Alkaline polishing method for silicon wafer, PERC battery and preparation method thereof
Through multiple batches of alkali polishing and adjusting the alkali polishing solution formula, the problems of high fragmentation rate and low photoelectric conversion efficiency caused by thinning of silicon wafers have been solved, efficient polishing and low-cost processing of silicon wafers have been achieved, and PERC cells have been improved. photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202210231922.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-03-09
AI Technical Summary
In the context of the thinning of silicon wafers, debris is easily generated during the alkali polishing process, which affects the photoelectric conversion efficiency of the silicon wafer and increases the processing difficulty.
A multi-batch alkali polishing treatment method is adopted, including pre-cleaning, alkali polishing, post-cleaning, pickling, slow pulling and drying steps. By adjusting the formula of the alkali polishing solution, the weight loss and fragmentation rate of the silicon wafers are reduced, and the back surface is improved. The flatness of the polished surface.
It effectively reduces the fragmentation rate during alkali polishing of silicon wafers, improves the photoelectric conversion efficiency of silicon wafers, and reduces the amount and cost of chemicals used in the preparation process.
Smart Images

Figure CN114628252B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to an alkali polishing method for a silicon wafer, a PERC cell and a preparation method thereof. Background Art
[0002] PERC (Passivated Emitter and Rear Cell) is the passivated emitter and rear cell technology. PERC technology improves the conversion efficiency by adding a dielectric passivation layer on the rear side of the cell, which requires the back surface of the silicon wafer to have good flatness. PERC cell technology has obvious performance and cost advantages, which has promoted the application of P-type solar-grade silicon wafers. However, due to the trend of thinning cells, the thickness of monocrystalline silicon wafers is also gradually becoming thinner. The amount of silicon wafers that can be produced with the same quality of silicon material has greatly increased, which can reduce the cost of raw materials, but the processing difficulty of downstream cells has also increased accordingly.
[0003] Alkali polishing is a common process for back polishing of silicon wafers. The principle of alkali polishing is that alkali reacts with the back of the silicon wafer to polish. The front of the silicon wafer is not reacted due to the protection of the oxide layer, and the velvet surface on the back of the silicon wafer reacts with the alkali to form a back polished surface with higher flatness. As the thickness of the silicon wafer raw material used becomes thinner, it is easier to generate fragments in the alkali polishing process, which affects the photoelectric conversion efficiency of the silicon wafer. Summary of the invention
[0004] Based on this, it is necessary to provide an alkali polishing method for silicon wafers that has less weight loss, is not easy to break, and can improve battery efficiency.
[0005] In addition, a PERC cell processed by the above-mentioned silicon wafer alkali polishing method and a preparation method thereof are also provided.
[0006] In one aspect of the present invention, there is provided an alkali polishing method for a silicon wafer, the alkali polishing method comprising a plurality of batches of alkali polishing treatments performed sequentially, each batch of alkali polishing treatments comprising the following steps:
[0007] Pre-cleaning: cleaning the silicon wafer in a first mixed solution, wherein the first mixed solution includes an alkaline reagent and H2O2;
[0008] Alkali polishing: the silicon wafer after pre-cleaning is subjected to alkaline polishing in an alkaline polishing solution;
[0009] Post-cleaning: cleaning the silicon wafer after alkali polishing in a second mixed solution, wherein the second mixed solution includes an alkaline reagent and H2O2;
[0010] Pickling: soaking the silicon wafer after post-cleaning in an acid solution to remove the oxide layer;
[0011] Slow pulling: washing the pickled silicon wafer in water and slowly pulling it out; and
[0012] dry;
[0013] The alkali polishing liquid in the first batch of alkali polishing treatment is an initial alkali polishing liquid, and the components of the initial alkali polishing liquid include: water, alkali solution and alkali polishing additive in a volume ratio of (320-340): (9.5-12.5): (2.5-3.5);
[0014] The alkali polishing solution of the nth batch of alkali polishing treatment is prepared by adding a replenishing solution to the alkali polishing solution of the n-1th batch; the components of the replenishing solution include: (5.5 ~ 6.5): (0.24 ~ 0.28): (0.17 ~ 0.20) of water, alkali solution and alkali polishing additive; the volume ratio of the replenishing solution of the nth batch to the initial alkali polishing solution is (5.91 ~ 6.98): (332 ~ 356); wherein 2≤n≤60;
[0015] The alkali solution is selected from an aqueous solution of at least one of sodium hydroxide and potassium hydroxide, and the concentration of the alkali solution is 45wt% to 48wt%.
[0016] In some of the embodiments, in the initial alkali polishing solution, the volume ratio of the water, the alkali solution and the alkali polishing additive is (327 ~ 329): (10.5 ~ 11.5): (2.8 ~ 3.2).
[0017] In some of the embodiments, in the replenishing solution, the volume ratio of the water, the alkali solution and the alkali polishing additive is (5.9 ~ 6.1): (0.265 ~ 0.275): (0.19 ~ 0.20).
[0018] In some embodiments, the temperature of the alkali polishing step is 60° C. to 66° C., and the time is 140 s to 160 s.
[0019] In some embodiments, the temperature of the alkali polishing step is 64° C. to 66° C., and the time is 145 s to 155 s.
[0020] In some embodiments, the alkali polishing additive is selected from BP51.
[0021] In some embodiments, the pre-cleaning step is performed at a temperature of 45° C. to 60° C. and for a time of 40 s to 50 s.
[0022] In some embodiments, the post-cleaning step is performed at a temperature of 25° C. to 40° C. and for a time of 120 s to 180 s.
[0023] Another aspect of the present invention provides a method for preparing a PERC cell, comprising the steps of sequentially performing texturing, diffusion, SE, thermal oxidation, alkali polishing, annealing, micro-conduction and coating on a silicon wafer; the alkali polishing step is performed using the above-mentioned alkali polishing method for silicon wafers.
[0024] Another aspect of the present invention further provides a PERC cell produced by the above-mentioned PERC cell production method.
[0025] In the above-mentioned alkali polishing method for silicon wafers, the alkali polishing liquid used in the alkali polishing step includes: the initial alkali polishing liquid includes water, alkali solution and alkali polishing additives in a volume ratio of (320 ~ 340): (9.5 ~ 12.5): (2.5 ~ 3.5); the volume ratio of water, alkali solution and alkali polishing additives in the replenishing solution is (5.5 ~ 6.5): (0.24 ~ 0.28): (0.17 ~ 0.20). By adjusting the formula of the alkali polishing liquid, the weight loss of the silicon wafer in the above-mentioned alkali polishing method for silicon wafers is small, and the weight loss is about 0.15 g / g, which can reduce the weight loss of silicon wafers by alkali polishing, thereby reducing the fragmentation rate in the preparation process. The above-mentioned alkali polishing method for silicon wafers is used to prepare PERC cells, and the prepared PERC cells have good photoelectric conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A tower base diagram of the back polished surface of a single crystal silicon wafer prepared by the alkali polishing method of the silicon wafer in Example 1 of the present invention;
[0027] Figure 2 This is a tower base diagram of the back polished surface of a single crystal silicon wafer prepared by the alkali polishing method of the silicon wafer in Comparative Example 1 of the present invention;
[0028] Figure 3 The weight loss and fragmentation rate results of the single crystal silicon wafers obtained by the alkali polishing method of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3;
[0029] Figure 4 is the consumption of alkali solution and alkali polishing additive in the alkali polishing method of Example 3 of the present invention and Comparative Example 3;
[0030] Figure 5 This is a bar chart of the efficiency of PERC cells prepared in Examples 4 to 6 of the present invention and Comparative Examples 4 to 6. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0033] An embodiment of the present invention provides an alkali polishing method for a silicon wafer, the alkali polishing method comprising a plurality of batches of alkali polishing treatments performed sequentially, each batch of alkali polishing treatments comprising the following steps S110 to S160. Specifically, the silicon wafer can be selected from a single crystal silicon wafer and a polycrystalline silicon wafer.
[0034] Step S110: Pre-cleaning: Clean the silicon wafer in a first mixed solution, wherein the first mixed solution includes an alkaline reagent and H2O2.
[0035] In some embodiments, in step S110, the alkaline agent is selected from at least one of sodium hydroxide and potassium hydroxide. In some embodiments, in the first mixed solution, the mass ratio of the alkaline agent to H2O2 is (230-460): (960-1920). Further, in the first mixed solution, the mass ratio of the alkaline agent to H2O2 is (368-460): (1280-1920).
[0036] In some embodiments, the temperature of the pre-cleaning step in step S110 is 45° C. to 60° C., and the time is 40 s to 50 s.
[0037] Step S120: Alkali polishing: The silicon wafers obtained in step S110 are subjected to alkali polishing in an alkali polishing solution. The alkali polishing solution in the first batch of alkali polishing treatment is an initial alkali polishing solution, and the components of the initial alkali polishing solution include water, alkali solution and alkali polishing additives in a volume ratio of (320 ~ 340): (9.5 ~ 12.5): (2.5 ~ 3.5).
[0038] The alkali polishing solution of the nth batch of alkali polishing treatment is prepared by adding a replenishing solution to the alkali polishing solution of the n-1th batch; the components of the replenishing solution include water, alkali solution and alkali polishing additives in a volume ratio of (5.5 ~ 6.5): (0.24 ~ 0.28): (0.17 ~ 0.20). The volume ratio of the replenishing solution of the nth batch to the initial alkali polishing solution is (5.91 ~ 6.98): (332 ~ 356). Wherein, 2≤n≤60.
[0039] Specifically, after the n-1th batch of single crystal silicon wafers is processed through step S110 to step S160, replenishing solution is added to the alkaline polishing solution, and then the nth batch of single crystal silicon wafers is processed by repeating step S110 to step S160.
[0040] In some embodiments, the components of the initial alkali polishing solution include: 320 L ~ 340 L of water, 9.5 L ~ 12.5 L of alkali solution and 2.5 L ~ 3.5 L of alkali polishing additive. The components of the replenishing solution include: 5.5 L ~ 6.5 L of water, 240 mL ~ 280 mL of alkali solution and 170 mL ~ 200 mL of alkali polishing additive. It can be understood that the formula of the initial alkali polishing solution and the replenishing solution can be adjusted according to the ratio of water, alkali solution and alkali polishing additive according to the processing equipment or the number of single crystal silicon wafers processed in each batch.
[0041] The alkali solution is selected from an aqueous solution of at least one of sodium hydroxide and potassium hydroxide, and the concentration of the alkali solution is 45 wt% to 48 wt%. Optionally, the 45 wt% to 48 wt% sodium hydroxide aqueous solution is selected from one of Dongfeng 45 wt% sodium hydroxide solution and Jianghua 45 wt% sodium hydroxide solution.
[0042] In some embodiments, in step S120, the alkali polishing additive is selected from Tuobang BP51. In some embodiments, in step S120, the water used in the alkali polishing liquid formula is deionized water.
[0043] In some of the embodiments, in step S120, the volume ratio of water, alkali solution and alkali polishing additive in the initial alkali polishing solution is (327 ~ 329): (10.5 ~ 11.5): (2.8 ~ 3.2).
[0044] In some of the embodiments, in step S120, the volume ratio of water, alkali solution and alkali polishing additive in the replenishing solution is (5.9 ~ 6.1): (0.265 ~ 0.275): (0.19 ~ 0.20).
[0045] In some embodiments, in step S120, the temperature of the alkali polishing step is 60°C to 66°C, and the time is 140 s to 160 s. Optionally, the temperature of the alkali polishing step is 60°C, 61°C, 62°C, 63°C, 64°C, 65°C or 66°C; the time of the alkali polishing step is 140 s, 145 s, 150 s, 155 s or 160 s. Further, in step S120, the temperature of the alkali polishing step is 64°C to 66°C, and the time is 145 s to 155 s.
[0046] Compared with the traditional alkali polishing process, the alkali polishing step in the above-mentioned alkali polishing step shortens the time of the alkali polishing step. The alkali polishing step time is 140 s ~ 160 s, which can ensure the polishing effect of the wafer and obtain a silicon wafer with high back flatness. In addition, the weight loss of the silicon wafer in the alkali polishing method is smaller, which can avoid silicon wafer breakage, and the photoelectric conversion efficiency of the battery is higher.
[0047] In some embodiments, before step S120, a step of washing the silicon wafer obtained in step S110 is also included to clean the chemical residues on the surface of the silicon wafer. Specifically, the operation of the washing step is: immersing the silicon wafer obtained in step S110 in water for washing. In some embodiments, the washing step lasts for 120 s to 200 s.
[0048] Step S130: Post-cleaning: Clean the silicon wafer obtained in step S120 in a second mixed solution, wherein the second mixed solution includes an alkaline reagent and H2O2.
[0049] In some embodiments, in step S130, the alkaline agent is selected from at least one of sodium hydroxide and potassium hydroxide. In some embodiments, in the second mixed solution, the mass ratio of the alkaline agent to H2O2 is (230-460): (960-1600). Further, in the second mixed solution, the mass ratio of the alkaline agent to H2O2 is (368-460): (1280-1600).
[0050] In some embodiments, the temperature of the post-cleaning step in step S130 is 25° C. to 60° C., and the time is 120 s to 180 s.
[0051] In some embodiments, before step S130, a step of washing the silicon wafer obtained in step S120 is also included. Specifically, the operation of the washing step is to soak the silicon wafer obtained in step S120 in water for washing. In some embodiments, the time of the washing step is 110 s to 200 s.
[0052] Step S140: Pickling: The silicon wafer obtained in step S130 is immersed in an acid solution for cleaning to remove the oxide layer.
[0053] In some embodiments, the acid solution in step S140 is a hydrofluoric acid solution, wherein the mass concentration of HF in the hydrofluoric acid solution is 40% to 55%.
[0054] In some embodiments, in step S140, the pickling time is 120 s to 200 s.
[0055] In some embodiments, before step S140, a step of washing the silicon wafer obtained in step S130 is also included. Specifically, the operation of the washing step is to soak the silicon wafer obtained in step S130 in water for washing. In some embodiments, the time of the washing step is 110 s to 200 s.
[0056] Step S150: Slow pulling: Wash the silicon wafer obtained in step S140 in water and slowly pull it out.
[0057] In some embodiments, the temperature of the slow pulling in step S150 is 20° C. to 35° C. The speed of the slow pulling is 3 mm / s to 5 mm / s.
[0058] In some embodiments, before step S150, a step of washing the silicon wafer obtained in step S140 is also included. Specifically, the operation of the washing step is to immerse the silicon wafer obtained in step S140 in water for washing. In some embodiments, the time of the washing step is 100 s to 200 s.
[0059] Step S160: Drying: Use clean air or nitrogen to dry the silicon wafer obtained in step S150.
[0060] In some embodiments, the drying temperature in step S160 is 95° C. to 120° C. and the drying time is 10 min to 12 min.
[0061] In the above-mentioned alkali polishing method for silicon wafers, the alkali polishing liquid used in the alkali polishing step includes: the initial alkali polishing liquid includes water, alkali solution and alkali polishing additives in a volume ratio of (320 ~ 340): (9.5 ~ 12.5): (2.5 ~ 3.5); the volume of water, alkali solution and alkali polishing additive in each batch of replenishing solution is (5.5 ~ 6.5): (0.24 ~ 0.28): (0.17 ~ 0.20). By adjusting the formula of the alkali polishing liquid, the weight loss of the silicon wafer in the above-mentioned alkali polishing method for silicon wafers is small, and the weight loss is about 0.15 g / g, which can reduce the weight loss of silicon wafers during alkali polishing, reduce the fragmentation rate during the preparation process, and the back polished surface of the silicon wafer after alkali polishing is bright and flat.
[0062] In some embodiments, the weight loss of the silicon wafer prepared by the alkali polishing method of the silicon wafer is 0.150 g / g to 0.159 g / g. In some embodiments, the weight loss of the silicon wafer prepared by the alkali polishing method of the silicon wafer is 0.150 g / g, 0.151 g / g, 0.152 g / g, 0.154 g / g, 0.155 g / g, 0.156 g / g, 0.158 g / g or 0.159 g / g.
[0063] In some of the embodiments, the tower base size of the back-polished surface of the silicon wafer prepared by the alkali polishing method of the silicon wafer is 9 μm to 11 μm.
[0064] Another embodiment of the present invention also provides a method for preparing a PERC battery, comprising the steps of texturing, diffusion, SE, thermal oxidation, alkali polishing, annealing, micro-conduction and coating on a silicon wafer in sequence; the alkali polishing step is carried out using the above-mentioned alkali polishing method for silicon wafers.
[0065] In the preparation method of the above-mentioned PERC battery, the alkaline polishing is carried out using the alkaline polishing method of the above-mentioned silicon wafer. The back polished surface of the prepared silicon wafer has a higher flatness, and the weight loss in the alkaline polishing process of the silicon wafer is small, and the fragmentation rate is low. Therefore, the photoelectric conversion efficiency of the prepared battery cell is higher.
[0066] In some embodiments, the method for preparing a PERC cell comprises the following steps:
[0067] Texturing: The silicon wafer is subjected to surface texturing to obtain a good velvet structure;
[0068] Diffusion: Phosphorus oxychloride is introduced into the silicon wafer to react and achieve diffusion bonding;
[0069] SE process: The selective emitter is on a lightly doped silicon substrate, and impurity atoms are selectively heavily doped by a micron-sized laser beam;
[0070] Thermal oxidation: A high-temperature thermal oxidation process is added after the SE process to produce and deposit a silicon dioxide protective layer on the surface of the silicon wafer;
[0071] PSG removal: Use HF to remove the oxide layer and phosphosilicate glass on the back of the silicon wafer;
[0072] Alkali polishing: using the above-mentioned batch alkali polishing method for silicon wafers for treatment;
[0073] Annealing: Annealing the silicon wafer after alkali polishing to produce and deposit a silicon dioxide film layer on the surface of the silicon wafer;
[0074] Microguide: Deposit aluminum oxide passivation film on the back of silicon wafer by ALD method;
[0075] Coating: growing and depositing silicon nitride film on the front and back of silicon wafers;
[0076] Laser grooving: laser grooving on the back of the coated silicon wafer;
[0077] Printing and sintering: The back and front sides are printed by screen printing, and then the sintering process is carried out;
[0078] Electric injection: Electric injection is carried out through a light decay furnace or an electric injection furnace;
[0079] Test and sorting: Finally, the battery cells are tested and sorted.
[0080] Another embodiment of the present invention further provides a PERC cell produced by the above-mentioned PERC cell production method.
[0081] The following are specific embodiments. Example
[0082] The single crystal silicon wafer of this embodiment is alkaline polished according to the following steps:
[0083] (1) Take a single crystal silicon wafer that has been processed by texturing, diffusion, SE, thermal oxidation, and PSG removal for use. The size of the single crystal silicon wafer is 158.75 mm*158.75 mm.
[0084] (2) Pre-cleaning: Soak the single crystal silicon wafer in a first mixed solution at 45°C for 40 seconds. The first mixed solution is an aqueous solution with a mass ratio of sodium hydroxide to H2O2 of 400:1600.
[0085] (3) Water washing: Soak the single crystal silicon wafer prepared in step (2) in pure water for 120 s.
[0086] (4) Alkali polishing: Soak the single crystal silicon wafers in step (3) in an alkaline polishing solution at 65°C for 150 s. The formula of the alkaline polishing solution is as follows: the initial alkaline polishing solution is prepared from 328 L of deionized water, 11.0 L of Jianghua 45 wt% sodium hydroxide solution and 3.0 L of alkaline polishing additive Tuobang BP51; each batch of replenishing solution is prepared from 6.0 L of deionized water, 270 mL of Jianghua 45 wt% sodium hydroxide solution and 200 mL of alkaline polishing additive Tuobang BP51.
[0087] (5) Water washing: Soak the single crystal silicon wafer obtained in step (4) in pure water for 120 s.
[0088] (6) Post-cleaning: Soak the single crystal silicon wafer in step (5) in a second mixed solution at 25° C. for 120 s. The second mixed solution is an aqueous solution with a mass ratio of sodium hydroxide to H2O2 of 400:1600.
[0089] (7) Water washing: Soak the single crystal silicon wafer obtained in step (6) in pure water for 110 s.
[0090] (8) Pickling: Immerse the single crystal silicon wafer obtained in step (7) in a 40 wt% hydrofluoric acid solution for 120 s.
[0091] (9) Water washing: Soak the single crystal silicon wafer prepared in step (8) in pure water for 100 s.
[0092] (10) Slow pulling: The single crystal silicon wafer from step (9) is cleaned in pure water at 25°C, and the single crystal silicon wafer is slowly lifted at a speed of 3 mm / s.
[0093] (11) Drying: Dry the single crystal silicon wafer obtained in step (10) at 95° C. in clean air for 11 min.
[0094] Each batch of single crystal silicon wafers completes steps (1) to (11), i.e., replenishes the alkali polishing solution, and then performs alkali polishing on the next batch of single crystal silicon wafers. Three batches of 400 single crystal silicon wafers in each batch are subjected to alkali polishing according to steps (1) to (11). Example
[0095] The alkali polishing method for single crystal silicon wafers in this embodiment is basically the same as that in Embodiment 1, except that in this embodiment, alkali polishing is performed on 15 batches of 400 single crystal silicon wafers in each batch according to steps (1) to (11). Example
[0096] The alkali polishing method for single crystal silicon wafers in this embodiment is basically the same as that in Embodiment 1, except that in this embodiment, 600 batches of 400 single crystal silicon wafers are subjected to batch alkali polishing according to steps (1) to (11). Example
[0097] The PERC cell of this embodiment is prepared according to the following steps:
[0098] (1) taking the single crystal silicon wafer obtained by the batch alkali polishing method in Example 1 for use;
[0099] (2) Annealing the alkali-polished silicon wafer to produce a silicon dioxide film layer on the surface of the silicon wafer; the annealing process time is 22 minutes, and the volume ratio of oxygen to nitrogen is 2000:500;
[0100] (3) The micro-conducting process is that trimethylaluminum and ozone react to form aluminum oxide on the back of the silicon wafer. The trimethylaluminum flow rate is 18 sccm, the ozone flow rate is 18 sccm, and the ozone concentration is 18.5wt%;
[0101] (4) Deposit a silicon nitride film on the back of the silicon wafer. The back film process time is 33 min, with 2 layers of film. The film thickness is controlled at 95±10nm and the refractive index is 2.13±0.12.
[0102] (5) Deposit a silicon nitride film on the front side of the silicon wafer. The positive film process time is 34 min, with 3 layers of film, the film thickness is controlled at 72±10nm, and the refractive index is 2.15±0.05;
[0103] (6) Laser grooving is performed on the back side of the coated silicon wafer. The laser back side grooving light power is 99%, the pulse frequency is 845kHz, the processing speed is 34 m / s, and the dust removal cabinet air pressure is 0.8 kPa;
[0104] (7) The temperature of the sintering and drying zone is 210℃~345℃, and the temperature settings of sintering zones 7 to 14 are 445℃, 450℃, 460℃, 520℃, 635℃, 800℃, 800℃, and 800℃ respectively.
[0105] (8) The process parameters of the electric injection at each station are current 9.5A, time 140s, CDA pressure 0.75mPa, and heat exhaust air 175Pa. Example
[0106] The preparation method of the PERC cell of this embodiment is basically the same as that of Example 4, except that the PERC cell of this embodiment is prepared from the monocrystalline silicon wafer obtained by the alkaline polishing method of Example 2. Example
[0107] The preparation method of the PERC cell of this embodiment is basically the same as that of Example 4, except that the PERC cell of this embodiment is prepared from the monocrystalline silicon wafer obtained by the alkaline polishing method of Example 3.
[0108] Comparative Example 1:
[0109] The alkali polishing method of the single crystal silicon wafer in this comparative example is basically the same as that in Example 1, except that in step (4) alkali polishing, the single crystal silicon wafer obtained in step (3) is immersed in an alkali polishing solution at 62°C for 200 s. The formula of the alkali polishing solution is as follows: the initial alkali polishing solution is prepared from 328 L of deionized water, 11.0 L of 45 wt% sodium hydroxide solution of Jianghua, and 3.0 L of alkali polishing additive Tuobang BP51; each batch of replenishing solution is prepared from 6.0 L of deionized water, 290 mL of 45 wt% sodium hydroxide solution of Jianghua, and 210 mL of alkali polishing additive Tuobang BP51.
[0110] Comparative Example 2:
[0111] The alkali polishing method for the single crystal silicon wafers in this comparative example is basically the same as that in comparative example 1, except that in this example, alkali polishing is performed on 15 batches of 400 single crystal silicon wafers in each batch according to steps (1) to (11).
[0112] Comparative Example 3:
[0113] The alkali polishing method for the single crystal silicon wafers in this comparative example is basically the same as that in comparative example 1, except that in this example, 600 batches of 400 single crystal silicon wafers are subjected to batch alkali polishing according to steps (1) to (11).
[0114] Comparative Example 4:
[0115] The preparation method of the PERC cell of this comparative example is basically the same as that of Example 4, except that the PERC cell of this example is prepared from the monocrystalline silicon wafer obtained by the alkaline polishing method of Comparative Example 1.
[0116] Comparative Example 5:
[0117] The preparation method of the PERC cell of this comparative example is basically the same as that of Example 4, except that the PERC cell of this example is prepared from the monocrystalline silicon wafer obtained by the alkaline polishing method of Comparative Example 2.
[0118] Comparative Example 6:
[0119] The preparation method of the PERC cell of this embodiment is basically the same as that of Example 4, except that the PERC cell of this embodiment is prepared from the monocrystalline silicon wafer obtained by the alkaline polishing method of Comparative Example 3.
[0120] See also Figure 1 and Figure 2 , Figure 1 This is a tower base diagram of the back polished surface of the single crystal silicon wafer obtained by the alkali polishing method in Example 1. Figure 2 The tower base diagram of the back polished surface of the single crystal silicon wafer obtained by the alkali polishing method in comparative example 1 was taken by Zeta 3D microscope. Figure 1 and Figure 2 It can be seen that the back polished surface of the single crystal silicon wafer prepared by the alkali polishing method in Example 1 has a high flatness, and the tower base size is 9 μm to 11 μm. The back polished surface of the single crystal silicon wafer prepared by the alkali polishing method in Comparative Example 1 has a high flatness, and the tower base size is 12 μm to 15 μm. The tower base size of the back polished surface of the single crystal silicon wafer prepared by the alkali polishing method of Example 1 is slightly reduced compared to the conventional process of Comparative Example 1.
[0121] The weight loss and fragmentation rate of the single crystal silicon wafers in the alkali polishing method of the single crystal silicon wafers of Examples 1 to 3 and Comparative Examples 1 to 3 are recorded in Table 1. The weight loss is the ratio of the mass difference before and after the alkali polishing of the silicon wafer to the mass of the silicon wafer before the alkali polishing.
[0122] Table 1 Weight loss and fragmentation rate of the single crystal silicon wafers in the alkali polishing method of the single crystal silicon wafers of Examples 1 to 3 and Comparative Examples 1 to 3.
[0123]
[0124] See also Figure 3 , are the weight loss and fragmentation rate results of the single crystal silicon wafers obtained by the batch alkali polishing method of Examples 1 to 3 and Comparative Examples 1 to 3. Figure 3It can be seen from the data in Table 1 that, relative to the traditional alkali polishing process of Comparative Examples 1 to 3, the alkali polishing method of Examples 1 to 3, by adjusting the formula of the alkali polishing liquid, reduces the weight loss of the single crystal silicon wafer in the alkali polishing process, and the weight loss is reduced from about 0.20 g / g to about 0.15 g / g. The fragmentation rate of Examples 1 to 3 is 0.27% to 0.28%, and the fragmentation rate of Comparative Examples 1 to 3 is 0.31% to 0.32%, indicating that the alkali polishing method of Examples 1 to 3 is beneficial to reducing the processing fragmentation rate of single crystal silicon wafers.
[0125] It can be seen from the weight loss data of Examples 1 to 3 that the weight loss of single crystal silicon wafers processed by the batch alkali polishing method described above is similar in weight to that of single crystal silicon wafers processed in different batches, ranging from 0.150 g / g to 0.158 g / g.
[0126] The consumption of alkali solution and alkali polishing additives in the alkali polishing method of the single crystal silicon wafer in Example 3 and Comparative Example 3 is recorded in Table 2.
[0127] Table 2 Consumption of alkali solution and alkali polishing additives in the alkali polishing method of the single crystal silicon wafer in Example 3 and Comparative Example 3.
[0128]
[0129] See also Figure 4 , which is a bar graph of the consumption of alkali solution and alkali polishing additives in the alkali polishing method of Example 3 of the present invention and Comparative Example 3. Figure 4 It can be seen from the data in Table 2 that, compared with the alkali polishing method of Comparative Example 3, the alkali polishing method of Example 3 reduces the amount of alkali solution and alkali polishing additives in each batch of replenishment, and can save 0.5 L of alkali solution and 0.25 L of alkali polishing additives per 10,000 single crystal silicon wafers, thereby reducing the amount of chemicals used and reducing processing costs.
[0130] The efficiency of the PERC cells prepared in Examples 4 to 6 and Comparative Examples 4 to 6 is recorded in Table 3. The test method for the efficiency of the PERC cell is as follows: the discharge of the host capacitor of the test system triggers the flashing of the xenon lamp, and the cell under test generates a photocurrent effect after being illuminated, and at the same time, the variable load collects 3000 to 5000 points of voltage and current data through load changes and draws an IV curve.
[0131] Table 3 Efficiency of PERC cells prepared in Examples 4 to 6 and Comparative Examples 4 to 6.
[0132]
[0133] See also Figure 5 , which is a bar graph of the PERC cell efficiency prepared in Examples 4 to 6 and Comparative Examples 4 to 6. Figure 5As can be seen from the data in Table 3, the PERC cell efficiencies of Examples 4 to 6 are close, ranging from 22.509% to 22.511%; the PERC cell efficiencies of Comparative Examples 4 to 6 are 22.483% to 22.502%. It can be seen that the PERC cell efficiencies of Examples 4 to 6 are increased by about 0.01% relative to the PERC cell efficiencies of Comparative Examples 4 to 6. It is generally believed that increasing the tower base size of the back polished surface of the monocrystalline silicon wafer is beneficial to improving the efficiency of the PERC cell. The tower base size of the back polished surface of the monocrystalline silicon wafer used in the PERC cell of Examples 4 to 6 is smaller than that of the monocrystalline silicon wafer used in Comparative Examples 4 to 6, and the PERC cell efficiency is improved. This shows that the alkali polishing method of the monocrystalline silicon wafer of the present invention can not only reduce the weight loss of the monocrystalline silicon wafer during alkali polishing, reduce the loss of raw materials, but also improve the efficiency of the downstream PERC cell.
[0134] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0135] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in detail, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the protection scope of the attached claims described in the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the contents of the attached claims, and the description and drawings can be used to interpret the contents of the claims.
Claims
1. A method for alkali polishing of a silicon wafer, characterized in that: The alkali polishing method comprises a plurality of batches of alkali polishing treatments performed sequentially, and each batch of alkali polishing treatments comprises the following steps: Pre-cleaning: cleaning the silicon wafer in a first mixed solution, wherein the first mixed solution includes an alkaline reagent and H2O2; Alkali polishing: the silicon wafer after pre-cleaning is subjected to alkaline polishing in an alkaline polishing solution; Post-cleaning: cleaning the silicon wafer after alkali polishing in a second mixed solution, wherein the second mixed solution includes an alkaline reagent and H2O2; Pickling: soaking the silicon wafer after post-cleaning in an acid solution to remove the oxide layer; Slow pulling: washing the pickled silicon wafer in water and slowly pulling it out; and dry; The alkali polishing liquid in the first batch of alkali polishing treatment is an initial alkali polishing liquid, and the components of the initial alkali polishing liquid include: water, alkali solution and alkali polishing additive in a volume ratio of (320-340): (9.5-12.5): (2.5-3.5); The alkali polishing solution of the nth batch of alkali polishing treatment is prepared by adding a replenishing solution to the alkali polishing solution of the n-1th batch; the components of the replenishing solution include: (5.5-6.5): (0.24-0.28): (0.17-0.20) of water, alkali solution and alkali polishing additive; the volume ratio of the replenishing solution of the nth batch to the initial alkali polishing solution is (5.91-6.98): (332-356); wherein 2≤n≤60; The alkali solution is selected from an aqueous solution of at least one of sodium hydroxide and potassium hydroxide, and the concentration of the alkali solution is 45wt% to 48wt%.
2. The alkali polishing method for silicon wafer according to claim 1, characterized in that: In the initial alkali polishing solution, the volume ratio of the water, the alkali solution and the alkali polishing additive is (327-329): (10.5-11.5): (2.8-3.2).
3. The alkali polishing method for silicon wafer according to claim 1, characterized in that: In the replenishing solution, the volume ratio of the water, the alkali solution and the alkali polishing additive is (5.9-6.1): (0.265-0.275): (0.19-0.20).
4. The alkali polishing method for silicon wafers according to any one of claims 1 to 3, characterized in that: The temperature of the alkali polishing step is 60° C. to 66° C., and the time is 140s to 160s.
5. The alkali polishing method for silicon wafer according to claim 4, characterized in that: The temperature of the alkali polishing step is 64° C. to 66° C., and the time is 145 s to 155 s.
6. The alkali polishing method for silicon wafers according to any one of claims 1 to 3 and 5, characterized in that: The alkali polishing additive is selected from BP51.
7. The alkali polishing method for silicon wafers according to any one of claims 1 to 3 and 5, characterized in that: The temperature of the pre-cleaning step is 45° C. to 60° C., and the time is 40s to 50s.
8. The alkali polishing method for silicon wafers according to any one of claims 1 to 3 and 5, characterized in that: The temperature of the post-cleaning step is 25° C. to 40° C., and the time is 120 s to 180 s.
9. A method for preparing a PERC battery, characterized in that: The method comprises the steps of texturing, diffusion, SE, thermal oxidation, alkali polishing, annealing, micro-conduction and coating on a silicon wafer in sequence; the alkali polishing step is carried out by the alkali polishing method for a silicon wafer according to any one of claims 1 to 8.
10. A PERC cell manufactured according to the method for manufacturing a PERC cell according to claim 9.
Citation Information
Cited By
A method for electrochemical mechanical polishing of semiconductor silicon wafer
CN119121368B