Composite solder balls for surface metallization and granulation of circuit board assembly
By using expanded polystyrene spherical carrier particles and performing multi-layer metallization to form composite solder balls, the problems of high granulation costs and mismatch in soldering thermal expansion caused by dense core materials are solved, and mechanical improvements in circuit board assembly are realized. Stable interconnection and cost reduction of stress-sensitive components.
Patent Information
- Application Number
- CN202080060917.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-12
- Filing Date
- 2020-09-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-09-11
Smart Images

Figure CN114599818B_ABST
Abstract
Description
[0001] The present invention generally relates to the manufacture of composite solder balls and the use of these solder balls as an interconnect solution for circuit board assembly.
[0002] The search for increasingly miniaturized, lead-free circuit board assembly technologies is increasingly encouraging industrial practitioners in this technology field to seek innovative solutions for interconnecting mechanically stress-sensitive components, such as CBGA (Ceramic Bail Grid Array) type ball grid arrays and micro-electromechanical systems (often denoted by the English abbreviation MEMS "Micro Electro Mechanical System").
[0003] Flexible ball (such as [ Figure 1 ] is a technology used to realize system-level packaging, usually represented by the English abbreviation SiP (System In Package). They have solder contacts, which makes them easy to assemble in the package.
[0004] However, the flexible spheres currently used in the field suffer from the drawback of having a dense core made of polymer material, which has a negative impact on the yield of the initial pelletizing and sizing process and on the manufacturing costs associated with the final density of the pellets. On the other hand, during the subsequent brazing operation, problems of different thermal expansion may be encountered between the core and the metal shell of the pellets.
[0005] In order to overcome this defect, the applicant has developed a method for manufacturing a composite solder ball with a surface metallized and granulated, wherein the solder ball comprises an inner core and an outer shell, wherein the inner core is composed of a spherical carrier particle of expanded polystyrene (EPS) with a diameter of D0 and an intragranular porosity of at least 50%, and the outer shell covers the carrier particle and is composed of a plurality of metal surface layers, in particular, a metal layer with a thickness of E0. cu Copper coating, at least one layer of thickness E Ni The nickel layer has a thickness of E Au The gold surface layer makes the finished particle have a diameter D f .
[0006] According to the invention, the method is characterized in that it comprises the following steps:
[0007] A) a first step of providing carrier particles, followed by
[0008] B) A first step of size sorting the carrier particles, comprising a step of physically and / or mechanically separating the carrier particles, the diameter of the carrier particles being D0 with a tolerance of + / -5%, for example D0=D f -2*(E Ni +E Cu +EAu ), D0 can be selected between 200μm and 1000μm;
[0009] C) a treatment step of activating the carrier particles thus selected, in order to obtain activated carrier particles;
[0010] D) subjecting the activated support particles to a first step of metallization by autocatalytic chemical deposition of one or more layers of copper, this step being repeated until the copper layer has a thickness of 15 μm to 35 μm, thereby obtaining copper-coated support particles;
[0011] E) a second step of metallizing the copper-coated support particles by autocatalytic chemical deposition of at least one nickel NiP layer alloyed with phosphorus, wherein the mass percentage of phosphorus relative to the total weight of the NiP layer is 7 to 10%, this step being carried out until the thickness of the chemical nickel layer is E Ni Reach 4 μm to 7 μm, thereby obtaining chemical nickel-coated carrier particles;
[0012] F) a third step of metallizing the chemical nickel-coated support particles (including a gold deposition step, the gold deposition step adopts an electro-displacement process, the electro-displacement process is achieved by immersing in an aqueous solution containing gold ions (usually achieved according to the prior art)), thereby obtaining a metallized composite solder ball, and the surface is coated with a thickness of E Au Gold surface layer between 0.05 μm and 0.12 μm;
[0013] G) A second step of size sorting the thus metallized particles to sort and select surface metallized composite solder balls (1) having a diameter D f , tolerance is + / -5%.
[0014] Expanded polystyrene (EPS) pellets have the advantage of being able to reduce particle size when heated, thus providing the possibility of pelletizing by heat treatment.
[0015] In the present invention, intragranular porosity refers to the internal porosity of the carrier particles, and different types of pores can be observed on the surface and / or inside thereof: channels, grids, "pocket holes", blind holes and surface convexoconcavities. It can be measured, for example, by a helium pycnometer.
[0016] The first step of the method according to the invention is to provide carrier particles (step A).
[0017] Advantageously, expanded polystyrene (EPS) pellets having an intra-pellet porosity greater than 90% may be used.
[0018] In the method according to the invention, a first step of size sorting of the carrier particles (step B) is first carried out, which comprises physically and / or mechanically separating out carrier particles (10) having a selected diameter D0 between 200 μm and 1000 μm. According to an advantageous embodiment of the method according to the invention, the size sorting step B) of the carrier particles may comprise mechanical sieving to sort out and select carrier particles having a selected diameter D0 between 200 μm and 1000 μm. In actual operation, carrier particles having a particle size corresponding to a target value D0 + / - 5% are selected.
[0019] If EPS pellets are used as carrier particles, the carrier particle size sorting step B) may include mechanical screening of the carrier particles. The thus sorted upper particles (that is to say particles with a particle size greater than D0+5%) may then advantageously be finally subjected to a heat treatment at a temperature between 100° C. and 120° C., preferably between 110° C. and 120° C., in order to increase the yield of whole particles of the initial population of pellets. In fact, since the diameter of EPS pellets decreases when heated, if mechanical screening is combined with heating, the diameter of the previously sorted upper pellets during screening is reduced, so that these initially rejected pellets reach the target diameter D0+ / -5%. This makes it possible to significantly reduce production costs, in particular by increasing the yield of the number of pellets with diameter D0. This heat treatment step may advantageously be carried out in a fluidized bed, either by gas or liquid, in order to maintain the initial sphericity of the pellets.
[0020] At the end of the size sorting step B), the previously selected support particles are subjected to an activation treatment (step C) to obtain activated support particles.
[0021] In the present invention, activation treatment refers to a treatment for activating the surface of the carrier particles, so that the subsequent metallization treatment can be well controlled.
[0022] A first advantageous embodiment of such an activation treatment may consist in depositing silver nuclei onto the previously selected surface of the support particles, for example by reducing silver ions in a solution, wherein the silver deposit is formed by germination-growth. This operation may be achieved, for example, by reducing ammoniacal silver nitrate in an ethylene glycol-based solution.
[0023] Another advantageous embodiment of this activation treatment may also consist in depositing a thin layer of copper less than or equal to 1 μm onto the surface of the previously selected support particles by physical vapor deposition (PVD).
[0024] Once the support particles have been activated, metallization of the particles is performed as described (steps D to F).
[0025] The first step (step D) of metallizing the activated support particles is an autocatalytic chemical deposition step of one or more layers of copper, which is repeated until the copper layer reaches a thickness of 15 μm to 35 μm, thereby obtaining copper-coated support particles. Multiple consecutive metallizations may be required to obtain the desired copper thickness.
[0026] If the solder balls are desired to be hollow or nearly hollow, the expanded polystyrene (EPS) constituting the carrier particles can be partially or completely dissolved or partially or completely thermally decomposed between metallization steps D and E. To this end, the copper layer formed in step E should be thin enough or porous enough to make the EPS disappear.
[0027] The second metallization step (step E) consists in metallizing the copper-coated support particles obtained in step D) (possibly converted into hollow or nearly hollow spheres) by autocatalytic chemical deposition of at least one nickel NiP layer alloyed with phosphorus, wherein the mass percentage of phosphorus relative to the total weight of the NiP (or chemical nickel) layer is 7% to 10%. This step E) is carried out until the thickness E of the chemical nickel layer (111) is Ni Reaching 4μm to 7μm, thereby obtaining chemical nickel-coated carrier particles.
[0028] The third step of metallization (step F) includes metallizing the chemical nickel-coated support particles by immersing them in a solution containing gold ions, thereby obtaining a metallized composite solder ball, and the surface of the ball is coated with a thickness of E. Au Gold surface layer between 0.05μm and 0.12μm.
[0029] Finally, the last step (step G) of the method according to the present invention is a second step of size sorting the thus metallized particles, in order to sort and select the surface metallized composite solder balls, whose diameter D f , tolerance is + / -5%.
[0030] The invention also has as its object the solder pellets obtainable by the production method according to the invention.
[0031] According to a first particularly advantageous embodiment of the invention, the solder spheres may have the following features:
[0032] - Diameter D0 is about 630 μm + / - 5%,
[0033] -The thickness of the copper layer is about 30μm,
[0034] -Thickness of NiP layer E Ni About 5μm,
[0035] -Thickness of the gold layer E Au Between 0.05μm and 0.12μm,
[0036] - Diameter Df is about 700 μm + / - 5%.
[0037] According to a second particularly advantageous embodiment of the invention, the solder spheres may have the following features:
[0038] - diameter D0 is about 350 μm + / - 5% μm,
[0039] -The thickness of the copper layer Ecu is about 20μm,
[0040] -Thickness of NiP layer E Ni About 5μm,
[0041] -Thickness of the gold layer E Au About 0.1μm,
[0042] - Diameter Df is about 400 μm + / - 5%.
[0043] Advantageously, the solder spheres according to the invention may be hollow (or nearly hollow) spheres comprising, in the case of expanded polystyrene (EPS), a core consisting of up to 50% by volume of polymer material. Such solder spheres are obtained by a process according to the invention, during which, between steps D) and E), a step of partial or complete dissolution, a step of partial or complete thermal decomposition of the expanded polystyrene (EPS) constituting the starting carrier particles is included.
[0044] The invention also aims at the use of the pellets according to the invention in the assembly of circuit boards. In fact, the structure of the pellets according to the invention makes it possible to realize interconnections between components that are sensitive to mechanical stresses (CBGA, MEMS, etc.). They also have the advantage of maintaining a controlled positioning on the one hand and limiting the mechanical stresses in the interconnection between substrate and component on the other hand.
[0045] Other advantages and features of the invention will be understood from the following description given as non-limiting examples, with reference to the accompanying drawings, in which:
[0046] [ Figure 1 ] is a schematic diagram of an example of a flexible ball known in the prior art, which includes solder contacts for assembling them into an integrated circuit package,
[0047] [ Figure 2 ] is a schematic diagram of an example of a flexible ball according to the present invention,
[0048] [ Figure 3 ] is also a schematic diagram of an example of a flexible ball according to the present invention, but for the sake of clarity, the gold surface layer is not shown.
[0049] [ Figure 4] is a photograph of the activated EPS spherical particles (coated with a thin layer of silver) obtained at the end of the activation step C) of the method according to the present invention,
[0050] [ Figure 5 ] is a photograph of EPS spherical particles activated and coated with a copper layer obtained at the end of the copper metallization step D) according to the method of the present invention,
[0051] [ Figure 6 ] is a photograph of EPS spherical particles activated and continuously coated with a copper layer and a chemical nickel (NiP) layer obtained at the end of the chemical nickel metallization step E) according to the method of the present invention,
[0052] [ Figure 7 ] is a photograph of a solder ball according to the invention, comprising an EPS spherical particle activated and successively coated with a copper layer, a chemical nickel (NiP) layer and a gold layer, obtained at the end of step F) of metallization with chemical nickel according to the method of the invention,
[0053] [ Figure 8 ] is an optical microscope image of a cross section of a pellet according to the invention, showing a support EPS pellet and successive copper, chemical nickel and gold layers obtained at the end of a first embodiment of the method according to the invention (EPS pellet diameter is about 655 μm, copper layer thickness is 17 μm),
[0054] [ Fig. 9 ] shows an optical microscope image (A) of a cross section of an EPS pellet obtained at the end of step D) of the second embodiment of the method according to the present invention (EPS pellet diameter is about 660 μm, copper layer thickness is 15 μm), and an optical microscope image (B) of a cross section of a copper-coated EPS pellet obtained at the end of step D) of the third embodiment of the method according to the present invention (EPS pellet diameter is about 630 μm, copper layer thickness is 31 μm),
[0055] [ Fig.10 ] shows a first image A taken under an optical microscope, which shows EPS carrier particles 10 whose particle size D0 is distributed between 0.5 and 1 mm, and a second image B taken under an optical microscope, which shows EPS carrier particles 10 obtained after particle size sorting with a selected diameter between 0.63 and 0.66 mm.
[0056] [ Fig.11 ] shows a metallized spherical particle according to the present invention, the diameter of which is about 400 μm + / - 5%,
[0057] [ Fig.12] shows an SEM image (A) of a metallized pellet according to the present invention before heat treatment at 360°C, and an SEM image (B) of a metallized pellet according to the present invention after subsequent heat treatment at 360°C for 20 minutes to confirm the heat resistance of the pellet.
[0058] [ Fig.13 ] is a SEM image of a pellet with a dense polystyrene core, which was metallized according to steps A to G of the method according to the present invention and subsequently heat treated at 360°C for 20 minutes to confirm the heat resistance of the pellet (B).
[0059] [ Figure 1 ] is described in the prior art background introduction. It specifically shows a flexible ball with welding contacts 1, 2 for easy assembly. Figures 2 to 12 Described in more detail, these examples illustrate the invention without limiting its scope. Example
[0060] Devices and instruments
[0061] -Autocatalytic chemical deposition equipment (for copper and chemical nickel deposition);
[0062] -Mechanical screening device
[0063] Starting material
[0064] - Expanded polystyrene pellets (EPS) with a diameter between 595 μm and 665 μm;
[0065] - Expanded polystyrene (EPS) pellets with a diameter of about 400 μm,
[0066] - chemical nickel (containing 7 to 10% by weight of P),
[0067] -copper,
[0068] -Silver nitrate,
[0069] -Gold ions.
[0070] Characterization: Morphological analysis
[0071] Optical microscopy is the use of an optical microscope to observe the surface ([ Figure 4 ]to[ Figure 7 ]) and cross-section ([ Figure 8 ]and[ Fig. 9 ]) is completed.
[0072] Fig.12 and 13 The observations in this paper were obtained using a scanning electron microscope (SEM).
[0073] Example 1 :
[0074] According to a first embodiment of the method according to the invention, a solder ball according to the invention is produced.
[0075] The solder ball according to the present invention is manufactured using expanded polystyrene (EPS) pellets according to the first embodiment of the method according to the present invention. The manufacturing is divided into the following steps:
[0076] -1) The EPS carrier particles 10 with a particle size distribution between 0.5 and 1 mm are subjected to a first mechanical sieving so as to retain only spherical particles with a diameter of about 630 μm ([ Fig.10 ]);
[0077] -2) Then, the EPS particles are surface activated so that they can have good adhesion in the subsequent metallization treatment. The activated spherical particles 10' are obtained by depositing silver nuclei on the surface of the spheres. This operation is carried out in a silver nitrate reduction bath. After the treatment, the following is obtained: Figure 4 ] The pellet 10' shown;
[0078] -3) The third step comprises metallization with copper. A copper layer 110 with a thickness Ecu of 30 μm is obtained by autocatalytic chemical deposition (see [ Figure 2 ]、[ Figure 3 ]). After the processing is completed, the following is obtained: Figure 5 ](surface view) or [ Fig. 9 ] The pellet 10" of part B (cross-sectional view) shown in FIG.
[0079] - The fourth step comprises depositing a 5 μm thick chemical nickel (NiP) layer 111 on the copper layer 110 (see [ Figure 2 ]、([ Figure 3 ]). The coating is also produced by autocatalytic chemical deposition. After the treatment, the following is obtained: Figure 6 ]Spherical particle 10'" shown;
[0080] - The last layer of metallization is a gold surface layer 112 (see [ Figure 2 ]). The deposition is achieved by galvanic displacement by immersing the chemical nickel-coated spheres 10'" in an aqueous solution containing gold ions. Thus, a thickness of E is deposited. Au Gold layers between 0.05 μm and 0.12 μm (see [ Figure 2 ]). After the processing is completed, the following is obtained: Figure 7 ]The composite solder ball 1 shown;
[0081] The last step is the size sorting of the pellets, so that only the pellets of diameter D according to the invention remain. fComposite solder ball 1 of 700 μm + / - 5%.
[0082] Example 2 :
[0083] According to a second embodiment of the method according to the invention, a solder ball according to the invention is produced
[0084] The solder balls according to the present invention were prepared using the same materials as in Example 1, wherein the diameter of the carrier spheres was 660 μm and the copper deposition thickness was about 15 to 17 μm (see Figure 8 and Fig. 9 A).
[0085] Example 3 :
[0086] According to a third embodiment of the method according to the invention, a solder ball according to the invention is produced.
[0087] The solder balls according to the present invention were prepared using the same materials as in Examples 1 and 2, thereby obtaining a diameter D f About 400 μm + / - 5% of the spherulites (see [ Fig.12 ]).
[0088] Example 4 :
[0089] Effect of heat treatment after the screening step
[0090] SEM analysis ([ Fig.12 ]) presents metallized and sized pellets according to the invention before (12a) and after (12b) heat treatment at 360° C. It was observed that the pellets did not degrade / modify after the heat treatment, which demonstrates their temperature stability.
[0091] Example 5 (control)
[0092] In order to establish a comparative analysis of the pellet weight, three batches of pellets (diameter D0 of 700 μm + / - 5%) were prepared according to steps A to G of the method according to the invention (Cu / NiP / Au metallization) and then subjected to a subsequent heat treatment (B) at 360°C for 20 minutes to confirm the heat resistance of the pellets. For this purpose, three different types of support pellets were used:
[0093] - The first batch was made of expanded polystyrene pellets (porosity about 95%),
[0094] - The second batch was made of cross-linked polystyrene pellets (dense),
[0095] - The third batch was made of copper metal pellets (dense).
[0096] 1000 pellets were sampled from each batch and weighed. The results are summarized in Table 1 below:
[0097] Table 1
[0098] Carrier pellets Weight of 1000 metallized pellets (g) Expanded polystyrene 0.225 Compacted polystyrene 0.390 Dense copper 2.100
[0099] The pellets made from expanded polystyrene (first batch) according to the invention have a mass reduction factor of between 1.7 and 9.4 compared to the prior art solutions (dense core made of organic or metallic material).
[0100] On the other hand, it has been noted that the thermal stability of the pellets is improved by the use of an EPS core (first batch of pellets according to the invention) compared to the pellets obtained with a dense core (second and third batches of pellets). In fact, it was found that, starting from 360°C, the pellets made of dense polystyrene (second and third batches of pellets) exhibit a behavioural defect, with the appearance of organic "droplets" on the surface of the pellets ( Figure 1 This phenomenon was not observed with the pellets made of expanded polystyrene according to the invention (first batch of pellets).
Claims
1. A method of manufacturing a surface metallized and sized particle with a diameter of D f A method for preparing a composite solder ball (1), wherein the composite solder ball (1) comprises: - an inner core, the inner core is composed of spherical expanded polystyrene EPS carrier particles (10) with a diameter D0 and an intragranular porosity of at least 50%, - a shell (11), which covers the carrier particle (10) and is composed of a plurality of metal surface layers (110, 111, 112), including a metal surface layer with a thickness of E Cu Copper coating, at least one layer with a thickness of E Ni The nickel layer and the thickness of E Au The method comprises the following steps: A) a first step of providing the carrier particles (10), followed by B) a first step of size sorting the carrier particles (10), comprising a step of physically and / or mechanically separating the carrier particles (10), wherein the diameter of the carrier particles is D0, D0=D f -2*(E Ni +E Cu +E Au ), the D0 is selected to be between 200 μm and 1000 μm; C) a treatment step of activating said carrier particles (10) thus selected, in order to obtain activated carrier particles (10'); D) a first step of metallizing the activated support particles (10') by autocatalytic chemical deposition of one or more layers of copper, said step being repeated until the thickness of the copper coating (110) is E Cu Reaching 15 μm to 30 μm, thereby obtaining copper-coated support particles (10"); E) a second step of metallizing the copper-coated support particles (10") by autocatalytic chemical deposition of at least one nickel NiP layer alloyed with phosphorus, wherein the mass percentage of phosphorus relative to the total weight of the NiP layer is 7 to 10%, said step being carried out until the thickness of the chemical nickel layer (111) is E Ni Reaching 4 μm to 7 μm, thereby obtaining chemical nickel-coated support particles (10'"); F) a third step of metallizing the chemical nickel coated support particles (10'"), comprising a gold deposition step, wherein the gold deposition step adopts an electro-displacement process, wherein the electro-displacement process is achieved by immersing the support particles in an aqueous solution containing gold ions, thereby obtaining a metallized composite solder ball, and the surface of the metallized composite solder ball is coated with a thickness of E Au A gold surface layer between 0.05 μm and 0.12 μm; and G) subjecting the thus metallized particles to a second step of size sorting to sort and select surface metallized composite solder balls (1) having a diameter D f , tolerance is + / -5%.
2. The method according to claim 1, wherein the particle size sorting step B) of the carrier particles (10) comprises mechanical sieving to sort and select the carrier particles (10) having a selected diameter D0 between 200 μm and 1000 μm.
3. A method according to claim 2, wherein after the mechanical sieving step B) of the carrier particles (10), the upper layer of particles thus sorted with a particle size greater than D0+5% are subjected to a heat treatment at a temperature between 100°C and 120°C.
4. The method according to claim 2, wherein after the mechanical sieving step B) of the carrier particles (10), the upper layer of particles having a particle size greater than D0+5% thus sorted are subjected to a heat treatment at a temperature between 110°C and 120°C.
5. The method according to any one of claims 1 to 4, wherein the activation treatment of the selected carrier particles (10) comprises adding silver nitrate to a bath so that silver nuclei are deposited on the surface of the selected carrier particles, or depositing a thin layer of copper less than or equal to 1 μm on the surface of the selected carrier particles by physical vapor deposition (PVD).
6. The method according to any one of claims 1 to 4, further comprising a step of partially or completely dissolving the expanded polystyrene EPS constituting the carrier particles (10) between steps D) and E), or a step of partially or completely thermally decomposing the expanded polystyrene EPS constituting the carrier particles (10).
7. A surface metallized and sized particle having a diameter D obtained by the method according to any one of claims 1 to 6 f The composite solder ball (1) is used in circuit board assembly.