Systems and methods for making carbon nanostructures

Through the electrochemical synthesis method of the molten carbonate method, carbon dioxide is used as a reactant, which solves the high energy consumption and high emission problems of the synthesis of spiral carbon nanostructures in the existing technology, and achieves low carbon footprint and low-cost spiral carbon nanostructures. production, providing a variety of high-performance applications.

CN114630926BActive Publication Date: 2024-10-25C2CNT LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080073487.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-29
Filing Date
2020-10-29
Publication Date
2024-10-25
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

The existing technology is energy intensive and costly when synthesizing spiral carbon nanostructures, and results in a large amount of carbon dioxide emissions, making it impossible to effectively utilize carbon dioxide as a reactant.

Method used

The molten carbonate method is used for electrochemical synthesis, using carbon dioxide as a reactant. By limiting the space between electrodes, applying high electrolysis current density, heating the space between electrodes, adding electrolyte additives and transition metal nucleating agents, the electrolysis reaction conditions are controlled to Synthesis of spiral carbon nanostructures.

Benefits of technology

It achieves low carbon footprint and low-cost production of spiral carbon nanostructures, consumes carbon dioxide in the atmosphere or flue, and provides various forms of spiral carbon nanostructures with high performance and multiple application potentials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114630926B_ABST
    Figure CN114630926B_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure relate to methods and systems for providing electrolytic reactions in molten carbonate electrolytes to synthesize spiral carbon nanostructures (HCNS). Electrolyte, electrode composition, current density, temperature and additives can all play an important role in the formation of HCNS. According to embodiments of the present disclosure, by controlling these parameters, various specific, uniform high-yield HCNS can be synthesized by molten carbonate electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 927,389, filed on October 29, 2019, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to making carbon nanostructures. In particular, the present disclosure relates to systems and methods for making helical carbon nanostructures using a molten carbonate process. Background Art

[0004] Carbon nanotubes (CNTs) consist of cylindrical walls of rolled graphene sheets. An occasionally reported and unusual variation of this morphology is called coiled or helical carbon nanotubes (HCNTs). Figure 1 Examples of such unusual HCNT allotropes are shown in (Zhang, M. and Li, J. Carbon nanotube in different shapes. Materials Today, 2009. 12(6), 12-18).

[0005] HCNTs were first predicted to exist in 1993 and then first discovered in 1994. The few reported examples of HCNT synthesis to date have been accomplished by chemical vapor deposition (CVD) of organic or organometallic precursors using metal catalysis. CVD is an energy-intensive and costly process that emits a large carbon footprint of up to 600 tons of carbon dioxide (CO2) for every ton of carbon nanomaterial produced. CO2 emissions are a growing global problem that we all face, as anthropogenic CO2 emissions are responsible for the increase in atmospheric CO2 concentrations and the resulting climate change. Summary of the invention

[0006] Embodiments of the present disclosure are directed to providing systems and methods for electrochemically synthesizing helical carbon nanostructures (HCNS), wherein the reactant for producing HCNS is carbon dioxide (CO2). In some embodiments of the present disclosure, the systems and methods have a negative carbon footprint.

[0007] Some embodiments of the present disclosure relate to a method for synthesizing helical carbon nanostructures (HCNS). The method comprises the steps of aligning an anode spaced apart from a cathode to define an inter-electrode space; introducing a molten carbonate electrolyte into the inter-electrode space; introducing a carbon input into the inter-electrode space; applying an electric current across the electrodes; and collecting a product comprising HCNS from the electrodes.

[0008] In some embodiments of the present disclosure, the method further comprises the step of applying at least two of the following parameters: applying an electric current having a high electrolysis current density; heating the inter-electrode space to at least 725° C.; adding an electrolyte additive to the inter-electrode space; adding iron oxide to the inter-electrode space.

[0009] Some embodiments of the present disclosure relate to a system for making a spiral carbon nanostructure. The system includes an anode and a cathode that together define an inter-electrode space. The system further includes a method for applying at least 0.2A / cm across the electrodes. 2 a current source for a current density, a heat source for conditioning the inter-electrode space at a temperature of at least about 725°C, and a carbon source for introducing carbon into the inter-electrode space.

[0010] Some embodiments of the present disclosure relate to HCNS, such as but not limited to: helical carbon nanotubes (HCNTs), helical carbon nanofibers (HCNFs), double-stranded HCNTs, braided HCNTs, helical nanosheets (HCNPs), sp3-defective CNTs, deformed CNTs, bent CNTs, curved CNTs, or combinations thereof.

[0011] In contrast to straight carbon nanotube (CNT) growth, the growth of HCNTs has been proposed to occur via two independent but non-exclusive mechanisms. A model that combines local stresses and anisotropic rates of carbon deposition on the catalyst particles has been widely accepted. The first mechanistic pathway for HCNT growth is heterogeneous growth leading to pentagonal and heptagonal defects, which result in bending. This can be due to the catalyst or substrate having different faces or using catalysts composed of different metals and thus promoting different growth rates. An example of such a heterogeneous metal catalyst is the tin and iron (Sn / Fe) catalyst or the indium and iron (In / Fe) catalyst, which promotes HCNT growth by chemical vapor deposition (CVD). For example, tin accelerates CNT growth, but iron appears to grow at a slower rate, resulting in defective CNTs during CVD growth. Our molten carbonate growth method has a complex mixture of metals from the electrodes that can cause this feature to appear.

[0012] The second proposed mechanistic pathway for HCNT growth is that strain or fast growth rates lead to coiling. For example, if CNTs grow faster on a catalyst, they can organize themselves in a straight fashion, coiling like yarn, coming out of the holes too fast to be laid straight down on a mat during chemical vapor deposition (CVD) growth. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] These and other features of the present disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings.

[0014] Figure 1 An image of a helical carbon nanotube (HCNT) is provided.

[0015] Figure 2 Transmission electron microscope (TEM) images of carbon nanotubes (CNTs) synthesized in molten carbonate are provided, wherein Figure (a) shows the CNTs after 15 minutes of synthesis; Figure (b) shows the CNTs after 30 minutes of synthesis; Figure (c) shows the CNTs after 90 minutes of synthesis; and Figure (d) shows a closer image of the CNTs shown in Figure (c).

[0016] Figure 3 is a schematic diagram showing an overview of the molten carbonate process for making various carbon nanostructures including HCNTs and helical carbon nanofibers (HCNFs).

[0017] Figure 4 An image of HCNS synthesized according to an embodiment of the present disclosure is shown, wherein: Figure 4 A shows a scanning electron microscope (SEM) image of HCNS, with a scale of 100 μm; Figure 4 B shows a TEM image of HCNS synthesized according to an embodiment of the present disclosure, wherein the scale bars of (i) and (ii) are 500 nm, the scale bar of (iii) is 100 nm, the scale bar of (iv) is 20 nm, and the scale bars of (v) and (vi) are 500 nm.

[0018] Figure 5 shows SEM images of CNTs synthesized by molten carbonate electrolysis in the presence or absence of iron oxide in molten carbonate, where Figure 5 A shows CNTs synthesized without using iron oxide and with a size of 50 μm; Figure 5 B shows CNTs synthesized without the use of iron oxide and the scale bar is 10 μm; Figure 5 C shows CNTs synthesized using 0.1% iron oxide and the scale bar is 100 microns; and, Figure 5 D shows CNTs synthesized using 0.1% iron oxide and the scale bar is 10 μm.

[0019] Figure 6 shows an SEM image of a mixture of HCNS and CNTs synthesized by molten carbonate electrolysis in the presence of iron oxide in molten carbonate, wherein Figure 6 A shows a photograph of the cooled and extracted product before removal from the cathode; Figure 6 B shows a mixture of HCNS and CNTs at a scale of 30 microns; and, Figure 6 C shows a 10 μm scale bar Figure 6 The same mixture of B.

[0020] Figure 7 A low magnification TEM image of HCNS synthesized according to an embodiment of the present disclosure is shown, wherein Figure 7 The scale bar in A is 200 nm; Figure 7 The scale bar in B is 100 nm; Figure 7 The scale bar of C is 200 nm; and, Figure 7 D scale bar is 200 nm.

[0021] Figure 8 A high-magnification TEM image of HCNS synthesized according to an embodiment of the present disclosure is shown, wherein Figure 8 A shows the Figure 7 A is the same image (with the target region identified by A) and the distance between the layers of HCNS; Figure 8 B shows the target area A with a scale bar of 1 nm; Figure 8 C shows the Figure 7 D. The same image with the target region identified by B. Figure 8 D shows a scale bar of 20 nm. Figure 8 Target area B in C; Figure 8 E shows another portion of HCNS synthesized according to an embodiment of the present disclosure, with a scale bar of 50 nm and a target region identified by F; Figure 8 F shows the scale bar of 20 nm Figure 8 target area F in E, and other target areas C1, C2, and C3; Figure 8 G is shown with a scale bar of 1 nm Figure 8 Target area C1 in E; Figure 8 H is shown with a scale bar of 1 nm Figure 8 The target area C2 in E and the distance between the HCNS layers therein measured at the black transverse line; Figure 8 I is shown with a scale bar of 1 nm Figure 8 The target area C3 in E and the distance between the HCNS layers measured at the black transverse line; Figure 8 J shows another portion of HCNS synthesized according to an embodiment of the present disclosure, with two target regions labeled D1 and D2; Figure 8 K is shown with a scale bar of 20 nm Figure 8 Target area D1 in J; Figure 8 L is shown with a scale bar of 20 nm Figure 8 target region D2 in J and a further target region denoted as d2; Figure 8 M shows Figure 8 The target region d2 in L and the distance between HCNS layers therein measured at the black transverse line; Figure 8N shows another portion of HCNS synthesized according to an embodiment of the present disclosure, with three target regions labeled E1, E2, and E3 and a scale bar of 50 nm; Figure 8 O is shown with a scale bar of 1 nm Figure 8 Target area E1 in N; Figure 8 P is shown with a scale bar of 1 nm Figure 8 Target area E2 in N; Figure 8 Q is shown with a scale of 1 nm Figure 8 Target region E3 in N and the distance between HCNS layers therein measured at the black transverse lines.

[0022] Fig. 9 Shows Figure 6 TEM image of a small portion of the mixture shown in Fig. 9 A shows a portion of HCNS and CNT with a scale bar of 500 nm; Fig. 9 B shows a portion of a single CNT with a scale bar of 100 nm; Fig. 9 C shows a portion of HCNS and CNT with a scale bar of 50 nm; Fig. 9 D shows another part of the CNT with a scale bar of 20 nm and two target areas marked with B1 and B2; Fig. 9 E is shown with a scale bar of 1 nm Fig. 9 D shows the target area B1 and the distance between CNT layers therein measured at the black horizontal line; Fig. 9 F is shown with a scale bar of 1 nm Fig. 9 D shows the target area B2 and the distance between CNT layers therein measured at the black transverse line; Fig. 9 G shows another part of the CNT with a scale bar of 20 nm and two target regions marked with C1 and C2; Fig. 9 H is shown with a scale bar of 1 nm Fig. 9 G shows the target area C1 and the distance between CNT layers therein measured at the black transverse lines; and Fig. 9 I is shown with a scale bar of 1 nm Fig. 9 G shows the target area C2 and the distance between CNT layers therein measured at the black transverse lines.

[0023] Fig.10 Shows Figure 6 Electron dispersive spectroscopy (EDS) results for a small portion of the mixture shown in Fig.10 A shows the EDS results inside the CNT wall; and, Fig.10 B shows the EDS results inside the CNT.

[0024] Fig.11A SEM image of HCNS synthesized according to an embodiment of the present disclosure is shown, wherein Fig.11 A shows HCNS with a 30 μm scale bar and a magnified inset with a 3 μm scale bar; Fig.11 B shows HCNS with a scale bar of 10 μm; Fig.11 C shows HCNS at a scale bar of 8 μm; and, Fig.11 D shows HCNS with a scale bar of 5 μm.

[0025] Fig.12 A SEM image of HCNS synthesized according to an embodiment of the present disclosure is shown, wherein Fig.12 A shows HCNS with a scale bar of 20 μm; Fig.12 B shows HCNS with a scale bar of 10 μm; Fig.12 C shows HCNS with a scale bar of 20 nm and the target region marked by the dashed rectangle and Fig.12 The distance between HCNS layers measured at the white horizontal line in D; Fig.12 D shows Fig.12 The target area in C; Fig.12 E shows another part of HCNS with a scale bar of 500 nm; and, Fig.12 F shows the scale bar of 20 nm Fig.12 Part of HCNS in E.

[0026] Fig.13 A SEM image of HCNS synthesized according to an embodiment of the present disclosure is shown, wherein Fig.13 A shows HCNS with a scale bar of 20 μm; Fig.13 B shows HCNS with a scale bar of 10 μm; Fig.13 C shows a portion of HCNS with a scale bar of 100 nm and the target area marked by a dashed rectangle; Fig.13 D is shown with a scale bar of 1 nm Fig.13 The target area in E and the distance between CNT layers therein measured at the white horizontal line; Fig.13 F shows a portion of HCNS with a scale bar of 20 nm and the target area marked by the dashed rectangle; and, Fig.13 G is shown with a scale bar of 1 nm Fig.13 The target area in F and the distance between CNT layers therein measured at the black transverse lines.

[0027] Fig.14 Figure A shows a TEM image and Figure B shows a DSEM image of a curved carbon nanoform synthesized according to an embodiment of the present disclosure, wherein Fig.14 A shows a bent carbon nanotube at a scale of 500 μm; Fig.14 B shows a curved carbon nanomaterial including a spiral morphology at a scale of 10 μm, wherein inset (i) is shown at a scale of 1 μm and inset (ii) is shown at a scale of 3 μm; Fig.14 C shows the curved carbon nanomaterial at a scale of 20 microns; and, Fig.14 D shows a curved carbon nanomaterial including a spiral morphology at a scale of 10 microns, and inset (i) is shown at a scale of 30 microns and inset (ii) is also shown at a scale of 30 microns. DETAILED DESCRIPTION

[0028] It is well known that molten carbonates have an affinity for absorbing CO2 from atmospheric and flue gas levels. For example, 13C isotopes have been used in CO2 to track and demonstrate that CO2 originating from the gas phase acts as a renewable carbon building block in the observed CNT products in an electrochemical process using molten lithium carbonate. The net reaction of this electrochemical process is as follows:

[0029] Dissolution: CO2 (gas) + Li2O (soluble) → Li2CO3 (molten) (1)

[0030] Electrolysis: Li2CO3(molten)→C(CNT)+Li2O(soluble)+O2 (2)

[0031] (gas)

[0032] Net: CO2(gas)→C(CNT)+O2(gas) (3)

[0033] An important component of the electrochemical process includes transition metal nucleation growth, such as the addition of nickel powder, which leads to Figure 2 Shown is a clearly observable non-helical carbon nanotube (CNT) wall. Figure 2 Included are transmission electron microscopy (TEM) images of CNT walls synthesized from CNTs synthesized in molten carbonate. Figure 2 The CNTs shown were synthesized by 2 This is achieved by electrolysis of a coiled copper wire with nickel powder in lithium carbonate (molten Li2CO3) at 770°C. Figure 2 Figure d shows a magnified view of the CNT product after 90 minutes of electrochemical synthesis reaction. The synthesis produced pure CNT products whose diameter increased with the increase of electrolysis time. TEM of CNT products synthesized after 15 minutes (Figure a), 30 minutes (Figure b) or 90 minutes (Figure c) of electrolysis reaction. For adjacent graphene layers, the graphene spacing between CNT walls is about 0.34 nanometers (nm). However, when the nucleation additive (nickel powder) is excluded during the synthesis process, the result is a high-yield synthesis of carbon nano onions (CNO) and carbon flakes.

[0034] Figure 3 A high-yield electrolytic synthesis route for carbon nanomaterials in molten carbonates is shown, which consumes CO2 directly as a reactant, either from air or from smoke / flue CO2.

[0035] Under appropriate electrochemical conditions, electrolysis reactions in molten carbonates convert CO2 from the atmosphere or flue gas into specific carbon nanomaterial products with high yields.

[0036] By varying the conditions of the electrolysis reaction, such as the materials used to form the electrodes and electrolyte additives, the electrolysis reaction can produce a variety of carbon nanostructure morphologies, including large diameter (between about 500 nm and about 1 μm), long (about 1 mm), wool-like CNTs; straight, medium diameter (about 175 nm), medium length (about 100 μm) CNTs; tangled, smaller diameter (about 125 nm) CNTs, short (about 50 μm) CNTs; much shorter (about 10 μm) CNTs and smaller diameter (about 50 nm) CNTs; thinner-walled, smaller diameter (about 50 μm) CNTs, or combinations thereof.

[0037] For example, different electrode materials can produce different CNT products ( Figure 3 ). Nickel-containing alloys are often used as anode materials in electrolytic processes for at least two reasons:

[0038] 1) The nickel in the electrode dissolved in the electrolyte acts as a good nucleation site, and

[0039] 2) Under oxidation, nickel forms a stable nickel oxide layer on the anode, which acts as an effective electrocatalyst to generate oxygen at the anode (see reaction (2) above).

[0040] Therefore, anodes made of various nickel-containing alloys have been studied. It is known that Nichrome (nickel-chromium-based alloys) (including stainless steels such as SS 304 or SS 316) and Inconel (such as Inconel 600, 625 and 718) or nickel-chromium alloys such as Chromel A, B or, as alloy components, co-nucleation can produce high-quality CNTs. Binary and ternary transition metal nucleating agents, including but not limited to Ni, Cr, Sn, In, Fe and Mo, can also affect CNT growth.

[0041] The cathode material composition also affects the electrolytic reaction for synthesizing CNTs, CNO and graphene. Examples of materials for making suitable cathodes include, but are not limited to: galvanized steel (which utilizes Fe, Zn and Ni from the anode to form nucleation sites); copper, monel and brass (which utilizes co-nucleation of Ni, Cu, Zn and trace Fe) or combinations thereof.

[0042] However, what has not been clearly demonstrated is how to manipulate the conditions of the electrolysis reaction to synthesize helical carbon nanostructures (HCNS) of various morphologies using CO 2 as a reactant and molten carbonate as an electrolyte.

[0043] Embodiments of the present disclosure relate to an efficient system and method for removing CO2 directly from the atmosphere or chemical / energy plants and converting the removed CO2 into useful products. In particular, embodiments of the present disclosure relate to synthesizing various forms of HCNS from CO2 or other carbon sources.

[0044] As a general category of carbon nanostructures, HCNS may include: helical carbon nanotubes (HCNTs), helical carbon nanofibers (HCNFs), double-stranded HCNTs, braided HCNTs, helical nanosheets (HCNPs), sp3-defective CNTs, deformed CNTs, bent CNTs, curved CNTs or combinations thereof. For clarity, the term HCNS includes regular repeating helical morphologies (both symmetrical and asymmetrical morphologies) and defective or deformed CNTs that do not have regular repeating helical morphologies but include bends, curves or other morphologies that distinguish them from non-defective or deformed CNTs.

[0045] HCNTs can have many uses, including but not limited to: high performance electromagnetic wave absorbers, sensors, resonators, nano-scale mechanical springs, electronic inductors, and magnetic beam generators as well as various medical applications.

[0046] HCNTs exhibit properties associated with high magnetization. For example, if an electric current is applied to the HCNT, the bends in the HCNT generate a magnetic field, acting much like a solenoid. When a high-frequency magnetic field is applied to the HCNT, the HCNT generates an electric current. These properties lead to a strong interaction with electromagnetic waves.

[0047] Furthermore, if HCNTs are compressed, the curves experience different strains and have different electronic properties in different regions, resulting in a strong piezoelectric effect, in which mechanical force can be converted into electricity and electric current can be converted into mechanical force, such as compression force or vibration. These properties of HCNTs can provide mechanically tunable electronic properties. Overall, all these properties may make HCNTs an ideal candidate for nanoelectronics, nanomechanical systems, and nanosensors. HCNTs can also be used as superconductors.

[0048] HCNT is also known to enhance early immune responses during Pseudomonas aeruginosa bacterial infection, affecting phagocytosis.

[0049] Embodiments of the present disclosure relate to electrochemical conditions that result in the conversion of CO2 into HCNS (including HCNTs, HCNFs (helical carbon nanofibers), HCNPs (helical carbon flakes), defective CNTs, bent CNTs, nearly or fully filled carbon nanotubes containing carbon nanofibers, or combinations thereof).

[0050] Some embodiments of the present disclosure relate to a system for providing an electrolytic reaction for synthesizing HCNS. The system includes a pair of electrodes, a cathode and an anode defining an inter-electrode space, which inter-electrode space may also be referred to as an electrolysis space, which may receive and accommodate an electrolyte. The system also includes a current source, a carbon input source, and a heat source.

[0051] In some embodiments of the present disclosure, the cathode is formed as a planar structure, a wire structure, a mesh, a porous structure, a conductive plate, a planar or folded gasket, a coiled structure, or the cathode can form at least a portion of the inside of the housing. The cathode can be formed of a variety of conductive materials that reflect the need for variations in nucleation sites and carbon products formed on the cathode. Such cathode forming materials include, but are not limited to, any conductive material, galvanized (zinc-coated) steel, titanium, graphite, iron, alloys containing copper and zinc, Monel (Ni 400, a Ni / Cu alloy), Inconel, nickel-chromium alloys, pure copper and brass alloys may also be suitable. It has been observed that each cathode material has an effect on linear (non-coiled) CNT products. For example, copper cathodes produce very small diameter tubes, steel cathodes produce very entangled CNTs, and Muntz brass (60% copper, 40% zinc alloy) cathodes produce high purity CNTs.

[0052] In some embodiments of the present disclosure, the anode is formed as a planar structure, a wire structure, a screen, a porous structure, a conductive plate, a plane or folded gasket, a coiled structure, or the anode can form at least a portion of the inner side of the shell. The anode can be formed of various conductive materials so that the anode can produce or not produce oxygen. Such anode forming materials include, but are not limited to: any conductive material, Ni, Ni alloy, galvanized (zinc-coated) steel, titanium, graphite, iron, and various metals that establish a highly stable oxide outer layer that is conducive to oxygen production during the electrolysis reaction performed according to the present disclosure. Examples of suitable materials for forming the anode include nickel-chromium alloys (nickel-chromium-based alloys), including stainless steel such as SS 304 or SS 316, and Inconel alloys such as Inconel 600, 625 and 718, alloy C-264, or nickel-chromium alloys such as Chromel A, B or as co-nucleation of alloy components is known to produce high-quality CNTs. Binary and ternary transition metal nucleators, including but not limited to: Ni, Cr, Sn, In, Fe, and Mo, can also affect carbon product growth.

[0053] In some embodiments of the present disclosure, a transition metal such as nickel can be added to the anode, which can be dissolved from the anode to migrate to the cathode through the electrolyte. The added transition metal can be used as a nucleating agent, which can be selected from nickel, iron, cobalt, copper, titanium, chromium, manganese, zirconium, molybdenum, silver, cadmium, tin, ruthenium or a mixture thereof. The transition metal can also be directly introduced into the electrolyte as a dissolved transition metal salt to migrate to the cathode. The transition metal nucleating agent can also be directly added to the cathode.

[0054] The cathode and anode can be aligned substantially parallel to each other in a housing, such as a stainless steel housing or a housing made of substantially pure or pure alumina. The housing can be made of any material suitable for accommodating molten carbonate and maintaining the temperature reached by the system. The electrodes can be oriented in any direction, including but not limited to substantially horizontal or substantially vertical, but spaced apart from each other so as to define an inter-electrode space between them. In some embodiments of the present disclosure, the inter-electrode space is about 0.1 cm to about 10 cm. In some embodiments of the present disclosure, the inter-electrode space is about 1 cm. As will be appreciated by those skilled in the art, the size of the inter-electrode space will depend on the scale of the system, such as the size of each electrode, the gas collecting chamber defined in the housing, the amount of current applied, and a combination thereof.

[0055] The current source may provide at least about 0.1 A / cm 2 Any source of alternating or direct current with a current density, which may be constant or non-constant. In some embodiments of the present disclosure, the current density provided between the electrodes is at least 0.2 A / cm 2 , 0.3A / cm 2 , 0.4A / cm 2 , 0.5A / cm 2 , 0.6A / cm 2 , 0.7A / cm 2 , 0.8A / cm 2 , 0.9A / cm 2 , 1.0A / cm 2 The power source for the current source can be any power source or a combination of multiple power sources, including electric power source, solar energy, etc.

[0056] The heat source may be any heat source that raises the temperature within the space within the housing to a temperature of at least about 725° C. In some embodiments of the present disclosure, the temperature within the housing may be raised to about 750° C. to about 800° C. or higher. In some embodiments of the present disclosure, the heat source is provided or supplemented by the exothermic reaction of carbon dioxide absorption and conversion to carbonate or the overpotential of the applied electrolysis current.

[0057] The carbon input source can be any carbon source including CO2. For example, ambient air can provide a CO2 source. Exhaust gases from various factories or chemical reactors may provide a CO2 source. For example, power plants, steam generation facilities or pyrolysis reactors can emit CO2. CO2 emitted from these types of systems or in the production of high carbon footprint materials can also be used as a CO2 source. In addition, CO2 products produced by the combustion or conversion of fossil fuels for heating and transportation, as well as carbon products such as polymers and plastics, can also be CO2 sources. The housing is configured to receive a carbon input, such as CO2, in the inter-electrode space.

[0058] In some embodiments of the present disclosure, the electrolyte may include a carbonate that can be heated by a heat source until it is converted into a molten phase. Conveniently, compared to carbon nanomaterials produced by other conventional techniques such as chemical vapor deposition (CVD) synthesis, flame synthesis or plasma synthesis, carbon nanomaterials produced by electrolysis from molten carbonates can be produced with a relatively low carbon footprint or even a negative carbon footprint because CO2 is consumed as a reactant and the cost is relatively low. For example, the carbonate can be lithium carbonate or a lithiated carbonate. Molten carbonates, such as lithium carbonate Li2CO3 with a melting point of 723°C, or lower melting point carbonates such as LiBaCaCO3 with a melting point of 620°C, when containing oxides produced by electrolysis, such as, but not limited to, the oxides illustrated in Equation 2, or when mixed with highly soluble oxides such as Li2O and BaO, maintain rapid absorption of CO2 from atmospheric or exhaust CO2. Suitable carbonates may include alkali metal carbonates and alkaline earth carbonates. The alkali carbonate may include carbonates of lithium, sodium, potassium, rubidium, cesium or francium, or mixtures thereof. The alkaline earth carbonate may include carbonates of beryllium, magnesium, calcium, strontium, barium or radium, or mixtures thereof. In some embodiments of the present disclosure, the electrolyte may be a mixed composition, such as a mixture of alkali and alkaline earth carbonates with one or more of oxides, borates, sulfates, nitrates, chlorides, chlorates or phosphates. Without being bound by any particular theory, mixed electrolytes may also induce HCNS growth for at least the following reasons: (i) complex mixtures may cause CNTs to extend more slowly than they are extruded from the catalyst, thereby improving spiral growth; (ii) more complex electrolyte mixtures may introduce anisotropic growth conditions by directly causing different growth rates or indirectly affecting the catalyst morphology or species present in the solution; (iii) more complex electrolyte mixtures may reduce the "correction" of pentagonal or heptagonal defects, or may even increase them, thereby producing repeated bending or defects that cause such bending; or (iv) combinations thereof. Eutectic mixtures of different carbonates can also provide different temperature states because of their lower melting points.

[0059] In some embodiments of the present disclosure, one or more additives can be supplemented to the molten carbonate electrolyte by adding one or more additives in the inter-electrode space, for example, by adding directly to the molten electrolyte, in a non-molten electrolyte precursor, or in a combination thereof. Metal oxide electrolyte additives can be used as sp3 defect inducers, increasing sp3 compared to sp2 bonds, and these defects can be compatible with the increased distortion observed in various HCNS forms. Some non-limiting examples of metal oxides used as sp3 defect inducers include lithium oxide, iron oxide, barium oxide, nickel oxide, cobalt oxide, and chromium oxide. Additive oxides can also increase CO2 absorption and can reduce electrolysis voltage requirements. Other electrolyte additives can include borates, sulfates, nitrates, and phosphates.

[0060] Transition metal nucleating agents can also affect the growth of helical carbon nanotubes by molten carbonate electrosynthesis. Ni is a known CNT nucleating agent, and nickel-containing metals such as nichrome and Inconel can provide a highly stable anode as well as a nickel source for nucleation during molten carbonate.

[0061] In some embodiments of the present disclosure, the electrolyte additives and transition metal nucleating agents may be placed in the inter-electrode space as separate components added to the inter-electrode space, added to the non-molten electrolyte precursor, or they may be placed in the inter-electrode space as part of one or more of the electrodes.

[0062] Example

[0063] Example 1 - General Procedure

[0064] Lithium carbonate (Li2CO3, 99.5%) and lithium oxide (Li2O, 99.5%) were combined or not with various additives and heated to form different molten electrolytes.

[0065] As further described below, the electrolytic reaction is driven at a constant current density. The electrolytic reaction is contained in a pure alumina or pure stainless steel 304 housing. Inconel, nickel-chromium alloy or stainless steel is used to form the oxygen-producing anode. Monsole brass or monel alloy is used to form the cathode.

[0066] During the electrolysis reaction (the details of which will be further described below), the synthesized carbon product accumulates on the cathode, which is then removed and cooled. After the electrolysis reaction, the carbon product remains on the cathode, but the carbon product falls off or flakes off when the cathode is removed from the stainless steel 304 housing, cooled, knocked or scraped.

[0067] The carbon product is then washed with deionized water (DI water) or in up to 6 mol of hydrochloric acid (HCl). Both washes produce similar products, but the acid solution speeds up the washing. The washed carbon product is then separated from the washing solution by paper filtration or centrifugation. Both separation techniques produce similar carbon products, but centrifugation speeds up the separation.

[0068] The washed and separated carbon product was then analyzed by PHENOM Pro Pro-X SEM, by FEI Teneo Talos F200X TEM and by scanning electron microscopy (SEM, PHENOM Pro-X SEM with EDS) using electron dispersive spectroscopy (EDS).

[0069] Example 2 - HCNS Synthesis

[0070] According to embodiments of the present disclosure, an unusual carbon product can be formed when the electrolysis reaction is carried out at high current density. For these electrolysis reactions, the cathode is 5 cm 2 Monel wire, located at 0.5cm 2 About 0.5 cm below the coiled Ni wire anode. In an alumina crucible, use about 0.4 A / cm in 770 °C Li2CO3 2 The current density (compared to about 0.05 A / cm when forming non-helical CNTs by known electrolytic reaction methods) 2 To about 0.3A / cm 2 ) for about 2.5 hours to synthesize the synthesized carbon product. Figure 4 A scanning electron microscope (SEM) of this unusual product is shown in . Figure 4 A shows the SEM image and Figure 4 Panel B shows a TEM image of this carbon product. The SEM image of the carbon product shows a mixture of conventional entangled CNTs and HCNTs.

[0071] Example 3 - CNT Synthesis

[0072] Figure 5 The SEM images of the clean and separated carbon products synthesized by electrolysis reaction according to the embodiments of the present disclosure are shown. In particular, the plane 27 cm 2 Montessori brass cathode with 27cm 2 The Nichrome C flat anodes were spaced about 1 cm apart vertically. These electrodes were charged at about 0.6 A / cm in a 750°C molten Li2CO2 electrolyte containing about 2 wt% dissolved Li2O. 2 The electrolysis reaction was run for about 30 minutes using CO2 as a reactant. Based on the product mass, the electrolysis occurred with a Coulombic efficiency of greater than 90% (4 e-conversion). Figure 5 C and Figure 5 The electrolysis reaction product shown in D contains an additional 0.1 wt% Fe2O3 in the molten electrolyte. As shown, the product is highly uniform and straight; based on the product mass, the product is formed with a Coulombic efficiency of over 98%. The purity of the carbon nanotube product is 97% and the length of the CNT is about 150 μm. Similar syntheses, in which the 2 wt% Li2O additive is replaced with 10 wt% dehydrated borax, and in which the Monel brass cathode is replaced with a monel alloy cathode, or in which Inconel 718 or SS 304 or C-264 is used to replace the NiCr anode, produce similar results.

[0073] Not bound by any particular theory, Figure 4 and Figure 5 The advantages of HCNS shown in can be produced by electrolytic splitting of molten carbon under growth conditions that: (1) maximize torsional stresses, such as those that may occur during rapid nucleation growth; (2) enhance defects that lead to the formation of heptagons, rather than the conventional pentagonal building blocks of graphene cylinder walls; (3) uniformly control those enhanced defects to repeatedly induce uniform helical conformations; and (4) employ a combination of (1), (2), and (3).

[0074] Example 4 - Further HCNS Synthesis

[0075] Surprisingly, it was found that HNCS synthesis can be achieved by applying at least two of the following four experimental parameters: (i) high electrolytic current density growth, e.g., about 0.35 A / cm 2 or higher; (ii) high temperature electrolysis temperature, such as 770°C or higher; (iii) use of sp3 defect inducing agents, such as added oxides; or (iv) addition of controlled concentrations of iron to the electrolyte or cathode surface. As will be appreciated by those skilled in the art, three or more of these experimental parameters are also considered.

[0076] Iron is an unusual transition metal carbon nanomaterial growth nucleating agent with very high oxide solubility in lithiated molten carbonates. For example, it is known that up to 50 wt% of iron can be dissolved in molten lithium carbonate. In embodiments of the present disclosure, it is surprisingly found that controlled concentrations of added Fe2O3 with added oxides such as Li2O can induce defects in the HCNS formation process and exert about 0.6 A / cm 2 The high current density leads to a high yield of HCNS.

[0077] Figure 6 The SEM images of the product are completely different from those of CNT Example 3, where the parameters of the electrolysis reaction are the same (Montgomery brass cathode, NiCrC anode, high current density 0.6 A / cm 2, in a molten Li2CO2 electrolyte containing about 2 wt% dissolved Li2O at 750°C). The electrolysis reaction of this Example 4 was run for the same 30 minutes using CO2 as the reactant, but the concentration of Fe2O3 in the electrolyte was increased from 0.1 wt% to 1 wt%. Before cleaning to remove excess electrolyte, the product looked the same (see Figure 6 A). However, unlike conventional CNTs, the carbon product now contains a mixture of small HCNTs (0.1 μm in diameter and 3 μm in length) with a purity of about 90% and about 10% straight CNTs.

[0078] Figure 7 A low magnification TEM image of the HCNT product (also referred to as the main product) is shown. The HCNT carbon product has a braided spiral geometry. Figure 8 High-magnification TEM of the HCNT product is shown. Using this higher magnification, the spacing of the graphene layers in the HCNT wall is consistently about 0.34 nm, a typical value for adjacent graphene layers, and the HCNT wall thickness observed in all TEM images varies from about 17 nm to about 38 nm.

[0079] Fig. 9 TEM of straight CNTs (also called secondary products) is shown. The secondary products contain CNTs, not HCNTs. Fig. 9 A and Fig. 9 As shown in Figure C, these CNTs are either hollow or partially filled with Fe, Ni and / or Cr.

[0080] Fig.10 EDS results for minor products at two points are shown: within the CNT wall and in the inner "dark" portion of the CNT, which indicates metal. The CNT wall is composed of essentially pure carbon ( Fig.10 A), and when not empty, contains iron and nickel (not shown) and / or chromium ( Fig.10 B). Straight CNTs in the secondary product appear to have almost no defects. The measured straight CNT diameters range from about 32 to about 200 nm, with diameter walls consisting of as few as 16 and as many as 72 walls consisting of cylindrical graphene shells spaced about 0.34 nm apart. Without being bound by any theory, it is assumed that iron regulates the rate at which nanocarbon components are available, and when properly controlled and combined with a high defect rate, heptagonal carbon is provided rather than pentagonal carbon, and highly controlled growth is used to adjust torsional stress, providing the first observed environment in which the primary product of molten carbonate electrolysis decomposition of CO2 is HCNT.

[0081] Example 5 - Further HCNS Synthesis

[0082] In this embodiment 5, the electrolysis reaction was carried out according to the following parameters: the plane 27cm 2Montessori brass cathode with 27cm 2 Nichrome alloy C plane anode vertically separated by 1 cm, about 0.6A cm -2 The electrolysis reaction in Example 5 was run for about 30 minutes using CO2 as a reactant and 1.7 wt% Fe2CO3 added to the molten electrolyte at a high current density of 1.5 wt% in a molten Li2CO2 electrolyte containing about 2 wt% dissolved Li2O at 750°C.

[0083] When a higher amount of Fe2O3 (1.7%) was added to the lithium carbonate electrolyte, the HCNT growth was interrupted. The HCNS continued to grow but in a planar spiral shape instead of a CNT spiral morphology, called spiral carbon nanosheets (HCNPs). Fig.11 An SEM image of the 1.7 wt% Fe2O3 HCNS product after about 30 minutes of melt electrolysis reaction according to an embodiment of the present disclosure is shown. The washed product consists of over 80% HCNP morphology, with the remainder of the product being a mixture of spiral sheets, nano-onions and nanotubes and a small portion of single (rather than double-helical) HCNTs. The observed spiral HCNP morphology resembles the classic macroscopic rotini or fusilli pasta shape, and it is noted that this shape can be formed as a solid or hollow tube, twisted into a spiral. Without being bound by any theory, it is assumed that the carbon components ejected by the combined carbon reduction and the formed iron carbide nucleation are produced at too high a rate to maintain the growth of the spiral nanotube morphology, which may result in the HCNP morphology.

[0084] Example 6 - Further HCNS Synthesis

[0085] At intermediate concentrations between 1% and 1.7% Fe2O3, high current densities (about 0.6 A / cm 2 ) Further phenomena were observed, and it was observed that high purity HCNTs were produced at 1% Fe2O3 concentration and high purity HCNPs were produced at 1.7% Fe2O3 concentration. Except for using 1.3% Fe2O3, all other electrolysis reaction parameters were the same as in Example 5 (plane 27 cm 2 Montessori brass cathode with 27cm 2 Nichrome C flat anode vertically separated by about 1 cm, 750 °C Li2CO3 with 2 wt% Li2O, at 0.6 A cm -2 At high current densities of 30 minutes (30 minutes), carbon building blocks can form more rapidly than at lower concentrations of Fe2O3 (such as in Example 4), and carbon nanotubes (whether regular or helical) tend to be filled with concentric cylindrical graphene shells, leaving no open core within the nanotube. This morphology has been previously described as carbon nanofibers (CNFs), although this helical CNF variant (HCNF) has not been observed.

[0086] like Fig.12 As shown, when 1.3% Fe2O3 is used, the carbon product consists of about 60% CNF, about 20% HCNF, about 15% HCNP and about 5% CNT with almost no defects. The diameter of the helical nanostructure is between about 300nm and about 700nm. Fig.13 As shown, increasing to 1.5% Fe2O3, the concentration of HCNPs in the product increases to about 30% and the remainder is observed to be mainly composed of a single irregularly coiled helical HCNS.

[0087] Example 7 - Further HCNS Synthesis

[0088] In the absence of: (i) high electrolytic current density growth; (ii) high temperature electrolytic growth (e.g., 725°C or higher); (iii) sp3 defect inducers, such as added oxides; or (iv) controlled concentrations of iron added to the electrolyte or cathode surface, deformed, curved, or bent CNTs can still be formed that are still HCNS but do not have a regularly repeating helical pattern.

[0089] In this Example 7, according to an embodiment of the present disclosure, HCNS was synthesized by electrolysis using the following parameters: a Montessori brass cathode and 30 cm 2 The flat NiCrC anodes of the area are spaced apart and about 0.5A / cm2 is applied in pure 750℃ Li2CO3 (without additives). -2 The current density was 2 hours using CO2 as the reactant. Fig.14 As shown in A, the HCNS product may not have a regular, repeating helical morphology, such as but not limited to: defective CNTs, deformed CNTs, bent CNTs, curved CNTs or combinations thereof.

[0090] The electrolysis reaction parameters described in this paper show high yields of HCNT, HCNP or CNT formation, but other molten electrolyte conditions can synthesize such nanomaterials, albeit in lower yields. For example, in pure Li2CO3 electrolyte (without any Li2O or Fe2O3 additives) at 0.5A cm -2 At relatively high current density, a small portion of about 20% HCNTs and HCNPs were produced, while the main curled CNTs were produced, such as Fig.14 As shown in B.

[0091] Fig.14 C and Fig.14D shows that HCNTs and HCNPs can be synthesized in certain ternary electrolytes even at lower current densities and in the absence of Fe2O3, albeit in lower yields. Specifically, the product of molten carbonate electrolysis containing 20 wt% Na2CO3 and 80 wt% Li2CO3 with an additional additive of about 8 wt% dehydrated borax was used to synthesize HCNTs and HCNPs at 0.2 A / cm -2 Splitting of CO2 at low current density. Fig.14 C shows that the main electrolysis product is curled CNT, and contains a large amount of by-products HCNT and HCNP ( Fig.14 D).

[0092] Electrolyte and electrode composition as well as (high) current density, defects and growth control additives can all play an important role in the formation of HCNS. Controlling these parameters, according to embodiments of the present disclosure, a variety of specific, uniform, high-yield HCNS can be synthesized through molten carbonate electrolysis reactions.

Claims

1. A method for synthesizing helical carbon nanostructure HCNS, the method comprising the following steps: (a) aligning an anode spaced apart from a cathode to define an inter-electrode space; (b) introducing a molten carbonate electrolyte into the inter-electrode space; (c) introducing a carbon input into the inter-electrode space; (d) applying a current across the electrodes; (e) applying at least (i), (ii) and (iv) of the following parameters: (i) applying said electric current at an electrolysis current density of at least 0.4 A / cm2; (ii) prior to the step of applying the current, heating the inter-electrode space to at least 725°C; (iii) adding an electrolyte additive into the inter-electrode space; and (iv) adding iron oxide in a concentration between 1% and 1.7% to the inter-electrode space; and (f) collecting the product containing the HCNS from the electrode, wherein the HCNS comprises one or more of the following: helical carbon nanotubes HCNTs, helical carbon nanofibers HCNFs, double-stranded HCNTs, braided HCNTs, helical nanosheets HCNPs, and combinations thereof.

2. The method according to claim 1, wherein: The HCNS also includes deformed CNTs, bent CNTs, curved CNTs, and combinations thereof.

3. The method according to claim 1, wherein: The inter-electrode space is heated to at least 750°C.

4. The method according to claim 1, wherein: The electrolyte additive is an sp3 defect inducer.

5. The method according to claim 4, wherein: The sp3 defect inducing agent is an oxide.

6. The method according to claim 5, wherein: The oxide is a metal oxide.

7. The method according to claim 1, wherein: The additive is one or more of borates, sulfates, nitrates, phosphates and combinations thereof.

8. The method according to claim 1, wherein: Iron oxide is added to the inter-electrode space by adding iron to the electrolyte, dissolving iron from the anode, an electrolyte precursor, including iron on the cathode surface, or a combination thereof.

9. The method according to claim 1, wherein: The molten carbonate electrolyte includes alkali metal carbonates, alkaline earth carbonates, or a combination thereof.