A room temperature based thermoelectric material containing metal organic polymer and preparation method thereof

By ball milling and hot-pressure discharge sintering metal-organic polymers and p-type bismuth telluride alloys to form composite materials, the problem of optimizing the performance of thermoelectric materials has been solved, the improvement of thermoelectric properties and mechanical properties have been achieved, and its application in thermoelectrics has been expanded. application prospects in the field.

CN114639770BActive Publication Date: 2024-10-25HARBIN INST OF TECH SHENZHEN GRADUATE SCHOOL
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210157806.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-21
Publication Date
2024-10-25
Estimated Expiration
2042-02-21

AI Technical Summary

Technical Problem

It is difficult to synergistically optimize the thermoelectric properties and mechanical properties of existing thermoelectric materials, especially the low electrical conductivity and insufficient thermal stability of metal-organic polymer materials, which limits their application in the field of thermoelectricity.

Method used

Metal-organic polymers and p-type bismuth telluride alloys are ball milled and hot-pressure discharge plasma sintered to form composite materials, which regulate the carrier concentration and lattice thermal conductivity to improve thermoelectric properties.

Benefits of technology

It has achieved dual optimization of the electrical and thermal properties of inorganic thermoelectric materials, improving the performance of thermoelectric materials, especially its application potential in the fields of medium and low-temperature waste heat power generation and thermoelectric refrigeration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114639770B_ABST
    Figure CN114639770B_ABST
Patent Text Reader

Abstract

The present invention provides a room temperature based thermoelectric material containing metal organic polymer and a preparation method thereof, the preparation method comprising: 2‑x Sb x Te3 is mixed and ball-milled to obtain a composite material powder, 0<x≤2; the composite material powder is subjected to hot pressing discharge plasma sintering at 400~500℃ to obtain a thermoelectric material; wherein the metal organic polymer is metal phthalocyanine or a metal phthalocyanine derivative. The technical scheme of the present invention combines a representative small molecule phthalocyanine or its derivative material in the metal organic polymer with an inorganic thermoelectric material, utilizes the advantages of the porous structure and structural diversity of the metal organic polymer material, and synergistically optimizes the electrical and thermal properties of the inorganic material, enriches the means of optimizing the inorganic thermoelectric material, and provides a new idea for obtaining high-performance thermoelectric materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of thermoelectric materials, and in particular relates to a room temperature-based thermoelectric material containing a metal organic polymer and a preparation method thereof. Background Art

[0002] Thermoelectric materials (TE) are environmentally friendly "green" energy conversion materials that can directly realize the mutual conversion of thermal energy and electrical energy. Thermoelectric conversion devices with thermoelectric materials as the core use the Seebeck effect and Peltier effect of semiconductors and have been widely used in refrigeration equipment, generators, thermal energy sensors, etc., covering the military, aviation, equipment, biology, medical, industrial, commercial and other fields.

[0003] The performance of thermoelectric materials is mainly measured by the dimensionless thermoelectric figure of merit zT = S 2 ·σ·T / κ, where σ is electrical conductivity, S is the Seebeck coefficient, κ is thermal conductivity, and T is absolute temperature. An ideal thermoelectric material should have a high Seebeck coefficient, high electrical conductivity, and low thermal conductivity. The larger the zT value, the higher the thermoelectric conversion efficiency of the material. Thermoelectric devices were first used in some special fields such as space exploration. The zT value of a thermoelectric material directly reflects the thermoelectric performance of the material. As can be seen from the formula, at a specific temperature, a thermoelectric material with excellent performance should have larger σ and S coefficients, as well as low κ. However, the three parameters that affect the performance of thermoelectric materials (electrical conductivity, Seebeck coefficient, and thermal conductivity) are coupled with each other. How to maximize the demodulation of electrical and thermal transport characteristics is a key scientific issue in improving thermoelectric performance.

[0004] As the earliest discovered compound semiconductor thermoelectric material, bismuth telluride alloy is the most widely used thermoelectric material in commercial applications. In recent years, the main research goal is to further improve the thermoelectric performance of the material and effectively control the zT peak temperature range of the material so that it can be more widely used in fields including medium and low temperature waste heat power generation and thermoelectric refrigeration. In actual material research, it is necessary to consider the electrical and thermal coupling effects in a coordinated manner. Therefore, it is of great significance to explore new research methods to optimize the thermoelectric properties of materials and obtain thermoelectric materials with enhanced mechanical properties for the application of thermoelectric devices. Since the 1950s and 1960s, bismuth telluride alloy semiconductor thermoelectric materials have been reported, and the highest zT value has been close to 1.0. In recent years, nanocomposites have been considered as an effective means to optimize the thermoelectric properties of inorganic materials. The basic idea is to reduce the size of the microstructure in the material to tens of nanometers or less, reaching the order of magnitude of the wavelength of electrons and phonons, so as to achieve coordinated optimization of carrier and phonon transport, and at the same time, nano second phase filling is expected to obtain enhanced mechanical properties.

[0005] Metal Organic Polymers (MOPs) are a type of porous material with a periodic network structure formed by the self-assembly of inorganic metal centers (metal ions or metal clusters) and bridging organic ligands. With the increasing number of MOPs materials and the gradual rise of composite materials, MOPs materials will have immeasurable application prospects. Therefore, the development of MOPs and composite materials with diverse functions and their application in different fields will greatly promote the mutual development of disciplines. However, the intrinsic low electrical conductivity of MOPs materials (10 -13 ~10 -1 S cm -1 ) makes it difficult to use it alone in the thermoelectric field. Another major problem that limits the application of MOPs materials in the thermoelectric field is that most MOPs have low thermal stability (decomposition temperature is less than 300 degrees), while most traditional inorganic thermoelectric materials undergo a high-temperature sintering process (greater than 400 degrees). From the perspective of processing technology, how to effectively combine the two is a difficult problem. Summary of the invention

[0006] In view of the above technical problems, the present invention discloses a room-temperature-based thermoelectric material containing a metal organic polymer and a preparation method thereof, which synergistically optimizes the electrical and thermal properties of inorganic materials and improves the performance of the thermoelectric material.

[0007] To this end, the technical solution adopted by the present invention is:

[0008] A method for preparing a room temperature based thermoelectric material containing a metal organic polymer, comprising:

[0009] Metal organic polymer, p-type bismuth telluride Bi 2-x Sb x Te3 is mixed and ball-milled to obtain composite material powder, 0<x≤2;

[0010] The composite material powder is subjected to hot pressing discharge plasma sintering at 400-500° C. to obtain a thermoelectric material;

[0011] Wherein, the metal organic polymer is metal phthalocyanine or a metal phthalocyanine derivative.

[0012] By adopting the technical solution of the present invention, nanomaterial composite technology is applied, and metal organic polymers are used to optimize the performance of inorganic thermoelectric materials. Through effective composite material processing technology, the material carrier concentration and lattice thermal conductivity are synergistically regulated to improve the thermoelectric performance.

[0013] As a further improvement of the present invention, the p-type bismuth telluride Bi 2-x Sb x Te3 is first ball-milled for 3-5 hours and then mixed with the metal organic polymer and ball-milled.

[0014] As a further improvement of the present invention, the pressure during hot pressure discharge plasma sintering is 40-60 MPa, and more preferably 50 MPa.

[0015] As a further improvement of the present invention, the ball milling time is 2 to 12 minutes.

[0016] As a further improvement of the present invention, the spark plasma sintering temperature is 450-500°C, more preferably 450°C.

[0017] As a further improvement of the present invention, x satisfies: 0.3≤x≤1.5.

[0018] As a further improvement of the present invention, the p-type bismuth telluride Bi 2-x Sb x Te3 is Bi 0.5 Sb 1.5 Te3、Bi 0.3 Sb 1.7 Te3 or Bi 1.5 Sb 0.5 Te3.

[0019] As a further improvement of the present invention, the coordination metal in the metal phthalocyanine is at least one of Cu, Pb, Mg, Zn and Co.

[0020] As a further improvement of the present invention, the metal organic polymer is copper phthalocyanine, lead phthalocyanine, magnesium phthalocyanine, zinc phthalocyanine, cobalt phthalocyanine or copper phthalocyanine.

[0021] As a further improvement of the present invention, the coordination metal of the metal organic polymer is Cu, and the metal organic polymer, p-type bismuth telluride Bi 2-x Sb x When Te3 is mixed and ball-milled, the mass percentage of the metal organic polymer is 1-5%.

[0022] As a further improvement of the present invention, the coordination metal of the metal organic polymer is Pb, and the metal organic polymer, p-type bismuth telluride Bi 2-x Sb x When Te3 is mixed and ball-milled, the mass percentage of the metal organic polymer is 0.5-5%.

[0023] The present invention also discloses a room temperature-based thermoelectric material containing a metal organic polymer, which is prepared by using any one of the above methods for preparing a room temperature-based thermoelectric material containing a metal organic polymer.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The technical solution of the present invention proposes a new strategy for optimizing inorganic thermoelectric materials. By compounding the representative small molecule phthalocyanine or its derivative materials in metal-organic polymers with inorganic thermoelectric materials, and utilizing the advantages of the porous structure and structural diversity of metal-organic polymer materials, the electrical and thermal properties of inorganic materials are synergistically optimized. Compared with the prior art that uses compounding to reduce the lattice thermal conductivity or doping to improve the electrical properties, the metal-organic polymer adopted in the technical solution of the present invention can comprehensively utilize the unique advantages of its material structure to achieve a dual optimization effect on its electrical and thermal properties, enriching the means of optimizing inorganic thermoelectric materials and providing a new idea for obtaining high-performance thermoelectric materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is the curve of the thermoelectric properties of different Bi 0.5 Sb 1.5 Te3 (BST)-based composite materials in the embodiments of the present invention varying with temperature; (a) electrical conductivity (σ), (b) carrier concentration (n H ), (c) Seebeck coefficient (S) and (d) power factor (PF) varying with temperature.

[0027] Figure 2 is the curve of the thermal conductivity and non-lattice thermal conductivity of different Bi 0.5 Sb 1.5 Te3 (BST)-based composite materials in the embodiments of the present invention including BST / CuPc x (x = 0, 1, 3, 5 and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3 (Cu 0.02 -BST) varying with temperature; (a) thermal conductivity (κ) and (b) non-lattice thermal conductivity (κ Latt + κ B ), (c) lattice thermal conductivity (κ Latt ), (d) bipolar diffusion thermal conductivity (κ B ).

[0028] Figure 3 is the electron micrograph of Bi 0.5 Sb 1.5 Te3, CuP bulk sample, and BST / CuPc5 bulk composite material in the embodiments of the present invention; (a) is the scanning electron microscope image of the cross-section of Bi 0.5 Sb 1.5 Te3, (b) is the scanning electron microscope image of the cross-section of the CuP bulk sample, (c) is the Bi 0.5 Sb 1.5EBSD images of Te3, where the inset shows the statistics of the pole figure and the average grain size; (d) SEM image of the cross-section of the BST / CuPc5 bulk composite, (e) enlarged image of the boxed part in (d), (f) EBSD image of BST / CuPc5, where the inset shows the statistics of the pole figure and the average grain size; (g) EBSD image of the polished surface of the BST / CuPc5 bulk material, (h) shows a schematic diagram of multiple scattering centers in the BST-based composite.

[0029] Figure 4 is Bi of the embodiment of the present invention 0.5 Sb 1.5 The Te3 (BST)-based composite includes BST / CuPc x (x = 0, 1, 3, 5 and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3 (Cu 0.02 -BST) thermal property variation curves with temperature; (a) thermal diffusivity (D), (b) specific heat capacity (C p ).

[0030] Figure 5 is Bi of the embodiment of the present invention 0.5 Sb 1.5 The Te3 (BST)-based composite includes BST / CuPc x (x = 0, 1, 3, 5 and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3 (Cu 0.02 -BST) μ w / κ Latt variation curve with temperature and histogram, (a) is the variation curve with temperature, (b) is the histogram.

[0031] Figure 6 is Bi of the embodiment of the present invention 0.5 Sb 1.5 The Te3 (BST)-based composite includes BST / CuPc x (x = 0, 1, 3, 5 and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3 (Cu 0.02 -BST) thermoelectric figure of merit (zT) variation curve with temperature.

[0032] Figure 7 is Bi of the embodiment of the present invention 0.5 Sb 1.5The average thermoelectric figure of merit (zT) of Te3(BST) based composites and BST avg ) comparison chart.

[0033] Figure 8 It is a thermoelectric performance diagram of the BST / CuPc5 single-leg device of an embodiment of the present invention; (a) is the relationship between the output voltage (U) (left) and output power (P) (right) of the BST / CuPc5 single-leg device and the change of current; (b) is the experimental and theoretical thermoelectric conversion efficiency (η) of the BST / CuPc5 single-leg device; (c) is a comparison curve of the theoretical and actual maximum tested thermoelectric conversion efficiency of the samples before and after optimization with the temperature difference; (d) is a comparison curve of the conversion efficiency of the BST / CuPc single-leg thermoelectric device and the commercial BST and some BST-based composite thermoelectric materials under different temperature difference conditions.

[0034] Fig. 9 Bi of the embodiment of the present invention 0.5 Sb 1.5 Te3(BST) based composite materials include BST / CuPc x (x=0,1 and 5), BST / PbPc x Curves of thermoelectric properties of (x = 1 and 5) as a function of temperature; (a) conductivity (σ), (b) Seebeck coefficient (S), (c) power factor (PF), (d) carrier concentration (n H ), (e) thermal conductivity (κ), and (f) thermoelectric figure of merit (zT).

[0035] Fig.10 TGA decomposition curves of Pc, CuPc and PbPc samples according to the embodiments of the present invention. DETAILED DESCRIPTION

[0036] The preferred embodiments of the present invention are described in further detail below.

[0037] p-type bismuth telluride Bi prepared by chemically synthesized metal organic polymer and smelting method 2-x Sb x Te3 (0<x≤2) is loaded into a ball mill according to the stoichiometric ratio and ball milled for 2 to 12 minutes to obtain a composite material powder; wherein, p-type bismuth telluride Bi 2-x Sb x Te3 is first subjected to high-energy ball milling for 4 hours. Then the obtained composite material powder is loaded into a graphite mold and hot-pressed in a discharge plasma sintering process at 450-500°C and 50MPa for 2-5 minutes.

[0038] The specific implementation of the present invention selects small molecule phthalocyanine and its derivatives as the research object, prepares high-performance bismuth telluride / metal organic polymer composite thermoelectric materials as the goal, and combines ball milling and spark plasma sintering processes to prepare a series of bismuth telluride-based composite thermoelectric materials. By adjusting the type, proportion and processing parameters of the wireless conjugated polymer in the composite material, the carrier concentration and lattice thermal conductivity of the composite material can be regulated.

[0039] The following describes the invention in conjunction with specific embodiments.

[0040] Example 1

[0041] Copper(II) phthalocyanine (CuPc) is a typical metal organic polymer with the characteristics of metal and organic porous framework. It is reported that single crystal CuPc exhibits high carrier mobility (~40cm 2 V -1 s -1 ) and high Seebeck coefficient (~900μV K -1 ). CuPc particles have an ultra-low thermal conductivity of about 0.15 W m -1 K -1 There is no research report on making full use of the structural and chemical composition diversity of CuPc materials to optimize the thermoelectric properties of traditional inorganic materials.

[0042] This example uses copper (II) phthalocyanine (CuPc) and p-type bismuth telluride Bi prepared by smelting method. 0.5 Sb 1.5 Te3 was loaded into a ball mill according to the stoichiometric ratio and ball milled for 6 minutes to obtain a composite material powder; wherein, p-type bismuth telluride Bi 0.5 Sb 1.5 Te3 was first subjected to high-energy ball milling for 4 hours. The resulting composite material powder was then placed in a graphite mold and hot-pressed in a spark plasma sintering process at 450°C and 50 MPa for 5 minutes.

[0043] In this embodiment, the mass percentage of CuPc is 1%, and the thermoelectric material obtained in this embodiment is recorded as BST / CuPc1.

[0044] Example 2

[0045] On the basis of Example 1, the mass percentage of CuPc is 3%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as BST / CuPc3.

[0046] Example 3

[0047] On the basis of Example 1, the mass percentage of CuPc is 5%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as BST / CuPc5.

[0048] Comparative Example 1

[0049] This comparative example is the existing Bi 0.5 Sb 1.5 Te3.

[0050] Comparative Example 2

[0051] Based on Example 1, the mass percentage of CuPc in this comparative example is 0.5%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as BST / CuPc 0.5 .

[0052] Comparative Example 3

[0053] Based on Example 1, the mass percentage of CuPc in this comparative example is 10%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as BST / CuPc 10 .

[0054] Comparative Example 4

[0055] Cu 0.02 Bi 0.5 Sb 1.5 Te3(Cu 0.02 -BST) is Comparative Example 4.

[0056] The steps are as follows: high-purity Bi powder (99.999%), Te powder (99.999%), Sb powder (99.999%), and Cu (granules, 99.99%, Alfa-Aesar) are mixed in a certain stoichiometric ratio and placed in a quartz tube with a diameter of 14 mm and vacuum-sealed. The quartz glass tube is placed in a box furnace and smelted at a high temperature of 800°C for 10 hours at a heating rate of 10°C / min. The smelted Cu 0.02 Bi 0.5 Sb 1.5 The Te3 ingot was pulverized using a high energy ball mill (SPEX 8000M) for 4 hours to obtain Cu 0.02 Bi 0.5 Sb 1.5 For the preparation of bulk materials, the obtained powder was loaded into a graphite mold with a diameter of 12.7 mm and subjected to spark plasma sintering (SPS) at 753 K vacuum conditions and a pressure of 50 MPa for 5 minutes to obtain Cu 0.02 Bi 0.5 Sb 1.5 Te3. The thermoelectric performance of Examples 1 to 3 and Comparative Examples 1-4 was compared. 0.5 Sb 1.5The Te3(BST)-based composites include BST / CuPc x (x = 0, 1, 3, 5, and 10, where x = 0 means without CuPc, that is, just BST, the same below), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3(Cu 0.02 -BST), the conductivity (σ), carrier concentration (n H ), Seebeck coefficient (S), and power factor (PF) as a function of temperature are shown as Figure 1 shown, and the curves of thermoelectric properties as a function of temperature are shown as Figure 2 shown.

[0057] Table 1

[0058]

[0059] Bi 0.5 Sb 1.5 The Te3(BST)-based composites include BST / CuPc x (x = 0, 1, 3, 5, and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3(Cu 0.02 -BST), the density (ρ), thermal diffusivity (D), and specific heat capacity (C p ) as a function of temperature are shown as Figure 4 shown, and the performance comparison table is shown in Table 1.

[0060] By Figure 1 、 Figure 2 、 Figure 4 and comparing with the data in Table 1, it can be seen that the examples adopting the technical solution of the present invention have better thermoelectric properties and better thermal properties.

[0061] Microstructural observations were carried out on Bi 0.5 Sb 1.5 Te3, CuPc bulk samples, and BST / CuPc5 bulk composites, and the results are shown as Figure 3 shown. The morphology can be observed from the fracture surfaces shown in Figure 3 (a) and (b). BST presents a layered crystal structure without obvious preferred orientation, while CuPc presents a two-dimensional flake structure. Figure 3 (d) shows a low-magnification SEM image of 5 wt.% CuPc composite BST bulk, in which the observed BST particles are significantly smaller than Figure 3 the original BST particles shown in (a), indicating that the introduction of CuPc may lead to a reduction in the grain size of BST. Figure 3 (e) shows the high-magnification SEM image of the BST / CuPc5 composite material, where the layered structure of BST and the long strip structure of CuPc are clearly visible. These results indicate that CuPc has high thermal stability.

[0062] To clearly reveal the effect of CuPc on the grain growth of BST, electron backscatter diffraction (EBSD) characterization was also carried out on the samples before and after the composite, and the results are shown in Figure 3 (c) and (f). It was found that pure BST presented a relatively large layered structure with an average grain size of about 1.5 μm. After adding CuPc, the average grain size decreased significantly to about 0.8 μm. Figure 3 (g) shows the EBSD image of the polished surface of the BST / CuPc5 sample. CuPc (black) is mainly distributed at the grain boundaries of BST (gray), which is beneficial to inhibiting the grain growth of BST and enhancing the interface phonon scattering. Figure 3 (h) is the optimization mechanism of CuPc for the thermoelectric properties of BST, that is, CuPc can introduce multi-scale scattering centers to enhance the phonon scattering effect. At the same time, Cu elements can diffuse and dope to optimize the electrical properties of the composite material.

[0063] Bi 0.5 Sb 1.5 Te3 (BST)-based composite materials include BST / CuPc x (x = 0, 1, 3, 5, and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb 1.5 Te3 (Cu 0.02 -BST)'s μ w / κ Latt The variation curves and histograms with temperature are shown in Figure 5 as shown. Through the comparison of the Figure 5 results, it can be seen that due to the significant reduction of the lattice thermal conductivity in the BST / CuPc composite material, it is beneficial to the increase of μ w / κ Latt With the increase of the CuPc content, the average value of μ w / κ Latt in the whole temperature range first increases and then decreases. At 3 wt%, it is nearly 55% higher than BST ( Figure 5 (b)).

[0064] Bi 0.5 Sb 1.5 Te3 (BST)-based composite materials include BST / CuPc x (x = 0, 1, 3, 5, and 10), BST / Pc5, Cu 0.02 Bi 0.5 Sb1.5 Te3(Cu 0.02 The curve of the thermoelectric figure of merit (zT) of -BST) changing with temperature is as follows Figure 6 shown; Bi 0.5 Sb 1.5 Thermoelectric figure of merit (zT) and average thermoelectric figure of merit (zT) of Te3(BST) based composites avg ) Comparison chart Figure 7 As shown. Figure 6 and Figure 7 It can be seen from the comparison that the embodiment adopting the technical solution of the present invention has better thermoelectric performance.

[0065] The BST / CuPc5 was made into a single-leg device and its electrical properties were measured. Figure 8 As shown in the figure, it can be seen that when the cold end temperature is fixed at 300K and the hot end temperature rises from 323K to 523K, the open circuit voltage increases from 3.1mV to 36.3mV. When ΔT = 223K, the maximum output power reaches 42.5mW, and the power density is ~0.18W cm -2 . Due to the interface heat flow loss and contact thermal resistance between the heating module and the hot end of the thermoelectric device, the actual hot end temperature is lower than the temperature heated by one end of the heater. Therefore, the measured maximum output voltage is 4-5% lower than the theoretical calculated value. In addition, due to the additional influence of contact resistance, the output power is reduced from the calculated value of ~58mW to the measured value of ~52mW. Figure 8 (b) shows the thermoelectric conversion efficiency as a function of current at different ΔT. Finally, at ΔT = 223K, the peak η max As high as about 6.8%, about 42% higher than pure BST (see Figure 8 (c)), which is also higher than that of previously reported BST-based composites (see Figure 8 (d)). Thermoelectric devices made of thermoelectric materials according to the technical solution of the present invention have higher conversion efficiency and better electrical performance than commercial BST and some BST-based composite thermoelectric materials.

[0066] Example 4

[0067] Based on Example 1, this example uses lead phthalocyanine (PbPc) and p-type bismuth telluride Bi prepared by smelting method. 0.5 Sb 1.5 Te3 is loaded into a ball mill according to the stoichiometric ratio and ball milled for 2 to 12 minutes to obtain a composite material powder; wherein, p-type bismuth telluride Bi 0.5 Sb 1.5 Te3 is first subjected to high-energy ball milling for 4 hours. The resulting composite material powder is then loaded into a graphite mold and hot-pressed at 400-500°C and 50 MPa during a discharge plasma sintering process for 2-5 minutes.

[0068] In this embodiment, the mass percentage of PbPc is 0.5%. The thermoelectric material obtained in this embodiment is recorded as Bi 0.5 Sb 1.5 Te3 / PbPc 0.5 BST / PbPc 0.5 .

[0069] Example 5

[0070] On the basis of Example 4, the mass percentage of PbPc is 1%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as Bi 0.5 Sb 1.5 Te3 / PbPc1 is BST / PbPc1.

[0071] Example 6

[0072] On the basis of Example 4, the mass percentage of PbPc is 3%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as Bi 0.5 Sb 1.5 Te3 / PbPc3 is BST / PbPc3.

[0073] Example 7

[0074] On the basis of Example 4, the mass percentage of PbPc is 5%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as Bi 0.5 Sb 1.5 Te3 / PbPc5 is BST / PbPc5.

[0075] Comparative Example 5

[0076] On the basis of Example 4, the mass percentage of PbPc is 10%, and the rest is the same as Example 1. The thermoelectric material obtained in this example is recorded as Bi 0.5 Sb 1.5 Te3 / PbPc 10 BST / PbPc 10 .

[0077] Bi 0.5 Sb 1.5 Te3(BST) based composite materials include BST / CuPc x (x=0,1 and 5), BST / PbPc x The thermoelectric performance curves of (x = 1 and 5) as a function of temperature are shown in Fig. 9 As shown in the figure, it can be seen that PbPc can effectively improve the conductivity of BST. At the same content, its conductivity is significantly higher than that of CuPc. This is mainly because the doping effect of Pb is more significant than that of Cu. The diffusion of Pb elements during the composite process causes the carrier concentration to increase from 1.0×1019 cm -3 to 2.4×10 20 cm -3 As a result, the Seebeck coefficient is sharply reduced and the thermal conductivity is increased to a higher level compared with the CuPc composite. Finally, both the PF and zT of the BST / PbPc composite are at a lower level, but this result is sufficient to confirm our speculation. In addition, under the same conditions, different types of metal elements can induce significantly different diffusion doping effects in all copper phthalocyanine analogs.

[0078] The TGA decomposition curves of Pc, CuPc and PbPc samples are shown in Fig.10 As shown, CuPc has good thermal stability, and its initial decomposition temperature is 783K, which is slightly higher than the SPS sintering temperature of 753K. The TGA decomposition curve of the composite material shows that the SPS process has little thermal damage to the composite material, and the composite material remains stable during the SPS sintering process. At the same time, PbPc and CuPc not only have similar crystal structures but also have similar thermal stability.

[0079] Example 9

[0080] Based on Example 1, in this example, the p-type bismuth telluride used is Bi 0.3 Sb 1.7 The mass percentage of Te3 and CuPc is 5%, and the rest is the same as in Example 1. The thermoelectric material obtained in this example is recorded as Bi 0.3 Sb 1.7 Te3 / CuPc5.

[0081] Comparative Example 6

[0082] This comparative example is Bi 0.3 Sb 1.7 Te3 is obtained by smelting method using existing technology.

[0083] Example 10

[0084] Based on Example 1, in this example, the p-type bismuth telluride used is Bi 1.5 Sb 0.5 The mass percentage of Te3 and CuPc is 5%, and the rest is the same as in Example 1. The thermoelectric material obtained in this example is recorded as Bi 1.5 Sb 0.5 Te3 / CuPc5.

[0085] Comparative Example 7

[0086] This comparative example is Bi 1.5 Sb 0.5Te3 is obtained by smelting method using existing technology.

[0087] Comparative Example 8

[0088] Based on Example 1, in this example, the p-type bismuth telluride used is Bi 1.5 Sb 0.5 Te3, phthalocyanine (Pc) and p-type bismuth telluride Bi prepared by smelting method 1.5 Sb 0.5 Te3 was loaded into a ball mill according to the stoichiometric ratio and ball milled for 6 minutes to obtain a composite material powder; wherein, p-type bismuth telluride Bi 1.5 Sb 0.5 Te3 was first subjected to high-energy ball milling for 4 hours. The obtained composite material powder was then placed in a graphite mold and hot pressed for 5 minutes in a discharge plasma sintering process at 450°C and 50MPa. The mass percentage of Pc was 5%. The thermoelectric material obtained in this example was recorded as Bi 1.5 Sb 0.5 Te3 / Pc5.

[0089] The thermoelectric performance comparison table of Examples 1 to 10 and Comparative Examples 1 to 8 is shown in Table 2.

[0090] Table 2

[0091]

[0092] From the data comparison in Table 2, it can be seen that by adopting the technical solution of the present invention, the electrical and thermal properties of the inorganic material are synergistically optimized by compounding the representative small molecule metal phthalocyanine or its derivative materials in the metal organic polymer with the inorganic thermoelectric material.

[0093] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for preparing a room temperature based thermoelectric material containing a metal organic polymer, Features: It includes: Metal organic polymer, p-type bismuth telluride Bi 2-x Sb x Te 3 Mixing and ball milling are performed to obtain composite material powder, 0<x<2; The composite material powder is subjected to hot pressing discharge plasma sintering at 400-500°C to obtain a thermoelectric material; Wherein, the metal organic polymer is metal phthalocyanine or a metal phthalocyanine derivative; The coordination metal of the metal organic polymer is Cu, and the metal organic polymer and p-type bismuth telluride Bi 2-x Sb x Te 3 During mixed ball milling, the metal organic polymer accounts for 1-5% by mass; Alternatively, the coordination metal of the metal organic polymer is Pb, and the metal organic polymer and p-type bismuth telluride Bi are 2-x Sb x Te 3 During mixed ball milling, the mass percentage of the metal organic polymer is 0.5-5%.

2. The method for preparing a room temperature based thermoelectric material containing a metal organic polymer according to claim 1, Features: The p-type bismuth telluride Bi 2-x Sb x Te 3 The mixture is first ball-milled for 3-5 hours and then mixed with the metal organic polymer and ball-milled.

3. The method for preparing a room temperature based thermoelectric material containing a metal organic polymer according to claim 1, Features: The pressure during hot-pressing spark plasma sintering is 40-60 MPa.

4. The method for preparing a room temperature based thermoelectric material containing a metal organic polymer according to claim 1, Features: The ball milling time ranged from 2 to 12 minutes.

5. The method for preparing a room temperature based thermoelectric material containing a metal organic polymer according to claim 1, Features: The p-type bismuth telluride Bi 2-x Sb x Te 3 for Bi 0.5 Sb 1.5 Te 3 、Bi 0.3 Sb 1.7 Te 3 Or Bi 1.5 Sb 0.5 Te 3 .

6. The method for preparing a room temperature based thermoelectric material containing a metal organic polymer according to claim 1, Features: The metal organic polymer is copper phthalocyanine or lead phthalocyanine.

7. A room temperature based thermoelectric material containing a metal organic polymer, Features: The material is prepared by the method for preparing a room temperature-based thermoelectric material containing a metal organic polymer as described in any one of claims 1 to 6.

Citation Information

Patent Citations

  • High-performance thermoelectric composite material and preparation method thereof

    CN102339946A

  • Halogenated metal phthalocyanine complex thermoelectric material and preparation method thereof

    CN110379915A

  • Two-dimensional transition metal carbide / bismuth telluride or derivative-based thermoelectric composite material and preparation thereof

    CN110767796A

  • N-type bismuth telluride-based room-temperature thermoelectric material and preparation method thereof

    CN113421959A

  • Thermoelectric conversion module

    JP2015144212A