Method for producing aqueous polymer dispersion

By optimizing the pore distribution and SUVA ratio control of the filtration membrane in the membrane filtration process, the problem of inner surface and internal fouling of the membrane is solved, the membrane life is extended and the production efficiency of the polymer dispersion is improved.

CN114641342BActive Publication Date: 2024-10-08KANEKA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080074831.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-25
Filing Date
2020-10-08
Publication Date
2024-10-08
Estimated Expiration
2040-10-08

AI Technical Summary

Technical Problem

In existing membrane filtration methods, suspended solids and dissolved components are easily adsorbed in the filtration membrane, leading to the formation of fouling and affecting the life and production efficiency of the membrane.

Method used

The total number of openings on the inner surface of the filter membrane is set to 100%, the openings with a pore diameter smaller than the minimum particle size of the polymer account for more than 50%, the surface opening diameter distribution is less than 0.2, and the initial SUVA ratio is controlled during the membrane filtration process. Above 0.8 and below 1.2, the difference between the secondary SUVA ratio and the initial SUVA ratio is below 0.2 to reduce the inner surface and internal fouling of the filter membrane.

Benefits of technology

It effectively extends the life of the filter membrane, reduces the cleaning frequency and the use of chemicals, improves the production efficiency of polymer dispersion, and reduces the cost of chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003614217300000011
    Figure HDA0003614217300000011
  • Figure HDA0003614217300000012
    Figure HDA0003614217300000012
  • Figure HDA0003614217300000013
    Figure HDA0003614217300000013
Patent Text Reader

Abstract

The present invention relates to a method for producing a polymer aqueous dispersion, the method comprising: a membrane filtration step, wherein a polymer aqueous dispersion containing a polymer and water is filtered using a filtration membrane to obtain a concentrated polymer aqueous dispersion and a filtrate containing no polymer, wherein the filtration membrane has openings on the inner surface, and when the total number of openings is set to 100%, there are more than 50% of the openings having a pore size smaller than the minimum particle size of the polymer, and the dispersion of the surface opening diameter distribution is 0.2 or less, and in the membrane filtration step, the initial SUVA ratio represented by the following mathematical formula (1) is 0.8 or more and 1.2 or less, and the absolute value of the difference between the initial SUVA ratio represented by the following mathematical formula (1) and the secondary SUVA ratio represented by the following mathematical formula (2) is 0.2 or less. Initial SUVA ratio = B1 / C1 (1) Secondary SUVA ratio = B2 / C2 (2) Thus, a method for producing a polymer aqueous dispersion by membrane filtration in which fouling on the inner surface of the filtration membrane and / or inside the filtration membrane is suppressed is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a polymer aqueous dispersion having a concentration step by membrane filtration, and more specifically, to a method for producing a polymer aqueous dispersion having a concentration step by membrane filtration in which fouling (membrane clogging) is reduced. Background Art

[0002] Solid-liquid separation has been performed by membrane filtration. For example, Patent Document 1 describes that suspended water can be deturbidified by external pressure filtration using a porous hollow fiber membrane with an outer surface opening rate of 20% or more and a minimum pore size of 0.03 μm or more and 1 μm or less. In addition, Patent Document 2 describes that a flow path with a flow path diameter of 1.5 mm or less is formed on the inner side of a separation membrane for solid-liquid separation, and the treated fluid is allowed to flow through the above-mentioned flow path under the condition that the membrane surface linear velocity is 6 m / s or more when the treated fluid is separated.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2001 / 053213

[0006] Patent Document 2: Japanese Patent Application Publication No. 2017-94310 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, the membrane filtration method described in Patent Document 1 has the following problems: suspended matter enters the filter membrane and generates dirt inside the filter membrane, or dissolved components in the suspension are adsorbed inside the filter membrane and generate dirt inside the filter membrane. In addition, the separation treatment method described in Patent Document 2 has the problem that dissolved components in the treated fluid are adsorbed inside the filter membrane and generate dirt inside the filter membrane.

[0009] In order to solve the above problems, the present invention provides a method for producing an aqueous polymer dispersion by membrane filtration in which fouling on the inner surface of the filtration membrane and inside the filtration membrane is suppressed.

[0010] Solution to the problem

[0011] In one or more embodiments, the present invention relates to a method for producing a polymer aqueous dispersion, the method comprising: a membrane filtration step, wherein a polymer aqueous dispersion containing a polymer and water is filtered using a filtration membrane to obtain a concentrated polymer aqueous dispersion and a filtrate not containing a polymer, the filtration membrane having openings on the inner surface, and when the total number of openings is set to 100%, more than 50% of the openings have a pore size smaller than the minimum particle size of the polymer, and the discreteness of the surface opening diameter distribution is less than 0.2. In the membrane filtration step, the initial SUVA ratio represented by the following mathematical formula (1) is greater than 0.8 and less than 1.2, and the absolute value of the difference between the initial SUVA ratio represented by the following mathematical formula (1) and the secondary SUVA ratio represented by the following mathematical formula (2) is less than 0.2.

[0012] [Mathematical formula 1]

[0013] Initial SUVA ratio = B1 / C1 (1)

[0014] Secondary SUVA ratio = B2 / C2 (2)

[0015] B1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the concentrated polymer aqueous dispersion

[0016] C1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the polymer-free filtrate

[0017] B2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the concentrated polymer aqueous dispersion is as follows:

[0018] C2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the polymer-free filtrate was

[0019] SUVA(L / mg·m)=UV(m -1 ) / DOC(mg / L)

[0020] UV(m -1 ): absorbance at wavelength 254nm

[0021] DOC (mg / L): Dissolved Organic Carbon concentration

[0022] Effects of the Invention

[0023] According to the present invention, in the filter membrane used in the method for producing a polymer dispersion, by reducing the dirt on the inner surface of the filter membrane and inside the filter membrane, the life of the membrane can be extended, and the productivity of the polymer dispersion can be improved. In addition, by reducing the dirt, the frequency of using the agent for cleaning the filter membrane can be reduced, and the membrane degradation caused by the agent can be prevented, so that the life of the membrane can be extended, and the productivity of the polymer dispersion can be improved. In addition, the frequency of using the agent for cleaning the filter membrane can be reduced, and the cost of using the agent can be reduced, and the productivity of the polymer dispersion can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a graph showing the solid content concentration of the PHBH aqueous dispersion measured in Example 1 and Comparative Example 1 and the ratio of the permeation flux (J) at each solid content concentration to the initial permeation flux (J0).

[0025] Figure 2 This is a graph showing the difference in permeate flow rate per unit membrane area and SUVA ratio of the PHBH aqueous dispersion measured in Example 1 and Comparative Example 1 (the absolute value of the difference between the initial SUVA ratio and the SUVA ratio at a given permeate flow rate per unit membrane area).

[0026] Figure 3 This is a graph showing the difference in solid content concentration and SUVA ratio of the PHBH aqueous dispersion measured in Example 1 and Comparative Example 1 (the absolute value of the difference between the initial SUVA ratio and the SUVA ratio at each solid content concentration).

[0027] Figure 4 A is a SEM photograph of a cross section of the filtration membrane used in Example 1 after the polymer dispersion was concentrated. Figure 4 B is a SEM photograph of a membrane cross section of the filtration membrane used in Comparative Example 1 after the polymer dispersion was concentrated.

[0028] Figure 5 A is a SEM photograph of a membrane cross section of the filtration membrane used in Example 1 before the polymer dispersion is concentrated. Figure 5 B is a SEM photograph of a membrane cross section of the filtration membrane used in Comparative Example 1 before the polymer dispersion was concentrated.

[0029] Figure 6 This is a graph of the total permeation flow rate per unit membrane area measured in Example 2 and Comparative Example 2 and the ratio of the permeation flux (J) at a given permeation flow rate to the initial permeation flux (J0).

[0030] Figure 7 This is a schematic diagram of a filtration device used for concentrating the PHBH aqueous dispersion in Example 1 and Comparative Example 1.

[0031] Figure 8 This is a schematic diagram of a filtration device used for circulation of the PHBH aqueous dispersion in Example 2 and Comparative Example 2. DETAILED DESCRIPTION

[0032] The inventors of the present invention have conducted intensive research on suppressing the fouling on the inner surface and inside of a filter membrane used for solid-liquid separation when producing a polymer dispersion. As a result, it was found that, when the total number of openings existing on the inner surface of the filter membrane is set to 100%, a filter membrane is used in which the openings having a pore size smaller than the minimum particle size of the polymer account for more than 50% and the dispersion of the surface opening diameter distribution is 0.2 or less, and in the membrane filtration process, the initial SUVA ratio (expressed by mathematical formula (1) described below) is set to 0.8 or more and 1.2 or less, and the absolute value of the difference between the initial SUVA ratio and the secondary SUVA ratio (expressed by mathematical formula (2) described below) is set to 0.2 or less, thereby effectively reducing the fouling on the inner surface and / or inside of the filter membrane. In one or more embodiments of the present invention, the "inner surface" of the filter membrane refers to the filtration surface in contact with the polymer dispersion.

[0033] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments.

[0034] In one or more embodiments of the present invention, the method for producing an aqueous polymer dispersion includes the following step (a) of concentrating the aqueous polymer dispersion as an essential step. Step (a) is a membrane filtration step of filtering the aqueous polymer dispersion with a filtration membrane to obtain a concentrated aqueous polymer dispersion and a filtrate containing no polymer.

[0035] In step (a), the polymer aqueous dispersion is sent to the inside of the filtration membrane, thereby filtering the polymer aqueous dispersion with the filtration membrane. The filtration method is not particularly limited, and includes a cross-flow method (a method in which the flow directions of the filtrate and the filtrate are orthogonal), a dead-end method (a method in which the flow directions of the filtrate and the filtrate are the same), etc. Among them, the cross-flow method is preferred from the viewpoint of suppressing fouling of the filtration membrane surface caused by polymer particles.

[0036] In one or more embodiments of the present invention, the polymer aqueous dispersion contains water and a polymer. Specifically, it is an aqueous dispersion in which polymer particles are dispersed in water. The polymer is not particularly limited, and polyhydroxyalkanoate (PHA), polyvinyl chloride, etc. can be preferably used.

[0037] In one or more embodiments of the present invention, PHA refers to a general term for polymers with 3-hydroxyalkanoic acid esters as monomer units. The above-mentioned 3-hydroxyalkanoic acid esters are not particularly limited, and examples thereof include: 3-hydroxypropionate, 3-hydroxybutyrate, 3-hydroxyvalerate, 3-hydroxyhexanoate, 3-hydroxyheptanoate and 3-hydroxyoctanoate. The above-mentioned PHA may be a homopolymer with one 3-hydroxyalkanoic acid ester as a monomer unit, or a copolymer with two or more 3-hydroxyalkanoic acid esters as monomer units. Specifically, there can be cited: copolymers of 3-hydroxybutyrate (3HB) and other 3-hydroxyalkanoic acids, copolymers of 3-hydroxyalkanoates containing at least 3-hydroxyhexanoate (3HH) as a monomer unit, and the like. Among them, from the aspect of physical properties, effective is a copolymer containing 3HH as a monomer unit, for example, a two-component copolymer of 3HB and 3HH (PHBH) (Macromolecules, 28, 4822-4828 (1995)), a three-component copolymer of 3HB, 3-hydroxyvalerate (3HV) and 3HH (PHBVH) (Patent No. 2777757, Japanese Patent Laid-Open No. 08-289797), etc. There is no particular limitation on the composition ratio of each monomer unit constituting the above-mentioned two-component copolymer PHBH of 3HB and 3HH. When the total of all monomer units is 100 mol%, the 3HH unit is preferably 1 mol% or more and 99 mol% or less, more preferably 1 mol% or more and 50 mol% or less, and further preferably 1 mol% or more and 25 mol% or less. In addition, there is no particular limitation on the composition ratio of each monomer unit constituting the three-component copolymer PHBVH of 3HB, 3HV and 3HH. When the total of all monomer units is set to 100 mol%, for example, the range of 3HB unit being 1 mol% to 95 mol%, 3HV unit being 1 mol% to 96 mol%, and 3HH unit being 1 mol% to 30 mol% is appropriate.

[0038] The polymer aqueous dispersion may contain one type of polymer or two or more types of polymers.

[0039] The polymer aqueous dispersion to be concentrated in step (a) may contain other components in addition to water and polymer (particles). Other components include solvents other than water, dispersants, surfactants, preservatives, etc. The content of other components may be appropriately selected according to the purpose, etc.

[0040] The polymer aqueous dispersion to be concentrated in step (a) may be a PHA suspension derived from a disrupted product of a PHA-containing microorganism. The PHA suspension can be obtained, for example, as described in International Publication No. 2010 / 116681.

[0041] The concentration of the polymer (solid content) in the polymer aqueous dispersion before filtration in step (a), i.e., the membrane filtration step, is not particularly limited, and may be, for example, 5% by weight (w / v%) or more and 40% by weight or less, or 10% by weight or more and 35% by weight or less. Step (a) can effectively concentrate the polymer aqueous dispersion.

[0042] The concentration of the polymer (solid content) in the concentrated polymer aqueous dispersion after filtration in step (a), i.e., the membrane filtration step, is not particularly limited, and may be, for example, 30% by weight (w / v%) or more and 65% by weight or less, or 35% by weight or more and 60% by weight or less. It becomes easy to remove water from the concentrated polymer aqueous dispersion.

[0043] In one or more embodiments of the present invention, when the total number of openings present on the inner surface of the filter membrane is set to 100%, the openings with a pore size smaller than the minimum particle size of the polymer account for 50% or more, and the dispersion of the surface opening diameter distribution is 0.2 or less (hereinafter also referred to as the surface opening diameter requirement). As a result, it is possible to effectively prevent polymer particles from entering the inside of the filter membrane from the surface of the filter membrane, and it is possible to suppress the pores inside the filter membrane from being blocked. For the filter membrane, when the total number of openings present on the inner surface is set to 100%, the openings with a pore size smaller than the minimum particle size of the polymer are preferably 55% or more, more preferably 60% or more, and further preferably 65% ​​or more. In addition, although not particularly limited, for example, from the viewpoint of further improving the effect of suppressing dirt on the surface and inside of the filter membrane, when the total number of openings present on the inner surface of the filter membrane is set to 100%, it is ideal that the openings with a pore size smaller than the minimum particle size of the polymer account for 100%, and it may be 85% or less. Specifically, it may be within the range of any of the lower limit and upper limit values ​​described above. The dispersion of the surface opening diameter distribution of the filtration membrane is preferably 0.15 or less, more preferably 0.10 or less, and even more preferably 0.05 or less. In addition, from the viewpoint of further improving the effect of suppressing the fouling on the surface and inside of the filtration membrane, the dispersion of the surface opening diameter distribution of the filtration membrane is preferably 0, but may be 0.02 or more. Specifically, it may be within the range of any of the lower limit and upper limit values ​​described above.

[0044] In one or more embodiments of the present invention, the minimum particle size of the polymer refers to the minimum particle size Dmin in the volume-based particle size distribution curve measured by the laser diffraction scattering method using the polymer aqueous dispersion before concentration in step (a) as a sample. In one or more embodiments of the present invention, the particle size distribution curve can be measured, for example, using a laser diffraction scattering particle size distribution measuring device "Microtrac MT3300EX II" manufactured by Microtrac BEL. It should be noted that the polymer aqueous dispersion that has not been concentrated based on step (a) is used as the measurement sample.

[0045] In one or more aspects of the present invention, the surface pore size of the filtration membrane can be measured, for example, as follows.

[0046] (1) Observe the inner surface of the filter membrane using a scanning electron microscope (SEM), and import the image into a computer. The scanning electron microscope is not particularly limited, and for example, "JSM-7001FA" manufactured by JEOL Ltd. can be used for observation at 3500 times. It should be noted that the type and magnification of the microscope can be appropriately changed according to the size of the pores.

[0047] (2) All the holes existing in the 5μm×5μm range selected arbitrarily in the obtained image are analyzed using image processing software (ImageJ, developer: National Institutes of Health, USA). Specifically, first, the SEM image is binarized to obtain an image in which the pores are black and the structure is white. It should be noted that when the pores and the structure cannot be binarized smoothly due to the difference in contrast in the analysis image, the pores are painted black and then the image is processed to obtain the Feret diameter of the holes within the obtained analysis range. At this time, in order to remove noise, the area of ​​0.0001μm 2 The following wells were excluded from the data.

[0048] It should be noted that, when the filter membrane is a tubular membrane, the tubular membrane is cut into a semi-cylindrical shape, and the inner surface of the filter membrane is observed with a scanning electron microscope in a state where the inner surface is exposed. In addition, when the filter membrane is a flat membrane, the surface on the side with a smaller pore size is observed with a scanning electron microscope.

[0049] In one or more embodiments of the present invention, in the membrane filtration process, the filtration membrane satisfies the requirements that the initial SUVA ratio (expressed by mathematical formula (1) described below) is greater than 0.8 and less than 1.2, and the absolute value of the difference between the initial SUVA ratio and the secondary SUVA ratio (expressed by mathematical formula (2) described below) is less than 0.2 (hereinafter also referred to as the SUVA ratio requirement).

[0050] [Mathematical formula 2]

[0051] Initial SUVA ratio = B1 / C1 (1)

[0052] Secondary SUVA ratio = B2 / C2 (2)

[0053] B1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the concentrated polymer aqueous dispersion

[0054] C1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the polymer-free filtrate

[0055] B2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the concentrated polymer aqueous dispersion is as follows:

[0056] C2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the polymer-free filtrate was

[0057] SUVA(L / mg·m)=UV(m -1 ) / DOC(mg / L)

[0058] UV(m -1 ): absorbance at wavelength 254nm

[0059] DOC (mg / L): Dissolved Organic Carbon concentration

[0060] The above-mentioned initial SUVA ratio is greater than 0.8 and less than 1.2, that is, the initial SUVA ratio is approximately 1, and the absolute value of the difference between the above-mentioned initial SUVA ratio and the above-mentioned secondary SUVA ratio is less than 0.2, that is, the secondary SUVA ratio is approximately equal to the initial SUVA ratio, which means that the water quality of the concentrated polymer dispersion and the filtrate is the same. In other words, the organic impurities contained in the concentrated polymer dispersion and the filtrate are at the same level. When the organic impurities contained in the concentrated polymer dispersion and the filtrate are at the same level, the adsorption of organic impurities on the inner surface and pores of the filtration membrane is reduced.

[0061] In one or more aspects of the present invention, "DOC" is measured using, for example, a total organic carbon analyzer (TOC-L) manufactured by Shimadzu Corporation. In addition, "UV" is measured using, for example, a spectrophotometer (U-3900) manufactured by Hitachi High-Tech Science Corporation.

[0062] In one or more embodiments of the present invention, as long as the filter membrane meets the requirements of the surface opening diameter requirements, its material is not particularly limited. It can be an organic material or an inorganic material. As an organic material, for example, resins such as polypropylene, fluororesin, cellulose ester, polysulfone resin, polyacrylonitrile, and polyimide can be listed. As a fluororesin, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, tetrafluoroethylene-hexafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, etc. can be listed. As cellulose ester, for example, cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, etc. can be listed. As a polysulfone resin, for example, polysulfone, polyether sulfone, etc. can be listed. As an inorganic material, for example, porous ceramics such as alumina, mullite, zirconia, cordierite, porous bodies made of porous sintered metals such as stainless steel, etc. can be listed. Among them. From the perspective of high roundness of the surface pores and easy to meet the above-mentioned SUVA ratio requirements, inorganic materials are preferred. In addition, the shape of the filter membrane is not particularly limited, and it can be any shape such as a tubular membrane, a flat membrane, and a hollow fiber membrane. Among them, a tubular membrane is preferred from the viewpoint that the flow path is less likely to be clogged by the polymer and that the above-mentioned SUVA ratio requirement is easily satisfied.

[0063] In one embodiment of the present invention, the aqueous polymer dispersion may be Figure 7 The filtration device shown is manufactured. Figure 7 As shown, the polymer aqueous dispersion a stirred by the stirrer 4 in the container 3 and supplied to the filter membrane 1 via the pump 2 is filtered through the filter membrane 1, thereby being separated into a concentrated polymer aqueous dispersion b and a filtrate c not containing a polymer. The concentrated polymer aqueous dispersion b is returned to the container 3, and the filtrate c is discharged from the system, thereby concentrating the polymer aqueous dispersion in the container 3.

[0064] In one embodiment of the present invention, the aqueous polymer dispersion may be Figure 8 The filtration device shown is manufactured. Figure 8 In the case of the device shown, Figure 8 As shown, the concentration of the aqueous polymer dispersion can be kept constant by returning the filtrate c to the container 3 .

[0065] The present invention includes, for example, one or more embodiments described below.

[0066] [1] A method for producing an aqueous polymer dispersion, the method comprising:

[0067] The membrane filtration step comprises filtering the polymer aqueous dispersion containing the polymer and water using a filtration membrane to obtain a concentrated polymer aqueous dispersion and a filtrate containing no polymer.

[0068] The filter membrane has openings on the inner surface, when the total number of the openings is 100%, more than 50% of the openings have a pore size smaller than the minimum particle size of the polymer, and the dispersion of the surface opening diameter distribution is less than 0.2,

[0069] In the membrane filtration step, the initial SUVA ratio represented by the following mathematical formula (1) is 0.8 or more and 1.2 or less, and the absolute value of the difference between the initial SUVA ratio represented by the following mathematical formula (1) and the secondary SUVA ratio represented by the following mathematical formula (2) is 0.2 or less.

[0070] [Mathematical formula 3]

[0071] Initial SUVA ratio = B1 / C1 (1)

[0072] Secondary SUVA ratio = B2 / C2 (2)

[0073] B1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the concentrated polymer aqueous dispersion

[0074] C1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the polymer-free filtrate

[0075] B2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the concentrated polymer aqueous dispersion is as follows:

[0076] C2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the polymer-free filtrate was

[0077] SUVA(L / mg·m)=UV(m -1 ) / DOC(mg / L)

[0078] UV(m -1 ): absorbance at wavelength 254nm

[0079] DOC (mg / L): concentration of dissolved organic carbon.

[0080] [2] The method for producing an aqueous polymer dispersion according to [1], wherein the polymer is a polyhydroxyalkanoate.

[0081] [3] The method for producing an aqueous polymer dispersion according to [1] or [2], wherein:

[0082] The above-mentioned filtration membrane is made of inorganic material.

[0083] [4] The method for producing an aqueous polymer dispersion according to any one of [1] to [3], wherein

[0084] The solid content concentration of the polymer aqueous dispersion before filtration in the membrane filtration step is 10% by weight or more and 35% by weight or less.

[0085] [5] The method for producing an aqueous polymer dispersion according to any one of [1] to [4], wherein

[0086] The concentration of the solid content of the concentrated aqueous polymer dispersion after filtration in the membrane filtration step is 35% by weight or more and 60% by weight or less.

[0087] [6] The method for producing an aqueous polymer dispersion according to any one of [1] to [5], wherein

[0088] The polymer aqueous dispersion to be filtered by the membrane filtration step is a suspension of polyhydroxyalkanoate derived from a disrupted product of a microorganism containing polyhydroxyalkanoate.

[0089] [7] The method for producing an aqueous polymer dispersion according to any one of [1] to [6], wherein

[0090] The above-mentioned filter membrane is a tubular membrane.

[0091] Example

[0092] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0093] (Measurement of polymer particle size)

[0094] The particle size distribution curve (volume basis) was measured using a laser diffraction and scattering particle size distribution measuring apparatus "Microtrac MT3300EX II" manufactured by Microtrac BEL, and the minimum particle size Dmin and the median particle size D50 were calculated.

[0095] (Determination of the surface opening diameter of the filtration membrane)

[0096] (1) The tubular membrane was cut into a semi-cylindrical shape, and the inner surface of the filtration membrane was observed at 3500 times using a scanning electron microscope ("JSM-7001FA" manufactured by JEOL Ltd.) with the inner surface exposed. The image was loaded into a computer.

[0097] (2) All pores within a range of 5 μm × 5 μm selected arbitrarily from the obtained image were analyzed using image processing software (ImageJ, developer: National Institutes of Health, U.S.A.). Specifically, first, the SEM image was binarized to obtain an image in which the pore portion was black and the structure portion was white. It should be noted that when the pore portion and the structure portion could not be binarized smoothly due to the difference in contrast within the analysis image, the pore portion was painted black and then image processing was performed to obtain the Feret diameter of the pores within the obtained analysis range. At this time, in order to remove noise, the area of ​​0.0001 μm 2 The following wells were excluded from the data.

[0098] (Determination of DOC)

[0099] The measurement was performed using a total organic carbon analyzer (TOC-L) manufactured by Shimadzu Corporation.

[0100] (UV measurement)

[0101] The measurement was performed using a spectrophotometer (U-3900) manufactured by Hitachi High-Tech Science.

[0102] (Example 1)

[0103] Ralstonia eutropha KNK-005 strain was cultured according to the method described in Example 1 of International Publication No. 2010 / 116681 to prepare a bacterial culture solution containing poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH). Then, the bacterial culture solution obtained above was sterilized by heating / stirring at an internal temperature of 60 to 80°C for 20 minutes. 0.2 wt% sodium dodecyl sulfate was added to the sterilized bacterial culture solution obtained above. After further adding an aqueous sodium hydroxide solution so that the pH reached 11.0, it was kept warm at 50°C for 1 hour. Then, a high-pressure crusher ("High-Pressure Homogenizer PA2K Model" manufactured by Nirosoabi) was used at 450 to 550 kgf / cm 2The high-pressure crushing was carried out at a pressure of . An equal amount of distilled water was added to the crushed liquid obtained after the high-pressure crushing. After centrifugation, the supernatant was removed and the liquid was concentrated twice. To the concentrated PHA water suspension, an equal amount of sodium hydroxide aqueous solution (pH11) as the removed supernatant was added and centrifuged. After removing the supernatant, water was added again to suspend it, and 0.2 wt% of sodium dodecyl sulfate and 1 / 100 weight of protease (Esperase manufactured by Novozyme) of PHA were added, and the mixture was stirred at 50°C for 2 hours at pH10. Then, the supernatant was removed by centrifugation and concentrated four times. Furthermore, by adding water, a PHBH water dispersion having a median particle size (D50) of 2 μm and a solid content concentration of 26 wt% (PHBH particle content: 260 g / L) was obtained. The minimum particle size (Dmin) of the polymer particles in the PHBH water dispersion is 0.75 μm. By using a tubular membrane (MEMBRALOX (registered trademark) 1T1-70, manufactured by PALL, material: alumina ceramic) as the filtration membrane Figure 7 The filtration device shown in the figure circulates the PHBH aqueous dispersion to the tubular membrane and performs concentration. For the tubular membrane, when the total number of openings is set to 100%, the proportion of the number of openings with a pore size smaller than the minimum particle size of the polymer particles in the PHBH aqueous dispersion is 67%, the dispersion of the surface opening diameter distribution is 0.02, the initial SUVA ratio is 0.83, and the absolute value of the difference between the initial SUVA ratio and the secondary SUVA ratio is greater than 0.05 and less than 0.2. Figure 7 As shown, the polymer aqueous dispersion a stirred by the stirrer 4 in the container 3 and supplied to the filter membrane 1 via the pump 2 is filtered at the filter membrane 1, thereby being separated into a concentrated polymer aqueous dispersion b and a filtrate c not containing a polymer. The concentrated polymer aqueous dispersion b is returned to the container 3, and the filtrate c is discharged out of the system, thereby concentrating the PHA aqueous dispersion in the container 3.

[0104] (Comparative Example 1)

[0105] Using the bacterial culture solution obtained by the same method as in Example 1, except for changing the amount of water added at the end, a PHBH aqueous dispersion having a median particle size D50 of 2 μm and a solid content concentration of 23 wt% (PHBH particle content: 230 g / L) was obtained in the same manner as in Example 1. The minimum particle size (Dmin) of the polymer particles in the PHBH aqueous dispersion was 0.75 μm. A tubular membrane (MICRODYN (registered trademark) MD020TP2N, manufactured by Microdyn-Nadir GmbH, material: polypropylene) was used as a filtration membrane. Figure 7The filtration device shown in the figure circulates the PHBH aqueous dispersion to the tubular membrane and performs concentration. For the tubular membrane, when the total number of openings is set to 100%, the proportion of the number of openings with a pore size smaller than the minimum particle size of the polymer particles in the PHBH aqueous dispersion is 38%, the dispersion of the surface opening diameter distribution is 0.50, the initial SUVA ratio is 0.90, and the absolute value of the difference between the initial SUVA ratio and the secondary SUVA ratio is 0.3. Figure 7 As shown, the polymer aqueous dispersion a stirred by the stirrer 4 in the container 3 and supplied to the filter membrane 1 via the pump 2 is filtered at the filter membrane 1, thereby being separated into a concentrated polymer aqueous dispersion b and a filtrate c not containing a polymer. The concentrated polymer aqueous dispersion b is returned to the container 3, and the filtrate c is discharged out of the system, thereby concentrating the PHA aqueous dispersion in the container 3.

[0106] The results are shown in Figure 1 to Figure 4 . Figure 1 This is a graph showing the solid content concentration of the PHBH aqueous dispersion measured in Example 1 and Comparative Example 1 and the ratio of the permeation flux (J) at each solid content concentration to the initial permeation flux (J0). Figure 2 This is a graph showing the difference between the permeate flow rate per unit membrane area and the SUVA ratio of the PHBH aqueous dispersion measured in Example 1 and Comparative Example 1 (the absolute value of the difference between the initial SUVA ratio and the SUVA ratio at the permeate flow rate per unit membrane area). Figure 3 This is a graph showing the difference in solid content concentration and SUVA ratio of the PHBH aqueous dispersion measured in Example 1 and Comparative Example 1 (the absolute value of the difference between the initial SUVA ratio and the SUVA ratio at each solid content concentration). Figure 4 A is a SEM photograph of a cross section of the filtration membrane used in Example 1 after the polymer dispersion was concentrated. Figure 4 B is a SEM photograph of a membrane cross section of the filtration membrane used in Comparative Example 1 after the polymer dispersion was concentrated.

[0107] according to Figure 1 It was confirmed that in Example 1, even when the solid content concentration of the polymer aqueous dispersion reached about 40 wt % after the concentration was completed, the ratio of the permeation flux to the initial permeation flux was 0.5 or more, and fouling was effectively suppressed. Figure 2 and Figure 3 It can be confirmed that in Example 1, by setting the initial SUVA ratio to 0.8 or more and 1.2 or less in the membrane filtration step and setting the absolute value of the difference between the initial SUVA ratio and the secondary SUVA ratio to 0.2 or less, adhesion of inclusions to the inside of the filtration membrane is suppressed and fouling inside the filtration membrane is reduced. Figure 5 A is a SEM photograph of the membrane cross section of the filtration membrane used in Example 1 before the polymer dispersion was concentrated. Figure 4 A and Figure 5 A comparison shows that, in Example 1, PHBH particles can be prevented from entering the interior of the filtration membrane, so the fouling inside the filtration membrane is reduced.

[0108] On the other hand, according to Figure 1 It is known that when the solid content concentration of the polymer aqueous dispersion reaches about 40 wt % after the concentration is completed, the ratio of the permeation flux to the initial permeation flux in Comparative Example 1 is less than 0.2, and fouling cannot be suppressed. Figure 2 and 3 It is found that in the membrane filtration step, since the absolute value of the difference between the initial SUVA ratio and the secondary SUVA ratio is 0.3 or more, adhesion of foreign matter to the inside of the filtration membrane cannot be suppressed, and fouling of the inside of the filtration membrane cannot be suppressed. Figure 5 B is a SEM photograph of a cross section of the filtration membrane used in Comparative Example 1 before the polymer dispersion was concentrated. Figure 4 B and Figure 5 As can be seen from the comparison with B, in Comparative Example 1, since the PHBH particles could not be prevented from entering the interior of the membrane, fouling inside the membrane could not be suppressed.

[0109] (Example 2)

[0110] Using the bacterial culture solution obtained by the same method as in Example 1, except for changing the amount of water added at the end, a PHBH aqueous dispersion having a median particle size D50 of 2 μm and a solid content concentration of 25 wt% (PHBH particle content: 250 g / L) was obtained in the same manner as in Example 1. The minimum particle size (Dmin) of the polymer particles in the PHBH aqueous dispersion was 0.75 μm. Using the same tubular membrane as in Example 1, the PHBH aqueous dispersion was circulated and supplied to the tubular membrane, and circulation was performed. Figure 8 As shown, the concentration of the PHBH aqueous dispersion was kept constant by returning the filtrate c to the container 3, and the fouling property was evaluated by circulating the filtrate c in a state where there were no factors that reduce the permeation flux other than fouling.

[0111] (Comparative Example 2)

[0112] A PHBH aqueous dispersion having a median particle size of 2 μm and a solid content concentration of 25 wt% (PHBH particle content: 250 g / L) was obtained in the same manner as in Example 2. The minimum particle size (Dmin) of the polymer particles in the PHBH aqueous dispersion was 0.75 μm. The same tubular membrane as that used in Comparative Example 1 was used, and the PHBH aqueous dispersion was circulated to the tubular membrane, and the circulation was carried out in the same manner as in Example 2. Figure 8As shown, the concentration of the PHBH aqueous dispersion was kept constant by returning the filtrate c to the container 3, and the fouling property was evaluated by circulating the filtrate c without any factors that reduce the permeation flux other than fouling.

[0113] The results are shown in Figure 6 . Figure 6 This is a graph showing the permeation flux per unit membrane area measured in Example 2 and Comparative Example 2 and the ratio of the permeation flux (J) at a given permeation flux to the initial permeation flux (J0). Figure 6 It can be seen that in Example 1, when the permeate volume relative to the membrane area is 10000 kg / m 2 In the stage of the membrane, the ratio of the permeate flux to the initial permeate flux is 0.8 or more, and fouling can be suppressed. On the other hand, in Comparative Example 2, the permeate volume relative to the membrane area is 10000 kg / m 2 At the stage, the ratio of the permeation flux to the initial permeation flux is less than 0.5, and fouling cannot be suppressed.

[0114] Explanation of symbols

[0115] 1 Filter membrane

[0116] 2 Pumps

[0117] 3 Container

[0118] 4. Blender

Claims

1. A method for producing an aqueous polymer dispersion, the method comprising: The membrane filtration step comprises filtering the polymer aqueous dispersion containing the polymer and water using a filtration membrane to obtain a concentrated polymer aqueous dispersion and a filtrate containing no polymer. The filter membrane has openings on the inner surface, when the total number of openings is set to 100%, more than 50% of the openings have a pore size smaller than the minimum particle size of the polymer, and the dispersion of the surface opening diameter distribution is less than 0.2, In the membrane filtration step, the initial SUVA ratio represented by the following mathematical formula (1) is greater than or equal to 0.8 and less than or equal to 1.2, and the absolute value of the difference between the initial SUVA ratio represented by the following mathematical formula (1) and the secondary SUVA ratio represented by the following mathematical formula (2) is less than or equal to 0.2, Initial SUVA ratio = B1 / C1(1) Secondary SUVA ratio = B2 / C2(2) B1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the concentrated polymer aqueous dispersion C1: The permeation flow rate per unit membrane area is less than 0.1kg / m 2 SUVA of the polymer-free filtrate B2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the concentrated polymer aqueous dispersion is as follows: C2: The permeation rate per unit membrane area is 0.1 kg / m 2 Above and 10kg / m 2 The SUVA of the polymer-free filtrate was SUVA(L / mg·m)=UV(m -1 ) / DOC(mg / L) UV(m -1 ): absorbance at wavelength 254nm DOC (mg / L): concentration of dissolved organic carbon. The polymer is a polyhydroxyalkanoate.

2. The method for producing an aqueous polymer dispersion according to claim 1, wherein: The filtration membrane is composed of inorganic materials.

3. The method for producing an aqueous polymer dispersion according to claim 1 or 2, wherein: The solid content concentration of the polymer aqueous dispersion before filtration in the membrane filtration step is 10% by weight or more and 35% by weight or less.

4. The method for producing an aqueous polymer dispersion according to claim 2, wherein: The solid content concentration of the polymer aqueous dispersion before filtration in the membrane filtration step is 10% by weight or more and 35% by weight or less.

5. The method for producing an aqueous polymer dispersion according to claim 1 or 2, wherein: The concentration of the solid content of the concentrated aqueous polymer dispersion after filtration in the membrane filtration step is 35% by weight or more and 60% by weight or less.

6. The method for producing an aqueous polymer dispersion according to claim 2, wherein: The concentration of the solid content of the concentrated aqueous polymer dispersion after filtration in the membrane filtration step is 35% by weight or more and 60% by weight or less.

7. The method for producing an aqueous polymer dispersion according to claim 3, wherein: The concentration of the solid content of the concentrated aqueous polymer dispersion after filtration in the membrane filtration step is 35% by weight or more and 60% by weight or less.

8. The method for producing an aqueous polymer dispersion according to claim 4, wherein: The concentration of the solid content of the concentrated aqueous polymer dispersion after filtration in the membrane filtration step is 35% by weight or more and 60% by weight or less.

9. The method for producing an aqueous polymer dispersion according to claim 1 or 2, wherein: The polymer aqueous dispersion to be filtered by the membrane filtration step is a suspension of polyhydroxyalkanoate derived from a disrupted product of a microorganism containing polyhydroxyalkanoate.

10. The method for producing an aqueous polymer dispersion according to claim 2, wherein: The polymer aqueous dispersion to be filtered by the membrane filtration step is a suspension of polyhydroxyalkanoate derived from a disrupted product of a microorganism containing polyhydroxyalkanoate.

11. The method for producing an aqueous polymer dispersion according to claim 3, wherein: The polymer aqueous dispersion to be filtered by the membrane filtration step is a suspension of polyhydroxyalkanoate derived from a disrupted product of a microorganism containing polyhydroxyalkanoate.

12. The method for producing an aqueous polymer dispersion according to claim 4, wherein: The polymer aqueous dispersion to be filtered by the membrane filtration step is a suspension of polyhydroxyalkanoate derived from a disrupted product of a microorganism containing polyhydroxyalkanoate.

13. The method for producing an aqueous polymer dispersion according to claim 1 or 2, wherein: The filter membrane is a tubular membrane.

14. The method for producing an aqueous polymer dispersion according to claim 2, wherein: The filter membrane is a tubular membrane.