A method for repairing high temperature anti-oxidation coating

By using MAX phase ceramic powder and ultra-high speed laser cladding on the surface of C/C composite materials, the problem of coating peeling off under high temperature oxidation environment of C/C composite materials was solved, and efficient and rapid coating repair and performance improvement were achieved.

CN114657551BActive Publication Date: 2024-11-01JIANGSU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111626413.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-11-01
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

In existing technologies, the coating of C/C composite materials is prone to peeling off under high-temperature oxidizing conditions, resulting in low repair efficiency and affecting product use.

Method used

A high-temperature antioxidant coating was prepared by using MAX phase ceramic powder to perform local repairs on the surface of carbon/carbon composite materials via ultra-high-speed laser cladding, combined with diamond paper polishing and argon protection.

Benefits of technology

It achieves efficient and rapid coating repair, enhances the bonding strength between the coating and the substrate, and has good thermal and electrical conductivity and antioxidant properties, with a short repair cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114657551B_ABST
    Figure CN114657551B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for repairing a high-temperature anti-oxidation coating, and belongs to the technical field of material preparation. The present invention uses MAX phase powder as the main raw material; ball-mills and dries the MAX phase powder; grinds the coating detached part; and adopts an ultra-high-speed laser cladding method to prepare the MAX phase high-temperature anti-oxidation coating, so as to achieve the purpose of repairing the detached high-temperature anti-oxidation coating on the surface of a carbon / carbon composite product. The present invention uses ultra-high-speed laser cladding technology to use MAX phase powder to repair the detached part of the anti-oxidation coating on the surface of a carbon / carbon composite product. This process not only enhances the interface bonding strength between the coating and the substrate, but also can perform local repair of the coating on the surface of the substrate at any time; on the other hand, this process method has a short preparation cycle and has high work efficiency compared to traditional processes such as magnetron sputtering and high-temperature sintering coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for repairing a high-temperature anti-oxidation coating and belongs to the technical field of material preparation. Background Art

[0002] C / C composites are widely used as aerospace and aviation materials due to their excellent thermal and mechanical properties. However, they are easily oxidized in an aerobic environment above 450°C, which affects their application in high-temperature fields. Therefore, the overall anti-oxidation and anti-ablation properties of composite materials can be achieved through surface coating modification technology. However, the surface anti-oxidation coating may partially or completely fall off during repeated use, seriously affecting the further use of the product. Therefore, it is necessary to repair the fallen coating area.

[0003] At present, the main method of coating repair is to repair the peeled parts by brushing, and then put the whole product into a high-temperature treatment furnace for sintering. This method has a long production cycle and low repair efficiency. Summary of the invention

[0004] The purpose of the present invention is to address the deficiencies of the prior art and provide a method for repairing a high-temperature anti-oxidation coating. The high-temperature anti-oxidation coating in the present invention has the advantages of low porosity, high bonding strength and excellent high-temperature anti-oxidation ability; because the ternary layered MAX phase ceramics have the characteristics of both metals and ceramics, they exhibit excellent thermal conductivity, electrical conductivity, anti-oxidation performance, fracture energy absorption capacity, and radiation resistance, and the anti-oxidation coating can be repaired locally at any time by using an ultra-high-speed laser cladding method, which is easy to use and highly efficient.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: a method for repairing a high-temperature anti-oxidation coating, characterized in that the method comprises the following steps:

[0006] Step 1: Place the MAX phase powder in a ball mill and then dry it.

[0007] Step 2: Grind the area where the antioxidant coating on the surface of the carbon / carbon composite material product has fallen off until the surface roughness Ra is less than 3.2 μm.

[0008] Step 3: Place the MAX phase powder dried in step 1 into the powder feeding device of the ultra-high-speed laser cladding machine, place the part where the anti-oxidation coating on the surface of the carbon / carbon composite material product in step 2 has fallen off on the workbench of the ultra-high-speed laser cladding machine, and turn on the equipment switch to perform coating treatment to achieve the purpose of repairing the high-temperature anti-oxidation coating of the carbon / carbon composite material.

[0009] The above-mentioned method for repairing a high-temperature anti-oxidation coating is characterized in that, in step one, the MAX phase powder is one or any two of Ti2SiC, Ti3SiC2, Ti4SiC3, Zr2SiC, Zr3SiC2, Zr4SiC3, Zr2AlC, Zr3AlC2, and Zr4AlC3, the particle size after ball milling is 40μm-100μm, the drying temperature is 80℃-250℃, and the drying time is 2h-8h.

[0010] The above-mentioned method for repairing a high-temperature anti-oxidation coating is characterized in that, in step 2, the polishing is performed using emery paper.

[0011] The above-mentioned method for repairing a high-temperature anti-oxidation coating is characterized in that, in step three, the powder feeding device of the ultra-high-speed laser cladding machine adopts coaxial powder feeding and is protected by argon gas, the laser cladding power is 60W-300W, the cladding head moving speed is 3mm / s-18mm / s, and the overlap rate is 30%-50%.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] 1. Since ternary layered MAX phase ceramics have the characteristics of both metals and ceramics, they exhibit excellent properties such as good thermal conductivity, electrical conductivity, oxidation resistance, fracture energy absorption capacity, and radiation resistance.

[0014] 2. Ultra-high-speed laser cladding is used to prepare MAX phase coating on the surface of carbon / carbon composite materials. This process not only enhances the interfacial bonding strength between the coating and the substrate, but also enables local repair of the coating on the surface of the substrate at any time. On the other hand, this process method has a short preparation cycle and has high work efficiency compared to traditional magnetron sputtering, high-temperature sintering coating and other process methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a process flow chart of a method for repairing a high-temperature anti-oxidation coating. DETAILED DESCRIPTION

[0016] Example 1

[0017] Step 1: Use Ti2SiC powder as the main raw material.

[0018] Step 2: Place the Ti2SiC powder prepared in step 1 in a ball mill for ball milling, and the particle size after ball milling is 40 μm.

[0019] Step 3: Place the Ti2SiC powder after ball milling in step 2 in a drying oven for drying at a temperature of 80°C for 8 hours.

[0020] Step 4: Set the density to 1.4 g / cm3 The surface of the carbon / carbon composite crucible where the anti-oxidation coating has fallen off is polished with emery paper until the surface roughness Ra is less than 3.2 μm.

[0021] Step 5: Place the dried Ti2SiC powder in step 3 into the powder feeding device of the ultra-high-speed laser cladding machine, place the part of the carbon / carbon composite material surface anti-oxidation coating that has fallen off in step 4 on the workbench of the ultra-high-speed laser cladding machine, turn on the equipment switch for coating treatment, the powder feeding device of the ultra-high-speed laser cladding machine adopts coaxial powder feeding and is protected by argon, the laser cladding power is 60W, the cladding head moving speed is 3mm / s, and the overlap rate is 30%. The purpose of repairing the high-temperature anti-oxidation coating of the carbon / carbon composite crucible is achieved.

[0022] The properties of the prepared coating: the coating strength grade tested by the scratch method is ≥ grade 2, the coating has no defects such as cracks and bulges, and the coating thickness is 50 μm. The weight loss rate in an oxygen atmosphere at 1500°C for 1 hour is ≤1.5%.

[0023] Example 2

[0024] Step 1: Use Zr4SiC3 powder as the main raw material.

[0025] Step 2: Place the Zr4SiC3 powder prepared in step 1 in a ball mill for ball milling, and the particle size after ball milling is 60 μm.

[0026] Step 3: Place the Zr4SiC3 powder after ball milling in step 2 in a drying oven for drying at a temperature of 150°C for 6 hours.

[0027] Step 4: Use emery paper to polish the peeling part of the anti-oxidation coating on the surface of the carbon / carbon composite throat lining product with a density of 1.8g / cm3 until the surface roughness Ra is less than 3.2μm.

[0028] Step 5: Place the dried Zr4SiC3 powder in step 3 into the powder feeding device of the ultra-high-speed laser cladding machine, place the part of the carbon / carbon composite material surface anti-oxidation coating that has fallen off in step 4 on the workbench of the ultra-high-speed laser cladding machine, turn on the equipment switch for coating treatment, the powder feeding device of the ultra-high-speed laser cladding machine adopts coaxial powder feeding and is protected by argon, the laser cladding power is 160W, the cladding head moving speed is 10mm / s, and the overlap rate is 40%. The purpose of repairing the high-temperature anti-oxidation coating of the carbon / carbon composite material is achieved.

[0029] The properties of the prepared coating: the coating strength grade tested by the scratch method is ≥ Grade 2, the coating has no defects such as cracking and bulging, and the coating thickness is 80 μm. The weight loss rate in an oxygen atmosphere at 1500°C for 1 hour is ≤1.0%.

[0030] Example 3

[0031] Step 1: A mixture of Ti3SiC2 powder and Zr3AlC2 powder in a weight ratio of 1:1 is used as a main raw material.

[0032] Step 2: Place the mixed powder in step 1 in a ball mill for ball milling, and the particle size after ball milling is 100 μm.

[0033] Step 3: Place the mixed powder after ball milling in step 2 in a drying oven and dry it at a drying temperature of 250° C. for 2 h.

[0034] Step 4: Use emery paper to polish the peeling part of the anti-oxidation coating on the surface of the carbon / carbon composite throat lining product with a density of 1.75g / cm3 until the surface roughness Ra is less than 3.2μm.

[0035] Step 5: Place the dried mixed powder in step 3 into the powder feeding device of the ultra-high-speed laser cladding machine, place the part where the anti-oxidation coating on the surface of the carbon / carbon composite material in step 4 falls off on the workbench of the ultra-high-speed laser cladding machine, turn on the equipment switch for coating treatment, the powder feeding device of the ultra-high-speed laser cladding machine adopts coaxial powder feeding and is protected by argon gas, the laser cladding power is 300W, the moving speed of the cladding head is 18mm / s, and the overlap rate is 50%. The purpose of repairing the high-temperature anti-oxidation coating of the carbon / carbon composite material is achieved.

[0036] The properties of the prepared coating: the coating strength grade tested by the scratch method is ≥ grade 2, the coating has no defects such as cracking and bulging, and the coating thickness is 100 μm. The weight loss rate in an oxygen atmosphere at 1500°C for 1 hour is ≤1.2%.

[0037] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for repairing a high temperature anti-oxidation coating, characterized in that: The method comprises the following steps: Step 1: Place the MAX phase powder in a ball mill and then dry it; Step 2: Grind the fallen-off part of the anti-oxidation coating on the surface of the carbon / carbon composite material product until the surface roughness Ra is less than 3.2µm; Step 3: Place the dried MAX phase powder in step 1 into the powder feeding device of the ultra-high-speed laser cladding machine, place the part where the anti-oxidation coating on the surface of the carbon / carbon composite material product in step 2 has fallen off on the workbench of the ultra-high-speed laser cladding machine, and turn on the equipment switch to perform coating treatment, so as to achieve the purpose of repairing the high-temperature anti-oxidation coating of the carbon / carbon composite material; The MAX phase powder is one or any two of Ti2SiC, Ti4SiC3, Zr2SiC, Zr3SiC2, Zr4SiC3, Zr2AlC, Zr3AlC2, and Zr4AlC3, and the particle size after ball milling is 40 μm-100 μm, the drying temperature is 80°C-250°C, and the drying time is 2h-8h; In step three, the powder feeding device of the ultra-high-speed laser cladding machine adopts coaxial powder feeding and is protected by argon gas. The laser cladding power is 60W-300W, the moving speed of the cladding head is 3mm / s-18mm / s, and the overlap rate is 30%-50%.

2. A method for repairing a high temperature anti-oxidation coating according to claim 1, characterized in that: In step 2, the grinding is performed using emery paper.