Electronic communication articles and methods comprising cross-linked fluoropolymers

By using a fluoropolymer composition and crosslinking it through photochemical radiation to form a patterned fluoropolymer layer, the problem of poor dielectric properties of perfluoropolymer materials in electronic communication products is solved, enabling its application in 5G products, reducing dielectric constant and dielectric loss, and improving mechanical properties.

CN114600201BActive Publication Date: 2024-10-013M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080075328.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-11
Filing Date
2020-11-03
Publication Date
2024-10-01
Estimated Expiration
2040-11-03

AI Technical Summary

Technical Problem

The lack of perfluoropolymer materials that can be cross-linked by photochemical radiation in existing technologies limits their application in electronic communication products, especially in 5G products where the dielectric constant and dielectric loss are high.

Method used

A fluoropolymer composition containing at least 80% perfluorinated monomer polymerization units is used to form a patterned fluoropolymer layer through photochemical radiation crosslinking. This layer is used to replace polyimide materials and reduce dielectric constant and dielectric loss.

Benefits of technology

It enables the reduction of dielectric constant and dielectric loss in electronic communication products, and improves mechanical properties. It is applicable to integrated circuits, printed circuit boards, antennas and fiber optic cables, etc., to meet the needs of 5G technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114600201B_ABST
    Figure CN114600201B_ABST
Patent Text Reader

Abstract

Electronic communication products comprising crosslinked fluoropolymer layers are described. In typical embodiments, the crosslinked fluoropolymer layer is a substrate, a patterned (e.g., photoresist) layer, an insulating layer, a passivation layer, a cladding, a protective layer, or a combination thereof. Methods for making electronic communication products and methods for forming patterned fluoropolymer layers are also described. The fluoropolymer preferably comprises at least 80%, 85%, or 90% by weight of polymerized units of perfluorinated monomers and a cure site selected from nitrile, iodine, bromine, and chlorine. Exemplary electronic communication products include integrated circuits, printed circuit boards, antennas, and fiber optic cables. Fluoropolymer compositions are also described.
Need to check novelty before this filing date? Find Prior Art

Description

Summary of the invention

[0001] In one embodiment, an electronic communication article comprising a crosslinked fluoropolymer layer is described. In typical embodiments, the crosslinked fluoropolymer layer is a substrate, a patterned (eg, photoresist) layer, an insulating layer, a passivation layer, a cladding layer, a protective layer, or a combination thereof.

[0002] In another embodiment, a method of manufacturing an electronic communication article is described, the method comprising providing a film or coating solution comprising a fluoropolymer; and applying the film or coating solution to a component of the electronic communication article. The coating solution typically also comprises a fluorinated solvent. The method also comprises crosslinking the fluoropolymer by subjecting it to heat, actinic radiation, or a combination thereof.

[0003] In another embodiment, a method of forming a patterned fluoropolymer layer is described, the method comprising applying a fluoropolymer film to a substrate; selectively crosslinking portions of the fluoropolymer film by exposure to actinic radiation; and removing the uncrosslinked portions of the fluoropolymer film.

[0004] In each of these embodiments, the fluoropolymer preferably comprises at least 80, 85, or 90 weight percent polymerized units of perfluorinated monomers and cure sites selected from the group consisting of nitrile, iodine, bromine, and chlorine.

[0005] Exemplary electronic communications articles include integrated circuits, printed circuit boards, antennas, and fiber optic cables. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Figure 1 is a schematic cross-sectional view of forming a patterned fluoropolymer layer by photolithography in an exemplary embodiment of the fabrication of an integrated circuit (IC).

[0007] Figure 2 is a perspective view of an exemplary printed circuit board (PCB) including an integrated circuit;

[0008] Figure 3A and Figure 3B is a cross-sectional view of an exemplary fluoropolymer passivation and insulation layer.

[0009] Figure 4 is a plan view of an exemplary antenna for a mobile computer device.

[0010] Figure 5A and Figure 5B is a perspective view of an exemplary antenna for a communications tower.

[0011] Figure 6 is a cross-sectional view of an exemplary fiber optic cable. DETAILED DESCRIPTION

[0012] Presently described are certain fluoropolymer compositions (e.g., films and coatings) for use in electronic communications articles. As used herein, electronic refers to devices that use the electromagnetic spectrum (e.g., electrons, photons); and communications is the transmission of symbols, signals, messages, words, text, images, and sounds or information of any nature by wire, radio, optical or other electromagnetic systems.

[0013] Polyimide materials are widely used in the electronic communications industry. The structure of polyoxydiphenylene-pyromellitimide "Kapton" is as follows:

[0014]

[0015] The polyimide film exhibits good insulating properties with dielectric constant values ​​in the range of 2.78-3.48 and dielectric loss between 0.01 and 0.03 at 1 Hz at room temperature.

[0016] Perfluoropolymers can have much lower dielectric constants and dielectric loss characteristics than polyimides, which is particularly important for fifth generation cellular network technology ("5G") products. For example, the crosslinked fluoropolymer compositions described herein can have a dielectric constant (Dk) of less than 2.75, 2.70, 2.65, 2.60, 2.55, 2.50, 2.45, 2.40, 2.35, 2.30, 2.25, 2.20, 2.15, 2.10, 2.05, 2.00, or 1.95. In some embodiments, the dielectric constant is at least 2.02, 2.03, 2.04, 2.05. In addition, the crosslinked fluoropolymer compositions described herein can have low dielectric losses, which are typically less than 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, 0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.0004, 0.0003. In some embodiments, the dielectric loss is at least 0.00022, 0.00023, 0.00024, 0.00025. Dielectric properties (e.g., constants and losses) can be determined according to the test methods described in the Examples. As the number of non-fluorine atoms increases (e.g., the number of carbon-hydrogen and / or carbon-oxygen bonds increases), the dielectric constant and dielectric loss also typically increase.

[0017] However, various electronic communication articles have not used perfluoropolymers to replace polyimides due, at least in part, to the lack of perfluoropolymer materials that can be crosslinked by exposure to actinic radiation and, more preferably, ultraviolet radiation. Crosslinked perfluoropolymer materials can have improved mechanical properties compared to non-crosslinked perfluoropolymer materials. Therefore, the described perfluoropolymer compositions are suitable for use in replacing polyimides in various electronic communication articles.

[0018] In one embodiment, the electronic communication article is an integrated circuit, or in other words a silicon wafer or microchip, which is an array of microscopic electronic circuits formed by fabricating various electrical and electronic components (resistors, capacitors, transistors, etc.) on a wafer of semiconductor material (silicon).

[0019] In one embodiment, the fluoropolymer compositions described herein can be used to form a patterned (e.g., photoresist) layer. Fluoropolymer compositions as described herein can be used as negative photoresists in various manufacturing techniques. In some embodiments, the (e.g., sacrificial) photoresist material is etched away and not retained in the finished article. In other embodiments, the photoresist material may be present in the finished article. Various integrated circuit designs have been described in the literature.

[0020] refer to Figure 1 In one embodiment, a method of forming a patterned fluoropolymer layer is described, the method comprising applying a fluoropolymer film 100 to a substrate (e.g., a silicon wafer 120 or a surface coated with a passivation (e.g., SiO2) layer 125); selectively cross-linking portions of the fluoropolymer film by exposure to actinic radiation; and removing uncross-linked portions of the fluoropolymer film.

[0021] In some embodiments, the method further includes providing a mask (e.g., a photomask) 130 having one or more openings between the fluoropolymer film 100 and an actinic (e.g., electron beam or UV) radiation source 140, and subjecting the fluoropolymer film to actinic radiation through at least one opening of the mask.

[0022] As is known in the art, the mask includes a portion that transmits actinic energy (e.g., UV light) and a portion that does not transmit actinic energy (e.g., UV light). A photomask typically includes a transparent substrate with a non-transmitting mask pattern on the surface of the substrate. The substrate is typically (e.g., high purity quartz) glass that is transparent to the illumination (i.e., wavelength and intensity) of the photolithography process employed. The mask is typically prepared by selectively depositing or selectively etching a mask material. Common non-light-transmitting mask materials include chromium metal, iron oxide, molybdenum silicide, etc., as is known in the art.

[0023] After receiving, the fluoropolymer film comprises a patterned fluoropolymer layer including portions of cured, or in other words cross-linked, fluoropolymer 150 and portions of uncured, or in other words non-cross-linked, fluoropolymer 175 .

[0024] In some embodiments, the method further comprises removing the portion of the fluoropolymer film that is not cross-linked by dissolving the portion that is not cross-linked in a solvent 160 (e.g., washing the fluoropolymer film with a fluorinated solvent). The portion of the solidified or in other words cross-linked fluoropolymer 150 remains on the surface of the substrate as a patterned fluoropolymer layer. In this embodiment, the substrate or its (e.g., SiO2) coated surface that is in contact with the solvent is substantially insoluble in the solvent used to remove the non-cross-linked portion of the fluoropolymer film. In an advantageous embodiment, the solvent is a fluorinated solvent.

[0025] In some embodiments, particularly when it is desired that a thin fluoropolymer film is applied to a substrate, the method includes applying a coating solution (e.g., spin coating) to the substrate, wherein the coating solution comprises a fluorinated solvent and a fluoropolymer. In some embodiments, the fluoropolymer preferably mainly comprises polymerized units of perfluorinated monomers and a cure site. The coating also comprises a curing agent, which reacts with the cure site in the presence of actinic (e.g., UV) radiation, thereby crosslinking the fluoropolymer. The method generally includes removing the fluorinated solvent (e.g., by evaporation). In this embodiment, the substrate in contact with the solvent or its (e.g., SiO2) surface coated is substantially insoluble in the fluorinated solvent of the coating solution. The fluorinated solvent for removing the uncrosslinked portion of the fluoropolymer film and the fluorinated solvent of the coating solution can be the same or different fluorinated solvents. In addition, the method generally includes recycling, or in other words, reusing the fluorinated solvent for removing the uncrosslinked portion of the fluoropolymer film and / or the fluorinated solvent of the coating solution.

[0026] In other embodiments, the uncured portion 175 may be removed using other solvent-free methods, such as laser ablation.

[0027] The patterned fluoropolymer layer can be used to make other layers, such as circuits of patterned electrode materials. Suitable electrode materials and deposition methods are known in the art. Such electrode materials include, for example, inorganic materials or organic materials or composite materials of the two. Exemplary electrode materials include polyaniline, polypyrrole, poly (3,4-ethylenedioxythiophene) (PEDOT) or doped conjugated polymers, other dispersions or pastes of graphite or metal (such as Au, Ag, Cu, Al, Ni or mixtures thereof) particles, and sputter-coated or evaporated metals (such as Cu, Cr, Pt / Pd, Ag, Au, Mg, Ca, Li or mixtures) or metal oxides such as indium tin oxide (ITO), F-doped ITO, GZO (gallium-doped zinc oxide) or AZO (aluminum-doped zinc oxide). Organic metal precursors can also be used and deposited from the liquid phase.

[0028] In another embodiment, a fluoropolymer (eg, photoresist) layer may be disposed on a metal (eg, copper) substrate in the manufacture of a printed circuit board (PCB). Figure 2 An exemplary perspective view of a printed circuit board is depicted in . A printed circuit board, or PCB, is used to mechanically support and electrically connect electronic components using conductive paths, tracks, or signal traces etched from a sheet of (e.g., copper) metal laminated to a non-conductive substrate. Such boards are typically made of an insulating material, such as fiberglass reinforced (fiberglass) epoxy or paper reinforced phenolic resin. The electrical paths are typically made of a negative photoresist, as previously described. Thus, in this embodiment, a cross-linked fluoropolymer is disposed on the surface of a (e.g., copper) metal substrate. Portions of the uncross-linked fluoropolymer are removed to form conductive (e.g., copper) paths. The cross-linked fluoropolymer (e.g., photoresist) remains present, disposed between the conductive (e.g., copper) paths of the printed circuit board. Solder is used to mount components on the surface of these boards. In some embodiments, the printed circuit board also includes an integrated circuit 200, such as Figure 2 Printed circuit board assemblies have applications in nearly every electronic product, including computers, computer printers, televisions, and cellular phones.

[0029] In another embodiment, the cross-linked fluoropolymer films described herein may be utilized as insulating layers, passivation layers, and / or protective layers in the manufacture of integrated circuits.

[0030] refer to Figure 3A In one embodiment, a thin fluoropolymer film 300 (eg, typically having a thickness of less than 50 nm, 40 nm, or 30 nm) may be disposed on a passivation layer 310 (eg, SiO 2 ) disposed on an electrode patterned 360 silicon wafer 320 .

[0031] refer to Figure 3B In another embodiment, a thicker fluoropolymer film 300 (e.g., typically having a thickness of at least 100 nm, 200 nm, 300 nm, 400 nm, 500 nm) may be disposed on the electrode patterned 360 silicon wafer 320. In this embodiment, the fluoropolymer layer may serve as both a passivation layer and an insulating layer. Passivation is the use of a thin coating to provide electrical stability by isolating the transistor surface from the electrical and chemical conditions of the environment.

[0032] In another embodiment, the crosslinked fluoropolymer films described herein can be used as a substrate for an antenna.The antenna of a transmitter transmits (eg, high frequency) energy into space, while the antenna of a receiver captures the energy and converts it into electricity.

[0033] The patterned electrodes of the antenna can also be formed by photolithography. Screen printing, flexographic printing and inkjet printing can also be used to form electrode patterns known in the art. Various antenna designs for (e.g., mobile) computing devices (smart phones, tablets, laptops, desktop computers) have been described in the literature. Figure 4 A representative split-loop monopole antenna is depicted in FIG. 5 with the following dimensions in micrometers.

[0034]

[0035] The low dielectric fluoropolymer films and coatings described herein may also be used as insulating and protective layers for transmitter antennas in cellular towers and other (eg, outdoor) structures. There are two main types of antennas used in cellular towers. Figure 5A A representative omnidirectional (eg, dipole) antenna for transmitting / receiving in any direction is depicted. Figure 5B It is a representative directional antenna for transmitting / receiving only in a specific desired direction, such as a circular and rectangular type horn antenna.

[0036] In another embodiment, the low dielectric fluoropolymer compositions described herein may also be used in optical fiber cables. Figure 6 , optical fiber cables typically include five main components: a core 620, typically high purity (e.g., silica) glass, a cladding 630, a coating (e.g., a first inner protective layer) 640, a reinforcing fiber 650, and an outer sheath (i.e., a second outer protective layer) 660. The function of the cladding is to provide a lower refractive index at the core interface to cause reflections within the core so that light waves are transmitted through the optical fiber. The coating on the cladding is typically present to strengthen the core, help absorb shock, and provide additional protection to prevent excessive cable bending. The low dielectric fluoropolymer composition described herein can be used as a cladding, a coating, an outer sheath, or a combination thereof.

[0037] In other embodiments, the low dielectric fluoropolymer films and coatings described herein can also be used in flexible cables and as insulating films on magnetic wires. For example, in a laptop computer, the cable connecting the main logic board to the display (which must be bent every time the laptop is opened or closed) can be a low dielectric fluoropolymer composition with copper conductors as described herein.

[0038] Electronic communications products are not typically hermetically sealed components of equipment used in wafer and chip production.

[0039] It will be appreciated by those skilled in the art that the low dielectric fluoropolymer compositions described herein can be used in a variety of electronic communication products, particularly in place of polyimide, and that such utility is not limited to the specific products described herein.

[0040] Fluoropolymers as described herein are copolymers that mainly comprise or only comprise (e.g., repeating) polymerized units derived from two or more perfluorinated comonomers. Copolymers refer to polymeric materials obtained by the simultaneous polymerization of two or more monomers. In some embodiments, comonomers include tetrafluoroethylene (TFE) and one or more unsaturated perfluorinated (e.g., alkenyl, vinyl) alkyl ethers.

[0041] In some advantageous embodiments, the one or more unsaturated perfluorinated alkyl ethers are selected from the general formula:

[0042] R f -O-(CF2) n -CF=CF2

[0043] wherein n is 1 (allyl ether) or 0 (vinyl ether), and R f represents a perfluoroalkyl residue which may be interrupted once or more than once by oxygen atoms. f It may contain up to 10 carbon atoms, for example 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms. f contains up to 8, more preferably up to 6 carbon atoms, and most preferably 3 or 4 carbon atoms. f has 3 carbon atoms. In another embodiment, R f Has 1 carbon atom. f R may be straight chain or branched, and it may or may not contain cyclic units. f Specific examples include residues having one or more ether functional groups, including but not limited to:

[0044] -(CF2)-O-C3F7,

[0045] -(CF2)2-O-C2F5,

[0046] -(CF2) r3 -O-CF3,

[0047] -(CF2-O)-C3F7,

[0048] -(CF2-O)2-C2F5,

[0049] -(CF2-O)3-CF3,

[0050] -(CF2CF2-O)-C3F7,

[0051] -(CF2CF2-O)2-C2F5,

[0052] -(CF2CF2-O)3-CF3.

[0053] R f Other specific examples include residues without ether functional groups, and include but are not limited to -C4F9; -C3F7, -C2F5, -CF3 residues, wherein the C4 and C3 residues may be branched or linear, but are preferably linear.

[0054] Specific examples of suitable perfluorinated alkyl vinyl ethers (PAVE) and perfluorinated alkyl allyl ethers (PAAE) include, but are not limited to, perfluoro(methyl vinyl) ether (PMVE), perfluoro(ethyl vinyl) ether (PEVE), perfluoro(n-propyl vinyl) ether (PPVE-1), perfluoro-2-propoxypropyl vinyl ether (PPVE-2), perfluoro-3-methoxy-n-propyl vinyl ether, perfluoro-2-methoxy-ethyl vinyl ether, CF2=CF-O-CF2-O-C2F5, CF2=CF-O-CF2-O-C3F7, CF3-(CF2)2-O-CF(CF3)-CF2-O-CF(CF3)-CF2-O-CF=CF2 and their allyl ether homologs. Specific examples of allyl ethers include CF2=CF-CF2-O-CF3, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-(CF3)3-O-CF3.

[0055] Other examples include, but are not limited to, the vinyl ethers described in European Patent Application EP 1,997,795 Bl.

[0056] Perfluorinated ethers as described above are commercially available, for example from Anles Ltd. St. Petersburg, Russia and other companies, or can be prepared according to the methods described in U.S. Patent 4,349,650 (Krespan) or European Patent 1,997,795 or by adaptation of methods known to the skilled person.

[0057] In some embodiments, the one or more unsaturated perfluorinated alkyl ethers include unsaturated cyclic perfluorinated alkyl ethers, such as 2,2-bis(trifluoromethyl)-4,5-difluoro-1,3 dioxole. In other embodiments, the fluoropolymer is substantially free of unsaturated cyclic perfluorinated alkyl ethers, such as 2,2-bis(trifluoromethyl)-4,5-difluoro-1,3 dioxole. By "substantially free" is meant that the amount is zero or sufficiently low so that the properties of the fluoropolymer are substantially the same.

[0058] In some advantageous embodiments, the fluoropolymer is mainly or only derived from a perfluorinated comonomer, which includes tetrafluoroethylene (TFE) and one or more unsaturated perfluorinated alkyl ethers described above. As used herein, "mainly" means that at least 80 weight %, 85 weight % or 90 weight % of the polymerized units of the fluoropolymer are derived from such perfluorinated comonomers, such as tetrafluoroethylene (TFE) and one or more unsaturated perfluorinated alkyl ethers, based on the total weight of the fluoropolymer. In some embodiments, the fluoropolymer comprises at least 81 weight %, 82 weight %, 83 weight %, 84 weight %, 85 weight %, 86 weight %, 87 weight %, 88 weight %, 90 weight %, 91 weight %, 92 weight %, 93 weight %, 94 weight %, 95 weight %, 96 weight % or 97 weight % or more of such perfluorinated comonomers, based on the total weight of the fluoropolymer. The fluoropolymer may contain at least 40 wt%, 45 wt%, or 50 wt% of polymerized units derived from TFE. In some embodiments, the maximum amount of polymerized units derived from TFE is no greater than 60 wt%.

[0059] Fluoropolymers typically include polymerized units derived from one or more of unsaturated perfluorinated alkyl ethers (PAVE) (e.g., PMVE, PAAE, or a combination thereof) in an amount of at least 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 45 wt%, or 50 wt% based on the total polymerized monomer units of the fluoropolymer. In some embodiments, based on the total polymerized monomer units of the fluoropolymer, the fluoropolymer includes not more than 50 wt%, 45 wt%, 40 wt%, or 35 wt% of polymerized units derived from one or more of unsaturated perfluorinated alkyl ethers (PMVE, PAAE, or a combination thereof). The molar ratio of the units derived from TFE to the above-mentioned perfluorinated alkyl ethers may be, for example, 1:1 to 5:1. In some embodiments, the molar ratio is in the range of 1.5:1 to 3:1.

[0060] Fluoropolymers may be thermoplastic, but in a preferred embodiment, the fluoropolymers are amorphous. As used herein, amorphous fluoropolymers are materials that are substantially free of crystallinity or have no significant melting point (peak maximum), as determined by differential scanning calorimetry in accordance with DIN EN ISO 11357-3:2013-04 in a nitrogen stream and at a heating rate of 10°C / min. Typically, amorphous fluoropolymers have a glass transition temperature (Tg) of less than 26°C, less than 20°C, or less than 0°C, and, for example, -40°C to 20°C, or -50°C to 15°C, or -55°C to 10°C. Fluoropolymers may typically have a Mooney viscosity (ML 1+10 at 121°C) of about 2 to about 150, for example 10 to 100, or 20 to 70. For amorphous polymers comprising cyclic perfluorinated alkyl ether units, the glass transition temperature is typically at least 70, 80 or 90° C. and may range up to 220, 250, 270 or 290° C. The MFI (297° C. / 5 kg) is between 0.1 and 1000 g / 10 min.

[0061] In other embodiments, the fluoropolymer may have a melting point of less than 150°C or 100°C.

[0062] The fluoropolymer is preferably a curable fluoropolymer containing one or more cure sites. A cure site is a functional group that reacts in the presence of a curing agent or curing system to crosslink the polymer. Cure sites are typically introduced by copolymerizing cure site monomers, which are functional comonomers of a precursor that already contains a cure site or cure site. One indication of crosslinking is that the dried and cured coating composition is insoluble in the fluorinated solvent of the coating.

[0063] Cure sites can be introduced into the polymer through the use of cure site monomers, ie, functional monomers, functional chain transfer agents, and initiator molecules as described below. Fluoroelastomers may contain cure sites reactive with more than one type of curative.

[0064] Curable fluoroelastomers may also contain cure sites in the backbone, as pendant cure sites, or at terminal positions. Cure sites within the fluoropolymer backbone may be introduced using suitable cure site monomers. Cure site monomers are monomers containing one or more functional groups that may act as cure sites, or contain precursors that may be converted into cure sites.

[0065] In some embodiments, the cure sites comprise iodine atoms or bromine atoms.

[0066] Iodine-containing cure site end groups can be introduced by using an iodine-containing chain transfer agent in the polymerization. Iodine-containing chain transfer agents are described in more detail below. Iodine end groups can be introduced using a halogenated redox system as described below.

[0067] In addition to the iodine cure sites, other cure sites may be present, such as Br-containing cure sites or cure sites containing one or more nitrile groups. The Br-containing cure sites may be introduced by Br-containing cure site monomers.

[0068] Examples of cure site comonomers include, for example:

[0069] (a) bromo(per)fluoroalkyl-(per)fluorovinyl ether or iodo(per)fluoroalkyl-(per)fluorovinyl ether, for example including those having the formula:

[0070] ZRf-O-CX=CX2

[0071] Wherein, each X may be the same or different and represents H or F, Z is Br or I, and Rf is a C1-C12 (per)fluoroalkylene group, which optionally contains chlorine and / or ether oxygen atoms. Suitable examples include ZCF2-O-CF=CF2, ZCF2CF2-O-CF=CF2, ZCF2CF2CF2-O-CF=CF2, CF3CFZCF2-O-CF=CF2 or ZCF2CF2–O-CF2CF2CF2-O-CF=CF2, wherein Z represents Br of I; and

[0072] (b) brominated perfluoroolefins or iodinated perfluoroolefins, such as those having the formula:

[0073] Z'-(Rf)r-CX=CX2

[0074] Wherein each X independently represents H or F, Z' is Br or I, and Rf is C1-C 12 a perfluoroalkylene group, which optionally contains a chlorine atom, and r is 0 or 1; and

[0075] (c) Non-fluorinated bromoolefins and non-fluorinated iodoolefins, such as vinyl bromide, vinyl iodide, 4-bromo-1-butene and 4-iodo-1-butene.

[0076] Specific examples include, but are not limited to, compounds that meet (b), wherein X is H, for example, compounds where X is H and Rf is a C1 to C3 perfluoroalkylene. Specific examples include: brominated or iodinated trifluoroethylene, 4-bromo-perfluorobutene-1, 4-iodo-perfluorobutene-1, or brominated or iodinated fluoroolefins such as 1-iodo, 2,2-difluoroethylene, 1-bromo-2,2-difluoroethylene, 4-iodo-3,3,4,4,-tetrafluorobutene-1 and 4-bromo-3,3,4,4-tetrafluorobutene-1; 6-iodo-3,3,4,4,5,5,6,6-octafluorohexene-1.

[0077] In some embodiments, the cure site comprises a chlorine atom. Such cure site monomers include those represented by the general formula: CX1X2=CY1Y2, wherein X1, X2 are independently H and F; Y1 is H, F or Cl; and Y2 is Cl, a fluorinated alkyl group (R) having at least one Cl substituent. F ), a fluoroether group having at least one Cl substituent (OR F ), or -CF2-OR F . Fluoroalkyl group (R F ) is typically a partially or fully fluorinated C1-C5 alkyl group. Examples of cure site monomers having chlorine atoms include CF2=CFCl, CF2=CF-CF2Cl, CF2=CF-O-(CF2) n -Cl, n=1–4; CH2=CHCl, CH2=CCl2.

[0078] Typically, the amount of iodine or bromine or chlorine or a combination thereof in the fluoropolymer is between 0.001 wt % and 5 wt %, preferably between 0.01 wt % and 2.5 wt %, or 0.1 wt % to 1 wt %, or 0.2 wt % to 0.6 wt %, relative to the total weight of the fluoropolymer. In one embodiment, the curable fluoropolymer contains between 0.001 wt % and 5 wt %, preferably between 0.01 wt % and 2.5 wt %, or 0.1 wt % to 1 wt %, more preferably between 0.2 wt % and 0.6 wt % iodine, based on the total weight of the fluoropolymer.

[0079] The composition may optionally further comprise a second fluoropolymer lacking a halogen cure site. The amount of the fluoropolymer lacking a halogen cure site is typically less than 50 wt%, 45 wt%, 40 wt%, 35 wt%, 30 wt%, 25 wt%, 20 wt%, 15 wt%, 10 wt% or 5 wt% of the total fluoropolymer. Therefore, the composition has a sufficient amount of fluoropolymer with a halogen cure site to achieve sufficient crosslinking.

[0080] In one embodiment, the composition further comprises a second fluoropolymer derived primarily or solely from two or more perfluorinated comonomers including tetrafluoroethylene (TFE) and one or more unsaturated cyclic perfluorinated alkyl ethers, such as 2,2-bistrifluoromethyl-4,5-difluoro-1,3-dioxole. Such fluoropolymers may be "TEFLON TM AF", "CYTOP TM ” and “HYFLON TM "Commercially available.

[0081] In some embodiments, the second fluoropolymer comprises a nitrile-containing cure site. When a combination of fluoropolymers having different cure sites is utilized, the composition can be characterized as dual cure, comprising different cure sites reactive to different cure systems.

[0082] Although fluoropolymers with halogen cure sites (iodine, bromine, and chlorine) favor UV curing in the case of thermal or electron beam curing, fluoropolymers with nitrile-containing cure sites may alternatively be employed.

[0083] Fluoropolymers having nitrile containing cure sites are known, such as described in US Pat. No. 6,720,360.

[0084] The nitrile-containing cure sites may be reactive toward other cure systems such as, but not limited to, bisphenol cure systems, peroxide cure systems, triazine cure systems, and especially amine cure systems. Examples of nitrile-containing cure site monomers conform to the following formula:

[0085] CF2=CF-CF2-O-Rf-CN;

[0086] CF2=CFO(CF2) r CN;

[0087] CF2=CFO[CF2CF(CF3)O] p (CF2) v OCF(CF3)CN;

[0088] CF2=CF[OCF2CF(CF3)] k O(CF2) u CN;

[0089] Wherein, r represents an integer of 2 to 12; p represents an integer of 0 to 4; k represents 1 or 2; v represents an integer of 0 to 6; u represents an integer of 1 to 6, and Rf is a perfluoroalkylene group or a divalent perfluoroether group. Specific examples of nitrile-containing fluorinated monomers include, but are not limited to, perfluoro(8-cyano-5-methyl-3,6-dioxa-1-octene), CF2=CFO(CF2)5CN, and CF2=CFO(CF2)3OCF(CF3)CN.

[0090] In some embodiments, the amount of nitrile-containing cure site comonomer is typically at least 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt% or 5 wt% and typically not more than 10 wt%; all based on the total weight of the fluoropolymer. Suitable curing agents for nitrile cure sites are known in the art, and include, but are not limited to, (e.g., fluorinated) amidines, amide oximes, and others described in WO2008 / 094758A1 incorporated herein by reference. Representative curing agents include, for example, perfluoroadipic acid bis-tetraphosphonium, methyl sulfone, tetrabutylphosphonium toluene-trifluoromethoxy hexafluoroisopropoxylate, and tetrafluoropropyl amidine.

[0091] In one embodiment, the fluoropolymer having nitrile-containing curing sites can be combined with peroxides and olefinically unsaturated compounds as curing agents, as described in WO 2018 / 107017. In this embodiment, suitable organic peroxides are those that generate free radicals at the curing temperature. Examples include, for example, dialkyl peroxides or bis(dialkyl peroxides), such as di-tert-butyl peroxide having a tertiary carbon atom connected to the peroxy oxygen. Specific examples include 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexyne-3 and 2,5-dimethyl-2,5-di(tert-butyl peroxy)hexane; dicumyl peroxide, dibenzoyl peroxide, tert-butyl perbenzoate, α,α'-bis(tert-butyl peroxy-diisopropylbenzene) and di[1,3-dimethyl-3-(tert-butyl peroxy)-butyl] carbonate. Generally speaking, about 1 to 5 parts of peroxide can be used per 100 parts of fluoropolymer.

[0092] In other embodiments, the composition is substantially free of fluoropolymers having nitrile-containing cure sites. In this embodiment, the composition is also free of curing agents that react with nitrile groups.

[0093] In other embodiments, halogenated chain transfer agents may be used to provide terminal cure sites. Chain transfer agents are compounds that react with growing polymer chains and terminate chain growth. Examples of chain transfer agents reported for use in producing fluoroelastomers include those having the formula RI xThose, wherein R is an x-valent fluoroalkyl or fluoroalkylene group having 1 to 12 carbon atoms, which may be inserted with one or more ether oxygens, and may also contain chlorine and / or bromine atoms. R may be Rf, and Rf may be an x-valent (per)fluoroalkyl or (per)fluoroalkylene group which may be interrupted once or more than once by ether oxygen. Examples include α-ω diiodoalkanes, α-ω diiodofluoroalkanes, and α-ω diiodoperfluoroalkanes, which may contain one or more catenary ether oxygens. "α-ω" means that the iodine atom is located at the terminal position of the molecule. Such compounds may be represented by the general formula XRY, X and Y are I, and R is as described above. Specific examples include diiodomethane, α-ω (or 1,4-) diiodobutane, α-ω (or 1,3-) diiodopropane, α-ω (or 1,5-) diiodopentane, α-ω (or 1,6-) diiodohexane, and 1,2-diiodoperfluoroethane. Other examples include fluorinated diiodoether compounds of the following formula:

[0094] R f -CF(I)-(CX2) n -(CX2CXR) m -OR"fO k -(CXR'CX2) p -(CX2) q -CF(I)-R' f

[0095] wherein X is independently selected from F, H and Cl; R f and R' f independently selected from F and a monovalent perfluoroalkane having 1 to 3 carbons; R is F or a partially fluorinated or perfluorinated alkane containing 1 to 3 carbons; R" f is a divalent fluorinated alkylene group having 1 to 5 carbons or a divalent fluorinated alkylene ether having 1 to 8 carbons and at least one ether linking group; k is 0 or 1; and n, m and p are independently selected from integers of 0-5, wherein n plus m is at least 1, and p plus q is at least 1.

[0096] Fluoropolymers may or may not contain units derived from at least one modifying monomer. The modifying monomer can introduce branching sites into the polymer architecture. Typically, the modifying monomer is a diene, diene ether or polyether. The diene and diene (poly) ether can be perfluorinated, partially fluorinated or non-fluorinated. Preferably, they are perfluorinated. Suitable perfluorinated diene ethers include those represented by the general formula:

[0097] CF2=CF-(CF2) n -O-(Rf)-O-(CF2) m -CF=CF2

[0098] wherein n and m are independently 1 or 0, and wherein Rf represents a perfluorinated linear or branched, cyclic or acyclic aliphatic or aromatic hydrocarbon residue which may be interrupted by one or more oxygen atoms and contains up to 30 carbon atoms. Particularly suitable perfluorinated bis-olefin ethers are divinyl ethers represented by the formula:

[0099] CF2=CF-O-(CF2) n -O-CF=CF2

[0100] wherein n is an integer between 1 and 10, preferably 2 to 6, for example n may be 1, 2, 3, 4, 5, 6 or 7. More preferably, n represents an even integer, for example 1, 3, 5 or 7.

[0101] Other specific examples include bisolefin ethers according to the general formula:

[0102] CF2=CF-(CF2) n -O-(CF2) p -O-(CF2) m -CF=CF2

[0103] wherein n and m are independently 1 or 0, and p is an integer from 1 to 10 or from 2 to 6. For example, n can be selected to represent 1, 2, 3, 4, 5, 6 or 7, preferably 1, 3, 5 or 7.

[0104] Other suitable perfluorinated bisolefin ethers can be represented by the formula:

[0105] CF2=CF-(CF2) p -O-(R af O) n (R bf O) m -(CF2) q -CF=CF2

[0106] Where R af and R bf R is a different straight-chain or branched perfluoroalkylene group having 1 to 10 carbon atoms, in particular 2 to 6 carbon atoms, which may or may not be interrupted by one or more oxygen atoms. af and / or R bf It may also be a perfluorinated phenyl group or a substituted phenyl group; n is an integer between 1 and 10, and m is an integer between 0 and 10, preferably m is 0. In addition, p and q are independently 1 or 0.

[0107] In another embodiment, the perfluorinated bisolefin ether can be represented by the formula just described, wherein m, n, and p are zero and q is 1-4.

[0108] The modifying monomers can be prepared by methods known in the art and are commercially available, for example, from Anles Ltd., St. Petersburg, Russia.

[0109] Preferably, no modifier is used or only used in lower amounts. Typical amounts include 0 wt % to 5 wt % or 0 wt % to 1.4 wt % based on the total weight of the fluoropolymer. The modifier may be present, for example, in an amount of about 0.1 wt % to about 1.2 wt % or about 0.3 wt % to about 0.8 wt % based on the total weight of the fluoropolymer. Combinations of modifiers may also be used.

[0110] Fluoropolymers may contain partially fluorinated or non-fluorinated comonomers and combinations of partially fluorinated or non-fluorinated comonomers, but this is not preferred. Typical partially fluorinated comonomers include but are not limited to 1,1-difluoroethylene (vinylidene fluoride, VDF) and fluoroethylene (VF) or trifluorochloroethylene or trichlorofluoroethylene. Examples of non-fluorinated comonomers include but are not limited to ethylene and propylene. Based on the total weight of the fluoropolymer, the amount of units derived from these comonomers includes 0 wt % to 8 wt %. In some embodiments, based on the total weight of the fluoropolymer, the concentration of such comonomers is not more than 7 wt %, 6 wt %, 5 wt %, 4 wt %, 3 wt %, 2 wt % or 1 wt %.

[0111] In a preferred embodiment, the curable fluoropolymer is a perfluoroelastomer comprising repeating units derived (only) from perfluorinated comonomers, but may contain units derived from cure site monomers and optionally modifying monomers. The cure site monomers and modifying monomers may be partially fluorinated, unfluorinated or perfluorinated, and are preferably perfluorinated. The perfluoroelastomer may contain 69% to 73%, 74% or 75% fluorine by weight (based on the total amount of perfluoroelastomer). The fluorine content can be achieved by selecting the comonomers and their respective amounts.

[0112] Such highly fluorinated amorphous fluoropolymers are typically insoluble in hydrogen-containing organic liquids (e.g., they are insoluble in any of methyl ethyl ketone ("MEK"), tetrahydrofuran ("THF"), ethyl acetate, or N-methylpyrrolidone ("NMP")) to an extent of at least 1 weight percent at room temperature and standard pressure.

[0113] Fluoropolymers can be prepared by methods known in the art, such as bulk, suspension, solution or aqueous emulsion polymerization. Various emulsifiers can be used as described in the art, including, for example, 3H-perfluoro-3-[(3-methoxy-propoxy) propionic acid. For example, the polymerization process can be implemented by free radical polymerization of monomers that are either alone or in the form of solutions, emulsions or dispersions in organic solvents or water. Seed polymerization may or may not be used. Useable curable fluoroelastomers also include commercially available fluoroelastomers, especially perfluoroelastomers.

[0114] Fluoropolymers may have a unimodal or bimodal or multimodal weight distribution. Fluoropolymers may or may not have a core-shell structure. Core-shell polymers are polymers in which at the end of polymerization, typically after consumption of at least 50 mol % of the comonomer, the comonomer composition or comonomer ratio or reaction rate is changed to produce a shell of different composition.

[0115] The fluorine content of the fluoropolymer is typically at least 60, 65, 66, 67, 68, 69, or 70 weight percent of the fluoropolymer, and typically no greater than 76, 75, 74, or 73 weight percent.

[0116] Fluoropolymer composition as herein described contains one or more ethylenically unsaturated curing agents.Based on the gross weight of fluoropolymer, ethylenically unsaturated curing agent is usually present in an amount of at least 1 wt %, 1.5 wt % or 2 wt %.For compositions with lower crosslinking amount, ethylenically unsaturated curing agent can be present in lower amount, such as at least 0.005 wt %, 0.1 wt %, 0.2 wt %, 0.3 wt %, 0.5 wt %.Based on the gross weight of fluoropolymer, the maximum amount of ethylenically unsaturated curing agent is usually not more than 10 wt %, 9 wt %, 8 wt %, 7 wt %, 6 wt % or 5 wt %.

[0117] The ethylenically unsaturated group of the curing agent is typically a (meth)acryloyl group, including (meth)acrylate RCH=CHCOO- and (meth)acrylamide RCH=CHCONH-, wherein R is methyl or hydrogen; an alkenyl group, including vinyl (CH2=CH-); or an alkynyl group.

[0118] Available multi-(meth)acrylate curing agents include:

[0119] (a) Monomers containing di(meth)acryloyl groups, such as 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol monoacrylate monomethacrylate, ethylene glycol diacrylate, alkoxylated aliphatic diacrylates, alkoxylated cyclohexanedimethanol diacrylate, alkoxylated hexanediol diacrylate, alkoxylated neopentyl glycol diacrylate, caprolactone-modified neopentyl glycol hydroxypivalate diacrylate, hexylene glycol diacrylate, alkoxylated cyclohexanedimethanol diacrylate, alkoxylated hexanediol diacrylate, alkoxylated neopentyl glycol diacrylate, caprolactone-modified neopentyl glycol hydroxypivalate diacrylate, caprolactone-modified Lactone-modified neopentyl glycol hydroxypivalate diacrylate, cyclohexanedimethanol diacrylate, diethylene glycol diacrylate, dipropylene glycol diacrylate, ethoxylated bisphenol A diacrylate, hydroxypivalaldehyde-modified trimethylolpropane diacrylate, neopentyl glycol diacrylate, polyethylene glycol diacrylate, propoxylated neopentyl glycol diacrylate, tetraethylene glycol diacrylate, tricyclodecane dimethanol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate;

[0120] (b) monomers containing a tri(meth)acryloyl group, such as glycerol triacrylate, trimethylolpropane triacrylate, ethoxylated triacrylates (e.g., ethoxylated trimethylolpropane triacrylate), propoxylated triacrylates (e.g., propoxylated glycerol triacrylate, propoxylated trimethylolpropane triacrylate), trimethylolpropane triacrylate, tris(2-hydroxyethyl)-isocyanurate triacrylate;

[0121] (c) Monomers containing higher functionality (meth)acryloyl groups, such as ditrimethylolpropane tetraacrylate, dipentaerythritol pentaacrylate, pentaerythritol triacrylate, ethoxylated pentaerythritol tetraacrylate and caprolactone-modified dipentaerythritol hexaacrylate.

[0122] In some embodiments, the ethylenically unsaturated curing agent comprises at least two or three ethylenically unsaturated groups. The maximum number of ethylenically unsaturated groups is typically 3, 4, 5 or 6. In this embodiment, the ethylenically unsaturated groups are preferably alkenyl groups. Therefore, in some embodiments, the composition is substantially free of (meth)acrylate groups.

[0123] The ethylenically unsaturated curing agent may be linear, branched or contain cyclic groups.The ethylenically unsaturated curing agent may be aliphatic or aromatic. Examples of useful ethylenically unsaturated curing agents include triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, tri(methylallyl) isocyanurate, tri(diallylamine)-s-triazine, triallyl phosphite, (N,N')-diallylacrylamide, hexallylphosphoramide, (N,N,N,N)-tetraalkyltetraphthalamide; (N,N,N',N'-tetraallylmalonamide, trivinyl isocyanurate, N,N'-m-phenylene bismaleimide, diallyl phthalate, and tris(5-norbornene-2-methylene)cyanurate. In some embodiments, the ethylenically unsaturated curing agent is heterocyclic, such as in the case of triallyl isocyanurate (TAIC).

[0124] In some embodiments, the ethylenically unsaturated curing agent comprises a silicone-containing moiety, such as a silane or a siloxane. When the curing agent comprises a silicone-containing moiety, the curing agent may also promote adhesion of the fluoropolymer to the substrate.

[0125] Suitable ethylenically unsaturated curing agents comprising a silicone-containing moiety include, for example, diallyldimethylsilane; and 1,3-divinyltetramethyldisiloxane.

[0126] In certain embodiment, the ethylenically unsaturated curing agent comprises at least one ethylenically unsaturated group and at least one alkoxysilane group. Suitable curing agents include, for example, (meth)acryloylalkoxysilanes, such as 3-(methacryloyloxy)propyltrimethoxysilane, 3-(methacryloyloxy)propylmethyldimethoxysilane, 3-(acryloyloxypropyl)methyldimethoxysilane, 3-(methacryloyloxy)propyldimethylmethoxysilane and 3-(acryloyloxypropyl)dimethylmethoxysilane. In some embodiments, the amount of (meth)acryloylalkoxysilane is at least 2 weight %, 3 weight %, 4 weight % or 5 weight % to achieve a highly crosslinked fluoropolymer.

[0127] Suitable alkenyl alkoxysilanes include vinyldimethylethoxysilane, vinylmethyldiacetoxysilane, vinylmethyldiethoxysilane, vinyltriacetoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltrimethoxysilane, vinyltriphenoxysilane, vinyltri-tert-butoxysilane, vinyltriisobutoxysilane, vinyltriisopropenoxysilane, vinyltri(2-methoxyethoxy)silane and allyltriethoxysilane.

[0128] In some embodiments, the ethylenically unsaturated curing agent may have the general formula

[0129] X 1 -L 1-SiR m (OR 1 ) 3-m ;

[0130] Where X 1 is an ethylenically unsaturated group, such as (meth)acryloyl or vinyl;

[0131] L 1 is an organic divalent linking group having 1 to 12 carbon atoms;

[0132] R is independently C1-C4 alkyl and most typically methyl or ethyl;

[0133] R 1 is independently H or C1-C4 alkyl and most typically methyl or ethyl; and

[0134] m is in the range of 0 to 2.

[0135] In typical embodiments, L 1 In some embodiments, L 1 is an alkylene group having 1, 2 or 3 carbon atoms. 1 Contains or consists of an aromatic group, such as a phenyl group or a (eg C1-C4)alkylphenyl group.

[0136] The composition may contain a single ethylenically unsaturated curing agent or a combination of ethylenically unsaturated curing agents as just described.

[0137] The compositions described herein also include an electron donor group or a precursor thereof.The electron donor group may be present on the same compound, such as in the case of an aminoolefin or vinylaniline, or the electron donor group may be present as a separate compound.

[0138] The fluoropolymer and / or curing agent contain a chromophore, ie, an atom or group that absorbs light at a specified frequency. In some embodiments, the fluoropolymer and / or curing agent may not have sufficient absorbance alone, but have sufficient absorbance when combined with each other.

[0139] In some embodiments, the fluoropolymer, curing agent, or a combination thereof has an absorbance of at least 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0 at a wavelength in the range of 190 nm to 400 nm. In some embodiments, such absorbance is measured at a wavelength of at least 200 nm, 210 nm, 220 nm, 230 nm, or 240 nm. In some embodiments, such absorbance is measured at a wavelength of no more than 350 nm, 340 nm, 330 nm, 320 nm, 310 nm, or 290 nm. In other embodiments, the fluoropolymer, curing agent, or a combination thereof has an absorbance of at least 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0 at a wavelength in the range of 150 nm to 200 nm.

[0140] Although not intending to be bound by theory, it is speculated that upon exposure to appropriate wavelength and intensity of actinic (e.g., ultraviolet) radiation, the halogen atoms of the cure sites of the fluoropolymer become excited and ionized. The ionized halogen atoms react with the electron donor groups, thereby replacing the previous halogen atoms with protonated cure sites. Such protonated cure sites are covalently bonded to the ethylenically unsaturated groups of the curing agent.

[0141] Although other electron donor groups may be used, the compound comprising the electron donor group is typically an amine or a precursor thereof. Suitable amines include primary amines, secondary amines, tertiary amines, and combinations thereof. The amines may be aliphatic or aromatic. Amine compounds may also be used to provide a crosslinked fluoropolymer layer by curing a fluoropolymer having (e.g., nitrile) curing sites using an amine curing agent (e.g., heat).

[0142] Exemplary amine compounds include diaminohexane, N,N,N',N'-tetramethyl-1,4-diaminobutane (TMDAB); N,N-dimethylaniline; triethylenetetramine; and diethylenetriamine. In some embodiments, the amine groups are separated by alkylene groups having at least 3, 4, 5, or 6 (e.g., carbon) atoms. Typically, the number of (e.g., carbon) atoms is not greater than 12. When the amine compound has insufficient chain length, it may be a less effective electron donor group. The alkylene group may optionally contain a substituent, such as a siloxane, provided that the compound is an electron donor or a precursor thereof.

[0143] In some embodiments, the electron donor compound can be characterized as an electron donor precursor, meaning that when the compound is initially mixed with the fluoropolymer, it is not an electron donor. However, the precursor compound decomposes or otherwise reacts to form a (eg, amine) electron donor prior to or during curing.

[0144] Electron donor precursors include nitrogen-containing nucleophilic compounds such as heterocyclic secondary amines; guanidines; compounds that decompose in situ at temperatures between 40°C and 330°C to produce guanidines; compounds that decompose in situ at temperatures between 40°C and 330°C to produce primary or secondary amines; nucleophilic compounds of the formula R1-NH-R2, wherein R1 is H-, C1-C 10 an aliphatic hydrocarbon group, or an aryl group having a hydrogen atom at the α position, R2 is C1-C 10 an aliphatic hydrocarbon group, an aryl group having a hydrogen atom at the α position, -CONHR3, -NHCO2R3 or -OH', and R3 is C1-C 10 an aliphatic hydrocarbon group; and a substituted amidine of the formula HN=CR4NR5R6, wherein R4, R5, R6 are independently H-, an alkyl or aryl group, and wherein at least one of R4, R5 and Re is not H-.

[0145] As used herein, "heterocyclic secondary amine" refers to an aromatic or aliphatic cyclic compound having at least one secondary amine nitrogen contained within the ring. Such compounds include, for example, pyrrole, imidazole, pyrazole, 3-pyrroline, and pyrrolidine.

[0146] Guanidine is a compound derived from guanidine, ie a compound containing the group -NHCNHNH-, such as, but not limited to, diphenylguanidine, diphenylguanidine acetate, aminobutylguanidine, biguanidine, isopentylguanidine, di-sigma-tolylguanidine, o-tolylbiguanidine and triphenylguanidine.

[0147] Other compounds that decompose in situ at temperatures between 40°C and 330°C to produce primary or secondary amines include, but are not limited to, disubstituted or polysubstituted ureas (e.g., 1,3-dimethylurea); N-alkyl or N-dialkylcarbamates (e.g., N-(tert-butoxycarbonyl)propylamine); disubstituted or polysubstituted thioureas (e.g., 1,3-dimethyl-thiourea); aldehyde-amine condensation products (e.g., 1,3,5-trimethylhexahydro-1,3,5-triazine); N,N'-dialkylphthalamide derivatives (e.g., N,N'-dimethylphthalamide); and amino acids.

[0148] When utilizing a thermally activated electron donor precursor compound as just described, the composition is typically heated prior to and / or during curing.

[0149] Other types of amine electron donors include bis(aminophenol) and bis(aminothiophenol) represented by the formula:

[0150]

[0151] as well as

[0152]

[0153] and a tetraamine represented by the formula:

[0154]

[0155] Wherein A is SO2, O, CO, an alkyl group having 1 to 6 carbon atoms, a perfluoroalkyl group having 1 to 10 carbon atoms, or a carbon-carbon bond connecting two aromatic rings. The amino and hydroxyl groups in the above formula can be interchanged in the meta and para positions relative to the group A.

[0156] In some embodiments, the amine electron donor compound is an aziridine compound. In some embodiments, the aziridine compound comprises at least two aziridine groups. The aziridine compound may comprise 3, 4, 5, 6 or more than 6 aziridine groups. The aziridine compound may be represented by the following structure:

[0157]

[0158] wherein R is a core moiety having a valence of Y;

[0159] L is a chemical bond, a divalent atom or a divalent linking group;

[0160] R1, R2, R3 and R4 are independently hydrogen or C1-C4 alkyl (eg, methyl); and

[0161] Y is usually 2, 3 or more.

[0162] In some embodiments, R is -SO2-. In some embodiments, RL is the residue of a poly(meth)acrylate compound. In some embodiments, L is a C1-C4 alkylene group, which is optionally substituted with one or more (e.g., adjacent or pendant) oxygen atoms, thereby forming an ether linking group or an ester linking group. In typical embodiments, R1 is methyl and R2, R3 and R4 are hydrogen.

[0163] Representative aziridine compounds include trimethylolpropane tris[β-(N-aziridinyl)-propionate, 2,2-bishydroxymethylbutanol tris[3-(1-aziridine)propionate]; 1-(aziridin-2-yl)-2-oxabut-3-ene; and 4-(aziridin-2-yl)-but-1-ene; and 5-(aziridin-2-yl)-pent-1-ene.

[0164] In some embodiments, polyaziridine compounds can be prepared by reacting divinyl sulfone with alkylene (e.g., ethylene) imine, as described in US 3,235,544 (Christena). A representative compound is di(2-propylene iminoethyl) sulfone, as described below:

[0165]

[0166] The above-mentioned polyaziridine compound comprises at least two aziridine groups when the compound is added to the coating composition. In other embodiments, the polyaziridine compound does not comprise two aziridine groups when the compound is added to the composition, and it still forms polyaziridine in situ. For example, a compound comprising a single aziridine group and a single (meth)acrylate group can form a dimer or oligomerization through the reaction of the (meth)acrylate group, thereby forming a polyaziridine (i.e., diaziridine) compound.

[0167] In some embodiments, the composition comprises an electron donor compound having at least one (e.g., primary, secondary, tertiary) amine group and at least one organosilane (e.g., alkoxysilane) group. Such compounds can improve bonding and independently crosslink the fluoroelastomers described herein, thereby providing a second fluoropolymer crosslinking mechanism. By combining the use of an ethylenically unsaturated curing agent with an amino-substituted organosilane, a highly crosslinked fluoropolymer can be provided using lower concentrations of curing agent and electron donor compound.

[0168] In some embodiments, the amine may be characterized as an amino-substituted organosilane ester or ester equivalent, which carries at least 1, preferably 2 or 3 ester or ester equivalent groups on the silicon atom. Ester equivalents are known to those skilled in the art and include compounds such as silane amides (RNR'Si), silane alkanoates (RC(O)OSi), Si-O-Si, SiN(R)-Si, SiSR and RCONR'Si compounds, which are replaced by R"OH through heat and / or catalysis. R and R' are independently selected and may include hydrogen, alkyl, aralkyl, alkenyl, alkynyl, cycloalkyl and substituted analogs such as alkoxyalkyl, aminoalkyl and alkylaminoalkyl. R" may be the same as R and R', except that it may not be H. These ester equivalents may also be cyclic, such as those derived from ethylene glycol, ethanolamine, ethylenediamine (e.g., N-[3-(trimethoxysilyl)propylene]ethylenediamine) and their amides.

[0169] Another such cyclic example of an ester equivalent is

[0170]

[0171] In this cyclic example, R' is as defined in the preceding sentence, except that it may not be an aryl group. 3-Aminopropylalkoxysilanes are well known to cyclize upon heating and these RNHSi compounds will find use in the present invention. Preferred amino-substituted organosilane esters or ester equivalents have an ester group such as a methoxy group, which is easily volatilized with methanol. The amino-substituted organosilane must have at least one ester equivalent; for example, it may be a trialkoxysilane.

[0172] For example, an amino-substituted organosilane may have the formula:

[0173] (Z2N-L-SiX'X”X”'), where

[0174] Z is hydrogen, alkyl or substituted aryl or alkyl, including amino-substituted alkyl; and L is a divalent straight chain C1-12 alkylene or may contain C3-8 cycloalkylene, 3-8 membered heterocyclic alkylene, C2-12 alkenylene, C4-8 cycloalkenylene, 3-8 membered heterocyclic alkenylene or heteroarylene units; and each of X', X' and X'' is C1-18 alkyl, halogen, C1-8 alkoxy, C1-8 alkylcarbonyloxy or amino group, provided that at least one of X', X' and X'' is a labile group. In addition, any two or all of X', X' and X'' may be joined by covalent bonds. The amino group may be an alkylamino group.

[0175] L may be divalent aromatic or may be intercalated with one or more divalent aromatic groups or heteroatom groups. Aromatic groups may include heteroaromatics. The heteroatom is preferably nitrogen, sulfur or oxygen. L is optionally substituted by the following groups: C1-4 alkyl, C2-4 alkenyl, C2-4 alkynyl, C1-4 alkoxy, amino, C3-6 cycloalkyl, 3-6 membered heterocycloalkyl, monocyclic aryl, 5-6 membered heteroaryl, C1-4 alkylcarbonyloxy, C1-4 alkyloxycarbonyl, C1-4 alkylcarbonyl, formyl, C1-4 alkylcarbonylamino or C1-4 aminocarbonyl. L is also optionally interrupted by -O-, -S-, -N(Rc)-, -N(Rc)-C(O)-, -N(Rc)-C(O)-O-, -OC(O)-N(Rc)-, -N(Rc)-C(O)-N(Rd)-, -OC(O)-, -C(O)-O-, or -OC(O)-O-. Each of Rc and Rd is independently hydrogen, alkyl, alkenyl, alkynyl, alkoxyalkyl, aminoalkyl (primary, secondary, or tertiary), or haloalkyl.

[0176] Examples of amino-substituted organosilanes include 3-aminopropyltrimethoxysilane (SILQUEST A-1110), 3-aminopropyltriethoxysilane (SILQUEST A-1100), bis(3-trimethoxysilylpropyl)amine, bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)n-methylamine, 3-(2-aminoethyl)aminopropyltrimethoxysilane (SILQUEST A-1120), SILQUEST A-1130, (aminoethylaminomethyl)phenethyltrimethoxysilane, (aminoethylaminomethyl)phenethyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane (SILQUEST A-2120), bis-(γ-triethoxysilylpropyl)amine (SILQUEST A-2130), and bis(γ-triethoxysilylpropyl)amine (SILQUEST A-2140). A-1170), N-(2-aminoethyl)-3-aminopropyltributoxysilane, 6-(aminohexylaminopropyl)trimethoxysilane, 4-aminobutyltrimethoxysilane, 4-aminobutyltriethoxysilane, p-(2-aminoethyl)phenyltrimethoxysilane, 3-aminopropyltris(methoxyethoxyethoxy)silane, 3-aminopropylmethyldiethoxysilane, oligomeric aminosilanes such as DYNASYLAN 1146. 3-(N-Methylamino)propyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyldimethylmethoxysilane, 3-aminopropyldimethylethoxysilane, and the following cyclic compounds:

[0177]

[0178] Bis-silylurea [RO)3Si(CH2)NR]2C=O is another example of an amino-substituted organosilane ester or ester equivalent.

[0179] In some embodiments, the curing agent may contain an amino group with a latent functional group. An example of such a curing agent is a blocked amine group such as

[0180] R 3 —N=C(R 1 )(R 2 )

[0181] Where R 1 and R 2 are independently selected from a linear or branched alkyl group containing 1 to 6 carbon atoms. In a typical embodiment, R1 is methyl, and R2 is a straight or branched chain alkyl group containing at least 2, 3, 4, 5 or 6 carbon atoms. 3 Typically an organic group (eg, having a molecular weight of less than 500 g / mol, 450 g / mol, 400 g / mol, 350 g / mol, 300 g / mol, or 250 g / mol).

[0182] The blocked amine can be activated by moisture provided by water or humidity adsorbed on the surface of the substrate to be coated. Deblocking begins within a few minutes and is generally complete within a few hours (e.g., two hours). During deblocking, —N═C(R 1 )(R 2 ) groups are converted to -NH2, which can then react with the fluoropolymer (e.g., nitrile cure site).

[0183] In some embodiments, the curing agent comprises a blocked amine group and an alkoxysilane group. Such blocked amine curing agents can be characterized by the following general formula:

[0184] (R 4 O)3—Si—(CH2) m —N=C(R1)(R2)

[0185] Where R 1 and R 2 R is independently selected from the above-mentioned straight chain or branched alkyl groups containing 1 to 6 carbon atoms. 1 are independently selected from a linear or branched alkyl group containing 1 to 6 carbon atoms, m is an integer from 1 to 4, and each R 4 are independently C1 or C2 alkyl groups.

[0186] An exemplary curing agent comprising a capped amine group and an alkoxysilane group is N-(1,3-dimethylbutylene)aminopropyltriethoxysilane, as shown below:

[0187]

[0188] This type of curing agent can be "3M TM Dynamer TM Rubber curing agent RC5125" is available from Gelest and 3M. Capped amines are additional examples of electron donor precursors.

[0189] In some embodiments, the amine curing agent comprises an aziridine group and an alkoxysilane group. Such compounds are known, for example, from US 3,243,429; which is incorporated herein by reference. The aziridine alkoxysilane compound may have the general structure:

[0190]

[0191] wherein R" is hydrogen or C1-C4 alkyl (e.g. methyl);

[0192] X is a chemical bond, a divalent atom or a divalent linking group;

[0193] n is 0, 1 or 2;

[0194] m is 1, 2 or 3; and

[0195] And the sum of n+m is 3.

[0196] One representative compound is 3-(2-methylaziridinyl)ethylcarboxypropyltriethoxysilane.

[0197] Various other suitable aziridine crosslinkers are known, such as described in WO 2014 / 075246, published on May 22, 2014, incorporated herein by reference, and "NEW GENERATION OF MULTIFUNCTIONAL CROSSLINKERS", (see https: / / www.pstc.org / files / public / Milker00.pdf).

[0198] The composition comprises a single (eg, amine) electron donor compound or a combination of amine electron donor compounds may be present.

[0199] The amount of the (e.g., amine) electron donor compound is typically at least 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5% by weight solids (i.e., excluding the solvent of the coating composition). In some embodiments, the amount of the (e.g., amine) electron donor compound is no greater than 5%, 4.5%, 4%, 3.5%, or 3% by weight solids.

[0200] In some embodiments, the fluoropolymer composition further comprises an alkoxysilane compound lacking amine functionality. In some embodiments, such alkoxysilanes may be characterized as "non-functional" having the following chemical formula:

[0201] R 2 Si(OR 1 ) m

[0202] in R 1 is independently the alkyl group described above;

[0203] R 2 are independently hydrogen, alkyl, aryl, aralkyl or OR 1 ;as well as

[0204] m is 1-3, and is usually 2 or 3 as previously described.

[0205] Suitable formula R 2 Si(OR 1 ) m Alkoxysilanes include, but are not limited to, tetraalkoxysilanes, trialkoxysilanes or dialkoxysilanes, and any combination or mixture thereof. Representative alkoxysilanes include propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, amyltrimethoxysilane, amyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, dimethyldimethoxysilane, and dimethyldiethoxysilane.

[0206] Preferably, the alkyl group of the alkoxysilane contains 1 to 6, more preferably 1 to 4 carbon atoms. Preferred alkoxysilanes for use herein are selected from tetramethoxysilane, tetraethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, and any mixture thereof. Preferred alkoxysilanes for use herein include tetraethoxysilane (TEOS). Alkoxysilanes lacking organic functional groups in the method for preparing the coating composition may be partially hydrolyzed, such as in the case of partially hydrolyzed tetramethoxysilane (TMOS) purchased from Mitsubishi Chemical Company under the trade name "MS-51".

[0207] When present, the amount of the alkoxysilane compound lacking (amine / electron donor) functionality (e.g., TESO) is typically at least 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5% by weight solids (i.e., excluding the solvent of the coating composition). In some embodiments, the amount of the alkoxysilane compound lacking functionality is no greater than 5%, 4.5%, 4%, 3.5%, or 3% by weight solids.

[0208] In some embodiments, the compositions described herein include a (e.g., UV) curing system comprising an olefinically unsaturated compound in combination with an electron donor compound (such as an amine) in the absence of an organic peroxide. The organic peroxide is an electron acceptor and therefore competes with ionized halogen atoms, thereby reducing the crosslinking of the fluoropolymer. In some embodiments, the composition is also substantially free of other electron acceptors that reduce crosslinking.

[0209] In other embodiments, the aminoorganosilane ester compounds or ester equivalents may be used to (e.g., UV) cure and / or thermally cure fluoropolymers in the absence of ethylenically unsaturated compounds, as described in PCT / US2019 / 036460, which is incorporated herein by reference.

[0210] Fluoropolymer (coating solution) composition comprises at least one solvent. The solvent can dissolve the fluoropolymer. Based on the total weight of the coating solution composition, the solvent is usually present in an amount of at least 25% by weight. In some embodiments, based on the total weight of the coating solution composition, the solvent is present in an amount of at least 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or more.

[0211] Based on the weight of the total coating solution composition, the fluoropolymer (coating solution) composition generally comprises at least 0.01 wt%, 0.02 wt%, 0.03 wt%, 0.03 wt%, 0.04 wt%, 0.04 wt%, 0.05 wt%, 0.06 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt% or 1 wt% of the fluoropolymer. In some embodiments, the fluoropolymer coating solution composition comprises at least 2 wt%, 3 wt%, 4 wt% or 5 wt% of the fluoropolymer. In some embodiments, the fluoropolymer coating solution composition comprises at least 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt% of the fluoropolymer. Based on the weight of the total coating solution composition, the fluoropolymer coating solution composition generally comprises no more than 50 wt%, 45 wt%, 40 wt%, 35 wt%, 30 wt%, 25 wt% or 20 wt% of the fluoropolymer.

[0212] The optimum amount of solvent and fluoropolymer may depend on the final application and may vary. For example, to provide a thin coating, a very dilute fluoropolymer solution in the solvent may be required, such as an amount of 0.01 wt % to 5 wt % fluoropolymer. In addition, for applications in spraying, low viscosity compositions may be preferred over solutions with high viscosity. The concentration of fluoropolymer in the solution affects the viscosity and may be adjusted accordingly. An advantage of the present disclosure is that solutions with high concentrations of fluoropolymer may also be prepared that still provide clear liquid compositions with low viscosity.

[0213] In some embodiments, the fluoropolymer coating solution composition may be a liquid. The liquid may have a viscosity of, for example, less than 2,000 mPas at room temperature (20°C + / - 2°C). In other embodiments, the fluoropolymer coating solution composition is a paste. The paste may have a viscosity of, for example, 2,000 to 100.000 mPas at room temperature (20°C + / - 2°C).

[0214] The solvent is liquid under ambient conditions and generally has a boiling point greater than 50° C. Preferably, the boiling point of the solvent is below 200° C. so that it can be easily removed. In some embodiments, the boiling point of the solvent is below 190° C., 180° C., 170° C., 160° C., 150° C., 140° C., 130° C., 120° C., 110° C., or 100° C.

[0215] The solvent is partially fluorinated or perfluorinated. Thus, the solvent is non-aqueous. A variety of partially fluorinated or perfluorinated solvents are known, including perfluorocarbons (PFCs), hydrochlorofluorocarbons (HCFCs), perfluoropolyethers (PFPEs) and hydrofluorocarbons (HFCs), as well as fluorinated ketones and fluorinated alkylamines.

[0216] In some embodiments, the solvent has a global warming potential (GWP, 100-year ITH) of less than 1000, 900, 800, 700, 600, 500, 400, 300, 200, or 100. The GWP is typically greater than 0 and can be at least 10, 20, 30, 40, 50, 60, 70, or 80.

[0217] As used herein, GWP is a relative measure of the global warming potential of a compound based on the compound's structure. The GWP of a compound, defined by the Intergovernmental Panel on Climate Change (IPCC) in 1990 and updated in subsequent reports, is calculated as the warming caused by the release of 1 kg of the compound relative to the warming caused by the release of 1 kg of CO2 over a specified integral time horizon (ITH).

[0218]

[0219] where F is the radiative forcing per unit mass of the compound (the change in the radiative flux through the atmosphere due to IR absorption by the compound), C o is the atmospheric concentration of the compound at the initial time, τ is the atmospheric lifetime of the compound, t is the time, and x is the compound of interest.

[0220] In some embodiments, the solvent comprises a partially fluorinated ether or a partially fluorinated polyether. The partially fluorinated ether or polyether can be linear, cyclic or branched. Preferably, it is branched. Preferably, it comprises a non-fluorinated alkyl group and a perfluorinated alkyl group, and more preferably, the perfluorinated alkyl group is branched.

[0221] In one embodiment, the partially fluorinated ether or polyether solvent conforms to the formula:

[0222] Rf-OR

[0223] wherein Rf is a perfluorinated or partially fluorinated alkyl or (poly)ether group and R is a non-fluorinated or partially fluorinated alkyl group. Typically, Rf may have from 1 to 12 carbon atoms. Rf may be a primary, secondary or tertiary fluorinated or perfluorinated alkyl residue. This means that when Rf is a primary alkyl residue, the carbon atom attached to the ether atom contains two fluorine atoms and is bonded to another carbon atom of the fluorinated or perfluorinated alkyl chain. In this case, Rf would correspond to R f 1 -CF2- and the polyether can be described by the general formula: R f 1 -CF2-OR.

[0224] When Rf is a secondary alkyl residue, the carbon atom attached to the ether atom is also attached to one fluorine atom and two carbon atoms of a partially fluorinated and / or perfluorinated alkyl chain and Rf satisfies (R f 2 R f 3 )CF-. The polyether will conform to (R f 2 R f 3 )CF-OR.

[0225] When Rf is a tertiary alkyl residue, the carbon atom attached to the ether atom is also attached to three moieties and / or three carbon atoms of a perfluorinated alkyl chain and Rf complies with (R f 4 R f 5 R f 6 )-C-. The polyether then complies with (R f 4 R f5 R f 6 )-C-OR. f 1 ; R f 2 ; R f 3 ; R f 4 ; R f 5 ; R f 6 The polyethers meet the definition of Rf and are perfluorinated or partially fluorinated alkyl groups which may be interrupted once or more than once by ether oxygens. They may be linear or branched or cyclic. Combinations of polyethers may also be used, and combinations of primary, secondary and / or tertiary alkyl residues may also be used.

[0226] Examples of solvents containing partially fluorinated alkyl groups include C3F7OCHFCF3 (CAS No. 3330-15-2).

[0227] An example of a solvent in which Rf comprises a polyfluorinated (poly)ether is C3F7OCF(CF3)CF2OCHFCF3 (CAS No. 3330-14-1).

[0228] In some embodiments, the partially fluorinated ether solvent conforms to the formula:

[0229] CpF2p+1-O-CqH2q+1

[0230] wherein q is an integer from 1 to 5, for example, 1, 2, 3, 4 or 5, and p is an integer from 5 to 11, for example, 5, 6, 7, 8, 9, 10 or 11. Preferably, C p F 2p+1 Preferably, C p F 2p+1 is branched, and q is 1, 2 or 3.

[0231] Representative solvents include, for example, 1,1,1,2,2,3,4,5,5,5-decafluoro-3-methoxy-4-(trifluoromethyl)pentane and 3-ethoxy-1,1,1,2,3,4,4,5,5,6,6,6-dodecafluoro-2-(trifluoromethyl)hexane. Such solvents can be purchased, for example, from 3M Company, St. Paul, MN, under the trade name NOVEC.

[0232] Fluorinated (e.g., ethers and polyethers) solvents can be used alone, or they can be used in combination with other solvents, which can be fluorochemical solvents or non-fluorochemical solvents. When non-fluorochemical solvents are combined with fluorinated solvents, the concentration of the non-fluorochemical solvent is generally less than 30 wt%, 25 wt%, 20 wt%, 15 wt%, 10 wt%, or 5 wt% relative to the total amount of solvent. Representative non-fluorochemical solvents include ketones such as acetone, MEK, methyl isobutyl ketone, methyl amyl ketone, and NMP; ethers such as tetrahydrofuran, 2-methyltetrahydrofuran, and methyltetrahydrofurfuryl ether; esters such as methyl acetate, ethyl acetate, and butyl acetate; cyclic esters such as delta-valerolactone and gamma-valerolactone.

[0233] In some embodiments, the composition further comprises crystallized fluoropolymer particles.

[0234] In one embodiment, such coating compositions are prepared by blending a latex containing crystallized fluoropolymer particles with a latex containing amorphous fluoropolymer particles. The fluoropolymer particles typically have a small average particle size, such as less than 400 nm, but may be larger if, particularly when the applied coating will be rubbed after curing. For example, the fluoropolymer particle size range may be from about 50 to about 1000 nm, or from about 50 to about 400 nm, or from about 50 to about 200 nm.

[0235] Latex can be combined by any suitable means, such as by vortex mixing for 1-2 minutes. The method also includes a mixture of latex particles coagulated. Coagulation can be implemented, for example, by cooling (for example, freezing) the blended latex or by adding suitable salt (for example, magnesium chloride). Cooling is particularly desirable for the coating to be used in semiconductor manufacturing and other applications where it is not desirable to introduce salt. The method also includes optionally washing the coagulated mixture of amorphous fluoropolymer particles and crystallized fluoropolymer particles. The washing step can substantially remove emulsifiers or other surfactants from the mixture, and can contribute to obtaining a well-mixed blend of substantially unagglomerated dry particles. In some embodiments, the surfactant content of the resulting dry particle mixture can be, for example, less than 0.1 wt %, less than 0.05 wt % or less than 0.01 wt %. The method also includes drying the coagulated latex mixture. The coagulated latex mixture can be dried by any suitable means (such as air drying or oven drying). In one embodiment, the coagulated latex mixture can be dried at 100° C. for 1 hour to 2 hours.

[0236] The dried coagulated latex mixture can be dissolved in a solvent suitable for dissolving the amorphous fluoropolymer particles to form a stable coating composition comprising a uniform dispersion of crystallized fluoropolymer particles in the amorphous fluoropolymer solution.

[0237] The coating solution can be used to provide a coating on a substrate by applying a layer of the coating composition to the surface of the substrate and drying (ie, removing the fluorinated solvent by evaporation) the coating composition.

[0238] In some embodiments, the method further comprises rubbing (eg, polishing) the dried layer, thereby forming an amorphous fluoropolymer binder layer containing crystallized submicron fluoropolymer particles.

[0239] The submicron crystallized fluoropolymer particles at the coating surface form a thin, continuous or nearly continuous fluoropolymer surface layer disposed on an underlying coating composed of an amorphous fluoropolymer. In a preferred embodiment, the thin crystallized fluoropolymer layer is relatively uniformly spread over the underlying coating and appears thinner and more uniform than if the fluoropolymer particles had merely undergone fibrillation (e.g., due to orientation or other stretching).

[0240] The average roughness (Ra) of the surface is the arithmetic mean of the absolute values ​​of the surface height deviations measured from the mean plane. In some embodiments, Ra is at least 40nm or 50nm before friction, and the range can reach 100nm. In some embodiments, the surface after friction is smoother by at least 10%, 20%, 30%, 40%, 50% or 60%. In some embodiments, after friction, Ra is less than 35 microns, 30 microns, 25 microns or 20 microns.

[0241] A variety of rubbing techniques may be employed when the coating is formed or when the coated article is later used or about to be used. Simply wiping or buffing the coating several times with cheesecloth or other suitable woven, nonwoven or knitted fabric will generally be sufficient to form the desired thin layer. Those skilled in the art will appreciate that many other rubbing techniques may be used. Rubbing may also reduce haze in the cured coating.

[0242] A variety of crystalline fluoropolymer particles may be employed, including mixtures of different crystalline fluoropolymer particles. Crystalline fluoropolymer particles generally have a high degree of crystallinity and thus a pronounced melting point (peak maximum), as determined by differential scanning calorimetry in accordance with DIN EN ISO 11357-3:2013-04 under nitrogen flow and a heating rate of 10°C / min.

[0243] For example, the crystallized fluoropolymer particles may include fluoropolymer particles having a Tm of at least 100° C., 110° C., 120° C., or 130° C. In some embodiments, the crystallized fluoropolymer particles may include fluoropolymer particles having a Tm of no greater than 350° C., 340° C., 330° C., 320° C., 310° C., or 300° C.

[0244] The crystallized fluoropolymer particles generally have a fluorine content greater than about 50% by weight. In addition, the fluoropolymer particles may include fluorine contents between about 50% by weight and about 76% by weight, between about 60% by weight and about 76% by weight, or between about 65% by weight and about 76% by weight.

[0245] Representative crystalline fluoropolymers include, for example, perfluorinated fluoropolymers such as 3M TM Dyneon TM PTFE dispersions TF 5032Z, TF 5033Z, TF 5035Z, TF 5050Z, TF 5135GZ and TF 5070GZ; and 3M TM Dyneon TM Fluorinated thermoplastic dispersions PFA 6900GZ, PFA 6910GZ, FEP 6300GZ and THV 340Z.

[0246] Other suitable fluoropolymer particles are available from suppliers such as Asahi Glass, Solvay Solexis, and Daikin Industries, and will be familiar to those skilled in the art.

[0247] Commercial aqueous dispersions typically contain nonionic and / or ionic surfactants at a concentration of up to 5% to 10% by weight. These surfactants are substantially removed by washing the coagulated blend. There may be a residual surfactant concentration of less than 1%, 0.05%, or 0.01% by weight. It is usually more convenient to use "virgin polymerized" aqueous fluoropolymer latexes because they do not contain such high levels of nonionic / ionic surfactants.

[0248] As previously mentioned, a crystalline fluoropolymer has a melting point that can be determined by DSC. The degree of crystallinity depends on the selection and concentration of the polymerized monomers of the fluoropolymer. For example, a PTFE homopolymer (containing 100% TFE units) has a melting point (Tm) above 340°C. The addition of comonomers such as unsaturated (per)fluorinated alkyl ethers reduces Tm. For example, when the fluoropolymer contains about 3 wt%-5 wt% of polymerized units of such comonomers, Tm is about 310°C. For another example, when the fluoropolymer contains about 15 wt%-20 wt% of polymerized units of HFP, Tm is about 260°C-270°C. For another example, when the fluoropolymer contains 30 wt% of polymerized units of (per)fluorinated alkyl ethers (e.g. PMVE) or other comonomers that reduce crystallinity, the fluoropolymer no longer has a melting point that can be detected by DSC and is therefore characterized as amorphous.

[0249] In some embodiments, the fluoropolymer particles of crystallization contain the fluorinated units of the TFE of at least 40 wt %, 45 wt %, 50 wt %, 55 wt %, 60 wt %, 65 wt %, 70 wt %, 75 wt %, 80 wt %, 85 wt %, 90 wt %, 95 wt % or 100 wt %. In addition, the fluoropolymer particles of crystallization usually comprise unsaturated (per) fluorinated alkyl ether (e.g. PMVE) of lower concentration than amorphous fluoropolymer. In typical embodiments, the fluoropolymer particles of crystallization contain the polymerization units of (per) fluorinated alkyl ether (e.g. PMVE) less than 30 wt %, 25 wt %, 20 wt %, 15 wt %, 10 wt % or 5 wt %.

[0250] In some embodiments, the crystalline fluoropolymer is a copolymer formed from component monomers known as tetrafluoroethylene ("TFE"), hexafluoropropylene ("HFP"), and vinylidene fluoride ("VDF", "VF2"). The monomer structures of these components are shown below:

[0251] TFE: CF2=CF2 (1)

[0252] VDF: CH2=CF2 (2)

[0253] HFP: CF2=CF–CF3 (3)

[0254] In some embodiments, the crystalline fluoropolymer is composed of at least two of the component monomers (HFP and VDF), and in some embodiments, all three of the component monomers in different amounts.

[0255] Tm depends on the amount of TFE, HFP and VDF. For example, a fluoropolymer containing about 45 wt% of polymerized units of TFE, about 18 wt% of polymerized units of HFP and about 37 wt% of polymerized units of VDF has a Tm of about 120°C. For another example, a fluoropolymer containing about 76 wt% of polymerized units of TFE, about 11 wt% of polymerized units of HFP and about 13 wt% of polymerized units of VDF has a Tm of about 240°C. By increasing the polymerized units of HFP / VDF while reducing the polymerized units of TFE, the fluoropolymer becomes amorphous. An overview of crystalline and amorphous fluoropolymers is given in Ullmann's Encyclopedia of Industrial Chemistry (7th edition, 2013, Wiley, 10.1002 / 14356007, a11 393 pub 2) chapter: Fluoropolymers, Organics thEdition,2013 Wiley-VCH Verlag.10.1002 / 14356007.a11 393 pub 2)Chapter:Fluoropolymers,Organic).

[0256] Fluoropolymer particles of crystallization and amorphous fluoropolymer particles can be mixed in multiple ratios. For example, based on the total weight percentage of solid (that is, not including solvent), the coating composition contains about 5 wt % to about 95 wt % of fluoropolymer particles of crystallization and about 95 wt % to about 5 wt % of amorphous fluoropolymer. In some embodiments, the coating composition contains about 10 wt % to about 75 wt % of fluoropolymer particles of crystallization and about 90 wt % to about 25 wt % of amorphous fluoropolymer.

[0257] In some embodiments, the coating composition contains about 10% to about 50% by weight of crystallized fluoropolymer particles and about 90% to about 50% by weight of amorphous fluoropolymer. In some embodiments, the coating composition contains about 10% to about 30% by weight of crystallized fluoropolymer particles and about 90% to about 70% by weight of amorphous fluoropolymer.

[0258] The composition containing the curable fluoroelastomer may also contain additives as known in the art. Examples include acid acceptors. Such acid acceptors may be inorganic acid acceptors or blends of inorganic acid acceptors and organic acid acceptors. Examples of inorganic acceptors include magnesium oxide, lead oxide, calcium oxide, calcium hydroxide, dibasic lead phosphate, zinc oxide, barium carbonate, strontium hydroxide, calcium carbonate, hydrotalcite, etc. Organic acceptors include epoxides, sodium stearate and magnesium oxalate. Particularly suitable acid acceptors include magnesium oxide and zinc oxide. Blends of acid acceptors may also be used. The amount of acid acceptor will generally depend on the nature of the acid acceptor used. Typically, the amount of acid acceptor used is between 0.5 and 5 parts per 100 parts of fluorinated polymer.

[0259] The fluoropolymer composition may contain additional additives such as stabilizers, surfactants, ultraviolet ("UV") absorbers, antioxidants, plasticizers, lubricants, fillers, and processing aids commonly used in fluoropolymer processing or compounding, provided that they have sufficient stability under the expected conditions of use. Specific examples of additives include carbon particles, such as carbon black, graphite, soot. Additional additives include, but are not limited to, pigments, such as iron oxide, titanium dioxide. Other additives include, but are not limited to, clay, silica, barium sulfate, silicon dioxide, glass fibers, or other additives known and used in the art.

[0260] In some embodiments, the fluoropolymer composition comprises silicon dioxide, glass fiber, thermally conductive particles or a combination thereof. Any amount of silicon dioxide and / or glass fiber and / or thermally conductive particles may be present. In some embodiments, the amount of silicon dioxide and / or glass fiber is at least 0.05 weight %, 0.1 weight %, 0.2 weight %, 0.3 weight % of the total solids of the composition. In some embodiments, the amount of silicon dioxide and / or glass fiber is not more than 5 weight %, 4 weight %, 3 weight %, 2 weight % or 1 weight % of the total solids of the composition. Small concentrations of silicon dioxide may be used to thicken the coating composition. In addition, small concentrations of glass fiber may be used to improve the strength of the fluoropolymer film. In other embodiments, the amount of glass fiber may be at least 5 weight %, 10 weight %, 15 weight %, 20 weight %, 25 weight %, 35 weight %, 40 weight %, 45 weight % or 50 weight % of the total solids of the composition. The amount of glass fiber is generally not more than 55 wt%, 50 wt%, 45 wt%, 40 wt%, 35 wt%, 25 wt%, 20 wt%, 15 wt% or 10 wt%. In some embodiments, the average length of glass fiber is at least 100 microns, 150 microns, 200 microns, 250 microns, 300 microns, 350 microns, 400 microns, 450 microns, 500 microns. In some embodiments, the average length of glass fiber is at least 1mm, 2mm or 3mm, and is generally not more than 5mm or 10mm. In some embodiments, the average diameter of glass fiber is at least 1 micron, 2 microns, 3 microns, 4 microns or 5 microns, and is generally not more than 10 microns, 15 microns, 30 microns or 25 microns. The aspect ratio of glass fiber can be at least 3: 1, 5: 1, 10: 1 or 15: 1.

[0261] In some embodiments, the fluoropolymer composition does not contain (for example, silicon dioxide) inorganic oxide particles. In other embodiments, the fluoropolymer composition includes (for example, silicon dioxide and / or heat conduction) inorganic oxide particles. In some embodiments, the amount of (for example, silicon dioxide and / or heat conduction) inorganic oxide particles is at least 5 weight %, 10 weight %, 15 weight %, 20 weight %, 25 weight %, 30 weight %, 35 weight %, 40 weight %, 45 weight % or 50 weight % of the total solid of the composition. In some embodiments, the amount of (for example, silicon dioxide and / or heat conduction) inorganic oxide particles is not more than 90 weight %, 85 weight %, 80 weight %, 75 weight %, 70 weight % or 65 weight % of the total solid of the composition. Various combinations of silicon dioxide and heat conductive particles can be utilized. In some embodiments, the total amount of (e.g., silica and thermally conductive) inorganic oxide particles or the amount of a particular type of silica particles (e.g., fused silica, fumed silica, glass bubbles, etc.) or thermally conductive particles (e.g., boron nitride, silicon carbide, alumina, aluminum trihydrate) is no greater than 60 wt%, 55 wt%, 50 wt%, 45 wt%, 40 wt%, 35 wt%, 30 wt%, 25 wt%, 20 wt%, 15 wt%, 10 wt%, or 5 wt% of the total solids of the composition. Higher concentrations of (e.g., silica) inorganic oxide particles can be beneficial in further reducing dielectric properties. Thus, a composition comprising (e.g., silica) inorganic oxide particles can have lower dielectric properties than the cross-linked fluoropolymer alone.

[0262] In some embodiments, the (e.g., silica) inorganic oxide particles and / or glass fibers have a dielectric constant at 1 GHz of no greater than 7, 6.5, 6, 5.5, 5, 4.5, or 4. In some embodiments, the (e.g., silica) inorganic oxide particles and / or glass fibers have a dissipation factor at 1 GHz of no greater than 0.005, 004, 0.003, 0.002, or 0.0015.

[0263] In some embodiments, the composition comprises inorganic oxide particles or glass fibers that mainly comprise silicon dioxide. In some embodiments, the amount of silicon dioxide is generally at least 50 weight %, 60 weight %, 70 weight %, 75 weight %, 80 weight %, 85 weight % or 90 weight % of inorganic oxide particles or glass fibers. In some embodiments, the amount of silicon dioxide is generally at least 90 weight %, 91 weight %, 92 weight %, 93 weight %, 94 weight %, 95 weight %, 96 weight %, 97 weight %, 98 weight %, 99 weight % or greater (for example, at least 99.5 weight %, 99.6 weight % or 99.7 weight %) silicon dioxide. Higher silicon dioxide concentrations generally have lower dielectric constants. In some embodiments, (for example, melting) silicon dioxide particles may also include other metals / metal oxides of small concentrations, such as Al2O3, Fe2O5, TiO2, K2O, CaO, MgO and Na2O. In some embodiments, the total amount of such metals / metal oxides (e.g., Al2O3, CaO, and MgO) is independently no more than 30 wt%, 25 wt%, 20 wt%, 15 wt%, or 10 wt%. In some embodiments, the inorganic oxide particles or glass fibers may include B2O3. The amount of B2O3 may range up to 25 wt% of the inorganic oxide particles or glass fibers. In other embodiments, (e.g., pyrogenic) silica particles may also include small concentrations of additional metals / metal oxides such as Cr, Cu, Li, Mg, Ni, P, and Zr. In some embodiments, the total amount of such metals or metal oxides is no more than 5 wt%, 4 wt%, 3 wt%, 2 wt%, or 1 wt%. In some embodiments, silica may be described as quartz. The amount of non-silicon dioxide metals or metal oxides may be determined using inductively coupled plasma mass spectrometry. (e.g., silica) inorganic oxide particles are typically dissolved in hydrofluoric acid and distilled as H2SiF6 at low temperatures.

[0264] In some embodiments, the inorganic particles can be characterized as "agglomerates," meaning weak associations between primary particles (such as particles held together by charge or polarity). During the preparation of the coating solution, the agglomerates are typically physically broken down into smaller entities, such as primary particles. In other embodiments, the inorganic particles can be characterized as "aggregates," meaning strongly bonded or fused particles, such as covalently bonded particles or thermally bonded particles prepared by methods such as sintering, electric arc, flame hydrolysis, or plasma. During the preparation of the coating solution, the aggregates are typically not broken down into smaller entities, such as primary particles. "Primary particle size" refers to the average diameter of a single (non-aggregated, non-agglomerated) particle.

[0265] The (e.g., silica) particles can have various shapes, such as spherical, ellipsoidal, linear or branched. Fused silica aggregates and fumed silica aggregates are more typically branched. The aggregate size is typically at least 10 times the primary particle size of the discrete portion.

[0266] In other embodiments, the (e.g., silica) particles may be characterized as glass bubbles. The glass bubbles may be prepared from soda-lime borosilicate glass. In this embodiment, the glass may contain about 70% silica (silicon dioxide), 15% soda (sodium oxide), and 9% lime (calcium oxide), with smaller amounts of various other compounds.

[0267] In some embodiments, inorganic oxide particles can be characterized as (for example, silicon dioxide) nanoparticles, and their average or median particle size is less than 1 micron. In some embodiments, (for example, silicon dioxide) average or median particle size of inorganic oxide particles is 500nm or 750nm. In other embodiments, (for example, silicon dioxide) average particle size of inorganic oxide particles can be at least 1 micron, 1.5 microns, 2 microns, 2.5 microns, 3 microns, 3.5 microns, 4 microns, 4.5 microns, 5 microns, 5.5 microns, 6 microns, 6.5 microns, 7 microns, 7.5 microns, 8 microns, 8.5 microns, 9 microns, 9.5 microns or 10 microns. In some embodiments, average particle size is not more than 30 microns, 25 microns, 20 microns, 15 microns or 10 microns. In some embodiments, composition comprises a small amount of or does not comprise (for example, colloidal silica) nanoparticles with 100 nanometers or smaller particles. The concentration of (e.g., colloidal silica) nanoparticles is typically less than 10 wt%, 9 wt%, 8 wt%, 7 wt%, 6 wt%, 5 wt%, 4 wt%, 3 wt%, 2 wt%, or 1 wt%. The inorganic oxide (e.g., silica particles) may include a normal distribution of particle sizes having a single peak or a particle distribution having two or more peaks.

[0268] In some embodiments, no more than 1% by weight of the (e.g., silica) inorganic oxide particles have a particle size greater than or equal to 3 microns or 4 microns. In some embodiments, no more than 1% by weight of the (e.g., silica) inorganic oxide particles have a particle size greater than or equal to 5 microns or 10 microns. In other embodiments, no more than 5%, 4%, 3%, 2%, or 1% by weight of the particles have a particle size greater than 45 microns. In some embodiments, no more than 1% by weight of the particles have a particle size ranging from 75 microns to 150 microns.

[0269] In some embodiments, the average or median particle size refers to the "primary particle size," which refers to the average or median diameter of discrete, non-aggregated, non-agglomerated particles. For example, the particle size of colloidal silica or glass bubbles is typically the average or median particle size. In a preferred embodiment, the average or median particle size refers to the average or median diameter of the aggregates. The particle size of inorganic particles can be measured using a transmission electron microscope. The particle size of a fluoropolymer coating solution can be measured using dynamic light scattering.

[0270] In some embodiments, the (eg, silica) inorganic particles have a specific gravity ranging from 2.18 g / cc to 2.20 g / cc.

[0271] Aggregate particles, such as in the case of pyrogenic and fused (e.g., silica) particles, can have a lower surface area than primary particles of the same size. In some embodiments, the BET surface area of ​​the (e.g., silica) particles ranges from about 50 m 2 / g to 500m 2 / g. In some embodiments, the BET surface area is less than 450 m 2 / g, 400m 2 / g, 350m 2 / g、300m 2 / g, 250m 2 / g, 200m 2 / g, 150m 2 / g or 100m 2 / g.

[0272] In some embodiments, the inorganic nanoparticles may be characterized as colloidal silica. It should be appreciated that unmodified colloidal silica nanoparticles typically contain hydroxyl or silanol functional groups on the surface of the nanoparticles and are typically characterized as hydrophilic.

[0273] In some embodiments, (e.g., silica aggregates) inorganic particles, particularly colloidal silica nanoparticles, are surface treated with a hydrophobic surface treatment. Common hydrophobic surface treatments include compounds such as alkoxysilanes (e.g., octadecyltriethoxysilane), silazanes, or siloxanes. Various hydrophobic fumed silicas are available from AEROSIL TM , Evonik, and various other suppliers. Representative hydrophobic fumed silicas include AEROSIL grades R 972, R 805, RX 300, and NX 90 S. TM .

[0274] In some embodiments, (e.g., silica aggregates) inorganic particles are surface treated with fluorinated alkoxysilane silane compounds. Such compounds typically include perfluoroalkyl or perfluoropolyether groups. Perfluoroalkyl or perfluoropolyether groups typically have no more than 4, 5, 6, 7, 8 carbon atoms. Alkoxysilane groups can be bonded to alkoxysilane groups with various divalent linking groups (including alkylene, carbamate and -SO2N(Me)-). Some representative fluorinated alkoxysilanes are described in US5274159 and WO2011 / 043973, which are incorporated herein by reference. Other fluorinated alkoxysilanes are commercially available.

[0275] The fluoropolymer composition can be prepared by mixing a polymer, a curing agent comprising at least one ethylenically unsaturated curing agent, at least one compound having an electron donor group, optional additives, and a fluorinated solvent. In some embodiments, the fluoropolymer is first dissolved in the fluorinated solvent, and then other additives, including the curing agent and the electron donor compound, are added.

[0276] In some embodiments, the fluoropolymer composition comprises thermally conductive particles.

[0277] In some embodiments, the thermally conductive inorganic particles are preferably non-conductive materials. Suitable non-conductive thermally conductive materials include ceramics, such as metal oxides, hydroxides, oxyhydroxides, silicates, borides, carbides and nitrides. Suitable ceramic fillers include, for example, silicon oxide, zinc oxide, aluminum trihydrate (ATH) (also referred to as hydrated aluminum oxide, aluminum oxide and aluminum trihydrate), aluminum nitride, boron nitride, silicon carbide and beryllium oxide. Other thermally conductive fillers include carbon-based materials (such as graphite) and metals (such as aluminum and copper). Combinations of different thermally conductive materials can be used. Such materials are not electrically conductive, that is, have an electronic band gap greater than 0eV and at least 1eV, 2eV, 3eV, 4eV or 5eV in some embodiments. In some embodiments, such materials have an electronic band gap not greater than 15eV or 20eV. In this embodiment, the composition may also optionally include low-concentration thermally conductive particles having an electronic band gap less than 0eV or greater than 20eV.

[0278] In an advantageous embodiment, the thermally conductive particles comprise a material having a bulk thermal conductivity > 10 W / m*K. The thermal conductivities of some representative inorganic materials are set forth in the table below.

[0279] Thermally conductive materials

[0280]

[0281] In some embodiments, the thermally conductive particles comprise one or more materials having a bulk thermal conductivity of at least 15 W / m*K or 20 W / m*K. In other embodiments, the thermally conductive particles comprise one or more materials having a bulk thermal conductivity of at least 25 W / m*K or 30 W / m*K. In other embodiments, the thermally conductive particles comprise one or more materials having a bulk thermal conductivity of at least 50 W / m*K, 75 W / m*K, or 100 W / m*K. In other embodiments, the thermally conductive particles comprise one or more materials having a bulk thermal conductivity of at least 150 W / m*K. In typical embodiments, the thermally conductive particles comprise one or more materials having a bulk thermal conductivity of no greater than about 350 W / m*K or 300 W / m*K.

[0282] Thermally conductive particles can be obtained in a variety of shapes, such as spheres and needle-like shapes, which can be irregular or plate-like. In some embodiments, the thermally conductive particles are crystals, typically having a geometric shape. For example, hexagonal crystals of boron nitride are commercially available from Momentive. In addition, alumina trihydrate is described as hexagonal platelets. Combinations of particles with different shapes can be utilized. Thermally conductive particles generally have an aspect ratio of less than 100: 1, 75: 1, or 50: 1. In some embodiments, thermally conductive particles have an aspect ratio of less than 3: 1, 2.5: 1, 2: 1, or 1.5: 1. In some embodiments, roughly symmetrical (e.g., spherical, hemispherical) particles can be used.

[0283] Boron nitride particles can be used as "3M TM Boron nitride cooling filler is commercially available from 3M Company.

[0284] In some embodiments, the boron nitride particles have a bulk density of at least 0.05 g / cm 3 , 0.01g / cm 3 , 0.15g / cm 3 , 0.03g / cm 3 , ranging up to about 0.60 g / cm 3 、0.70g / cm 3 or 0.80g / cm 3 The surface area of ​​the boron nitride particles can be <25m 2 / g, <20m 2 / g, <10m 2 / g, <5m 2 / g or <3m 2 / g. The surface area is usually at least 1m 2 / g or 2m 2 / g.

[0285] In some embodiments, the particle size d(0.1) of the boron nitride (e.g., platelets) particles is in the range of about 0.5 microns to 5 microns. In some embodiments, the particle size d(0.9) of the boron nitride (e.g., platelets) particles is at least 5 microns, ranging up to 20 microns, 25 microns, 30 microns, 35 microns, 40 microns, 45 microns, or 50 microns.

[0286] The coating compositions comprising fluorinated solvents described herein are "stable", meaning that the coating compositions remain homogeneous when stored in a sealed container at room temperature for at least 24 hours. In some embodiments, the coating compositions are stable for a week or longer. "Homogeneous" refers to a coating composition that does not exhibit a distinctly separate precipitate or distinctly separate layers when freshly shaken, placed in a 100 ml glass container and allowed to stand at room temperature for at least 4 hours.

[0287] In some embodiments, the fluoropolymer is first mixed with other solid ingredients, particularly with the electron donor (e.g., amine) compound and ethylenically unsaturated curing agent described herein, and (e.g., silica) inorganic particles (when present). The fluoropolymer and amine compound can be mixed in conventional rubber processing equipment to provide a solid mixture, i.e., a solid polymer containing additional ingredients, also referred to as a "compound" in the art. Typical equipment includes a rubber mill, an internal mixer (such as a Banbury mixer), and a mixing extruder. During the mixing process, the components and additives are evenly distributed throughout the resulting fluorinated polymer "compound" or polymer flakes. The compound is then preferably comminuted (e.g., by cutting into smaller pieces) and then dissolved in a solvent.

[0288] Fluoropolymer coating solution compositions provided herein are suitable for coating substrates.Depending on the presence or absence of solvent and fluoropolymer content and optional additives, fluoropolymer coating solution compositions can be formulated to have different viscosities.Fluoropolymer coating solution compositions generally contain or are solutions of fluoropolymers, and can be in the form of liquids or pastes.However, the compositions may contain dispersed or suspended materials, but these materials are preferably additives and are not fluoropolymers of the type described herein.Preferably, the compositions are liquids, and more preferably, they are solutions containing one or more fluoropolymers dissolved in solvents as described herein as described herein.

[0289] The fluoropolymer compositions provided herein are suitable for coating substrates and can be adjusted (via solvent content) to a viscosity that allows application by different coating methods, including but not limited to spraying or printing (such as but not limited to inkjet printing, 3D-printing, screen printing), painting, dipping, roller coating, rod coating, dip coating, and solvent casting.

[0290] Coated substrates and articles can be prepared by adding the fluoropolymer composition to a substrate and removing the solvent. Curing can occur when, during or after the solvent is removed. The solvent can be reduced or completely removed, for example by evaporation, drying or by boiling it off. After the solvent is removed, the composition can be characterized as "dry".

[0291] The method for preparing the crosslinked fluoropolymer described herein comprises curing the fluoropolymer with actinic radiation (e.g., ultraviolet or electron beam). The fluoropolymer composition, the substrate, or both may transmit the curing radiation. In some embodiments, a combination of UV curing and thermal (e.g., post) curing is utilized. Curing is performed at an effective temperature and effective time to produce a cured fluoroelastomer. The optimal conditions may be tested by examining the mechanical and physical properties of the fluoroelastomer. Curing may be performed in an oven under pressure or without pressure. A post-curing cycle at elevated temperature and or pressure may be applied to ensure that the curing process is fully completed. Curing conditions depend on the curing system used.

[0292] In some embodiments, the composition is cured by UV curing. The fluoropolymer of the composition described herein contains little or no polymerized units of vinylidene fluoride (VDF) (i.e., CH2=CF2) or VDF coupled to hexafluoropropylene (HFP). The polymerized units of VDF can undergo dehydrofluorination (i.e., HF elimination reaction) as described in US2006 / 0147723. The reaction is limited by the number of polymerized VDF groups coupled to the HFP groups contained in the fluoropolymer. The double bonds formed by dehydrofluorination can then react (via Michael addition) with aminoalkoxysilanes to graft fluorinated side chain alkoxysilane groups onto the fluoropolymer backbone. When irradiated with ultraviolet light, such side groups can undergo free radical copolymerization with multifunctional (meth)acrylate compounds.

[0293] However, because the fluoropolymers of the compositions described herein contain few or no polymerized units of VDF (i.e., CH2=CF2) coupled to HFP groups, the fluoropolymers are not susceptible to the reaction scheme just described. As demonstrated in the examples that follow, amine compounds alone can initiate UV curing in the absence of free radical photoinitiators. Addition of free radical photoinitiators generally does not increase crosslinking of fluoropolymers. This result indicates that the fluoropolymers do not crosslink via a free radical mechanism.

[0294] Although conventional free radical initiators are not required, the composition may also optionally include a photoinitiator. In other embodiments, the composition is substantially free of free radical initiators, including such free radical photoinitiators.

[0295] In some embodiments, the ultraviolet radiation may have sufficient intensity at a wavelength of at least 190nm, 200nm, 210nm, 220nm, 230nm, or 240nm. In some embodiments, the ultraviolet radiation may have sufficient intensity at a wavelength of no more than 350nm, 340nm, 330nm, 320nm, 310nm, or 290nm. In some embodiments, (e.g., ultraviolet) actinic radiation has sufficient intensity at a wavelength in the range of 270nm-290nm so that in the presence of (e.g., amine) electron donors, wavelength-induced single electron transfer reactions may occur between C-I bonds. In some embodiments, the ultraviolet radiation may have sufficient intensity at a wavelength in the range of less than 240nm (e.g., 150-200nm) so that in the presence of (e.g., amine) electron donors, wavelength-induced single electron transfer reactions may occur between C-I or C-Br bonds.

[0296] UV light sources can be of various types. Low intensity light sources such as black lights typically provide 0.1 mW / cm 2 or 0.5mW / cm 2 (mW / cm2) to 10mW / cm 2 The intensity of the high-intensity light source is in the range of 10 mW / cm2 (measured according to procedures approved by the National Institute of Standards and Technology, such as, for example, using a UVIMAP UM 365L-S radiometer manufactured by Electronic Instrumentation & Technology, Inc., Sterling, VA). High-intensity light sources typically provide greater than 10 mW / cm2. 2 、15mW / cm 2 or 20mW / cm 2 , range up to 450mW / cm 2 In some embodiments, the high intensity light source provides up to 500 mW / cm 2 、600mW / cm 2 , 700mW / cm 2 、800mW / cm 2 , 900mW / cm 2 or 1000mW / cm 2The ultraviolet light for polymerizing the ethylenically unsaturated monomers can be provided by various light sources, such as light emitting diodes (LEDs), fluorescent blacklights, arc lamps (such as xenon arc lamps), and medium and low pressure mercury lamps (including germicidal lamps), microwave driven lamps, lasers, etc., or combinations thereof. The composition can also be polymerized with a higher intensity light source obtained from Fusion UV Systems Inc. Lamps that emit ultraviolet or blue light are generally preferred. The UV acceptance time for polymerization and curing can vary depending on the intensity of the light source used. For example, full curing using a low intensity light process can be completed at an acceptance time in the range of about 30 seconds to 300 seconds; while full curing using a high intensity light source can be completed at a shorter acceptance time in the range of about 5 seconds to 20 seconds. Partial curing using a high intensity light source can typically be completed at an acceptance time in the range of about 2 seconds to about 5 seconds or 10 seconds. In some embodiments, post-curing can be performed at a temperature between 170°C and 250°C for a period of 0.1 hours to 24 hours.

[0297] In some embodiments, the post-curing of the fluoropolymer may be optionally carried out at a lower temperature. Post-curing at a lower temperature is suitable for coating heat-sensitive substrates. In some embodiments, post-curing occurs in a temperature range of 100°C, 110°C, 120°C, 130°C, 135°C or 140°C to a maximum of 170°C, for a period of 5 minutes to 10 minutes to 24 hours. In some embodiments, the temperature is no more than 169°C, 168°C, 167°C, 166°C, 165°C, 164°C, 163°C, 162°C, 161°C or 160°C. In some embodiments, the temperature is no more than 135°C, 130°C, 125°C or 120°C. In advantageous embodiments, after curing, the fluoropolymer is sufficiently crosslinked that at least 80 weight percent, 85 weight percent, 90 weight percent, 95 weight percent, or 100 weight percent or more is insoluble in a fluorinated solvent (e.g., 3-ethoxyperfluorinated 2-methylhexane) at a weight ratio of 5 grams of fluoropolymer in 95 weight percent of the fluorinated solvent (at 25° C. within 12 hours).

[0298] The composition can be used for impregnating substrates, printing (e.g., screen printing) or coating substrates on substrates, such as, but not limited to, spraying, painting dip coating, roller coating, rod coating, solvent casting, paste coating. The substrate can be organic, inorganic, or a combination thereof. Suitable substrates can include any solid surface, and can include substrates selected from glass, plastics (e.g., polycarbonate), composite materials, metals (stainless steel, aluminum, carbon steel), metal alloys, wood, paper, and other substrates. If the composition contains a pigment, such as titanium dioxide or a black filler (e.g., graphite or soot), the coating can be colored, or if there is no pigment or black filler, it can be colorless.

[0299] Binders and primers can be used to pretreat the surface of the substrate prior to coating. For example, the bonding of the coating to the metal surface can be improved by applying a binder or primer. Examples include commercial primers or binders, such as those commercially available under the trade name CHEMLOK.

[0300] The articles containing the coating from the composition provided herein include, but are not limited to, impregnated textiles, such as protective clothing. Another example of impregnated textiles is a glass scrim impregnated with (e.g., containing silicon dioxide) fluoropolymer compositions as described herein. Textiles may include woven or nonwoven fabrics. Other articles include articles that accept corrosive environments, such as seals and seals for chemical processing and parts of valves, such as but not limited to chemical reactors, molds, chemical processing equipment (e.g., for etching) parts or linings, or valves, pumps and pipelines, especially for corrosive substances or hydrocarbon fuels or solvents Pipelines; Internal combustion engines, electrodes, fuel transportation, containers for acids and alkalis and for acid and alkali transportation systems, electronic batteries, fuel cells, electrolytic cells and articles for or etching.

[0301] The advantage of the coating compositions described herein is that these coating compositions can be used to prepare high thickness or low thickness coatings or fluoropolymer sheets. In some embodiments, the dried and cured fluoropolymer has a thickness of 0.1 micron to 1 or 2 mils. In some embodiments, the dried and cured fluoropolymer thickness is at least 0.2 micron, 0.3 micron, 0.4 micron, 0.5 micron or 0.6 micron. In some embodiments, the dried and cured fluoropolymer thickness is at least 1 micron, 2 microns, 3 microns, 4 microns, 5 microns or 6 microns.

[0302] In typical embodiments, the dried and cured (i.e., cross-linked) composition has a low dielectric constant (Dk), which is generally less than 2.75, 2.70, 2.65, 2.60, 2.55, 2.50, 2.45, 2.40, 2.35, 2.30, 2.25, 2.20, 2.15, 2.20, 2.15, 2.10, 2.05, 2.00, 1.95, 1.90. In some embodiments, the dielectric constant is at least 2.02, 2.03, 2.04, 2.05. The dried and cured (ie, cross-linked) composition has a low dielectric loss, which is generally less than 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, 0.001, 0.0009, 0.0008, 0.0007, 0.0006, 0.0005, 0.0004, 0.0003. In some embodiments, the dielectric loss is at least 0.00022, 0.00023, 0.00024, 0.00025.

[0303] The dried and cured coatings can exhibit good adhesion to various substrates (e.g., glass, polycarbonate), as demonstrated by coatings that exhibit a 2, and preferably a 3 or 4, according to the boiling water test described in PCT / US2019 / 036460. In advantageous embodiments, the dried and cured coatings are durable, as demonstrated by coatings that exhibit a 2, and preferably a 3 or 4, according to the abrasion test described in the previously cited PCT / US2019 / 036460. In some embodiments, the coating is durable according to an abrasion test after being subjected to a boiling water test.

[0304] The dried and cured coating can exhibit good adhesion to metals such as copper. For example, in some embodiments, the T-peel of copper foil is at least 0.1 N / mm, 0.2 N / mm, 0.3 N / mm, 0.4 N / mm, 0.5 N / mm, or 0.6 N / mm, ranging up to at least 1 N / mm (i.e., 10 N / cm), 1.5 N / mm, 2 N / mm, or 2.5 N / mm, as determined by the test method described in the Examples.

[0305] In some embodiments, the dried and cured coating has good hydrophobicity and oleophobicity according to the black permanent marker resistance test (i.e., marker liquid bead) described in previously cited PCT / US2019 / 036460, and is easily removed with a paper towel or cloth.

[0306] In some embodiments, the dried and cured coating has good hydrophobicity and oleophobicity, as determined by contact angle measurement (as determined according to the test method described in the examples). In some embodiments, the static advancing and / or receding contact angle with water may be at least 100 degrees, 105 degrees, 110 degrees, 115 degrees, 120 degrees, 125 degrees, and generally not more than 130 degrees. In some embodiments, the advancing and / or receding contact angle with hexadecane may be at least 60 degrees, 65 degrees, 70 degrees, or 75 degrees. In some embodiments, the coating exhibits such contact angles after being subjected to a boiling water test or after being subjected to a boiling water test and an abrasion test (as determined according to the test method described in the previously cited PCT / US2019 / 036460).

[0307] In some embodiments, the dried and cured coating exhibits good corrosion resistance (i.e., does not corrode) according to the acid / base corrosion test described in previously cited PCT / US2019 / 036460.

[0308] In some embodiments, the dried and cured coating (eg, film) exhibits low water absorption, eg, less than 0.5, 0.4, 0.3, 0.2, or 0.1, as determined by the Moisture Absorption Test Method described in the Examples.

[0309] In some embodiments, the composition exhibits a low coefficient of thermal expansion, for example, less than 150, 100, 50, 40, 30, 20, or 10, as determined by the test method described in the Examples. For some insulation layer applications, the coefficient of thermal expansion is less important and can range up to 175, 200, or 225.

[0310] As used herein, the term "partially fluorinated alkyl" refers to an alkyl group in which some but not all of the hydrogens bonded to the carbon chain have been replaced by fluorine. For example, a F2HC- or FH2C- group is a partially fluorinated methyl group. The term "partially fluorinated alkyl" also encompasses alkyl groups in which the remaining hydrogen atoms have been partially or completely replaced by other atoms (e.g., other halogen atoms, such as chlorine, iodine and / or bromine), as long as at least one hydrogen is replaced by fluorine. For example, a residue of the formula F2ClC- or FHClC- is also a partially fluorinated alkyl residue.

[0311] "Partially fluorinated ethers" are ethers containing at least one partially fluorinated group or ethers containing one or more perfluorinated groups and at least one non-fluorinated or at least one partially fluorinated group. For example, F2HC-O-CH3, F3C-O-CH3, F2HC-O-CFH2 and F2HC-O-CF3 are examples of partially fluorinated ethers. The term "partially fluorinated alkyl" also encompasses ether groups whose remaining hydrogen atoms have been partially or completely replaced by other atoms (e.g., other halogen atoms, such as chlorine, iodine and / or bromine), as long as at least one hydrogen is replaced by fluorine. For example, ethers of formula F2ClC-O-CF3 or FHClC-O-CF3 are also partially fluorinated ethers.

[0312] The term "perfluorinated alkyl" or "perfluoroalkyl" is used herein to describe an alkyl group in which all hydrogen atoms bonded to the alkyl chain have been replaced by fluorine atoms. For example, F3C- represents a perfluoromethyl group.

[0313] A "perfluorinated ether" is an ether in which all hydrogen atoms have been replaced by fluorine atoms. An example of a perfluorinated ether is F3C-O-CF3.

[0314] The following examples are provided to further illustrate the present disclosure and are in no way intended to limit the present disclosure to the specific examples and embodiments provided.

[0315] Example

[0316] Unless otherwise indicated or readily apparent from the context, all parts, percentages, ratios, etc. in the examples and the remainder of the specification are by weight.

[0317] Table 1: Materials :

[0318]

[0319]

[0320]

[0321] Preparation of Fluorinated Ether Dienes

[0322] A fluorinated ether diol HO-CH2-CF2-O-(CF2CF2)CF2-CH2-OH (0.16 mol) having an average molecular weight of 1500 and an average hydroxyl functionality of 1.8 as described in US5384374 was reacted with sodium methoxide (0.34 mol) and then with allyl bromide (40 g, 0.36 mol) in a 250 mL 3-necked flask equipped with a condenser at 60° C. overnight. After the reaction, the reaction mixture was washed with water and the pale yellow liquid was first dried over CaCl2 and then subjected to rotary evaporation to remove any residues of allyl bromide.

[0323] General Procedure - Preparation of Perfluoroelastomer PFE Coating Solutions Using Multifunctional Olefin / Aminosilane Ester Photocrosslinkers :

[0324] Perfluoroelastomer PFE-1 and PFE-2 solutions were prepared by cutting the glue into small pieces individually and adding them to HFE solvent (HFE-7300 or HFE-7500) to prepare HFE solutions (10 g PFE and 90 g HFE) containing 10 wt % PFE. The containers were sealed with PTFE tape and parafilm. The solution was vigorously shaken overnight (about 12 hours) to make it completely homogeneous.

[0325] All aminosilanes, initiators are dissolved or dispersed in HFE to form a 1 wt% or 5 wt% solution or suspension (e.g., 0.5 g TAIC is added to 9.5 g HFE in a vial to form a 5 wt% suspension). Amines (e.g., aminosilanes), olefins, and optionally photoinitiators are added to the PFE solution. For example, a sample (5% TAIC, 1% APES, 2% TMOS) is prepared by adding 0.3157 g TAIC suspension (5 wt% in HFE), 0.0606 g APES suspension (5 wt% in HFE), and 0.1224 g TMOS solution (5 wt% in 7500) to 3 g PFE-1 solution (10 wt% in PFE-1). Many silanes form suspensions in HFE, rather than solutions. Such suspensions are homogenized at 1000 rpm for 10 seconds using a vortex shaker to form a well-dispersed slurry, which is then added to the PFE-HFE solution. In addition, the percentages in the formula (e.g., 5%, 3%, 1%) are based on the mass fraction of the PFE solid content (e.g., PFE-1+5%APES+2%1173 means: solid content of PFE-1 / APES=95:5 and solid content of PFE-1 / 1173=98:2).

[0326] General Procedure - Preparation of Perfluoroelastomer PFE Coating Solutions Using Fluorinated Olefin / Aminosilane Ester Photocrosslinkers :

[0327] In a similar manner as described above, perfluoroelastomer PFE-1 and PFE-2 solutions were prepared by the following steps: the glue was cut into small pieces individually and placed in an HFE solvent in a glass jar to obtain an HFE solution containing 10 wt % PFE. The glass jar was sealed with Teflon tape and paraffin film. The solution was shaken vigorously overnight (about 12 hours) until it was completely uniform. Most of the olefins were dissolved or dispersed in HFE to form a 1 wt % or 5 wt % solution or suspension. When there was a rapid phase separation between the olefin and the HFE solution and when the olefin sample was solid at room temperature and could not be completely dispersed in HFE-7500, the olefin was dissolved in methanol or methoxypropanol instead. These olefins include 4,4'-bis((1,2,2-trifluorovinyl)oxy)-1,1'-biphenyl (dissolved in methanol), chloro-1,2-phenylene diacrylate (dissolved in methanol), perchloro-1,2-phenylene diacrylate (dissolved in methoxypropanol), 2,4,6-tribromobenzene-1,3,5-triyl triacrylate (dissolved in methoxypropanol). In addition to the olefins, all silanes and photoinitiators are dissolved or dispersed in HFE to form 1 wt% or 5 wt% solutions or suspensions. Olefins or multifunctional olefins and other chemicals (including silanes and initiators as indicated in the table) are added to PFE.

[0328] Split-Pin Dielectric Resonator Measurements at 25 GHz

[0329] All split-column dielectric resonator measurements were performed at frequencies close to 25 GHz according to standard IEC 61189-2-721. Each thin material or membrane is inserted between two fixed dielectric resonators. The resonant frequency and quality factor of the column are affected by the presence of the sample, and this enables the direct calculation of the complex permittivity (dielectric constant and dielectric losses). The geometry of the split dielectric resonator fixture used in our measurements was designed by Company QWED, Warsaw Poland. The 25 GHz resonator is operated with a TE having only the azimuthal electric field component. 01d The dielectric constant of the sample is measured in the plane of the dielectric resonator. The dielectric constant of the sample is measured in the form of a dielectric constant. The dielectric constant of the sample is measured in the plane of the dielectric resonator ...

[0330] Coefficient of Thermal Expansion (CTE) Measurement

[0331] CTE measurements were performed using a thermomechanical analyzer (TMA) TMA Q400 from TA Instruments. Film samples were cut into rectangular shapes (4.5 mm x 24 mm) and mounted on a tension fixture. The sample was heated to at least 150°C using a ramp rate of 3.00°C / min and then cooled to room temperature at the same rate. The sample was then heated again to the target temperature. The CTE calculated from the second cycle is reported.

[0332] Moisture absorption rate measurement

[0333] The water absorption measurements were performed using a vapor absorption analyzer Q500SA from TA Instruments. The samples were placed in a quartz pan located in a programmable chamber. Approximately 5 mg of sample was used in each measurement. The sample was first dried in the chamber until the weight remained constant for 20 minutes. The sample was then placed at 60°C and 50% humidity until weight equilibrium was achieved. The water absorption value was calculated based on the weight gain / original weight of the sample.

[0334] T-peel measurement

[0335] The film was laminated with Cu foil at 24° C. for 20 minutes. The laminated sample was cut into strips with a width of 0.5 inches for T-peel measurement. The measurement was performed using an INSTRON electromechanical universal testing machine using the ASTM D1876 standard method.

[0336] Static contact angle

[0337] Static contact angle measurements were performed using deionized water on a drop shape analyzer DSA100 from KRUSS, Germany. The recorded value is the average of the measured values ​​obtained by measuring at least three drops on their respective left and right sides. The drop volume for static measurement is 5 μL.

[0338] Table 2: Crosslinking yield of cured fluoropolymers

[0339] For cross-linking yield study, samples were prepared in the following manner: 3 g of solution was deposited onto PET film. The coated film was dried at ambient temperature for 2 hours and at 50° C. for 20 minutes. After the sample was completely dried, the PET film sample was placed on a wooden board or stainless steel plate and placed under a single 500 watt H bulb or 500 watt D bulb UV lamp and run 5 to 10 times at a speed of 30 feet per minute for curing (as indicated in the table). After UV curing, many samples were also placed in an oven for heat curing at 120° C. for 5 minutes (as indicated in the table). Some of these samples were also subjected to heat curing conditions without UV curing.

[0340] UV-cured samples (1 to 2 mils thick) were peeled off the PET film, weighed, and then placed in a vial for dissolution with HFE. The mass ratio of cured PFE sample / HFE solvent was 5 / 95. The vials were subjected to vigorous shaking overnight (about 12 hours) before any observations were recorded, as described in the table below. The precipitated samples (i.e., cross-linked PFE) in the HFE solution were collected, dried, and weighed. In some cases, gels (i.e., PFE with a lower degree of cross-linking) were collected, dried, and weighed.

[0341]

[0342] Table 3: Effect of aminosilane esters on the photochemical crosslinking of PFE-1 and TAIC

[0343]

[0344]

[0345] Table 4: Effect of organic amines on the photochemical crosslinking of PFE-1 and TAIC

[0346] Example TAIC+Organic Primary Amine UV curing 10 times + 120℃ 5 minutes 4.1 5%TAIC 1%Diaminohexane Precipitation 81.33 wt% TAIC+Organic tertiary amine 4.2 5%TAIC 1%TMDAB Precipitation 87.14 wt% 4.3 5%TAIC 1%N,N-dimethylaniline Swelling 75.44 wt% TAIC+organic primary amine+organic secondary amine 4.4 5%TAIC 1%Triethylenetetramine Precipitation 98.95 wt% 4.5 5%TAIC 1%Diethylenetriamine Swelling 80.05 wt%

[0347] Table 5: Effect of olefins on the photochemical cross-linking of PFE-1 and TAIC

[0348]

[0349] Table 6: Effect of wavelength (H bulb and D bulb) and number of UV curing runs on the UV curing performance of PFE-1+TAIC+APES The impact of the alliance

[0350]

[0351]

[0352] Table 7: Effect of wavelength (H bulb and D bulb) on UV crosslinking of PFE-1 + olefin + amine

[0353]

[0354] Table 8: Effect of aminosilane esters on the photochemical crosslinking of PFE-2 with olefins

[0355]

[0356] Table 9. Effect of wavelength (H bulb and D bulb) on UV crosslinking of PFE-2+TAIC

[0357]

[0358] Table 10: PFE-1 photochemically crosslinked at 120°C for 5 minutes (UV curing only or UV curing + heat curing)

[0359]

[0360] Preparation of fluoropolymer solutions having dispersed crystalline fluoropolymer particles :

[0361] The perfluoroelastomer latex PFE-1 was mixed with a crystallized fluoropolymer latex PFA, PTFE or THV in the weight ratio described in Table 11. The solution was vortex mixed for 1-2 minutes. Subsequently, the well-mixed solution was frozen at -20°C for 4 hours, then taken out and thawed in warm water. After thawing, the precipitate was filtered and washed with deionized (DI) water. The obtained solid was then dried in an oven at 100°C for 1 hour to 2 hours. The dried condensed solid was mixed with HFE to form a 10 wt % solution in HFE. TAIC and APS were also added to the HFE composition as indicated in Table 11. Each composition was placed in a shaker for 3-4 hours to obtain a stable and uniformly dispersed uniform composition.

[0362] The samples were prepared by depositing 3 g of the solution onto a PET film. The coated film was dried at ambient temperature for 2 hours and at 50° C. for 20 min. After the sample was completely dry, the PET film sample was placed on a wooden or stainless steel plate and placed under a single 500 watt H bulb for 5 to 10 passes at 30 feet per minute for curing (as indicated in the table). After UV curing, some samples were also placed in an oven for heat curing at 120° C. for 5 min (as indicated in Table 11).

[0363] UV-cured samples (1 to 2 mils thick) were peeled off the PET film, weighed, and then placed in a vial for dissolution with HFE. The mass ratio of cured PFE sample / HFE solvent was 5 / 95. The vial was subjected to vigorous shaking overnight (about 12 hours) before any observations were recorded, as described in the table below. The precipitated samples (i.e., cross-linked PFE) in the HFE solution were collected, dried, and weighed.

[0364] Table 11: Crystalline fluoropolymer particles coated with photochemically crosslinked PFE-1

[0365]

[0366] Table 12: Effect of aminosilane esters on UV-cured PFE-1

[0367] The perfluoroelastomer PFE-1 solution was prepared by cutting the glue into small pieces individually and adding them to the HFE solvent (HFE-7300 or HFE-7500) to prepare the HFE solution (10 g PFE and 90 g HFE) containing 10 wt % PFE as described above. Aminosilane, alkoxysilane and 1173 were dissolved or dispersed in HFE to form a 1 wt % or 5 wt % solution or suspension, and mixed with the PFE-1 solution as described above.

[0368]

[0369]

[0370] Table 13: Effect of aminosilane esters on UV-cured PFE-2

[0371]

[0372] Some of the compositions of Examples 12-1 to 13-1 were cured with D bulbs instead of H bulbs and provided similar crosslinking results.

[0373] General Procedure - Compounding Fluoropolymers (CFP) with Inorganic Fillers :

[0374] Compounded fluoropolymer (CFP) was prepared by mixing 100 g of perfluoroelastomer with filler according to Table 14 using conventional rubber processing equipment to provide a well mixed solid mixture of perfluoroelastomer and filler. Glass bubbles were treated with a fluorinated hydrophobic surface treatment prior to use.

[0375] Table 14: Compounded Fluoropolymers (CFP) Prepared

[0376] CFP illustrate CFP-1 Fluoropolymer containing PFE-3 and FG-Si in a ratio of 70 / 30 by weight CFP-2 Fluoropolymer with a 50 / 50 weight ratio of PFE-3 and FG-Si CFP-3 Fluoropolymer with a weight ratio of 80 / 20 of PFE-3 and FG-Si CFP-4 Fluoropolymer with a weight ratio of 80 / 20 of PFE-3 and glass bubbles CFP-5 Fluoropolymer with a weight ratio of 70 / 30 of PFE-3 and FS20 CFP-6 Fluoropolymer with a weight ratio of 70 / 30 for PFE-3 and FS550 CFP-7 Fluoropolymer containing PFE-1 and FG-Si in a ratio of 70 / 30 by weight CFP-8 Fluoropolymer with a weight ratio of 80 / 20 of PFE-1 and glass bubbles

[0377] SRC220 surface treated glass bulb

[0378] A solution was prepared by adding 9 g of 3M antifouling additive SRC220 (aqueous fluorinated polyurethane dispersion, 15% solids) to 50 g of DI water, stirring for 5 minutes, and transferring the solution to a 60 mL syringe with an 18 gauge needle syringe.

[0379] To a 1 gallon size Lodige Popenmier mixer, 900 g of iM16K glass bubbles were added. The surface treatment solution was sprayed while mixing at a mixing rate of 400 rpm. After mixing at room temperature for 15 minutes, the mixing vessel was heated to 120°C-130°C for 1.5 hours.

[0380] General procedure for coatings from PFE-3 and CQ0382 or CQ1082 :

[0381] The PFE coating solution was prepared as generally described above to obtain a 9 wt % HFE solution. The fused silica filler was dispersed separately in HFE with a high-speed mixer to form a 50 wt % solid dispersion. The PFE solution and the fused silica dispersion were mixed with each other, and then a curing agent, an alkoxysilane, and glass fibers were added. The PFE composite membrane was obtained by coating the solution with a comma bar coater having a gap of 300um to 350um. The obtained coating was applied to a release liner (pre-coated with a fluorinated release coating) and then dried in an oven at 100°C to remove the solvent. The membrane was then separated from the liner and placed in a Teflon-coated metal tray and baked at 160°C to 200°C to crosslink the system. The thickness of the obtained membrane ranged from 230um to 290um. The membrane was characterized using different test methods. The concentrations of the components (i.e., solids) and the results are summarized in Tables 15 to 17.

[0382] Table 15: PFE-3 composition and CTE results

[0383]

[0384] Table 16: Dielectric constant (Dk), dissipation loss (Df), T-stripping with copper and static water contact of PFE-3 compositions Corner Results

[0385] Example Dk Df T-stripping with copper Water contact angle 15.1 2.45 0.0019 0.6N / mm 103°-106° 15.2 2.37 0.0018 0.6N / mm 103°-106° 15.3 2.24 0.0017 0.6N / mm 103°-106° 15.4 1.98 0.002 0.6N / mm 103°-106° 15.5 2.23 0.0019 0.6N / mm 103°-106°

[0386] Table 17: PFE-3 compositions with different silica sizes and CTE results

[0387]

[0388] General procedure for coatings from PFE-3 and fused silica (SF550) :

[0389] As generally described above, a solution of PFE-3 and fused silica in HFE was prepared using PFE-3 glue (20 g, cut into small pieces), 3M fused silica (8.6 g, FS550) and HFE (290 g). The stable coating solution had 6.45% by weight of PFE-3, and the ratio of PFE-3 to FS550 was 70 / 30 by weight. Similarly, a coating solution of 6.45% PFE-3 and fused silica was prepared using 20 g PFE-3, 6.0 g FS550 and 290 g HFE.

[0390] All crosslinkers (e.g., BTESPA) were dissolved in HFE to form a 5% or 10% solution. Based on the amount of PFE, 3% to 5% BTESPA crosslinker was prepared in the PFE-3 / FS550 solution. Based on the weight of FS550, the alkoxysilane compound was prepared with the PFE-3 / FS550 solution as shown below. After complete mixing, the solution was coated on the RL film or DuPontPFA film at different thicknesses and then cured in an oven at 140°C for 5 hours. The coating on the release liner was removed from the liner before testing, and the coating on the PFA film was tested directly on the PFA film. The CTE of the film peeled from the liner was tested. The formulations and test results are summarized in Tables 18 and 19. For some embodiments, the moisture absorption rate (23°C / 5%-95%RH) was measured. The moisture absorption rate of sample 18.6 was 0.11%.

[0391] Table 18: Coating compositions from PFE-3 and SF550 fused silica

[0392]

[0393] Table 19: Test results of coating compositions from PFE-3 and SF550 fused silica

[0394]

[0395] Coatings from compounded fluoropolymers :

[0396] For the coating solution formulation, all CFP (20g, cut into small pieces) were first dissolved in HFE (180g) to obtain a 10% solution after vigorous shaking overnight in a sealed glass bottle. All crosslinking agents (e.g., BTESPA) were dissolved in HFE to have a 5% or 10% solution. As shown in Table 20, all crosslinking agents were prepared in CFP solutions based on the gross weight of CFP. After complete mixing, the solution was coated on RL film or DuPont PFA film or FEP film with different thicknesses and then cured in a 140°C oven for 5 hours before testing. The coating on the release liner was removed from the liner before testing, and the coating on the PFA film was directly tested on the PFA film. The CTE of the film peeled off from the liner was tested. The results are summarized in Tables 20 and 21. For some embodiments in the embodiments, moisture absorption (23°C / 5%-95%RH) was measured. Two examples that exhibited good moisture absorption were 20.12 and 20.14, which had moisture absorptions of 0.15% and 0.13%, respectively.

[0397] Table 20: Compounded Fluoropolymer Coating Formulations

[0398]

[0399]

[0400] Table 21: Dk, Df and CTE of Compounded Fluoropolymer Coatings

[0401]

[0402] Compounded fluoropolymer coatings cured by UV :

[0403] The 10% coating solution of the compounded fluoropolymer and (for example, silica) inorganic filler is prepared as generally described above by 20g PFE-1 base CFP glue (cut into small pieces) and 180g HFE in a sealed glass bottle at room temperature after vigorous shaking overnight. Cross-linking agents (BTESPA and TAIC) are dispersed in HFE to produce a 5% solution. As shown below, based on the gross weight of CFP, all cross-linking agents (BTESPA and TAIC) are prepared in CFP solution. After complete mixing, the solution is coated on DuPont PFA film or FEP film with different thicknesses. First the coating is dried in a 100°C oven for 5 minutes, then cured by 10 times with 30fpm under nitrogen with H bulb UV at 100% power. The results are summarized in Table 22.

[0404] Table 22: Compounded Fluoropolymer Coating Formulations and Dk / Df / CTE Results

[0405]

[0406] General procedure for coating from PFE-3 and silica particles :

[0407] The PFE coating solution was prepared as generally described above to obtain a 5 wt % solution of PFE-3 in HFE-7300. A fused silica filler was separately dispersed in HFE using a high speed mixer to form a 50 wt % solids dispersion.

[0408] Dissolve or disperse bis(3-trimethoxysilylpropyl)amine (BTMSPA) in HFE-7300 to form a 10 wt % solution or suspension. Add BTMSPA and silica particles as indicated in Table 23 to the PFE-3 solution. Homogenize the HFE-7300 solution of BTMSPA for 10 seconds at 1000 revolutions per minute (rpm) using a vortex shaker to form a well-dispersed slurry, which is then added to the PFE-3 / HFE-7300 solution. The percentages shown in the formula (e.g., 5%, 2%) are mass fractions based on the solid content of PFE-3. For example, PFE-3+5% BTMSPA means: PFE-3 / APES=95:5 solid content. The solution prepared above is typically stirred at 2500 rpm under vortex for 1-2 minutes. All solutions prepared above were coated onto a clean PET release liner or copper foil using a No. 24 Meyer rod and the resulting coatings were typically cured for 20 minutes to 1 hour at 165° C. The cured films were peeled from the liner and evaluated for Dk, Df, moisture absorption and CTE.

[0409] Table 23: Perfluoropolymer Composite Coating Formulations and Dk / Df / Moisture Absorption / CTE Results

[0410]

[0411] General Procedure for Preparation of Coating Solutions of Perfluoroelastomer-Perfluoroplastic Nanoparticle Dispersions: PFE-PFA or PFE- Preparation of PTFE coagulation and dispersion solutions

[0412] The perfluoroelastomer PFE-3 (30.5 wt%) was co-coagulated with PFA latex (30 wt%, PFA-2 latex) or with PTFE latex (30 wt%, obtained from the dilution of 55 wt% TFM-2 latex) in the ratios described in Table 24. The latex solutions were mixed and placed on a roller for 20 minutes. Subsequently, the well-mixed solution was frozen in a refrigerator overnight. It was taken out and thawed in warm water or in an oven at 60°C. After melting, the precipitate was filtered and washed with deionized (DI) water at least three times. The obtained solid was dried in an air circulating oven at 55°C-65°C overnight. The dried PFE / PFA-2 and PFE / PTFE co-coagulated solids were mixed with HFE-7300 in 5 wt%-20 wt% solutions, respectively. They were placed on a shaker or roller at 80 cycles / min overnight or longer to obtain a stable and well-dispersed solution in HFE-7300 (Table 24).

[0413] General procedure for the preparation of perfluoropolymer coating solutions, optionally with aminosilane ester or fluorinated amidine curing agents and inorganic fillers, including spherical silica, glass fiber particles for coating, electrical property measurements, and copper bond adhesion measurements. Pellets and Boron Nitride Pellets :

[0414] PFE-3, PFE-3 / PFA-2 or PFE-3 / PTFE was dissolved / dispersed in HFE-7300 by cutting the fluoropolymer material into small pieces and placing them in separate glass jars and adding HFE-7300 solvent to each of the glass jars. The containers were fully sealed with PTFE tape and parafilm. The solution was then shaken vigorously overnight (about 12 hours) to obtain a completely uniform solution of 5 wt%-8 wt% PFE-3 in HFE-7300 (e.g., 5 g PFE-3 and 95 g HFE-7300), 10 wt% PFE-3 / PTFE or PFE-3 / PFA-2 in HFE-7300.

[0415] BTMSPA, aminosilane or fluorinated amidine curing agent were added to PFE-3, PFE-3 / PTFE or PFE-3 / PFA-2 dispersion solutions at the percentages described in Table 24 to prepare perfluorinated polymer HFE solutions for coating. In the case of a coating solution containing an inorganic filler, the inorganic filler or mixed filler was weighed in a glass jar, and a small amount of HFE solvent was added to each of the inorganic filler or mixed filler and vortexed for 1-2 minutes. The fluorinated polymer HFE solution and curing agent prepared above were added to the HFE-7300 filler or mixed filler slurry, respectively, and the ratio of the added amount was as described in Table 24.

[0416] An alternative way to prepare the above-mentioned fluoropolymer-HFE solution containing inorganic fillers is to first mix the fluoropolymer PFE-3, PFE-3 / PFA-2 or PFE-3 / PTFE with one or more inorganic fillers in a certain ratio, and then add a certain amount of HFE-7300 to make the solution concentration reach a certain weight % as described in Table 24. The prepared solution is placed in a shaker or roller at a speed of 80 cycles / minute overnight or longer. The resulting solution is uniform. Aminosilane BTMSPA or other curing agents are added to the freshly prepared fluoropolymer-inorganic filler-HFE-7300 solution at the ratio described in Table 24. In addition, the percentages in the formula (e.g., 5%, 2%) are mass fractions based on the solid content of PFE-3. For example, PFE-3+5%BTMSPA means: PFE-3 / APES=95:5 solid content. The above-prepared solution is usually stirred at 2500rpm under vortex for 1 minute to 2 minutes. All of the above prepared solutions were coated onto a 3M release liner with a #24 Meyer rod, or the solutions were simply poured onto the liner to obtain thicker coating samples, and the resulting coatings were typically dried overnight at room temperature or cured at 120°C-165°C for 20 minutes-105 minutes. The cured films were peeled off the liner and used for adhesion to copper, Dk / Df measurements, and CTE measurements as shown in Table 24.

[0417] The perfluoropolymer solution was coated on a release liner and dried overnight at room temperature or cured at 120° C. to 165° C. for 30 minutes to 105 minutes. The resulting film, with an average thickness of 15 microns to 40 microns, was peeled from the liner and then laminated against a Cu foil in a sandwich structure for bonding at the temperature indicated in the table and under a pressure of 1 ton to 2 tons, typically for 30 minutes.

[0418] Table 24: Cu-bondable perfluorinated polymer films obtained by coating

[0419]

[0420]

[0421]

[0422]

[0423] General Procedure for Preparation of Perfluoropolymer Coating Solutions with Inorganic Fillers :

[0424] The solution containing the co-coagulated perfluoropolymer and one or more inorganic fillers (e.g., silica nanoparticles, quartz fibers, and boron nitride) is called a fluoropolymer resin and is dissolved / dispersed in HFE-7300. The solution is prepared in the following step-by-step procedure: the dried inorganic and fluoropolymer resins are mixed in a container and HFE-7300 is added. The container is then sealed and placed on a roller to gently stir overnight or longer until it is determined that the solution is completely mixed and ready for coating. The solution is then transferred to a shear mixing container and mixed at 2500rpm-3500rpm for 3 minutes-4 minutes. BTMSPA (5% by mass of resin in the solution) is added to the well-mixed solution. After adding BTMSPA, the solution is vortexed to mix thoroughly and then placed on a shaker for 30 minutes-60 minutes. The solution is then coated on a release liner using a No. 24 Meyer rod and a belt guide to control the film thickness. The film is air-dried at room temperature, then removed from the release liner, and thermally cured at 165°C for 1 hour. The cured samples were then ready for testing.

[0425] Table 25: Perfluorinated polymer composite coatings*

[0426]

[0427]

[0428] *Average film thickness is 100 microns.

[0429] Table 26: Perfluorinated polymer composite coatings*

[0430]

[0431] *Average film thickness is 100 microns - 130 microns.

Claims

1. An electronic communication article comprising a crosslinked fluoropolymer layer, wherein the fluoropolymer comprises at least 80% by weight of polymerized units of a perfluorinated monomer and cure sites; and i) crystallized fluoropolymer particles, ii) fumed silica or fused silica having an aggregate particle size of at least 500 nm, or A combination of i) and ii); The article is an integrated circuit, a printed circuit board, an antenna or an optical cable.

2. The electronic communication article of claim 1, wherein the cross-linked fluoropolymer layer is a substrate, a patterned layer, an insulating layer, a passivation layer, a cladding layer, a protective layer, or a combination thereof.

3. The electronic communication article of claim 1, wherein the antenna is an antenna of a computer device or an outdoor structure.

4. The electronic communication product according to claim 1, wherein the cross-linked fluoropolymer layer has i) a dielectric constant less than 2.75; ii) Dielectric loss less than 0.01; or a combination thereof.

5. The electronic communication article of claim 1, wherein the fluoropolymer further comprises a cure site selected from the group consisting of nitrile, iodine, bromine, and chlorine.

6. The electronic communication article of claim 1, wherein the perfluorinated monomer is selected from tetrafluoroethylene and one or more unsaturated perfluorinated alkyl ethers.

7. The electronic communication product according to claim 6, wherein the unsaturated perfluorinated alkyl ether of the fluorine-containing polymer has the general formula: R f -O-(CF2) n -CF=CF2 Where n is 1 or 0, and R f is a perfluoroalkyl group or a perfluoroether group.

8. The electronic communication article of claim 1, wherein the cross-linked fluoropolymer is cross-linked using a curing agent selected from: i) peroxides and ethylenically unsaturated compounds; ii) one or more compounds comprising an electron donor group and an ethylenically unsaturated group; or iii) Aminoorganosilane ester compound or ester equivalent.

9. The electronic communication article of claim 8, wherein the curing agent comprises at least two ethylenically unsaturated groups or at least one ethylenically unsaturated group and at least one alkoxysilane group.

10. The electronic communication article of claim 1, wherein the crosslinked fluoropolymer is crosslinked with an amine curing agent.

11. The electronic communication article of claim 1, wherein the fluoropolymer comprises 40 wt% to 60 wt% of polymerized units of TFE based on the total weight of the fluoropolymer.

12. The electronic communication article of claim 1, wherein the crosslinked fluoropolymer comprises no more than 5 weight percent of polymerized units derived from non-fluorinated or partially fluorinated monomers and / or comprises no more than 5 weight percent of ester-containing linking groups.

13. The electronic communication article of claim 1, wherein the cross-linked fluoropolymer is insoluble in 3-ethoxyperfluorinated 2-methylhexane or 3-methoxyperfluorinated 4-methylpentane.

14. The electronic communication article of any one of claims 1 to 13, wherein the cross-linked fluoropolymer layer further comprises glass fibers or glass bubbles.

15. The electronic communication article of any one of claims 1 to 13, wherein the cross-linked fluoropolymer layer further comprises a thermally conductive filler.

16. The electronic communication article of claim 1, wherein the fumed silica or the fused silica has an aggregate particle size of at least 1 micron.

17. The electronic communication article of claim 1 wherein the silicon dioxide comprises a hydrophobic surface treatment optionally comprising a fluorinated alkoxysilane compound.

18. The electronic communication article of claim 1, wherein the silicon dioxide is present in an amount of at least 10 wt. % based on the total amount of the cross-linked fluoropolymer layer.