A bipolar plate and a method for preparing the same
Through 3D printing technology, the bipolar plates are printed layer by layer, and the problems of complex bipolar plate preparation process and complex runner processing are solved, achieving efficient and low-cost precision preparation and high mechanical performance bipolar plate manufacturing.
Patent Information
- Application Number
- CN202210200562.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-03-01
AI Technical Summary
The existing bipolar plate preparation methods are complex in technology, and it is difficult to meet the complex runner processing requirements and mass production problems.
通过建立双极板立体模型,分层处理并设置不同成形工艺参数,利用3D打印技术逐层打印双极板结构,筛选和烘干钛或钛合金粉末,预处理基板,并根据打印路径和成形工艺参数逐层打印流道和非流道区。
The precision preparation of bipolar plates is realized, the manufacturing process is simplified, the cost is reduced, and the efficiency is improved. It can effectively solve the complexity of traditional processes and complex runner processing problems, while improving the mechanical properties and material utilization of molded parts.
Smart Images

Figure CN114635149B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water electrolysis, and in particular to a bipolar plate and a preparation method thereof. Background Art
[0002] The bipolar plate is the core component of SPE water electrolysis, accounting for the vast majority of the weight and cost of the electrolyzer. Its main functions are to transport and distribute reactant water to the anode, collect hydrogen and oxygen produced after the reaction, transmit current, and support the entire electrolyzer. The choice of bipolar plate material needs to have good electrical and thermal conductivity, high mechanical strength, corrosion resistance, and gas impermeability. Metal materials not only have good electrical and thermal conductivity, but also have sufficiently high mechanical strength, good toughness, and are easy to process. They have become common materials for SPE water electrolysis bipolar plates, especially titanium metal and its alloys, because they are very easy to form a dense oxide film on their surface and have good corrosion resistance, and are favored by researchers in the field of SPE water electrolysis bipolar plates.
[0003] In order to ensure that water can be evenly distributed and fully supplied on the surface of the anode membrane electrode, and that the gases (oxygen and hydrogen) and heat generated by the reaction are removed in time, a flow field structure is generally set on the bipolar plate so that the water flows evenly through the entire electrode without any "blank area". At the same time, the heat is taken away in time through the circulation of water and the discharge of gas to balance the temperature inside the electrolyzer. Simple flow fields, such as parallel flow fields and serpentine flow fields, are relatively easy to process and have good heat dissipation capabilities when used in small electrolyzers. However, as the electrode surface increases or the number of stacks increases, the mass transfer resistance increases significantly. Complex flow fields such as gradient flow channels with variable cross-sectional dimensions, irregular bionic flow fields, and composite flow fields with multiple structural combinations will have greater advantages.
[0004] However, complex flow channels have many fine structures and complex designs, and high precision is required in the manufacturing process of metal bipolar plates. The traditional bipolar plate preparation method is complex and requires processes such as casting and electroplating. The manufacturing process is complicated and time-consuming, and it is difficult to meet the processing requirements of complex flow channels, making it difficult to industrialize and apply. Summary of the invention
[0005] The purpose of the present invention is to provide a bipolar plate and a method for preparing the same, so as to solve the problem that the existing bipolar plate preparation method is complicated in process and difficult to meet the requirements of complex flow channel processing and batch production.
[0006] In order to achieve the above object, the present invention provides a method for preparing a bipolar plate, which comprises:
[0007] S1. Establish a three-dimensional model of a bipolar plate, perform layered processing on the three-dimensional model of the bipolar plate to obtain a printing path for each layer, set different forming process parameters for the flow channel area and the non-flow channel area, and import the printing path and the forming process parameters into a printing device;
[0008] S2, screening and drying titanium or titanium alloy powder, and pre-treating the substrate;
[0009] S3. Pre-painting powder on the substrate according to the three-dimensional model information of each layer of the bipolar plate;
[0010] S4, printing the structure of each layer of the bipolar plate according to the printing path and the forming process parameters;
[0011] S5. Repeat steps S3 and S4 until the bipolar plate printing is completed.
[0012] Preferably, in step S1, the three-dimensional model of the bipolar plate is established, the three-dimensional model of the bipolar plate is layered to obtain a printing path for each layer, different forming process parameters are set for the flow channel area and the non-flow channel area, and the specific steps of importing the printing path and the forming process parameters into the printing device include:
[0013] Design a three-dimensional model of a bipolar plate with a flow channel using three-dimensional design software;
[0014] The three-dimensional model of the bipolar plate is imported into the slicing software for slicing and layering processing to obtain the contour data of each cross section and the filling scanning path to obtain the printing path of each layer;
[0015] Different forming process parameters are set for the flow channel area and the non-flow channel area respectively, and the printing path and the forming process parameters are imported into the printing device.
[0016] Preferably, after the three-dimensional model of the bipolar plate is imported into the slicing software for slicing and layering, a support structure for supporting the bipolar plate is added.
[0017] Preferably, the specific steps of screening and drying the titanium or titanium alloy powder and pre-treating the substrate in step S2 include:
[0018] Select titanium or titanium alloy powder with a particle size range of 15 to 53 μm, and dry the selected titanium or titanium alloy powder in a drying oven at 100 to 150° C. for 6 to 8 hours;
[0019] The substrate is surface polished, cleaned, and dried.
[0020] Preferably, before step S3, the method further includes: introducing an inert gas into the printing device until the oxygen content in the printing device is less than or equal to 0.08%.
[0021] Preferably, in step S3, the specific steps of pre-fabricating powder on the substrate according to the three-dimensional model information of each layer of the bipolar plate include:
[0022] According to the three-dimensional model information of each layer of bipolar plates, the working platform of the printing equipment is lowered by one layer thickness and a layer of alloy powder is laid;
[0023] The thickness of the laid alloy powder is equal to the height to which the working platform descends.
[0024] Preferably, in step S4, according to the printing path and the forming process parameters, the specific steps of printing the structure of each layer of the bipolar plate include:
[0025] According to the printing path and forming process parameters, the printing equipment begins to selectively melt each layer of alloy powder to complete the printing of each layer structure of the bipolar plate.
[0026] Preferably, the forming process parameters of the flow channel area are: laser power is 150-200W, laser scanning speed is 1000-1200mm / s, laser scanning spacing is 100-110μm, single layer thickness is 30-40μm, and the interlayer angle is 45°;
[0027] The forming process parameters of the non-flow channel area are: laser power is 200-250W, laser scanning speed is 1200-1500mm / s, laser scanning spacing is 60-80μm, single layer thickness is 30-40μm, and the interlayer angle is 67°.
[0028] The present invention also provides a bipolar plate, which is prepared by the above-mentioned bipolar plate preparation method.
[0029] The present invention provides a bipolar plate and a preparation method thereof, which has the following beneficial effects compared with the prior art:
[0030] The present invention provides a method for preparing a bipolar plate. First, a three-dimensional model of a bipolar plate is established, and the three-dimensional model of the bipolar plate is layered to obtain a printing path for each layer. Different forming process parameters are set for a flow channel area and a non-flow channel area, respectively, and the printing path and the forming process parameters are introduced into a printing device. At the same time, titanium or titanium alloy powder is screened and dried to pre-treat a substrate. Then, according to the three-dimensional model information of each layer of the bipolar plate, powder is pre-made on the substrate, and then the structure of each layer of the bipolar plate is printed according to the printing path and the forming process parameters, and the powder is repeatedly spread and the single-layer structure is printed until the printing of the bipolar plate is completed.
[0031] The above method adopts different process parameters to form the flow channel area and non-flow channel area of the bipolar plate respectively, among which the geometric size and surface quality of the flow channel area affect the normal operation function of the bipolar plate, and high-precision forming process parameters are selected. The non-flow channel area is a non-functional area, and high-efficiency forming process parameters are selected. In this way, the precise preparation of the bipolar plate can be achieved. The preparation method is simple, the production cost is low, and the efficiency is high. It can effectively solve the problem that the existing preparation technology and process of the bipolar plate are complex and it is difficult to meet the requirements of complex flow channel processing. At the same time, it has advantages in mechanical properties of molded parts, integrated molding, material utilization, processing flexibility and economy. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 Schematic diagram of a process for preparing a bipolar plate according to an embodiment of the present invention. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments.
[0034] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a bipolar plate, comprising the following steps:
[0035] S1. Establish a three-dimensional model of a bipolar plate, perform layered processing on the three-dimensional model of the bipolar plate to obtain a printing path for each layer, set different forming process parameters for the flow channel area and the non-flow channel area, and import the printing path and the forming process parameters into a printing device;
[0036] S2, screening and drying titanium or titanium alloy powder, and pre-treating the substrate;
[0037] S3. Pre-painting powder on the substrate according to the three-dimensional model information of each layer of the bipolar plate;
[0038] S4, printing the structure of each layer of the bipolar plate according to the printing path and the forming process parameters;
[0039] S5. Repeat steps S3 and S4 until the bipolar plate printing is completed.
[0040] Specifically, in step S1, a three-dimensional model of a bipolar plate with a flow channel part is first established using three-dimensional design software, and the three-dimensional model of the bipolar plate is imported into a slicing software for slicing and layering to form layered slices with a certain thickness and order. Preferably, necessary support structures are added between the layered slices, and the scanning path is reasonably planned according to the contour information of each cross section of the bipolar plate, and different process parameters are set for the flow channel area and the non-flow channel area respectively, and input into a printing device. Preferably, the printing device is an SLM (Selective laser melting) device, thereby obtaining a printing path and forming process parameters, and saving them in an STL file format recognizable by the SLM device, and finally importing them into the SLM device.
[0041] Specifically, in step S2, first, the titanium or titanium alloy powder needs to be screened and dried. It should be noted that by screening and drying the titanium or titanium alloy powder, the required metal bipolar plate can be prepared in one molding while meeting the printing requirements. The prepared metal bipolar plate has good flexibility and excellent mechanical and electrical properties, which can meet the requirements of the metal bipolar plate. Among them, a vacuum furnace or an atmosphere protection furnace can be used to dry the titanium or titanium alloy powder. The temperature and time depend on the weather and the powder particle size. Preferably, in this embodiment, titanium or titanium alloy powder with a particle size range of 15 to 53 μm is selected, and the selected titanium or titanium alloy powder is placed in a drying oven at 100 to 150°C for 6 to 8 hours; In addition, the substrate needs to be surface polished and cleaned. Preferably, the substrate surface is polished with sandpaper, and the oxides and oil stains on the substrate surface are cleaned with acetone to obtain the required surface roughness, and the substrate surface can be ensured to be free of pollution.
[0042] After the preparations in the above steps, the titanium or titanium alloy powder processed in step S2 can be poured into the powder supply cabin. At the same time, the SLM equipment is prepared, and the SLM equipment prepares and installs the substrate and the powder spreading device to pre-prepare the powder spreading.
[0043] Specifically, the SLM equipment is cleaned and pre-inspected, and the substrate is fixed in the forming chamber of the SLM equipment. In order to ensure the accuracy of printing, the substrate in the forming cylinder is first leveled, that is, it is necessary to ensure that the substrate is parallel to the printing plane of the SLM equipment. Preferably, the height error between the substrate and the printing plane is less than or equal to 0.02mm. In actual operation, a vernier caliper can be used to measure the height difference between the substrate and the printing plane at the four corners, so that the height difference at the four corners is less than or equal to 0.02mm. It should be noted that during the SLM forming process, large stress is easily generated inside the product, causing the product to warp and deform. In order to reduce the warping and deformation of parts, the product is usually sintered on the substrate so that the product and the substrate become one; before the forming begins, the substrate must first be leveled. If the substrate is not flat, the bonding strength between the formed part and the substrate will be reduced, affecting the forming quality.
[0044] After installing the substrate and the powder spreading device, lower the substrate by 2 mm and adjust the height of the powder spreading device to ensure that the knife does not get stuck during printing. Further, spread powder on the substrate according to the thickness of each slice layer. At the same time, the uniformity and flatness of the powder spreading also have a great influence on the quality of the product. If the powder is not spread evenly, the internal porosity of the product will increase and the quality of the product will be reduced. Therefore, it is necessary to further improve the flatness of the powder spreading and improve the quality of the product. Spread the alloy powder evenly on the substrate and ensure that the gaps around the substrate are also filled with powder.
[0045] Preferably, before step S3, the method further includes: introducing an inert gas into the SLM device until the oxygen content in the SLM device is less than or equal to 0.08%; further preferably, the inert gas is argon. In specific implementation, argon is introduced into the forming chamber of the SLM device to ensure that the product is not oxidized during the forming process.
[0046] Specifically, in steps S3 and S4, according to the printing path and forming process parameters imported into the SLM device, the SLM device calls in the contour information layer by layer under the control of computer instructions, and starts selective melting, which specifically includes turning on the laser, rotating the polarizer to control the laser to selectively irradiate the powder bed, and the unmelted titanium powder can continue to be used after screening; after processing the current layer, the forming cylinder drops a layer thickness, the powder supply cylinder rises a certain distance, and the powder spreading device further spreads the metal powder on the processed current layer, and the device calls in the data of the next layer of contour for processing, and processes layer by layer until the entire part is processed. Preferably, the powder spreading device can be a scraper. As a result, the metal powder is completely melted under the heat of the laser beam, cooled and solidified, and accumulated layer by layer to form a three-dimensional solid product. The high-energy beam laser is used to directly melt the metal powder to form a high-performance metal bipolar plate.
[0047] Preferably, after the SLM device prints the bipolar plate according to the printing path and the forming process parameters, the method further includes: after the bipolar plate is cooled, taking it out of the forming chamber, removing the supporting structure, and then performing corresponding post-processing.
[0048] Using large-scale selective laser melting rapid prototyping equipment, after a large number of rigorous and complex experiments, the process parameters suitable for bipolar plates with complex flow channels printed on titanium-based metals are obtained. Preferably, the forming process parameters include: the laser power used in the flow channel printing process is 150-200W, the laser scanning speed is 1000-1200mm / s, the laser scanning spacing is 100-110μm, the single layer thickness is 30-40μm, and the interlayer turning angle is 45°. The laser power used in the non-flow channel printing process is 200-250W, the laser scanning speed is 1200-1500mm / s, the laser scanning spacing is 60-80μm, the single layer thickness is 30-40μm, and the interlayer turning angle is 67°.
[0049] The traditional bipolar plate preparation method cannot be formed in one time, and usually two monopolar plates are spliced, bonded or welded. There are problems such as high resistivity at the bonding part, poor liquid resistance and fast aging rate. At the same time, most of the existing bipolar plate preparation methods use mold manufacturing, which has the problems of high mold opening cost and long cycle, and the entire set of molds will be scrapped due to minor appearance adjustments, which is not conducive to the research and development of new products. The present invention overcomes the shortcomings of the traditional preparation method and adopts SLM technology to realize the integrated forming of metal bipolar plates and their flow channels, reducing the traditional process of multi-part split design, manufacturing, welding, heat treatment, machining and other multi-process manufacturing solutions; at the same time, because 3D printing adopts a layer-by-layer stacking forming method to print metal components, there is no need for mold and tooling design and processing, which saves high mold opening costs, is not subject to process design restrictions such as casting parting and slope, and can produce complex structure titanium alloy castings that cannot be produced by traditional processes. The more complex the component structure, the greater the processing advantage, and it is very suitable for bipolar plate processing with complex flow channels.
[0050] In addition, it should be noted that the currently disclosed 3D printed bipolar plates are mainly used in hydrogen fuel cells, which are different from the environment in which SPE electrolysis of water is located. They use graphite and resin as the raw materials for the bipolar plate substrate, print the substrate and the flow field separately, and then perform bonding treatment; even if metal sheets are used, the cathode plate and the anode plate are printed separately, and then welded, and there are still problems such as high resistivity of the bonding or welding parts; while in this embodiment, the cathode plate and the anode plate are printed at the same time, formed in one time, without welding or bonding, and the strength of the processed parts is relatively large, which is convenient for the later development of the electrolytic cell to high pressure.
[0051] Example 1
[0052] Step 1: Use CAD drawing software to design a three-dimensional model of a bipolar plate with complex flow channels. Use the slicing software Magic to discretize the three-dimensional model into layered slices with a certain thickness and order and add necessary support structures. According to the part contour information, the scanning path is reasonably planned and the corresponding process parameters are input: the corresponding process parameters are input in the flow channel area (laser power 170W, scanning speed 1000mm / s, scanning spacing 105μm, single layer thickness 30μm, and interlayer angle 45°), and the corresponding process parameters are input in the non-flow channel area (laser power 200W, scanning speed 1200mm / s, scanning spacing 60μm, single layer thickness 30μm, and interlayer angle 67°, and saved in the STL file format recognized by the equipment, and then imported into the BLT-S200 type selective laser melting forming equipment. The system converts the part contour information and parameter file package into the corresponding computer instructions;
[0053] Step 2: Dry the pure titanium powder with a particle size of 15-53 μm in a vacuum environment at 120°C for 6 hours, polish the pure titanium substrate with 500# sandpaper, clean it with acetone, and then blow it dry;
[0054] Step 3: Add the dried pure titanium powder (composition: 99.6Ti-0.15Fe-0.1Si-0.15O (mass percentage)) into the powder supply cylinder, fix the surface-treated pure titanium substrate, use a vernier caliper to measure the height H from the substrate to the printer plane (the error of the four corners cannot be greater than 0.02), then lower the substrate and adjust the scraper height to ensure that the scraper does not get stuck during printing;
[0055] Step 4: Start spreading powder. First, raise the powder bin to be almost flush with the substrate, scrape it back and forth with a scraper, and then raise it 0.5mm each time. When spreading powder, use a shovel to fill the gaps around the processing platform with powder. After spreading the powder, install all the components and import the file;
[0056] Step 5: Open the pure argon gas bottle and start gas washing until the oxygen content in the SLM equipment forming chamber is lower than 0.08%;
[0057] Step 6: The SLM forming equipment calls in the contour information layer by layer under the control of computer instructions. The forming cylinder drops a corresponding distance according to the preset powder thickness. The scraper spreads the powder. The polarizer rotates to control the laser to melt the pure titanium powder, forming a molten pool that solidifies and spreads on the substrate. The unmelted pure titanium powder can continue to be used after screening. After the two-dimensional contour scanning of the sample on the current powder bed is completed, the servo motor drives the powder supply cylinder to rise 30μm, and the forming cylinder drops 30μm accordingly. The scraper spreads the powder from the powder supply cylinder to the forming substrate, and the laser melts the newly spread titanium powder. The whole process is repeated until the entire forming process is completed.
[0058] Step 7: After the pure titanium bipolar plate product has cooled, take it out of the forming chamber, remove the supporting structure, clean the powder in the flow channel, and then perform the corresponding post-processing.
[0059] Example 2
[0060] Step 1: Use CAD drawing software to design a three-dimensional model of a bipolar plate with complex flow channels. Use the slicing software Magic to discretize the three-dimensional model into layered slices with a certain thickness and order and add necessary support structures. According to the part contour information, the scanning path is reasonably planned and the corresponding process parameters are input: the corresponding process parameters are input in the flow channel area (laser power 180W, scanning speed 1200mm / s, scanning spacing 105μm, single layer thickness 30μm, and interlayer turning angle 45°), and the corresponding process parameters are input in the non-flow channel area (laser power 250W, scanning speed 1500mm / s, scanning spacing 80μm, single layer thickness 40μm, and interlayer turning angle 67°), and saved in the STL file format recognized by the equipment, and then imported into the BLT-S200 selective laser melting forming equipment. The system converts the part contour information and parameter file package into the corresponding computer instructions;
[0061] Step 2: Dry Ti-6Al-4V powder (composition: 88.94Ti-6.51Al-4.29V-0.074O-0.186Fe (mass percentage)) with a particle size of 15-53 μm in a vacuum environment at 120°C for 8 hours to remove moisture from the powder, and polish the titanium alloy substrate with 500# sandpaper, clean it with acetone, and then blow it dry;
[0062] Step 3: Add the dried Ti-6Al-4V powder into the powder supply cylinder, fix the titanium alloy substrate with surface treatment, use a vernier caliper to measure the height H from the substrate to the printer plane (the error of the four corners cannot be greater than 0.02), then lower the substrate and adjust the scraper height to ensure that the scraper does not get stuck during printing;
[0063] Step 4: Start spreading powder. First, raise the powder bin to be almost flush with the substrate, scrape it back and forth with a scraper, and then raise it 0.5mm each time. When spreading powder, use a shovel to fill the gaps around the processing platform with powder. After spreading the powder, install all the components and import the file;
[0064] Step 5: Open the pure argon gas bottle and start gas washing until the oxygen content in the SLM equipment forming chamber is lower than 0.08%;
[0065] Step 6: The SLM forming equipment calls in the contour information layer by layer under the control of computer instructions. The forming cylinder drops a corresponding distance according to the preset powder thickness. The scraper spreads the powder. The polarizer rotates to control the laser to melt the titanium alloy powder, forming a molten pool that solidifies and spreads on the substrate. The unmelted titanium alloy powder can continue to be used after screening. After the two-dimensional contour scanning of the sample on the current powder bed is completed, the servo motor drives the powder supply cylinder to rise 40μm, and the forming cylinder drops 40μm accordingly. The scraper spreads the powder from the powder supply cylinder to the forming substrate, and the laser melts the newly spread titanium alloy powder. The whole process is repeated until the entire forming process is completed.
[0066] Step 7: After the titanium alloy bipolar plate sample has cooled, it is taken out of the forming chamber, the supporting structure is removed, and the powder in the flow channel is cleared, and then the corresponding post-processing is performed.
[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a bipolar plate, It is characterized in that The following steps are involved: S1. Establish a three-dimensional model of a bipolar plate, perform layered processing on the three-dimensional model of the bipolar plate to obtain a printing path for each layer, set different forming process parameters for the flow channel area and the non-flow channel area, and import the printing path and the forming process parameters into a printing device; Design a three-dimensional model of a bipolar plate with a flow channel using three-dimensional design software; The three-dimensional model of the bipolar plate is imported into the slicing software for slicing and layering processing to obtain the contour data of each cross section and the filling scanning path to obtain the printing path of each layer; Different forming process parameters are set for the flow channel area and the non-flow channel area respectively, and the printing path and the forming process parameters are imported into the printing device; The forming process parameters of the flow channel area are: laser power of 150-200W, laser scanning speed of 1000-1200mm / s, laser scanning spacing of 100-110μm, single layer thickness of 30-40μm, and interlayer angle of 45°; The forming process parameters of the non-flow channel area are: laser power of 200-250W, laser scanning speed of 1200-1500mm / s, laser scanning spacing of 60-80μm, single layer thickness of 30-40μm, and interlayer rotation angle of 67°; S2, screening and drying titanium or titanium alloy powder, and pre-treating the substrate; S3. Pre-painting powder on the substrate according to the three-dimensional model information of each layer of the bipolar plate; S4, printing the structure of each layer of the bipolar plate according to the printing path and the forming process parameters; According to the printing path and forming process parameters, the printing equipment starts to selectively melt each layer of alloy powder to complete the printing of each layer structure of the bipolar plate; S5. Repeat steps S3 and S4 until the bipolar plate printing is completed.
2. The method for preparing a bipolar plate according to claim 1, Features: After the three-dimensional model of the bipolar plate is imported into the slicing software for slicing and layering, a support structure for supporting the bipolar plate is added.
3. The method for preparing a bipolar plate according to claim 1, Features: The specific steps of screening and drying the titanium or titanium alloy powder and pre-treating the substrate in step S2 include: Select titanium or titanium alloy powder with a particle size range of 15 to 53 μm, and dry the selected titanium or titanium alloy powder in a drying oven at 100 to 150° C. for 6 to 8 hours; The substrate is surface polished, cleaned, and dried.
4. The method for preparing a bipolar plate according to claim 1, Features: Before step S3, the method further includes: introducing an inert gas into the printing device until the oxygen content in the printing device is less than or equal to 0.08%.
5. The method for preparing a bipolar plate according to claim 1, Features: In step S3, the specific steps of pre-fabricating powder on the substrate according to the three-dimensional model information of each layer of the bipolar plate include: According to the three-dimensional model information of each layer of bipolar plates, the working platform of the printing equipment is lowered by one layer thickness and a layer of alloy powder is laid; The thickness of the laid alloy powder is equal to the height to which the working platform descends.
6. A bipolar plate, Features: The bipolar plate is prepared by the method for preparing the bipolar plate according to any one of claims 1 to 5.