-1 to 5) prepared above were coated on a silicon substrate, calcined at 250°C for 60 seconds, and the film thickness was measured. PGMEA solvent was dispensed thereon, left for 30 seconds and spun dry, and baked at 100°C for 60 seconds to evaporate the PGMEA solvent. The film thickness was measured again, and the difference in film thickness before and after PGMEA treatment was calculated to evaluate solvent resistance. The results are shown in Table 9.
[0293] [Table 9]
[0294]
[0295] As shown in Examples 1-1 to 1-18 in Table 9, when the compounds of the present invention were used, almost no film loss was observed in all resist underlayer film materials due to solvent treatment, and films with good solvent resistance were obtained. In particular, those having a naphthalene-type terminal group structure as a triple-bond-containing terminal group had a better residual film rate than Examples 1-1, 1-12, and 1-13 having a benzene-type terminal group structure, and the curing reaction proceeded more efficiently. In addition, when comparing Examples 1-9, 1-10, and Comparative Example 1-2, which have different terminal group ratios, more than 2% of film loss occurred in Comparative Example 1-2 because the terminal group ratio contributing to the crosslinking reaction was reduced, and deterioration of curability was observed.
[0296] [Example 2 Evaluation of film forming properties (Examples 2-1 to 2-18, Comparative Examples 2-1 to 2-5)]
[0297] The resist underlayer film materials (UDL-1 to 18, comparative UDL-1 to 5) prepared above were coated on the bare Si substrate, the substrate treated with hexamethyldisilazane (HMDS), and the substrate treated with SiON shown in Table 10, respectively, and calcined at 250°C for 60 seconds to form a resist underlayer film with a film thickness of 100 nm. The formed organic film was observed using an optical microscope (ECLIPSE L200 manufactured by Nikon Corporation) to see if there was coating abnormality. In addition, in this evaluation, the film thickness was made thin in advance in order to evaluate the coating quality, which is a severe evaluation condition that easily causes film formation abnormality.
[0298] [Table 10]
[0299]
[0300] As shown in Table 10, in Examples 2-1, 2-6, and 2-8 without catechol terminal structures, slight pinholes are generated on the substrate treated with HMDS, but in other examples with catechol-type terminal structures, a uniform resist lower layer film can be formed without substrate dependence and coating abnormalities. However, in Examples 2-1, 2-6, and 2-8, compared with Comparative Example 2-1, due to the introduction effect of the terminal structure with multiple phenolic hydroxyl groups, the film forming property on the SiON-treated substrate is improved, and the number of pinholes on the HMDS-treated substrate is also reduced, and the improvement effect can be confirmed. In addition, when Examples 2-9, 2-10, and 2-11 are compared with Comparative Examples 2-1, 2-3, and 2-4, it can be seen that the film forming property is improved by introducing the catechol-type terminal structure. It is believed that this is because the film condensation during calcination suppresses the formation of pinholes due to the effect of improving the adhesion with the substrate.
[0301] [Evaluation of landfill characteristics in Example 3 (Examples 3-1 to 3-18, Comparative Examples 3-1 to 3-5)]
[0302] The resist underlayer film materials (UDL-1 to 18, comparative UDL-1 to 5) prepared above were coated on SiO2 wafer substrates with dense hole patterns (hole diameter 0.16 μm, hole depth 0.50 μm, center distance between two adjacent holes 0.32 μm), and calcined at 250°C for 60 seconds to form resist underlayer films. The substrates used were as follows Figure 2 (G) (top view) and (H) (cross-sectional view) are base substrates 7 (SiO2 wafer substrates) having a dense hole pattern. The cross-sectional shape of each wafer substrate obtained was observed using a scanning electron microscope (SEM) to confirm whether the resist underlayer film 8 was filled inside the hole without pores (voids). The results are shown in Table 11. When a resist underlayer film material with poor filling characteristics was used, pores were generated inside the hole in this evaluation. When a resist underlayer film material with good filling characteristics was used, in this evaluation, Figure 2As shown in (I), the resist underlayer film is filled in the pores without any voids.
[0303] [Table 11]
[0304]
[0305] As shown in Examples 3-1 to 3-18 in Table 11, the resist underlayer film materials of the present invention can fill the hole pattern without voids and have excellent filling properties. On the other hand, since the polymer used in Comparative Example 3-5 undergoes a violent hardening reaction due to the action of the thermal acid generator, it is believed that the thermal fluidity is insufficient, resulting in voids due to poor filling.
[0306] [Example 4 Evaluation of Flattening Characteristics (Examples 4-1 to 4-18, Comparative Examples 4-1 to 4-5)]
[0307] The resist underlayer film materials (UDL-1 to 18, comparative UDL-1 to 5) prepared above were coated on the surfaces having huge isolated trench patterns ( Figure 3 (J), a base substrate 9 (SiO2 wafer substrate) with a groove width of 10 μm and a groove depth of 0.1 μm) was calcined at 250°C for 60 seconds, and the height difference of the resist lower layer film 10 between the groove part and the non-groove part was observed using an NX10 atomic force microscope (AFM) manufactured by Park Systems ( Figure 3 (K) delta10). The results are shown in Table 12. In this evaluation, the smaller the height difference, the better the planarization characteristics. In addition, in this evaluation, a trench pattern with a depth of 0.10 μm was planarized using a resist underlayer film material with a film thickness of about 0.2 μm, which was a strict evaluation condition for evaluating the quality of the planarization characteristics.
[0308] [Table 12]
[0309]
[0310] As shown in Examples 4-1 to 4-18 of Table 12, when the resist underlayer film material of the present invention is used, the height difference of the resist underlayer film between the trench portion and the non-trench portion is small compared to Comparative Examples 4-1 to 4-5, and the flattening property is excellent. In particular, those having a naphthalene-type terminal group structure form a dense film as shown in Example 1, and the film shrinkage is suppressed, and the flattening performance is improved compared to Examples 4-1, 4-12, and 4-13 having a benzene-type terminal group structure. In addition, when Examples 4-9 and 4-10 having different terminal group structures are compared with Comparative Examples 4-1, 4-3, and 4-4, it can be seen that the flatness is improved by the effect of the catechol terminal group. When Examples 4-9 and 4-10 are compared with Comparative Example 4-2, it can be seen that when an excessive amount of catechol terminal structure is introduced, the curing property is deteriorated as in Example 1, so the heat resistance is also deteriorated, and the flatness is deteriorated due to the influence of film shrinkage. In addition, Comparative Example 4-5 used a polymer and therefore had insufficient thermal fluidity, and thus did not achieve the same good flattening performance as Example 3. Comparison of Examples 4-17 and 4-18 to which a high boiling point solvent was added and Examples 4-10 and 4-15 to which no high boiling point solvent was added also showed that the addition of a high boiling point solvent further improved the flattening performance.
[0311] [Example 5 Pattern Formation Test (Examples 5-1 to 5-13, Comparative Examples 5-1 to 5-5)]
[0312] The UDL-2 to 5, 7, 9 to 11, 14 to 18 and comparative example UDL-1 to 5 prepared above were coated on a SiO2 substrate having a trench pattern (trench width 10 μm, trench depth 0.10 μm) formed with a SiO2 film having a thickness of 200 nm after HMDS treatment, and calcined at 250°C for 60 seconds in the atmosphere to form a resist lower layer film with a thickness of 200 nm on the bare Si substrate. A silicon-containing resist intermediate layer material (SOG-1) was coated thereon and baked at 220°C for 60 seconds to form a resist intermediate layer film with a thickness of 35 nm, and a resist upper layer film material (SL resist for ArF) was coated thereon and baked at 105°C for 60 seconds to form a resist upper layer film with a thickness of 100 nm. A wet protection film (TC-1) was applied on the resist upper layer and baked at 90° C. for 60 seconds to form a protection film with a film thickness of 50 nm.
[0313] The resist upper film material (SL resist for ArF) is prepared by dissolving a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass % FC-430 (manufactured by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 13, and filtering using a 0.1 μm fluororesin filter.
[0314] [Table 13]
[0315]
[0316] The structural formulas of the polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used are shown below.
[0317] [Chemistry 31]
[0318]
[0319] The wet protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent at the ratio shown in Table 14 and filtering the solution through a 0.1 μm fluororesin filter.
[0320] [Table 14]
[0321]
[0322] The structural formula of the polymer (PP1) used is shown below.
[0323] [Chemistry 32]
[0324]
[0325] The silicon-containing anti-etching intermediate layer material (SOG-1) is prepared by dissolving a polymer represented by an ArF silicon-containing intermediate film polymer (SiP1) and a cross-linking catalyst (CAT1) in an organic solvent containing 0.1 mass % FC-4430 (produced by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 15, and filtering using a fluororesin filter with a pore size of 0.1 μm.
[0326] [Table 15]
[0327]
[0328] The structural formulas of the ArF silicon-containing intermediate film polymer (SiP1) and the crosslinking catalyst (CAT1) used are shown below.
[0329] [Chemistry 33]
[0330]
[0331] Then, exposure was performed using an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA1.30, σ0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% half-step phase shift mask) while changing the exposure amount, and the pattern was baked (PEB) at 100°C for 60 seconds and developed with a 2.38 mass % tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a positive line and space pattern with a pitch of 100 nm and a resist line width of 50 nm to 30 nm.
[0332] Then, using the etching device Telius manufactured by Tokyo Electron, the resist pattern obtained by dry etching was used as a mask to process the silicon-containing intermediate layer, the silicon-containing intermediate layer was used as a mask to process the lower film, and the lower film was used as a mask to process the SiO2 film.
[0333] The etching conditions are as follows.
[0334] Transfer conditions for transferring the resist pattern to the SOG film.
[0335]
[0336] Transfer conditions for SOG film pattern transfer to underlying film.
[0337]
[0338]
[0339] Transfer conditions for transferring the lower film pattern to the SiO2 film.
[0340]
[0341] The pattern cross-section was observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd., and the shapes were compared and summarized in Table 16.
[0342] [Table 16]
[0343]
[0344] As shown in Table 16, as the results of the resist lower film material of the present invention (Examples 5-1 to 5-13), the resist upper film pattern was finally well transferred to the substrate, confirming that the resist lower film material of the present invention can be ideally used in micro-processing using a multilayer resist method. On the other hand, in Comparative Examples 5-1, 5-3, and 5-4, due to pinholes generated during film formation as shown in the results of the film forming test of Example 2, pattern collapse occurred during pattern processing and a pattern could not be formed. In Comparative Example 5-2, as in the results of Example 1, the hardening property was slightly insufficient, so when the SOG film was formed, cross-mixing with the upper layer occurred, and pattern transfer could not be performed. In Comparative Example 5-5, as in Examples 3 and 4, the filling characteristics and planarization characteristics were poor, so pattern collapse occurred during pattern processing and a pattern could not be formed.
[0345] From the above, it can be seen that if the resist underlayer film material of the present invention has good film-forming properties and excellent filling / planarization characteristics, it is extremely useful as an organic film material used in a multilayer resist method. Furthermore, if the pattern forming method of the present invention uses the resist underlayer film material, even if the processed body is a substrate with height differences, a fine pattern can be formed with high precision.
[0346] The present invention is not limited to the above-described embodiments. The above-described embodiments are illustrative, and those having substantially the same configuration as the technical concept described in the claims of the present invention and having the same functions and effects are all within the technical scope of the present invention.
[0347] Description of Reference Numerals
[0348] 1:Substrate
[0349] 2: Processing layer
[0350] 2a: Pattern formed on the processed layer
[0351] 3: Resist lower layer film
[0352] 3a: Resist lower film pattern
[0353] 4: Resist interlayer film
[0354] 4a: Resist interlayer film pattern
[0355] 5: Resist upper film
[0356] 5a: Resist upper film pattern
[0357] 6: Used part (exposed part)
[0358] 7: Base substrate with dense hole pattern
[0359] 8: Resist lower layer film
[0360] 9: Base substrate with large isolated trench patterns
[0361] 10: Resist lower layer film
[0362] delta10: height difference between the resist lower layer film in the trench part and the non-trench part
Claims
1. A resist underlayer film material, which is a resist underlayer film material used in a multilayer resist method, Its characteristics are that it contains: (A) one or more compounds represented by the following general formula (1); and (B) an organic solvent; In the formula, W is an n-valent organic group having 2 to 50 carbon atoms, X is any one of the terminal group structures represented by the following general formula (2) and the following general formula (3), and when the ratios of the structures of the following general formula (2) and the following general formula (3) constituting X are a and b, respectively, the relationship of a+b=1.0, 0.70≤a≤0.99, and 0.01≤b≤0.30 is satisfied; n is an integer of 1 to 10; In the formula, the dotted line represents an atomic bond; Z represents a (k+1)-valent aromatic group with 6 to 20 carbon atoms; A is a single bond, or -O-(CH2) p -; k is an integer from 1 to 5; p is an integer from 1 to 10; In the formula, the dotted line represents an atomic bond; L is a single bond or -(CH2) r -; l is 2 or 3, and r is an integer from 1 to 5; in, The general formula (2) is any one of the following formulas (4), (5), and (6); In the formula, the dotted lines represent atomic bonds; Wherein, the general formula (3) is any one of the following formulas (7) or (8); In the formula, the dotted lines represent atomic bonds.
2. The resist underlayer film material according to claim 1, wherein W in the general formula (1) is represented by the following general formula (9); In the formula, the dotted lines represent atomic bonds; R 1 W is a hydrogen atom, or an alkyl or acyl group having 1 to 20 carbon atoms which may contain an oxygen atom or a nitrogen atom; 1 is an n-valent organic group having 1 to 47 carbon atoms; Y is a single bond or a carbonyl group; and n is an integer of 1 to 10.
3. The resist underlayer film material according to claim 2, wherein In the general formula (9), W 1 A structure represented by any one of the following formulae: In the formula, the dotted lines represent atomic bonds.
4. The resist underlayer film material according to claim 1 or 2, wherein The (B) organic solvent is a mixture of one or more organic solvents having a boiling point of less than 180 degrees and one or more organic solvents having a boiling point of 180 degrees or more.
5. The resist underlayer film material according to claim 1 or 2, further comprising one or more of (C) an acid generator, (D) a surfactant, (E) a crosslinking agent, (F) a plasticizer, and (G) a pigment.
6. A method for forming a pattern on a processed substrate. It is characterized by the following steps: (I-1) coating a resist underlayer film material according to any one of claims 1 to 5 on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film; (I-2) forming a resist upper film on the resist lower film using a photoresist material; (I-3) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film; (I-4) using the patterned resist upper film as a mask, transferring the pattern to the resist lower film by dry etching; and (I-5) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
7. A method for forming a pattern on a processed substrate. The method is characterized by having the following steps: (II-1) coating a resist underlayer film material according to any one of claims 1 to 5 on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film; (II-2) forming a resist intermediate film on the resist underlayer film; (II-3) forming a resist upper film on the resist intermediate film using a photoresist material; (II-4) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film; (II-5) using the patterned resist upper film as a mask, transferring the pattern to the resist intermediate film by dry etching; (II-6) using the resist intermediate film having the transferred pattern as a mask, transferring the pattern to the resist lower layer film by dry etching; and (II-7) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
8. A method for forming a pattern on a processed substrate. The method is characterized by having the following steps: (III-1) coating a resist underlayer film material according to any one of claims 1 to 5 on a substrate to be processed, and then performing a heat treatment to form a resist underlayer film; (III-2) forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film on the resist underlayer film; (III-3) forming an organic thin film on the inorganic hard mask intermediate film; (III-4) forming a resist upper film on the organic thin film using a photoresist material; (III-5) exposing the resist upper layer film to pattern exposure, and then developing the resist upper layer film with a developer to form a pattern on the resist upper layer film; (III-6) using the patterned resist upper layer film as a mask, transferring the pattern to the organic thin film and the inorganic hard mask intermediate film by dry etching; (III-7) using the inorganic hard mask intermediate film having the transferred pattern as a mask, transferring the pattern to the resist underlayer film by dry etching; and (III-8) The substrate to be processed is processed using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed.
9. The pattern forming method according to any one of claims 6 to 8, wherein: As the substrate to be processed, a substrate having a structure with a height of 30 nm or more or a height difference is used.
10. A method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in a manufacturing step of a semiconductor device, characterized in that: The resist underlayer film material according to any one of claims 1 to 5 is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat treated at a temperature of 100° C. to 600° C. for 10 to 600 seconds to form a cured film.
11. A method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in a manufacturing step of a semiconductor device, characterized in that: The resist underlayer film material according to any one of claims 1 to 5 is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated in an environment with an oxygen concentration of 1% to 21% to form a cured film.
12. A method for forming a resist underlayer film, which is a method for forming a resist underlayer film that functions as an organic flat film used in a manufacturing step of a semiconductor device, characterized in that: The resist underlayer film material according to any one of claims 1 to 5 is spin-coated on a substrate to be processed, and the substrate coated with the resist underlayer film material is heat-treated in an environment with an oxygen concentration of less than 1% to form a cured film.
13. The resist underlayer film forming method according to any one of claims 10 to 12, wherein: As the substrate to be processed, a substrate having a structure with a height of 30 nm or more or a height difference is used.