Plant charcoal pigment and its liquid dispersion
By using a combination of biochar and a specific dispersant, high-quality black pigment dispersions were prepared, solving the problem that traditional methods are difficult to use to produce biochar pigment dispersions that meet standards, and achieving a pigment solution with high coloring strength and environmental friendliness.
Patent Information
- Application Number
- CN202080081471.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Existing technologies make it difficult to obtain high-quality black pigment dispersions from renewable sources, especially biochar-type materials, and traditional methods are insufficient to produce pigment dispersions that meet industry standards.
Using biochar as raw material, a black pigment dispersion with uniform submicron particles, spherical morphology and high coloring strength is prepared through specific dispersants and grinding processes. This includes using sodium lignosulfonate or modified acrylate copolymer as dispersants and reducing biochar particles to submicron size through wet milling.
It achieves high-quality black pigment dispersions with excellent blackness and tinting strength, meeting industry standards, and reduces the content of polycyclic aromatic hydrocarbons, providing an environmentally friendly and sustainable pigment solution.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
[0001] Related Applications
[0002] This application claims priority to currently pending provisional application serial number 62 / 907,411 filed on September 27, 2019. Background Art
[0003] Black pigments used in inks, paints, coatings, resins and printing pastes are primarily derived from petroleum. There remains a need to obtain high quality and comparable black pigments from renewable sources. For decades, pigment manufacturers have been trying to produce high quality pigment dispersions with charcoal-type materials and have been unsuccessful. Prior to working with the present applicant, major pigment manufacturers attempted to produce dispersions of carbonaceous particles derived from biochar. They were unsuccessful in producing a product that met industry standards. In fact, they said it was impossible. Other pigment manufacturers have also tried and claimed to obtain at best only weak tinting strength from charcoal-type materials. Compositions that meet the excellent standards of the industry and these manufacturers have been obtained using the chemistry and methods disclosed herein. Summary of the invention
[0004] The compositions and methods described herein relate to black pigments for coloring. More specifically, disclosed herein is a pigment dispersion formulation comprising carbonaceous particulate matter derived from biochar and a dispersant. In some embodiments, the biochar is wood biochar. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] The novel features of the present invention are particularly set forth in the appended claims. A better understanding of the features and advantages of the present invention will be obtained by referring to the following detailed description and the accompanying drawings, which set forth illustrative embodiments utilizing the principles of the present invention, wherein:
[0006] Figure 1A Shown is a scanning electron microscope image at 10,000 times magnification from the sputtering process showing a random sample of pigment particles that have been ground with a fluid and dried.
[0007] Figure 1B A scanning electron microscope image at 50,000x magnification from the sputtering process is shown showing a random sample of pigment particles that have been ground with a fluid and dried. Two representative particles are represented by the surrounding oval circles, with the particle in the upper right of the image having a diameter of 46.62 nm and the more numerous particles in the lower right of the image having a diameter of 40.80 nm.
[0008] Figure 2A Shown is a scanning electron microscope image at 10,000 times magnification from the sputtering process showing a random sample of pigment particles that have been ground with a fluid and dried.
[0009] Figure 2B A scanning electron microscope image at 50,000x magnification from the sputtering process is shown showing a random sample of pigment particles that have been ground with a fluid and dried. Two representative particles are represented by the surrounding oval circles, with the particle in the middle right of the image having a diameter of 53.45 nm and the more numerous particles in the lower right of the image having a diameter of 64.11 nm.
[0010] Figure 3 A scanning transmission electron microscopy image at 50,000 times magnification from a scanning transmission electron microscopy (STEM) process is shown showing a random sample of pigment particles wherein at least 95% of the particles by number, or at least 100 particles, are 15-25 nm in diameter.
[0011] Figure 4 A scanning transmission electron microscope image at 100,000 times magnification from a STEM process is shown showing a random sample of pigment particles wherein at least 95% of the particles by number, or at least 100 particles, are 15-25 nm in diameter.
[0012] Figure 5 A scanning transmission electron microscope image at 50,000 times magnification from a Lacey STEM process is shown showing a random sample of pigment particles wherein at least 95% of the particles by number, or at least 100 particles, are 15-25 nm in diameter.
[0013] Figure 5A is a scanning transmission electron microscope image at 50,000x magnification from the Lacey STEM process showing interconnected particles demonstrating a chain-like grape bunch-like morphology.
[0014] Figure 6 A scanning transmission electron microscope image at 100,000 times magnification from a Lacey STEM process is shown showing a random sample of pigment particles wherein at least 95% of the particles by number, or at least 100 particles, are 15-25 nm in diameter.
[0015] Figure 7-8 A scanning electron microscope image of a raw material of a particulate solid of plant char that can be used as a raw material for making submicron carbonaceous particles is shown.
[0016] Fig. 9A Shown is a scanning transmission electron microscope image of a prior art petroleum carbon black sample exhibiting a globular habit.
[0017] Figure 9B-9CShown is a scanning transmission electron microscope image of a prior art petroleum carbon black sample exhibiting clustering behavior.
[0018] Fig.10 Uncorrected Raman spectra of three random samples from Formulation 1 (Spectra 1-3) and three random samples from Formulation 2 (Spectra 4-6) are shown.
[0019] Fig.11 Baseline corrected Raman spectra of three random samples from Formulation 1 (Spectra 1-3) and three random samples from Formulation 2 (Spectra 4-6) are shown.
[0020] Fig.12 A graphical representation of the detected hues plotted in the CIE Lab color space is shown.
[0021] Figure 13-18 Shown are profiles of measurements performed using dynamic light scattering to assess the particle size distribution of Samples 1A-3B according to embodiments of the present disclosure.
[0022] Fig.19 Shown is a scanning transmission electron microscope image at 50,000X magnification from a Lacey STEM process showing biomass-derived pigment particles from a commercially available reference source not associated with the present applicants.
[0023] Figure 20-21 Some schematic diagrams showing the chain-like grape bunch-like morphology of pigment products according to the present disclosure.
[0024] Fig. 22 Shown is a scanning transmission electron microscope image at 100,000X magnification from a Lacey STEM process showing clusters of a reference commercial petroleum-derived carbon black.
[0025] Fig.23 Shown is a scanning transmission electron microscope image at 100,000x magnification from a Lacey STEM process showing biomass-derived pigment particles from a commercially available reference source.
[0026] Fig.24 shows the image at 30,000x magnification without electron transmission. Fig.23 of the image.
[0027] Fig.25 Shown is a scanning transmission electron microscope image at 30,000x magnification from the Lacey STEM process showing biomass-derived pigment particles from a commercially available reference source.
[0028] Fig.26 shows no electron transmission Fig.25 of the image.
[0029] Fig. 27 Shown is a scanning transmission electron microscope image from a Lacey STEM process showing particles from Formulation 11 disclosed herein.
[0030] Fig.28 Shown is a scanning transmission electron microscope image from the Lacey STEM process showing reference petroleum carbon black particles. DETAILED DESCRIPTION
[0031] As used herein, the term "about" refers to an amount that is close to 10%, 5%, or 1% of the stated amount, including increments therein. The term "about" refers to a value or range of values that follows the term. For example, "about 1-2" and "about 1 to 2" should be understood as "about 1 to about 2". Similarly, the term "between about 1 and 2" should be understood as "between about 1 and about 2".
[0032] Various embodiments may specify information about the weight of certain components (e.g., pigment particles or dispersants) and the weight of the total composition (e.g., dispersion) containing such components. In some cases, a subscript may be used to specify the part being referenced. For example, W P Can be used to refer to the weight of the particle, W D can be used to indicate the weight of the dispersant, and WT can be used to indicate the total weight of the composition. In some cases, fractions with subscript designations may be used, such as W P / W T , and the fractional value can be multiplied by 100 to express it as a weight percentage, such as "60% W P / W T ”. When the weight percentage of a component of a composition is expressed herein without explicit reference to an associated comparator, for example “[the specified component] is present at 10 wt %”, this means that the specified component is 10% of the total weight of the composition. Similarly, when the weight percentage of a chemical element or compound (such as ash content) in a specified component (such as a plant charcoal feedstock) is expressed without reference to an associated comparator, this means that the specified element or compound is present as a percentage of the total weight of the specified component.
[0033] Pigments have been used for artistic, functional, and decorative purposes for thousands of years, dating back to cave paintings and continuing to this day. The technology discussed in this article relates to pigments for black coloration. Black is a color whose perception is caused by the complete absence of light stimulating any of the three types of color-sensitive cones in the human eye and has a very low brightness compared to the surrounding environment. A true black visual stimulus is the absence of hues and grayscale. Black is the darkest color possible. Prehistoric painters often used charcoal from wood or animal bones, which was partially burned for gray or near-black coloration. In modern times, similar pigments are also prepared by partial combustion or pyrolysis of vegetable and fruit waste, bones, horns, and similar materials. Pyrolysis involves placing the material in a chamber and heating it in the presence of little or no oxygen. This article describes materials derived from recently living plants or animals, which are called "charcoal" or "biochar."
[0034] In contrast to carbon, petroleum carbon black is a pigment derived from petroleum or natural gas. Petroleum carbon black, also known as lamp black, pigment black, soot or black carbon, is used for black coloring. Petroleum carbon black is a fine particle carbon pigment obtained as soot from the incomplete combustion of many different types of products (such as natural gas or petroleum). Petroleum carbon black is usually a fine and soft black powder. It is very stable and is not affected by light, acids and alkalis. It is commonly used in printing inks, coating dyes and Chinese ink. Petroleum carbon black is used as a pigment in coatings, rubber, plastics, paints, carbon paper and crayons. Some other synonyms for petroleum carbon black pigment are channel black; lamp black; pigment black 6 or 7; CI 77266; gas black; diamond black; smoke black; soot black; flame black; furnace black; acetylene black; thermal black; graphite; carbon black; coal black; soot ink (Japan); hiilimusta (Finland); nero di carbone (Italy); The American Society for Testing and Materials (ASTM) has defined various standard petroleum carbon blacks. For example: ASTM D209-81 (2012) Standard Specification for Lamp Black Pigment; ASTM D210-05 (2011) Standard Specification for Bone Black Pigment; ASTM D561-82 (2014) Standard Specification for Carbon Black Pigment for Coatings; ASTM D769-01 (2012) Standard Specification for Black Synthetic Iron Oxide.
[0035] Black pigments can be prepared from charcoal or petroleum carbon black. Charcoal is a renewable source of pigments, which is a desirable property from an ecological and sustainable perspective. However, historical or modern implementations of charcoal do not typically provide pigments with properties comparable to the coloring properties provided by petroleum carbon black. Difficulties specific to charcoal include producing uniform submicron particles, producing dispersions, and producing spherical particles. This article describes a carbon pigment dispersion formulation with properties comparable to petroleum carbon black dispersion formulations that avoids the harmful aspects of the production and use of petroleum carbon black.
[0036] Polycyclic aromatic hydrocarbons (PAH) are a class of chemicals, some of which have been exposed to low levels for a long time and have caused cancer in laboratory animals. PAHs are naturally present in coal, crude oil and gasoline. They are also produced when coal, oil, natural gas, wood, garbage and tobacco are burned. Therefore, it is expected that PAHs will be present in biochar raw materials. It is also expected that PAHs present in biochar raw materials will be retained in pigment dispersion preparations including carbonaceous particulate matter derived from biochar. The most effective way to reduce the presence of PAH in such dispersions is to use biochar with a minimum PAH content. In some embodiments, polycyclic aromatic hydrocarbons are present in biochar raw materials (and may be present in carbonaceous particulate matter derived from such raw materials) at a concentration of less than about 50 mg / kg. In some embodiments, polycyclic aromatic hydrocarbons are present in biochar at a concentration of less than about 10 mg / kg or at an undetectable concentration. It is very unexpected that PAH concentrations are so low in the pyrolysis or thermal decomposition of carbohydrate materials such as biochar.
[0037] Pigment compositions derived from pigment dispersion preparations
[0038] The pigment composition described herein includes particles. Random samples of pigment particles are obtained by sampling from a substantially uniformly mixed liquid pigment dispersion. Particles can be characterized by particle number, size, size distribution, surface area, shape, surface texture or any combination thereof. The observed properties can vary with the measurement technique. Various techniques for measuring certain properties are described herein. For example, the average diameter of particle size is described herein with respect to various measurement techniques, and the measurement techniques include scanning electron microscope (SEM) imaging, scanning transmission electron microscopy (STEM) imaging, dynamic light scattering (DLS) and laser scattering (LS) or image analysis software such as ImageJ. The term "STEM" as used herein is a broad term, which refers to general scanning transmission electron microscopy as defined herein and microscopy using "Lacey STEM process" and microscopy using "STEM process".
[0039] Characterization
[0040] In some embodiments, a random sample of particles is measured. In some embodiments, the diameter of particles of carbonaceous materials derived from biochar is measured on a scanning transmission electron micrograph (STEM) two-dimensional micrograph with a magnification of at least 50,000 times. In some embodiments, particles are measured by spatial analysis on a two-dimensional micrograph with a magnification of at least 50,000 times from a Lacey STEM process. In some embodiments, a confidence interval is calculated for a 90% confidence level. In some embodiments, the confidence level is calculated at a 95% confidence level. In some embodiments, the confidence interval is calculated at a 97.5% confidence level. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter of less than about 1000nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter of less than about 900nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter of less than about 800nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter of less than about 700nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 600 nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 500 nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 400 nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 300 nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 200 nm. Disclosed herein are pigment compositions having particles derived from biochar, wherein at least about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 100 nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 50 nm. In some embodiments, about 80% of the particles by number, or at least 100 particles, have an average diameter of less than about 25 nm. In some embodiments, about 80% of the particles, or at least 100 particles, by number have an average diameter within the range between 1000 nm and 25 nm, including all ranges contained therein. In some embodiments, about 95% of the particles, or at least 100 particles, by number have an average diameter less than about 1000 nm. In some embodiments, about 95% of the particles, or at least 100 particles, by number have an average diameter less than about 900 nm. In some embodiments, about 95% of the particles, or at least 100 particles, by number have an average diameter less than about 800 nm. In some embodiments, about 95% of the particles, or at least 100 particles, by number have an average diameter less than about 700 nm.In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 600nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 500nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 400nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 300nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 200nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 50nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 50nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is less than about 25nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range of 15-25nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 0.1 nm and 1000 nm and all ranges contained therein. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 0.1 nm and 500 nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 1 nm and 300 nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 1 nm and 200 nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 1 nm and 100 nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 10 nm and 50 nm. In some embodiments, about 80% of the particles or at least 100 particles by number have an average diameter in the range between about 50 nm and 100 nm. In some embodiments, about 80% of the particles, or at least 100 particles, by number have an average diameter in the range between about 15 nm and 25 nm. In some embodiments, about 90% of the particles, or at least 100 particles, by number have an average diameter in the range between about 0.1 nm and 1000 nm, including all ranges subsumed therein. In some embodiments, about 90% of the particles, or at least 100 particles, by number have an average diameter in the range between about 0.1 nm and 500 nm. In some embodiments, about 90% of the particles, or at least 100 particles, by number have an average diameter in the range between about 1 nm and 300 nm.In some embodiments, the average diameter of about 90% of the particles or at least 100 particles by number is within the range of about 1 nm and 200 nm. In some embodiments, the average diameter of about 90% of the particles or at least 100 particles by number is within the range of about 1 nm and 100 nm. In some embodiments, the average diameter of about 90% of the particles or at least 100 particles by number is within the range of about 10 nm and 50 nm. In some embodiments, the average diameter of about 90% of the particles or at least 100 particles by number is within the range of about 50 nm and 100 nm. In some embodiments, the average diameter of about 90% of the particles or at least 100 particles by number is within the range of about 15 nm and 25 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is within the range of about 0.1 nm and 1000 nm, including all ranges contained therein. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is within the range of about 0.1 nm and 500 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range between about 1 nm and 300 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range between about 1 nm and 200 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range between about 1 nm and 100 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range between about 10 nm and 50 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range between about 50 nm and 100 nm. In some embodiments, the average diameter of about 95% of the particles or at least 100 particles by number is in the range between about 15 nm and 25 nm. In some embodiments, the average diameter of about 99.7% of the particles or at least 100 particles by number is in the range between about 0.1 nm and 1000 nm, including all ranges contained therein. In some embodiments, the average diameter of about 99.7% of the particles or at least 100 particles by number is in the range of about 0.1 nm and 500 nm. In some embodiments, the average diameter of about 99.7% of the particles or at least 100 particles by number is in the range of about 1 nm and 300 nm. In some embodiments, the average diameter of about 99.7% of the particles or at least 100 particles by number is in the range of about 1 nm and 200 nm. In some embodiments, the average diameter of about 99.7% of the particles or at least 100 particles by number is in the range of about 1 nm and 100 nm.In some embodiments, about 99.7% of the particles, or at least 100 particles, by number have an average diameter in the range between about 10 nm and 50 nm. In some embodiments, about 99.7% of the particles, or at least 100 particles, by number have an average diameter in the range between about 50 nm and 100 nm. In some embodiments, about 99.7% of the particles, or at least 100 particles, by number have an average diameter in the range between about 15 nm and 25 nm. In some embodiments, about 80% to about 99.7% of the particles, or at least 100 particles, by number have an average diameter in the range between about 0.1 nm and 1000 nm, including all ranges subsumed therein.
[0041] In some embodiments, a particle size distribution is obtained from a random sample. Once a random sample is obtained, the particle size is estimated and then the particle size distribution is described. Typically, the terms D10, D50, and D90 are used to describe the particle size distribution. The D10 diameter has 10% of smaller particles and 90% of larger particles. D50 is the median diameter, where 50% of the particles are larger and 50% are smaller. D90 defines the diameter where 90% of the distribution has a smaller particle size and 10% has a larger particle size. A three-point specification characterized by D10, D50, and D90 diameters is considered complete and suitable for most particulate materials. How these points are expressed can vary. Some specifications use a format where D10, D50, and D90 must not exceed (NMT) a specified size. For example: a particle size distribution can be described as D10 NMT 20μm; D50 NMT 80μm and D90 NMT 200μm. Although only one size is stated for each point, there is an implied range of acceptable sizes (i.e., D50 passes if between 20 μm and 80 μm). Alternatively, a range of values may be explicitly stated. For example: D10 10-20 μm; D50 70-80 μm; and D90 180-200 μm.
[0042] In some embodiments, error bands are included. The term "total error band" is used herein to specify all sources including sampling and sample preparation calculated at a 95% confidence level. An example is D50 NMT 100 μm, where the total error band is + / -5% in size. Other statistics are sometimes used to describe particle size distribution. The most common calculations are standard deviation and variance. Standard Deviation (St Dev.). The standard deviation specification defines a diameter where approximately 68.27% of the total population is within + / -1 standard deviation and 95.45% is within + / -2 standard deviations.
[0043] In some embodiments, the particle size distribution is determined by laser scattering measurement. Disclosed herein is a pigment composition having particles derived from biochar, wherein the D90 particle size as determined by laser scattering measurement is equal to or less than about 1 micron. In some embodiments, the D90 particle size as determined by laser scattering measurement is from about 100 nm to about 1 micron. In some embodiments, the D90 particle size is equal to or less than about 950 nm. In some embodiments, the D90 particle size is equal to or less than about 900 nm. In some embodiments, the D90 particle size is equal to or less than about 800 nm. In some embodiments, the D90 particle size is equal to or less than about 700 nm. In some embodiments, the D90 particle size is equal to or less than about 600 nm. In some embodiments, the D90 particle size is equal to or less than about 500 nm. In some embodiments, the D90 particle size is equal to or less than about 400 nm. In some embodiments, the D90 particle size is equal to or less than about 300 nm. In some embodiments, the D90 particle size is equal to or less than about 200 nm. In some embodiments, the D90 particle size is equal to or less than about 100 nm. In some embodiments, the D90 particle size is equal to or less than about 50nm. In some embodiments, the D90 particle size is equal to or less than about 25nm. In some embodiments, the D90 particle size is about 500nm to 1 micron. In some embodiments, the D90 particle size is about 400nm to 1 micron. In some embodiments, the D90 particle size is about 300nm to 900nm. In some embodiments, the D90 particle size is about 200nm to 800nm. In some embodiments, the D90 particle size is about 300nm to 500nm. In some embodiments, the D90 particle size is about 400nm to 800nm. In some embodiments, the D90 particle size is about 1nm to about 1,000nm. In some embodiments, the D90 particle size is at least about 1nm. In some embodiments, the D90 particle size is about 1nm to about 1,000nm, including all ranges contained therein. In some embodiments, the D50 particle size is about 100nm to 900nm, including all ranges contained therein.
[0044] Uniformity of pigment particle size is important because it stabilizes the fluid flow characteristics of inks, paints, coatings, resins and printing pastes, and because uniformity is important to the consistency and quality of the pigment's tinting and tinting strength properties. In many applications, it is desirable to have a particle size distribution that is characterized as "monodisperse" or nearly monodisperse. A monodisperse distribution is one in which all particles have essentially the same size. When dynamic light scattering (DLS) is used to estimate size distribution, the variation in particle size is often expressed as the polydispersity index (PDI), which is calculated as (standard deviation / mean) 2. For nanoparticles, it is generally understood that when the PDI is below 0.05, the distribution is "monodisperse". In some embodiments of the pigment compositions disclosed herein that include particles derived from biochar, the PDI value is between 0.1 and 0.2. Although this uniformity does not strictly represent a monodisperse nanoparticle distribution, it represents sufficient particle size uniformity to be characterized as near monodisperse and meet the requirements of many inks, paints, coatings, resins, and printing pastes. Other analytical techniques can be used to assess the monodisperse nature of the particles. For example, images from a scanning transmission electron microscope can be analyzed by various means including image analysis software such as ImageJ to estimate the variation in particle size and assess their monodisperse characteristics.
[0045] STEM images acquired using the Lacey STEM protocol can be used to estimate changes in the particle size and spherical properties of random samples of particles. The prescribed method for particle size estimation of the embodiments disclosed in the STEM images herein is called a "geometric protocol," which can be used to estimate the diameter of particles in the image. A particle with a roundness value of 1.0 represents a perfect circle. As the value approaches 0.0, it represents increasingly long polygons. Since the particles are at rest and in random orientations, roundness measurements accurately indicate the degree of sphericity of the particles. An example of image analysis software that can be used for this purpose is the "ImageJ" software available from the National Institutes of Health (https: / / imagej.nih.gov / ij / ). The following steps constitute a geometric protocol:
[0046] a. Using the Lacey STEM protocol, an image of a random sample of a dispersion of carbonaceous particles derived from biochar was acquired.
[0047] b. Measure the diameter of at least 100 particles in the image using ImageJ or equivalent software.
[0048] c. Measure the circularity of at least 100 particles in the image using ImageJ or equivalent software.
[0049] d. Calculate the average diameter of the at least 100 particles using statistical software.
[0050] e. Calculate the standard deviation of the average diameter of the at least 100 particles using statistical software.
[0051] f. Calculate the average roundness of the at least 100 particles using statistical software.
[0052] g. Calculate the standard deviation of the average roundness of the at least 100 particles using statistical software.
[0053] A sample of pigment particles in a dispersion formulation including a carbonaceous particulate material derived from biochar as disclosed herein was evaluated according to a geometric scheme. Fig. 27 The results are as follows:
[0054] Biochar samples Average diameter of 100 particles (μm) 0.0586087 The standard deviation of the diameters of the 100 particles 0.0103 The average roundness of at least 100 particles 0.824 Standard deviation as a percentage of the mean diameter 17.6% The standard deviation of the average circularity of the 100 particles 0.2387087 Standard deviation expressed as a percentage of mean circularity 28.97%
[0055] For comparison, a commercial petroleum-derived carbon black sample was tested using the geometry scheme. Fig.28 The results are as follows:
[0056] PCB Samples Average diameter of 100 particles (μm) 0.0253 The standard deviation of the diameters of the 100 particles 0.0193 Standard deviation as a percentage of the mean diameter 76.3% The average roundness of at least 100 particles 0.630 The standard deviation of the average circularity of the 100 particles 0.2529455 Standard deviation expressed as a percentage of mean circularity 40.1%
[0057] Surprisingly, the average diameter of the particles in the dispersion formulations including the carbonaceous particulate matter derived from biochar as disclosed herein is only slightly larger than the average diameter of the particles in commercial petroleum-derived carbon black. Even more surprisingly, the particles from the dispersion formulations including the carbonaceous particulate matter derived from biochar as disclosed herein are more spherical than the particles in commercial petroleum-derived carbon black.
[0058] In some embodiments, the particle size distribution is determined by dynamic light scattering measurement based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard. In some embodiments, 80% of the particles have a size less than 1 micron. In some embodiments, 90% of the particles have a size less than 1 micron. In some embodiments, 95% of the particles have a size less than 1 micron. In some embodiments, 99% of the particles have a size less than 1 micron. In some embodiments, 99.9% of the particles have a size less than 1 micron. Disclosed herein is a pigment composition having particles derived from biochar, wherein the particle size distribution has a maximum intensity of less than about 500 nm, as determined by dynamic light scattering measurement. In some embodiments, the particle size distribution has a maximum intensity of less than about 400 nm. In some embodiments, the particle size distribution has a maximum intensity of less than about 300 nm. In some embodiments, the particle size distribution has a maximum intensity of less than about 200 nm. In some embodiments, the particle size distribution has a maximum intensity of less than about 100 nm. In some embodiments, the particle size distribution has a maximum intensity of less than about 50 nm. In some embodiments, the particle size distribution has a maximum intensity of less than about 20 nm. In some embodiments, the particle size distribution has a maximum intensity between about 0.01-1000 nm, including all ranges subsumed therein. In some embodiments, the particle size distribution has a maximum intensity between about 165-171 nm.
[0059] As a practical matter, any statement of the size distribution of a given particle is an estimate. One consideration in specifying a particle size distribution is an estimate of the variation in particle size. One way the variation can be expressed is in terms of standard deviation (the "sigma" statistic) or equivalent percentage. One standard deviation or one sigma, plotted above or below the mean, includes 68% of all data points. Two sigma includes 95%, and three sigma includes 99.7%. Another way to express the variation is in terms of the percentage of particles below a certain size. For example, a D90 value of 900 nm means that 90% of the particles are estimated to be 900 nm or smaller.
[0060] Another consideration when specifying particle size parameters involves statements about the accuracy and reliability of the reported parameters. Typically, the precision of a parameter is reported in terms of "about" the specified value. Often, the reliability of a parameter is reported in terms of a confidence level, such as "95% confidence level." The science of particle size characterization is well developed, and particle size parameters cited herein will be interpreted accordingly.
[0061] In some embodiments, the particles are characterized by Raman measurements with a 1800 gr / mm grating under laser excitation at a wavelength of 514.5 nm. In some embodiments, the particles exhibit a Raman spectrum with a G position between about 1590 (cm-1) and about 1605 (cm-1) and an I(D) / I(G) ratio between about 2.54 and about 3.02. In some embodiments, the particles exhibit a Raman spectrum with a G position between about 1580 (cm-1) and about 1605 (cm-1) and an I(D) / I(G) ratio between about 2.49 and about 3.07.
[0062] In some embodiments, the surface area of the particles is determined by static pressure gas adsorption, also known as specific surface area analysis by gas physical adsorption (static volume method). In some embodiments, the surface area of the particles is greater than or equal to about 100 m 2 In some embodiments, the surface area of the particles is greater than or equal to about 200 m 2 In some embodiments, the surface area of the particles is greater than or equal to about 300 m 2 In some embodiments, the surface area of the particles is greater than or equal to about 350 m 2 In some embodiments, the surface area of the particles is about 100 m 2 g-1 to about 1000m 2 g-1, including all ranges contained therein.
[0063] The biochar feedstock includes carbon, and in some embodiments, the carbon content in the biochar feedstock is in the range of about 55% to about 80%, including all ranges subsumed therein. In some embodiments, the carbon content is in the range of about 80% to about 95%, including all ranges subsumed therein. In some embodiments, the carbon content is greater than or equal to about 95%. In some embodiments, the carbon content is greater than or equal to about 95%.
[0064] In some embodiments, the pigment dispersion formulation has no more than about 75% by weight of carbonaceous biochar particles, and no more than about 40% by weight of dispersant, and no more than about 20% by weight of optional anticoagulant, and no more than about 5% by weight of optional defoamer, and no more than about 5% by weight of optional preservative or biocide. In some embodiments, the biochar particles are no more than about 70% by weight. In some embodiments, the biochar particles are no more than about 65% by weight. In some embodiments, the biochar particles are no more than about 55% by weight. In some embodiments, the biochar particles are no more than about 50% by weight. In some embodiments, the biochar is no more than about 45% by weight. In some embodiments, the biochar is no more than about 40% by weight. In some embodiments, the biochar is no more than about 30% by weight. In some embodiments, the biochar is no more than about 25% by weight. In some embodiments, the dispersant is no more than about 35% by weight. In some embodiments, the dispersant is no more than about 30% by weight. In some embodiments, the dispersant is no more than about 25% by weight. In some embodiments, the dispersant is no more than about 20% by weight. In some embodiments, the dispersant is no more than about 15% by weight. In some embodiments, the dispersant is no more than about 10 weight percent. In some embodiments, the dispersant is no more than about 5 weight percent. In some embodiments, the anticoagulant is no more than about 20 weight percent. In some embodiments, the anticoagulant is no more than about 15 weight percent. In some embodiments, the anticoagulant is no more than about 10 weight percent. In some embodiments, the anticoagulant is no more than about 5 weight percent. In some embodiments, the defoamer is no more than about 2.5 weight percent. In some embodiments, the defoamer is no more than about 1.0 weight percent. In some embodiments, the composition is used as a coloring ink. A dispersion is disclosed herein, which includes the biochar pigment of any one of the above embodiments. In some embodiments, the biochar raw material carbon content is greater than or equal to about 70%. In some embodiments, the biochar raw material carbon content is in the range of about 70% to about 99.9%, including all ranges contained therein.
[0065] In some embodiments, the char is biochar and includes ash. Ash is any material that is not pure carbon. In some embodiments, the ash is a mixture of calcium, magnesium, potassium or phosphorus and their compounds. In some embodiments, the ash content is less than or equal to about 30%. In some embodiments, the ash content is less than or equal to about 25%, or less than or equal to about 20%, or less than or equal to about 15%, or less than or equal to about 10%, or less than or equal to about 9%, or less than or equal to about 8%, or less than or equal to about 7%, or less than or equal to about 6%, or less than or equal to about 5%, or less than or equal to about 4%, or less than or equal to about 3%. Or less than or equal to about 2%, or less than or equal to about 1%, or less than or equal to about 0.1%. In some embodiments, the ash content is about 1% to about 30%. In some embodiments, the ash content is at most about 30%. In some embodiments, the ash content is from about 1% to about 3%, or from about 1% to about 5%, or from about 1% to about 10%, or from about 1% to about 15%, or from about 1% to about 20%, or greater than 20%.
[0066] Characteristics of Black Pigment Dispersions
[0067] Pigments are typically manufactured as dispersions, "pigment dispersions," which are essentially concentrated forms of liquid colorants in water, solvents, UV curable liquids or oils, which are subsequently diluted by manufacturers of inks, paints, printing pastes, coatings, resins and other coloring media that use the pigments.
[0068] "Dispersion formulations" are disclosed herein. In various embodiments, dispersion formulations can be used in a mill to reduce particles derived from biochar in a homogeneous mixture from a size of a few microns or larger to a smaller size, even a submicron size. In various embodiments, the dispersion formulation is discharged from the mill and then prepared for use as a pigment dispersion. Dispersion formulations may include a grinding fluid. The grinding fluid is typically advantageous in a grinding operation to produce small (e.g., submicron) particle sizes, and at least a portion of the grinding fluid is retained when the dispersion formulation is discharged from the mill for use as a pigment dispersion. The grinding fluid can be water, a solvent, a carrier / activator, or an oil. Dispersion formulations typically include a dispersant. Among other functions, a dispersant can improve the grinding process.
[0069] The unexpected characterization of some embodiments of the dispersion formulations disclosed herein is excellent jetness [My] and excellent jetness [Mc], as well as excellent tinting strength [T]. Jetness My is a measure of jetness, directly related to reflectivity. Taking into account the exact base color or hue of the black pigment, the color-related jetness value Mc is different from My. The higher the values of My and Mc, the greater the perceived jetness or blackness. Jetness My and jetness Mc values exceeding 250 are generally considered to exhibit high jetness (blackness) and jetness (jetness). It is expected that the pigment derived from biochar will be similar to charcoal, which is dark gray rather than black, with expected jetness My and jetness Mc values below 200. Unexpectedly, some embodiments of the pigment dispersions disclosed herein exhibit jetness My and jetness Mc values of 300 or more.
[0070] Tinting strength (T) is another quality factor of the pigment. For black pigments, tinting strength is its efficiency in reducing reflectivity when mixed with white pigments. Tinting strength (T) is a measure of relative reflectivity when the pigment content in the printing paste formula is reduced. In some embodiments, tinting strength (T) is greater than or equal to about 75%. In some embodiments, tinting strength (T) is greater than or equal to about 80%. In some embodiments, tinting strength (T) is greater than or equal to about 85%. In some embodiments, tinting strength (T) is greater than or equal to about 90%. In some embodiments, tinting strength (T) is greater than or equal to about 91%. In some embodiments, tinting strength (T) is greater than or equal to about 92%. In some embodiments, tinting strength (T) is greater than or equal to about 93%. In some embodiments, tinting strength (T) is greater than or equal to about 94%. In some embodiments, tinting strength (T) is greater than or equal to about 95%. In some embodiments, tinting strength (T) is greater than or equal to about 96%. In some embodiments, tinting strength (T) is greater than or equal to about 97%. In some embodiments, tinting strength (T) is greater than or equal to about 98%. In some embodiments, tinting strength (T) is greater than or equal to about 99%. In some embodiments, the tint strength (T) is from about 80% to about 99%. In some embodiments, the tint strength (T) is at least about 80%.
[0071] Samples of the embodiments of the pigment dispersion formulations disclosed herein for use including carbonaceous particulate matter derived from biochar were tested for tint strength (T) according to the following "Tin Strength Protocol".
[0072] The test is carried out according to ASTM D-2066-"Test Method for Relative Tinting Strength of Paste-Type Printing Ink Dispersion", as follows:
[0073] The standard dispersion and the unknown dispersion were each brought down to the same concentration in a suitable color base as follows:
[0074] 975g standard printing base formula
[0075] 25g pigment dispersion
[0076] Standards are made with equivalent grade of carbon black pigment.
[0077] Drawing was done on bleached 100% cotton fabric using a No. 7 Meyer rod; drying at 105°C for 1 minute; curing at 150°C for 5 minutes. The reduction in tinting strength of the shade was evaluated by Test Method B - Instrumental Evaluation:
[0078] Reflectance Measurement Instrument: Spectrophotometer with hemispherical (integrating sphere) geometry in accordance with Test Method E1331
[0079] The tinting strength of unknown dispersions was calculated according to the Kubelka-Munk equation.
[0080] Compared to the standard, the embodiments disclosed herein record tinting strength (T) values of 94% to 99%. Tinting strength T values of more than 90% are considered excellent and unexpected for pigments made from biochar. It should be noted that the test according to ASTM D-2066 is carried out with a dispersion reduced to a finished ink formulation. Among other chemicals or additives, the finished ink formulation contains a pigment dispersion for printing, coating or painting applications. In these embodiments, only one-tenth of the pigment dispersion is required to achieve the same coloring in the finished ink formulation compared to commercially available pigments made from biomass. As an example, a finished ink formulation made from biochar commercially available from a competitive source has a pigment loading of 20%. In contrast, the finished ink formulation made from the embodiments disclosed herein achieves significantly higher blackness (My) and blackness (Mc) values at only 2% pigment loading.
[0081] Colour fastness is a characteristic of materials that have been coloured with pigments. One industry standard is the International Standard ISO 105 - Textiles - Tests for colour fastness. Of particular interest is Part B02: "Colour fastness to artificial light: Xenon arc fading lamp test". This part of ISO 105 specifies a method for determining the effect of an artificial light source (D65) representative of natural daylight on the colour of textiles of all kinds and in all forms. ISO standard 105 Part B02 is the basis for testing colour fastness according to the following "UV protocol":
[0082] Light source: As specified in ISO 105B02
[0083] Standard: Blue Wool
[0084] Equipment setup: Exposure cycle A1:
[0085] Humidity: Normal
[0086] Climate conditions repeat: Temperate
[0087] Black standard temperature: (47±3)℃
[0088] Blackboard temperature: (47±3)℃
[0089] Sample: 100% cotton dyed strips
[0090] Exposure time: 100h
[0091] The rating scale from ISO standard section 105B02 ranges from 1 (very low lightfastness) to 8 (very high lightfastness), with each higher number being quoted about twice as fast as the previous number. Five specimens dyed with the pigment dispersion formulation disclosed herein were tested according to the UV protocol. Four samples were rated 8, which is equivalent to the commercial petroleum carbon black test sample. One sample of the examples disclosed herein was rated between 5 and 6. Unexpectedly, a pigment derived from biochar would achieve a score of 8.
[0092] Several standardized tests can be used to assess how black a pigment is. Jetness (My) is a measure of blackness and is directly related to reflectivity. For the best black, typical reflectivity values are usually below 5%, and can be below 1%. In some embodiments, the Jetness is greater than or equal to about 200. In some embodiments, the Jetness is greater than or equal to about 250. In some embodiments, the Jetness is greater than or equal to about 350.
[0093] Blackness (Mc) is a complex function of surface area, primary particle size and dispersion. Black pigments with smaller primary particle sizes tend to impart higher blackness than black pigments with larger primary particle sizes. In some embodiments, the blackness is greater than or equal to about 200. In some embodiments, the blackness is greater than or equal to about 260. In some embodiments, the blackness is greater than or equal to about 350.
[0094] Background color (dM) quantifies the neutrality of the black pigment plus binder. Background color is calculated as dM=Mc-My. If dM<0, the background color is brownish red. A dM value=0 would indicate that the black is completely achromatic or neutral. If dM>0, the black exhibits a generally preferred light blue background color. In some embodiments, the background color is greater than 0.
[0095] In some embodiments, the blackness (My) is greater than or equal to about 50. In some embodiments, the blackness (My) is greater than or equal to about 100. In some embodiments, the blackness (My) is greater than or equal to about 150. In some embodiments, the blackness (My) is greater than or equal to about 200. In some embodiments, the blackness (My) is greater than or equal to about 250. In some embodiments, the blackness (My) is greater than or equal to about 300. In some embodiments, the blackness (My) is greater than or equal to about 350. In some embodiments, the blackness (My) is greater than or equal to about 400. In some embodiments, the blackness (My) is from about 50 to about 400.
[0096] In some embodiments, the blackness (Mc) is greater than or equal to about 50. In some embodiments, the blackness (Mc) is greater than or equal to about 100. In some embodiments, the blackness (Mc) is greater than or equal to about 150. In some embodiments, the blackness (Mc) is greater than or equal to about 200. In some embodiments, the blackness (Mc) is greater than or equal to about 250. In some embodiments, the blackness (Mc) is greater than or equal to about 300. In some embodiments, the blackness (Mc) is greater than or equal to about 315. In some embodiments, the blackness (Mc) is greater than or equal to about 350. In some embodiments, the blackness (Mc) is greater than or equal to about 400.
[0097]
[00136] Samples of embodiments of pigment dispersion formulations disclosed herein for use including carbonaceous particulate matter derived from biochar were tested for blackness (My) and blackness (Mc) according to the following "Black Protocol".
[0098] Tested using a Hunber LabScanXE instrument or equivalent 45 / 0 geometry instrument with a black glass tile as a black reference
[0099] Create the following setup:
[0100] XYZ color space D65 light source
[0101] 10 degree observer 45 / 0 geometry
[0102] 1.2" port size
[0103] The samples were tested as is in a polystyrene (PS) petri dish as sample container / window. Where the sample had sufficient viscosity to maintain a large enough gap on the petri dish surface to keep the sample opaque and in place between the windows. In the case where the sample did not have the required viscosity, an "O" ring spacer was used to maintain a fixed sealed gap that held the sample and provided sufficient sample path length for opacity.
[0104] The following results in the table below were obtained for the 5 composition examples disclosed herein (identified by "ID"). Note that composition 2019-006343-01 was tested twice.
[0105]
[0106] In some embodiments, the background color (dM) is greater than 0. In some embodiments, the background color (dM) is 0.
[0107] An alternative method of evaluating black pigments is to utilize the CIELAB color space (also known as CIE L*a*b* or sometimes simply "Lab" color space), which is a color space defined by the International Commission on Illumination (CIE) in 1976. It represents color as three values: L* represents lightness from black (0) to white (100), a* represents from green (-) to red (+), and b* represents from blue (-) to yellow (+). CIELAB is designed so that the same amount of numerical change in these values corresponds to approximately the same amount of visual perception change. dL* (ΔL*) represents the lightness / darkness difference or shade of gray (black / white). These values represent the hue (color) in a black pigment sample. A perfect black sample reflects no hue and absorbs all wavelengths of light.
[0108] In some embodiments, the black pigments described herein have an L* value read relative to a TiO2 reference blank suspension having an L* value of 84.99. In some embodiments, the L* value is about 30 to about 75. In some embodiments, the L* value is at least about 30. In some embodiments, the L* value is at most about 75. In some embodiments, the L* value is about 30 to about 35. The black pigments described herein have an a* value read relative to a TiO2 reference blank suspension having an a* value of -0.16. In some embodiments, the a* value is about -0.47 to about -0.2. In some embodiments, the a* value is at least about -0.47. In some embodiments, the a* value is at most about -0.2. The black pigments described herein have a b* value read relative to a TiO2 reference blank suspension having a b* value of +0.69. In some embodiments, the b* value is about 0.1 to about 1.5. In some embodiments, the b* value is at least about 0.1. In some embodiments, the b* value is at most about 1.5. The black pigments described herein have a dL* value read relative to a TiO2 reference blank suspension having a dL* value of 84.99. In some embodiments, the dL* value is about -50 to about -15. In some embodiments, the dL* value is about -50 or less (more negative values). In some embodiments, the dL* value is about -15 or more (less negative values).
[0109] In some embodiments of the technology disclosed herein, a random sample of the pigment particles in the liquid dispersion is further characterized as having L* values in a range between 48.0 and 58.0, as read relative to a TiO2 reference blank suspension having an L* value of 84.99, and having a* values in a range between -0.23 and -0.42, as read relative to a TiO2 reference blank suspension having an a* value of -0.16, and having b* values in a range between 0.15 and 1.25, as read relative to a TiO2 reference blank suspension having a b* value of 0.69, and having dL* values in a range between -26 and -37, as read relative to a TiO2 reference blank suspension having a dL* value of 84.99, when tested according to the black pigment color analysis test described herein.
[0110] In some embodiments of the technology disclosed herein, a random sample of the pigment particles in the liquid dispersion is further characterized as having L* values in the range between 40.0 and 65.0, as read relative to a TiO2 reference blank suspension having an L* value of 84.99 and having a* values in the range between -0.15 and -0.50, as read relative to a TiO2 reference blank suspension having an a* value of -0.16 and having b* values in the range between 0.1 and 1.5, as read relative to a TiO2 reference blank suspension having a b* value of 0.69 and having dL* values in the range between -20 and -45, as read relative to a TiO2 reference blank suspension having a dL* value of 84.99, when tested according to the black pigment color analysis test described herein.
[0111] In some embodiments, the dispersion evenly distributes individual pigment particles throughout the liquid medium for a period of time. In some embodiments, the dispersion has no settled pigment particles at the bottom of the container or no phase separation between the components of the dispersion. In some embodiments, phase separation occurs when water or solvent separates from the dispersion. In some embodiments, the dispersion maintains its density over a period of time and does not change or deform in consistency. For example, in some embodiments, the dispersion does not gel after a period of time. In some embodiments, the pigment dispersion increases color strength, produces higher color fastness, has low or high opacity and has other performance characteristics.
[0112] A specific type of material referred to as a "pigment dispersion preparation" is disclosed herein. When referring to the technology disclosed herein, the terms "pigment dispersion" and "dispersion" refer to the pigment dispersion preparation. During the wet grinding process, a mechanical mill is loaded with media (usually beads or spheres), and in the embodiments disclosed herein, is also loaded with biochar feedstock and chemicals, such as a grinding fluid or carrier / activator for facilitating the grinding of biochar into submicron carbonaceous particles. The mill has a high-speed rotating agitator shaft. As the agitator rotates, it transfers kinetic energy to the media. The charge of biochar feedstock and chemicals is pumped through the mill at a process flow rate. The energy from the medium acts on the biochar solids suspended in the liquid (slurry) to tear (shear) or crush it, reducing it to a tiny size. The particles are simultaneously dispersed in the liquid to form a dispersion preparation. The components of the dispersion preparation are homogenized in the mill.
[0113] In various embodiments, the dispersion formulation can be used as a grinding base in a mill to reduce its biochar-derived particles from a size of a few microns or larger to smaller sizes, even submicron sizes. These results are unexpected because conventional wet and dry milling processes and chemistries are stable, in which particle size is never reduced to any practical extent below a few microns in diameter. Additional milling time only serves to increase the viscosity of the mixture, which ultimately forces termination of the process. The inclusion of microfibrillated cellulose in the grinding base may be part of the reason for this success.
[0114] In various embodiments, when the grinding process is complete, the dispersion preparation is discharged from the mill and is then ready for use as a pigment dispersion. The microfibrillated cellulose helps keep the pigment particles suspended. In some embodiments, the dispersion preparation can be dried and the resulting micro-sized particles used in other products.
[0115] In some embodiments, the composition includes a dispersant. In some embodiments of the technology disclosed herein, the dispersion includes about 15-60% W P / W T Pigment particles and about 15-60% W D / W T dispersants such as sodium lignin sulfonate or lignin sulfonic acid dispersants or unstructured or structured acrylic polymer or copolymer dispersants or unstructured or structured acrylate polymer or copolymer dispersants or hydroxyl functional carboxylate dispersants or styrene maleic anhydride dispersants, wherein W P is the weight of the pigment particles, and W D is the weight of the dispersant, and W T is the total weight of the dispersion, and the fraction is expressed as a percentage. In some embodiments, the dispersion is about 20-60% W P / W T Pigment particles and about 15-55% WD / W T In some embodiments, the dispersion is about 25-55% W P / W T Pigment particles and about 15-50% W D / W T In some embodiments, the dispersion is about 30-50% W P / W T Pigment particles and about 15-45% W D / W T In some embodiments, the dispersion is about 30-50% W P / W T Pigment particles and about 15-40% W D / W T In some embodiments, the dispersion is about 20-50% W P / W T Pigment particles and about 20-50% W D / W T In some embodiments, the dispersion is about 20-55% W P / W T Pigment particles and about 25-45% W D / W T of dispersant.
[0116] In some embodiments of the technology disclosed herein, the dispersion includes pigment particles and a dispersant including a modified acrylic acid or acrylate copolymer having a pigment affinity group. In some embodiments, the dispersion also includes a dispersion including a hydroxyl-functional carboxylic acid ester having a pigment affinity group.
[0117] In some embodiments of the technology disclosed herein, a dispersion includes pigment particles and sodium lignin sulfonate or a sodium lignin sulfonate salt-based dispersant and a hydroxy-functional carboxylic acid ester having a pigment-affinic group.
[0118] In some embodiments, the dispersant may include commercial products sold or produced under the trade names EFKA, Dispex, Dispers, METOLAT, ZETASPERSE, DISPERBYK, BYKJET, E-SPERSE, Solsperse, Solplus, JEFFSPERSE, K-SPERSE, DISPARLON, DISPERSOGEN, AJISPER, LUCRAMUL, or any combination thereof. In some embodiments, the dispersant may include any dispersant sold or produced in BASF's EFKAPX line, EFKA FA line, EFKAPU line, EFKA PA line, DispexUltra PA line, Dispex Ultra FA line, Dispex Ultra PX line, Dispex AA line, Dispex CX line, or any combination thereof. In some embodiments, the dispersant may include TEGO Dispers 745W, TEGO Dispers 750W, TEGO Dispers 760W, METOLAT 392 (MUNZING), BYKJET 9170 (BYK), BYKJET 9151 (BYK), BYKJET 9152 (BYK), BYK-9076, BYK-9077, or any combination thereof. In some embodiments, the dispersant may include any dispersant sold or produced by BASF, TEGO, EVONIK, MUNZING, BYK, Ethox, Lubrizol, Huntsman, King Industries, Clariant, Ajinomotofine Technologies, Silok, Levaco, or any combination thereof.
[0119] In some embodiments, the dispersant may include a high molecular weight dispersant and may include a low molecular weight dispersant. In some embodiments, the dispersant may include an acrylic dispersant, an acrylate, an acrylic acid, an acrylic acid, a carboxylic acid dispersant, a carboxylic acid, a polymer dispersant, a polyacrylic acid and a copolymer dispersant, a polyacrylic acid, a polycarboxylic acid copolymer, a polycarboxylic acid, a hydrophobic polycarboxylic acid copolymer, a polyacrylate, a sodium polyacrylate, a potassium polyacrylate, an ammonium salt amphiphile, a phosphate with a sodium cationic polyacrylate, an ammonium salt of a polycarboxylic acid, a polyphosphate, a polyelectrolyte, a polyurethane, a star dispersant, a comb-branched copolymer dispersant, a block copolymer, a block copolymer based on controlled free radical polymerization (CFRP) or CRP), quaternary ammonium salts, high molar volume (HMV) dispersants, styrene / maleic anhydride copolymer dispersants, sodium salts of styrene / maleic anhydride, tertiary amines, alkanol-amines, synthetic esters, ammonium naphthalenesulfonate dispersants, ethoxylated linear fatty alcohols, ethoxylated fatty acid esters, sorbitan monolaurate, Tween 20, Tween 80, stearic acid, oleic acid, diglycerides, saponified vegetable oils, ether alcohols, alkyl ammonium salts of high molecular weight polymers, pine distillates, kraft lignin, amphiphilic block copolymers, acrylate diblock copolymers, phosphonate polymer dispersants, neutralized phosphonate polymers dispersants, aromatic polyglycol ether phosphates, anionic polyether sulfates, aliphatic polycarboxylic acid amine salts, modified polymers containing carboxylic acids, polycarboxylates, preparations of polar acid esters and high molecular weight alcohols, polar acid esters, high molecular weight alcohols, polyaminoamides, polyethers, nitrogen grafted polymers, fatty acid calcium, polyolefins, naphthylic acid, naphthalenesulfonic acid, polymers with formaldehyde, surface functionalized dispersants, terpolymers, terpolymers of benzyl methacrylate, methacrylic acid, potassium silicate, ammonium lignin sulfonate, purified lignin sulfonate, hydroxypropyl sulfonated lignin, monofunctional oil-alkylene oxide block copolymers dispersants, alkylphenol ethoxylate dispersants, alkyd resins, calcium sulfonates, calcium salts, mineral spirits, zinc sulfonates, 2-butoxyethanol, butyl acetate, amine salts of polyester phosphates, amine phosphates, polyether phosphates, polymers with phosphate groups, liposomes, surfactant-based dispersants, polymer-based dispersants, alkylpolyamines, polyethylene waxes, aqueous solutions of sulfated castor oil or sulfonated organic substances, sulfonated polymers, dispersants with pigment-affinity groups or binder-compatible chains, oligomeric dispersants, including fatty acid-based dispersants and fatty acid-modified emulsifying dispersants, or any combination thereof.
[0120] In some embodiments, the dispersant may include amphiphilic block copolymers, polycarboxylates and polyaminoamides, ammonium polyacrylates, sodium lignin sulfonate, polyurethane-based, lecithin, polyvinyl acetate, controlled polymerization structured acrylate copolymers with pigment-affinity groups, controlled polymerization copolymers, controlled polymerization structured copolymers, polyester phosphates, alkanol-amines, monostearate glycerol, styrene / maleic anhydride copolymers, nitrogen grafting, terpolymers of benzyl methacrylate, block copolymers with free radical polymerization, 2-amino-2-methyl-1-propanol, ethoxylated linear fatty alcohols, monofunctional oil-alkylene oxide block copolymers, cationic polyacrylates with phosphates, 100% active dispersants, inactive or semi-active dispersants, monomeric dispersants, or any combination thereof.
[0121] In some embodiments, the dispersant may include a controlled polymerized structured acrylate copolymer with pigment-affinity groups, a controlled polymerized acrylic block copolymer, a controlled polymerized copolymer, a controlled polymerized acrylic block copolymer with pigment-affinity groups, a sodium salt of lignin sulfonate, a controlled free radical polymerized acrylate block copolymer, or any combination thereof.
[0122] In some embodiments, the dispersant may include acrylic acid and acrylate dispersants, lignin-based dispersants, hydroxypropyl cellulose, hydroxyethyl cellulose, polylysine, sodium lauryl sulfate, decyl glucoside, carboxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose, dioctyl sodium sulfosuccinate, chitosan, alginate sodium alginate, solsperse 4300, tannic acid, aspartic acid, alum sulfate, alum acetate, polyquaternium 10, glycerol, glyceryl monostearate, mono- and di-glycerides, fumaric acid, cinnamic acid, and any combination thereof. In some embodiments of the technology disclosed herein, the dispersion includes rapeseed oil.
[0123] In some embodiments, the dispersant may include anionic, cationic, electrically neutral, nonionic, electrostatic, sterically hindered, non-ionizable, polar, nonpolar, neutral polar, amphoteric surfactants, surfactants, soy lecithin, soybean oil, linseed oil, phosphate ester salts of high molecular weight copolymers with pigment-affinity groups, or any combination thereof.
[0124] In some embodiments, the dispersant may include a commercial dispersant. In some embodiments, the commercial dispersant includes Vanisperse CB, AMP 95, KRAFTSPERSE, BYKJET 9171, BYK 190, BYK 191, BYKJET 9152, DISPERBYK 2015, BYKJET 9151, BASF Dispex Ultra PX 4585, Marasperse CBOS-4, and any combination thereof.
[0125] In some embodiments, the composition further comprises an optional defoamer. In some embodiments, the defoamer is molecular-based, oil-based (mineral or plant-based), siloxane-based, polysiloxane-based, silicone-based, oil-wax-based, oil-silica-based, glycol emulsion-based, polyacrylate-based, modified fatty acid-based, polyether-based, modified amine-based, or any combination thereof. In some embodiments, the defoamer is BYK 1740.
[0126] In some embodiments, the composition includes an optional anticoagulant. In some embodiments, the anticoagulant includes cellulose. In some embodiments, the cellulose is microfibrillated cellulose.
[0127] In some embodiments, the composition includes an optional solvent. In some embodiments, the solvent is n-butyl acetate, methyl soyaate, ethyl lactate, ethyl acetate, isopropyl acetate, mineral spirits, aromatic compounds, esters, ketones, ethanol, or any combination thereof.
[0128] In certain embodiments, composition includes optional activator / carrier.In certain embodiments, described activator / carrier includes oligomer, monomer or photoinitiator.In certain embodiments, described activator / carrier is unsaturated polyester, acrylated polyester, acrylated epoxy resin, aliphatic acrylated carbamate, aromatic acrylated carbamate, acrylated silicone resin, acrylated polyether, acrylated melamine, acrylated oil, N-vinyl carbamate, thiol, vinyl monomer, vinyl acetate, N-vinyl pyrrolidone, monoacrylate, diacrylate, triacrylate, tetraacrylate, pentaacrylate, allyl monomer, plasticizing monomer, plasticizing diluent, aromatic ketone, synergistic amine, alkyl benzoin ether, thioxanthone and derivative, benzyl ketal, acylphosphine oxide, ketone oxime ester, acyl oxime ester, quaternary ammonium salt, acetophenone derivative, engineered microorganism, fatty acid, carboxylic acid, biorenewable or biomass derived, or any combination thereof.
[0129] In some embodiments, the composition further comprises an optional preservative or biocide. In some embodiments, the preservative or biocide is octanoyl hydroxamic acid, koralone, propyl gallate, thymol, eugenol, citral, cinnamaldehyde, carvacrol, o-phthalaldehyde, peracetic acid, cassonon (MIT / CMIT), DMDM hydantoin or any combination thereof.
[0130] Source Material
[0131] In some embodiments, the charcoal is made from plants or animals. Plant charcoal is derived from plants (e.g., trees, grasses), while animal charcoal is derived from animals (e.g., bones, teeth, poultry litter). Plant charcoal is identified as being different from animal charcoal by one or more of the following characteristics: (1) animal charcoal typically contains more than 40 g / kg of total phosphorus, while typical plant charcoal contains less than 0.3 g / kg of total phosphorus, and (2) microscopic examination of charcoal from animal feedstock, litter, and digesta is essentially free of pores, while plant substrates become porous charcoals.
[0132] In some embodiments, plant charcoal is biochar. In some embodiments, biochar is produced by intentionally planted crops such as kenaf, switchgrass, Miscanthus and corn. In some embodiments, biochar is produced by waste biomass materials such as animal manure, sewage sludge and agricultural and forestry residues. Agricultural and forestry residues that can be used to produce biochar include stubble from crops (such as corn, wheat, oats, sorghum, maize, canola and triticale), harvest residues such as rice husks, corn cobs, seeds, peels, nut shells, coffee pulp and by-products. Agricultural and forestry residues that can be used to produce biochar include stubble from crops (such as corn, wheat, oats, sorghum, maize, canola and triticale), harvest residues such as rice husks, corn cobs, seeds, peels, nut shells and coffee pulp. In some embodiments, biochar can also be produced by by-products such as bark, sawdust, shavings and pruned branches from trees produced by trees. Tree types include hardwoods and softwoods, with some species of trees being classified as both hardwoods and softwoods. Hardwoods include oak (including white oak, red oak, ash (including black ash and Honshu ash), eucalyptus, bamboo, maple (including Florida maple, black maple and sugar maple), walnut, hickory (including water hickory, bitter hickory, smooth hickory, American hickory, rough hickory, small rough hickory, black hickory and downy hickory), cherry, cottonwood, sycamore, willow, birch, floribunda, and tamarisk. Ash, Persimmon, Beech, Aquatic Honey Locust, American Honey Locust, Kentucky Coffee, American Holly, Walnut (including Black Walnut), Orange, Apple, Mulberry (including White Mulberry and Red Mulberry) and Sassafras. Softwoods include Pine, Loblolly Pine, Silver Bell, Walnut, Sweet Gum, Poplar (including Yellow Boxwood and Silver Poplar), Magnolia, Laurel, Purple Tree and Black Gum, Paulownia, Red Laurel, Sycamore, Cottonwood, Balsam, Poplar (including Bigtooth aspen and quaking aspen), feather maple, cedar, cypress, spruce, Douglas fir, fir, maple (including red maple and silver maple), horse chestnut (including glossy and yellow horse chestnut), birch (including river birch, water birch, paper birch, gray birch), chestnut (including Allegheny chestnut and Ozark chestnut), cottonwood (including eastern cottonwood, cottonwood, black cottonwood, Limon cottonwood, and narrow-leaved cottonwood), basswood (including American basswood and white basswood) ), elm (including rock elm, winged elm, American elm, thick-leaved elm, Siberian elm, slippery elm and autumn elm), catalpa, larch, coast redwood, hackberry, Mississippi hackberry, cherry (including needle cherry and black cherry), hemlock, ash (including American ash, foreign ash and downy ash), willow (including peach leaf willow, black willow and diamond willow), Japanese cedar and kauri. The above biochar sources can be used alone or in combination.For example, methods and apparatus for producing biochar are disclosed in US Pat. No. 8,361,186 B1-“Biochar”, US Pat. No. 8,772,559 B2-“Biochar generator and related methods” and US Pat. No. 9,809,502 B2-“Enhanced biochar”.
[0133] In some embodiments, disclosed herein is a composition having about 1-75% by weight of particles derived from biochar, 10-40% by weight of a dispersant, about 1-20% by weight of an optional anticoagulant, about 0.01-5% by weight of an optional defoamer, and about 0.001-5% of an optional preservative or biocide. In some embodiments, the amount of biochar is 5-70% by weight.
[0134] In some embodiments, the amount of biochar is about 20-60% by weight. In some embodiments, the amount of biochar is about 30-50% by weight. In some embodiments, the amount of biochar is about 20-80% by weight, including all ranges contained therein.
[0135] In some embodiments, the amount of the dispersant is about 15-35% by weight. In some embodiments, the amount of the dispersant is about 15-30% by weight. In some embodiments, the amount of the dispersant is about 10-30% by weight. In some embodiments, the amount of the dispersant is about 20-30% by weight. In some embodiments, the amount of the dispersant is about 15-35% by weight. In some embodiments, the amount of the dispersant is about 20-25% by weight. In some embodiments, the amount of the dispersant is about 25-30% by weight. In some embodiments, the amount of the dispersant is about 1-40% by weight, including all ranges contained therein. In some embodiments, the amount of the dispersant is about 5-30% by weight. In some embodiments, the amount of the dispersant is about 5-40% by weight.
[0136] In some embodiments, the amount of the anticoagulant is about 5-20% by weight. In some embodiments, the amount of the anticoagulant is about 1-15% by weight. In some embodiments, the amount of the anticoagulant is about 1-20% by weight, including all ranges contained therein.
[0137] In some embodiments, the amount of the defoaming agent is about 0.01-5.0 wt %, including all ranges subsumed therein.
[0138] In some embodiments, the amount of preservative or biocide is about 0.001-5% by weight, including all ranges subsumed therein.
[0139] In some embodiments, the biochar is no greater than about 70% by weight. In some embodiments, the biochar is no greater than about 65% by weight. In some embodiments, the biochar is no greater than about 55% by weight. In some embodiments, the biochar is no greater than about 50% by weight. In some embodiments, the biochar is no greater than about 45% by weight. In some embodiments, the biochar is no greater than about 40% by weight. In some embodiments, the biochar is no greater than about 30% by weight.
[0140] In some embodiments, the dispersant is no greater than about 35 wt %. In some embodiments, the dispersant is no greater than about 30 wt %. In some embodiments, the dispersant is no greater than about 25 wt %. In some embodiments, the dispersant is no greater than about 20 wt %. In some embodiments, the dispersant is no greater than about 15 wt %. In some embodiments, the dispersant is no greater than about 10 wt %.
[0141] In some embodiments, the anticoagulant is no more than about 20% by weight. In some embodiments, the anticoagulant is no more than about 15% by weight. In some embodiments, the anticoagulant is no more than about 10% by weight. In some embodiments, the anticoagulant is no more than about 5% by weight.
[0142] In some embodiments, the defoamer is no greater than about 2.5 wt %. In some embodiments, the defoamer is no greater than about 1.0 wt %. In some embodiments, the defoamer is no greater than about 0.75 wt %.
[0143] In some embodiments, the preservative or biocide is not more than about 5.0 weight %. In some embodiments, the preservative or biocide is not more than about 2.5 weight %. In some embodiments, the preservative or biocide is not more than about 1.0 weight %. In some embodiments, the preservative or biocide is not more than about 0.1 weight %. In some embodiments, the preservative or biocide is not more than about 0.01 weight %.
[0144] In some embodiments, the composition is petroleum-free and includes 1-75 wt% biochar, 10-40 wt% dispersant, optionally 1-20 wt% anticoagulant, and optionally 0.01-5 wt% defoaming agent.
[0145] Pigment particles
[0146] Disclosed herein are various embodiments of pigments and pigment dispersions that include carbonaceous particulate matter derived from biochar. As used herein, the term "particle" refers to a single particle of the type typically referred to as a primary particle in a description of a carbon black pigment. As used herein, the term "particulate matter" refers to (1) a cluster of particles, (2) a chain of particles, or (3) a single particle, either alone or in a combination of two or all three.
[0147] The following characteristics and features that are characteristic of the technology disclosed herein may be applied as independent features or characteristics, and may be applied in combinations of two or more features or characteristics.
[0148] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles wherein at least 99.7% of the particles by number have a maximum diameter less than 25 nm as measured on a scanning transmission electron microscopy (STEM) two-dimensional micrograph at a magnification of at least 50,000 times.
[0149] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles wherein at least 95% of the particles by number have a maximum diameter less than 25 nm as measured on a scanning transmission electron microscopy (STEM) micrograph at a magnification of at least 50,000 times.
[0150] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles wherein at least 99.7% of the particles by number have a maximum diameter less than 50 nm as measured on a scanning transmission electron microscopy (STEM) two-dimensional micrograph at a magnification of at least 50,000 times.
[0151] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles wherein at least 95% of the particles by number have a maximum diameter less than 50 nm as measured on a scanning transmission electron microscopy (STEM) micrograph at a magnification of at least 50,000 times.
[0152] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles, wherein at least 99.7% of the particles by number have a maximum diameter within the range between 15 nm and 25 nm, as measured on a scanning transmission electron microscopy (STEM) two-dimensional micrograph at a magnification of at least 50,000 times.
[0153] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles wherein at least 95% of the particles by number have a maximum diameter in the range of 15 nm to 25 nm as measured on a scanning transmission electron microscopy (STEM) micrograph at a magnification of at least 50,000 times.
[0154] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles, wherein at least 99.7% of the particles by number have a maximum diameter within the range between 10 nm and 50 nm, as measured on a scanning transmission electron microscopy (STEM) two-dimensional micrograph at a magnification of at least 50,000 times.
[0155] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment spherical particles wherein at least 95% of the particles by number have a maximum diameter in the range of 5 nm to 500 nm as measured on a scanning transmission electron microscopy (STEM) micrograph at a magnification of at least 50,000 times.
[0156] Figure 5 and Figure 6 Particles having a spherical shape are shown. The spherical shape is characterized by appearing as a sphere with no significant ellipsoidal deformation.
[0157] As used herein, the term "carbon pigment particles" refers to particles that are at least 80% pure elemental carbon.
[0158] In some embodiments of the technology disclosed herein, the submicron carbon pigment particles are plant carbon pigment particles.
[0159] As used herein, the terms "submicron" carbon pigment particles and "submicron" carbon particles refer to particles wherein at least 99.9% of the particles are less than 1 micron in size as measured by dynamic light scattering based on a polystyrene latex standard having a refractive index of 1.590 and an absorbance of 0.010.
[0160] It is important to recognize that for the submicron-sized carbon particles derived from biochar with spherical or quasi-spherical shapes, high Mc and My values, and tinting strength as disclosed herein, the particles are the result of the wet milling process and chemistry disclosed herein. These particle characterizations are unexpected because it is found that conventional wet milling and dry milling processes and chemistry cannot achieve uniformity of shape or near-monodisperse quality, which leads to low tinting strength and low My and Mc values. Additional grinding time cannot produce uniform spherical or quasi-spherical shapes, high Mc or My values, or high tinting strength. In addition, in the typical manufacturing method disclosed herein, the step includes using a filter with an aperture larger than the typical particle size of the embodiments disclosed herein (which is generally much smaller than 1 micron), and the filtrate forms a dispersion. This relatively large aperture filtration proves that this method, rather than screening, is the cause of the submicron particle size distribution, shape uniformity, and near-monodisperse quality in the pigment composition.
[0161] For example, Fig.19is an image produced using the Lacey Stem process showing biomass-derived pigment particles from a commercially available source not associated with the present applicant. Although these particles are milled (according to the company's website), they do not achieve the same superior features of the embodiments disclosed herein. Instead, the small scale fiber features are Fig.19 The particles in the competitive material are apparent on the surface. The competitive material does not exhibit a smooth surface as defined herein, such as Fig. 27 As shown, Fig. 27 The smooth surface of the embodiment disclosed herein is shown. In addition, the spherical shape of the embodiment disclosed herein is shown. Figure 5 and Figure 6 compared to, Fig.19 The particles shown in show considerable size variation and deviations from spherical geometry.
[0162] Some embodiments of the technology disclosed herein provide a random sample of carbon pigment particles having a particle size distribution as measured by intensity-based dynamic light scattering based on polystyrene latex with a refractive index of 1.590 and an absorbance of 0.010 as a standard, with an average particle size in the range between 115 and 120 nm and a polydispersity index in the range between 0.170 and 0.200.
[0163] Some embodiments of the technology disclosed herein provide a random sample of submicron carbon pigment particles having a particle size distribution as measured by intensity-based dynamic light scattering based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard, with an average particle size in the range between 165 nm and 171 nm and a polydispersity index in the range between 0.10 and 0.15.
[0164] Some embodiments of the technology disclosed herein feature a random sample of submicron carbon pigment particles having a particle size distribution measured by intensity-based dynamic light scattering based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard, with an average particle size in the range of 115 to 120 nm and a polydispersity index in the range of 0.170 to 0.200.
[0165] Some embodiments of the technology disclosed herein feature a random sample of submicron carbon pigment particles having a particle size distribution measured by intensity-based dynamic light scattering based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard, with an average particle size in the range between 165 nm and 171 nm and a polydispersity index in the range between 0.10 and 0.15.
[0166] Some embodiments of the technology disclosed herein feature a random sample of submicron carbon pigment particles having a particle size distribution measured by intensity-based dynamic light scattering based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard, with an average particle size in the range of 115 to 120 nm and a polydispersity index in the range of 0.170 to 0.200.
[0167] Some embodiments of the technology disclosed herein feature a random sample of submicron carbon pigment particles having a particle size distribution measured by intensity-based dynamic light scattering based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard, with an average particle size in the range between 165 nm and 171 nm and a polydispersity index in the range between 0.10 and 0.15.
[0168] In some embodiments disclosed herein, under laser excitation at a wavelength of 514.5 nm using a 1800 gr / mm grating, the composition having carbonaceous particles exhibits a Raman spectrum with a G position between 1590 (cm-1) and 1595 (cm-1) and an I(D) / I(G) ratio between 2.54 and 3.02. In some embodiments disclosed herein, under laser excitation at a wavelength of 514.5 nm using a 1800 gr / mm grating, the composition having carbonaceous particles exhibits a Raman spectrum with a G position between 1585 (cm-1) and 1600 (cm-1) and an I(D) / I(G) ratio between 2.49 and 3.08. In some embodiments disclosed herein, under laser excitation at a wavelength of 514.5 nm using a 1800 gr / mm grating, the composition having carbonaceous particles exhibits a Raman spectrum with a G position between 1580 (cm-1) and 1605 (cm-1) and an I(D) / I(G) ratio between 2.43 and 3.14.
[0169] In some embodiments of the technology disclosed herein, the dispersion comprises 15-50% W P / W T Pigment particles and 15-50% W D / W T Sodium lignin sulfonate or lignin sulfonic acid dispersant or unstructured or structured acrylic polymer or copolymer dispersant or unstructured or structured acrylate polymer or copolymer dispersant or hydroxyl functional carboxylate dispersant or styrene maleic anhydride dispersant, wherein W P is the weight of the pigment particles, W D is the weight of the dispersant, W T is the total weight of the dispersion, and the fraction is expressed as a percentage.
[0170] In some embodiments of the technology disclosed herein, the dispersion includes 15-50% W P / W T Pigment particles, and 15-50% W D / W T The dispersion is characterized by an L* value in the range of 48.0 to 58.0, as read relative to a TiO2 reference blank suspension having an L* value of 84.99, and an a* value in the range of -0.23 to -0.42, as read relative to a TiO2 reference blank suspension having an a* value of -0.16, and a b* value in the range of 0.15 to 1.25, as read relative to a TiO2 reference blank suspension having a b* value of 0.69, and a dL* value in the range of -26 to -37, as read relative to a TiO2 reference blank suspension having a dL* value of 84.99, when tested according to the black pigment color analysis described herein. P is the weight of the pigment particles, W D is the weight of the dispersant, W T is the total weight of the dispersion and the fraction is expressed as a percentage.
[0171] In some embodiments of the technology disclosed herein, the dispersion includes 15-50% W P / W T Pigment particles, and 15-50% W D / W T The dispersion is characterized by an L* value in the range of between 40.0 and 65.0, as read relative to a TiO2 reference blank suspension having an L* value of 84.99, an a* value in the range of between -0.15 and -0.50, as read relative to a TiO2 reference blank suspension having an a* value of -0.16, a b* value in the range of between 0.1 and 1.5, as read relative to a TiO2 reference blank suspension having a b* value of 0.69, a dL* value in the range of between -20 and -45, as read relative to a TiO2 reference blank suspension having a dL* value of 84.99, when tested according to the black pigment color analysis described herein. P is the weight of the pigment particles, W D is the weight of the dispersant, W T is the total weight of the dispersion, and the fraction is expressed as a percentage.
[0172] In some embodiments of the technology disclosed herein, the dispersion includes pigment particles and a dispersant including a modified acrylic acid or acrylate copolymer having a pigment affinity group. In some embodiments, the dispersion also includes a dispersion including a hydroxyl-functional carboxylic acid ester having a pigment affinity group.
[0173] In some embodiments of the technology disclosed herein, a dispersion includes pigment particles and sodium lignin sulfonate or a sodium lignin sulfonate salt-based dispersant and a hydroxy-functional carboxylic acid ester having a pigment-affinic group.
[0174] In some embodiments of the technology disclosed herein, the dispersion includes rapeseed oil.
[0175] In some embodiments of the technology disclosed herein, the plant charcoal is biochar.
[0176] Particle morphology and identification
[0177] In some embodiments, disclosed herein are pigment dispersion compositions having carbonaceous particles derived from biochar, the carbonaceous particles being formed into particles having a smooth surface (e.g. Fig. 27 As used herein, the term "smooth surface" refers to a particle surface that shows approximate spatial uniformity and consistency when imaged using a Lacey STEM process, and in which local variations in surface height have a wavy form and the surface height variations have no roughness or angles.
[0178] Figure 1A , 1B , 2A and 2B show particles having a spheroidal morphology. The spheroidal morphology is characterized by a particle shape that may be slightly oblate or ellipsoidal compared to a perfect sphere.
[0179] In some applications of the technology disclosed herein, it may be desirable to use carbonaceous particles derived from biochar as a direct replacement for petroleum-derived carbon black. ASTM International maintains ASTM Standard D3053, "Standard Terminology Relating to Carbon Black," which specifically relates to carbon black derived from petroleum. D3053 defines carbon black as "an engineering material consisting essentially of elemental carbon, obtained by the partial combustion or thermal decomposition of hydrocarbons, existing as aggregates of spherical primary particles having a grape-like morphology, said spherical primary particles exhibiting uniformity of primary particle size within a given aggregate and turbostratic stratification within the primary particles." General scientific literature typically describes turbostratic structure as having carbon layers arranged in a randomly folded or broken manner. The turbostratic structure in the primary particles exhibits features on the nanoscale or smaller.
[0180] Most commercial carbon blacks are produced from petroleum. In some embodiments disclosed herein, the carbon particles derived from biochar substantially conform to most of the first part of the definition of carbon black in ASTM Standard D3053: "an engineered material consisting essentially of elemental carbon, obtained by the partial combustion or thermal decomposition of hydrocarbons, existing as aggregates of grape-like morphology composed of spherical primary particles, said spherical primary particles exhibiting uniformity of primary particle size within a given aggregate. One difference between the first part of the ASTM D3053 definition of carbon black and the embodiments of the carbon particles derived from biochar disclosed herein is that the carbon black defined in ASTM D3053 is "obtained by the partial combustion or thermal decomposition of hydrocarbons [C+H]," while the carbon particles derived from biochar are obtained by the pyrolysis or thermal decomposition of carbohydrates (C+H+O). Another difference is that in most applications of the carbon particles derived from biochar, the last part of the definition of carbon black (i.e., "turbostratified stratification within the primary particles") does not affect the pigment properties described herein and does not need to be evaluated.
[0181] The ASTM D3053 definition of carbon black refers to a "bunch of grapes morphology". The bunch of grapes morphology is generally understood to mean "shaped like a bunch of grapes". This section describes certain embodiments of the pigment compositions disclosed herein that include carbonaceous particles derived from biochar. However, a more complete term for the pigment composition that includes carbonaceous particles derived from biochar is a "chain-like bunch of grapes morphology". As used herein, the term "chain-like bunch of grapes morphology" refers to two clusters of grape-like particles that are interconnected by at least one particle that is connected to only two other particles.
[0182] Fig. 20 and 21 First particle clusters A, B, C and D and second particle clusters 1, 2, 3, 4 are shown. Fig. 20 In , the first particle cluster and the second particle cluster are connected by a particle "+" that is only connected to two other particles ("C" and "2"). Fig.21 In the embodiment, the first particle cluster and the second particle cluster are interconnected through particles "+" and "++". Particle "+" is only connected to particles "C" and "++", and particle "++" is only connected to particles "+" and "2".
[0183] Figure 5A (with Figure 5 ) shows grape-like clusters (shown as circles) and interconnected particles (identified by pointing arrows) that are connected to only two other particles, demonstrating the chain-like grape-bunch-like morphology.
[0184] It is generally known that petroleum-derived carbon black in liquids produces clusters called "structures". The term "high structure" refers to clusters with a large number of branches, while "low structure" refers to clusters with a small number of branches. These clusters are often referred to as "transient structures" because these structures can be broken up with grinding or force. In contrast, and surprisingly, some embodiments of carbonaceous particles derived from biochar disclosed herein form structures (e.g., chain-like grape bunch-like morphology) by grinding or force.
[0185] One measure of the structure in the carbon particles is the oil absorption number (OAN). The OAN is the number of cubic centimeters of dibutyl phthalate (DBP) or paraffin oil absorbed by 100 g of carbon black under specific conditions. The OAN value is proportional to the degree of aggregation at the structural level of the carbon black. A high OAN number corresponds to a high structure, i.e. a high degree of branching and clustering of the aggregates. The OAN value of a pigment sample having carbonaceous particles derived from biochar is determined using ASTM D2414 "Oil Absorption Number (OAN) of a Sample", in which dibutyl phthalate (DBP) is used as the oil. The procedure for conducting this test is sufficient in the standard and does not require further elaboration.
[0186] A raw material sample of a pigment dispersion formulation with carbonaceous particulates derived from biochar as disclosed herein was tested according to ASTM D2414 and resulted in an OAN value of 136.4 ml / 100 g. This is surprising because the OAN of loose black petroleum carbon black is typically less than about 132 ml / 100 g.
[0187] Reference is again made to commercially available biomass-derived pigment particles and micrographs depicting competitive products. Fig.19 , three separate particles were measured at 433.6 nm, 427.5 nm, and 549.5 nm. These particles are much larger than the embodiments disclosed herein having particles with diameters less than 100 nm. Fig.19 As shown, biomass-derived pigment particles from commercial sources not associated with the applicant do not exhibit the chain-like grape-bunch-like morphology disclosed herein. This difference is due to Fig.23 It is further evident in. Fig.23 Shown is a "web" featuring features in a micrograph image made from a Lacey STEM process. Fig.23 It is also shown that in some cases there may be portions of the image (labeled A, B, and C) that present some ambiguity in determining what represents a particle and what represents an inhomogeneity in the web. These ambiguities can be resolved by referencing an image processed without transmission so as not to see through the particles. This variation is shown in FIG. Fig.24 shown. Fig.24 The materials depicted in the images are Fig.23 Same materials as in Fig.24The image is magnified 30,000 times (with Fig.23 100,000 times as large as in Fig.24 However, from Fig.24 It is obvious that areas A, B and C are not images of particles.
[0188] Fig.25 Combination Fig.26 Particles from commercial sources of pigments derived from biomass do not show Fig. 27 The smooth surface of the embodiments of the present disclosure is evident in FIG. Fig.26 , solved Fig.25 any ambiguity in the roughness of the particle surface imaged from the Lacey STEM process, Fig.26 Depicts no electron transfer Fig.25 of the same particles.
[0189] The embodiments disclosed herein of biochar-derived carbonaceous particles having a chain-like grape bunch-like morphology are highly unexpected in view of the prior art of carbonaceous pigments at the priority date of the present disclosure.
[0190] In some embodiments, particularly in embodiments where the particles are milled with a fluid and dried and imaged by a sputtering method, the morphology of the aggregates of pigment particles made from plant carbon shows the particle surface and shape. In some embodiments, pigment carbon particles (e.g., Figure 1A , 1B , 2A and 2B). When imaged using the Lacey STEM process, such particles are expected to exhibit a chain-like grape-bunch-like morphology.
[0191] Disclosed herein are various biochars and combinations of biochars that were evaluated for effectiveness as potential pigments. The characteristics evaluated included surface area, surface groups, pure carbon content, ash content, compatibility with dispersants, amount of polyaromatic hydrocarbons, and size of particles produced by grinding the biochar. Suitable plant char feedstocks for grinding pigments were selected using one or more of the following criteria: surface area greater than 200 m 2 / g; carbon content ≥ 80%; ash content ≤ 20%; high compatibility with dispersants; polycyclic aromatic hydrocarbon (PAH) content ≤ 50 mg / kg; and the ability to grind the raw material to a D90 particle size of less than 1 micron. In some embodiments, high compatibility with dispersants is one or more of the following: minimum 20% pigment loading in the dispersion while also maintaining low viscosity during milling or grinding; minimal or no gelling during milling or grinding; almost no phase separation after milling; stable viscosity by oven testing at 60°C for 5 weeks; and stable storage for at least 1 month.
[0192] Petroleum carbon black (PCB) particles aggregate together to form small branches that fuse. If multiple branches are formed, this is sometimes referred to as a "high" structure, and if only one or two branches are formed, this is sometimes referred to as a "low" structure. In general, a high structure improves the dispersibility of the carbon, but reduces the blackness. Unexpectedly, embodiments of dispersions of carbonaceous particulates derived from biochar disclosed herein have relatively high structures and also exhibit excellent blackness.
[0193] PCBs can tend toward brown or other colors, often referred to as "blonding". In some embodiments, particles with a truer black are disclosed herein. This characteristic is referred to as ink color. Using PCBs, bluish black generally requires a minimum primary particle size, such as 10 nm. In some embodiments, primary particles with larger sizes, such as 25 nm, are disclosed herein that achieve bluish black. The advantage is that it is easier to disperse in the preferred black hue.
[0194] In some embodiments, the carbon particles disclosed herein are 100% biorenewable.
[0195] Biochar feedstock samples used in pigment dispersion formulations including carbonaceous particulate matter derived from biochar were tested for PAH content according to the following "PAH Protocol".
[0196] Samples were tested using the Environmental Protection Agency (EPA) method: SW846 8270C, Semivolatile Organic Compounds by Gas Chromatography / Mass Spectrometry (GC / MS)
[0197] Method 8270 is used to determine the concentration of semivolatile organic compounds in extracts prepared from many types of solid waste matrices, soils, air sampling media, and water samples.
[0198] Extraction by EPA method SW846 3546
[0199] The extract was tested for semi-volatile organic compounds or PAHs using EPA method SW846 8270C
[0200] In some embodiments, the carbon particles disclosed herein have non-detectable (ND) amounts of polycyclic aromatic hydrocarbons (PAHs), as shown in the test results below.
[0201]
[0202]
[0203] CAS Number Recovery rate of alternatives Run #1 Run #2 Limits 321-60-8 2-Fluorobiphenyl <![CDATA[21% b ]]> <![CDATA[1% b ]]> 23-130% 4165-60-0 Nitrobenzene-d5 31% <![CDATA[6% b ]]> 12-131% 1718-51-0 Terphenyl-d14 1% <![CDATA[0% b ]]> 29-141%
[0204] (a) Samples extracted beyond the holding time.
[0205] (b) Control limit exceeded due to matrix interference. Confirm by re-extraction and re-analysis.
[0206] ND = Not Detected
[0207] MDL = Method Detection Limit
[0208] RL = Reporting Limit
[0209] E indicates that the value is out of calibration range
[0210] J represents the estimated value
[0211] B indicates the analyte found in the relevant method blank
[0212] N indicates presumptive evidence for the compound
[0213] In some embodiments, the PAH content may be less than the following amounts in Table 1, which are typically 90% less than PCB.
[0214] Table 1
[0215]
[0216]
[0217] application
[0218] Some embodiments of pigment dispersion disclosed herein are applicable to digital (inkjet) printing. In certain embodiments, digital ink is used for consumer home printers, and / or for the coloring of textiles, banners, paper, packaging and other materials. In certain embodiments, dispersion disclosed herein is applicable to various types of printing and coloring, including but not limited to screen printing, rotary printing, offset printing, flexographic printing, gravure printing, continuous pigment dyeing, pad dyeing, stock solution dyeing, solution dyeing, foam coating, spraying or woodcut printing. In certain embodiments, dispersion disclosed herein is applicable to leather or polyurethane coating, paper coating, industrial coating, paint and wood coloring. In certain embodiments, dispersion disclosed herein is applicable to packaging, such as food packaging or cardboard box, and is applicable to embossed plastic or metal film. In certain embodiments, dispersion disclosed herein is applicable to colored non-aqueous polymers, including molded forms and fibers.
[0219] Manufacturing method
[0220] Various methods of making particles and dispersions for coloring can be used to make the pigments and dispersions disclosed herein. The pigment composition can be prepared by the method of any of the following examples.
[0221] In some embodiments, a method comprises the following steps:
[0222] (a) combining and mixing biochar and a dispersant to form a first mixture;
[0223] (b) adding water and optionally a defoaming agent and optionally an anticoagulant to the first mixture and mixing to form a second mixture;
[0224] (c) allowing the second mixture to stand for a settling time and optionally decanting water from the top to form a third mixture;
[0225] (d) grinding the third mixture in a media mill or ball mill having beads of 0.1-1.0 mm at a flow rate of 50-200 mL / min for 1-8 hours to form a fourth mixture; and
[0226] (e) filtering the fourth mixture through a 0.1-10 micron filter under vacuum;
[0227] Wherein steps (a) and (b) are optionally performed under vacuum, and the filtrate is a pigment dispersion composition.
[0228] In some embodiments, the first mixture is mixed manually or with a z-blade mixer. In some embodiments, the second mixture is mixed with a high shear agitator for 30-60 minutes. In some embodiments, the standing period is 1-24 hours, or water is allowed to evenly cover the surface of the second mixture. In some embodiments, the ball mill media is 0.5mm or 0.3mm. In some embodiments, the flow rate is 80-100mL / min. In some embodiments, the third mixture is ground for 3-4 hours. In some embodiments, the filter is a polypropylene bag. In some embodiments, the filter is a 1-5 micron polypropylene bag. In some embodiments, the filter is a screen at the exit point of a mechanical grinder. In some embodiments, the screen filter size is 1-10 microns.
[0229] In some embodiments, a method comprises the following steps:
[0230] (a) combining and mixing a dispersant and a grinding fluid, and optionally a defoaming agent, and optionally an anticoagulant to form a first mixture;
[0231] (b) adding a biochar feedstock to the first mixture and mixing to form a second mixture;
[0232] (c) grinding the second mixture with beads having a diameter of 0.1-1.0 mm at a flow rate of 7-200 mL / min for 1-8 hours to form a third mixture; and
[0233] (d) filtering the third mixture through a filter having an average pore size of 1 to 10 microns under vacuum, wherein the filtrate is the pigment composition.
[0234] In some embodiments, the grinding fluid of step (a) comprises water. In some embodiments, the grinding fluid of step (a) comprises solvent. In some embodiments, the mixing of step (b) is carried out in batches using a mechanical agitator for 30-60 minutes to form the second mixture. In some embodiments, step (b) is carried out under vacuum or a degasser. In some embodiments, the filter is a polypropylene bag. In some embodiments, the filter is a 1-5 micron polypropylene bag. In some embodiments, the filter is a screen at the exit point of a mechanical grinder. In some embodiments, the screen filter is a size of 1-10 microns. In some embodiments, the filtrate of step (d) is degassed under vacuum to form a pigment composition.
[0235] In some embodiments, a method comprises the following steps:
[0236] (a) combining and mixing a dispersant and optionally one or more monomers, and optionally one or more oligomers, and optionally an anticoagulant to form a first mixture
[0237] (b) adding the biochar feedstock to the first mixture and mixing to form a second mixture
[0238] (c) grinding the second mixture with a three-roll mill, wherein 1 to 8 passes of grinding are performed
[0239] (d) filtering the third mixture through a filter having an average pore size of 1 to 10 micrometers under vacuum, and the filtrate is the pigment composition.
[0240] Steps (a) and (b) are optionally performed under vacuum or a degasser.
[0241] In some embodiments, the raw material for the pigment particles produced with the technology disclosed herein is a plant charcoal raw material provided as a granular solid. In a preferred embodiment, the plant charcoal is biochar. In some embodiments, the granular solid is ground in a micromedia ball mill. In some embodiments, 0.3mm or 0.5mm beads can be used individually or one at a time to achieve a minimum particle size. In some embodiments, the grinding process incorporates these solid materials into a liquid carrier or grinding resin. In some embodiments, the granular solid is ground in a three-roll mill. In some embodiments, the granular solid is ground on a horizontal mill. During each of these processes, the biochar raw material of the granular solid is converted into a dispersion of particulate matter.
[0242] ExperimentalEvaluation of dispersions including biochar particles Dispersions were prepared according to the following general preparation steps.
[0243] Step 1 Pigment raw materials (eg wood biochar) and dispersant are weighed and added to a mixing container and mixed manually or with a z-blade mixer.
[0244] Step 2: Water and adjuvants such as defoamers, anticoagulants and optional biocides are added to the mixture. The mixture is mixed for 30-60 minutes using a high shear agitator such as a Ross mixer or a Cowles mixer. For some formulations, premixing is performed under vacuum to help wet the pigment.
[0245] Step 3: Allow the mixture to sit for 1-24 hours to "wet out" so that the water completely covers the surface area of the material. Decant the water from the top of the mixture.
[0246] Step 4 The decanted mixture is placed in a media mill or ball mill with 0.5 mm or 0.3 mm beads, depending on the pigment percentage in the mixture. The milling is started at a flow rate of 80-100 ml / min and run for 3-4 hours depending on the type of mill and formulation. A dispersion is formed.
[0247] Step 5 Using vacuum, filter the dispersion through a 1-5 micron polypropylene bag filter, depending on the end application needs, to remove any large particles.
[0248] preparation
[0249] Preparation 1
[0250] Formulation 1 is a dispersion prepared by the general method described above. The formulation is 35% bamboo biochar, 10% 100% active comb-branched copolymer dispersant, and the remainder isopropyl acetate.
[0251] Preparation 2
[0252] Formulation 2 is a dispersion prepared by the general method described above. The formulation is 40% oak biochar, 26% aromatic polyglycol ether phosphate dispersant, 9% microfibrillated cellulose, 0.5% oil-silica based defoamer, and the remainder is deionized water.
[0253] Preparation 3
[0254] Formulation 3 is a dispersion prepared by the general method described above. The formulation is 35% cottonwood biochar, 30% polyether phosphate dispersant, 8% microfibrillated cellulose, 0.5% molecular-based defoamer, and the remainder is deionized water.
[0255] Preparation 4
[0256] Formulation 4 is a dispersion prepared by the general method described above, which is 40% animal bone biochar, 10% carboxylic acid dispersant, 10% microfibrillated cellulose, 0.2% silicone-based defoamer, and the remainder is deionized water.
[0257] Preparation 5
[0258] Formulation 5 is a dispersion prepared by the general method described above, which is 70% blueberry wood biochar, 13% polyacrylate ammonium salt dispersant, 8% microfibrillated cellulose, 0.5% oil-wax based defoamer, and the rest is deionized water.
[0259] Preparation 6
[0260] Formulation 6 is a dispersion prepared by the general method described above. This formulation is 30% bamboo biochar, 5% 100% active structured acrylic copolymer, 30% oligomer, and 35% monomer blend.
[0261] Preparation 7
[0262] Formulation 7 is a dispersion prepared by the general method described above. The formulation is 50% cedar wood biochar, 15% polyurethane-based dispersant, 8% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is deionized water.
[0263] Preparation 8
[0264] Formulation 8 is a dispersion prepared by the general method described above. The formulation is 50% bamboo biochar, 20% lecithin dispersant, 8% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is deionized water.
[0265] Preparation 9
[0266] Formulation 9 is a dispersion prepared by the general method described above. The formulation is 50% cedar wood biochar, 25% polyvinyl acetate dispersant, 8% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is deionized water.
[0267] Preparation 10
[0268] Formulation 10 is a dispersion prepared by the general method described above. The formulation is 20% maple biochar, 10% phosphate ester salt of a high molecular weight copolymer having pigment affinity groups, 70% ethyl acetate.
[0269] Preparation 11
[0270] Formulation 11 is a dispersion prepared by the general method described above. This formulation is 40% pine biochar, 25% controlled polymerization structured acrylate copolymer dispersant with pigment affinity groups, 5% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is deionized water. See characterization data below.
[0271] Preparation 12
[0272] Formulation 12 is a dispersion prepared by the general method described above. This formulation is 68% birch biochar, 22% ethoxylated fatty acid ester dispersant, and the remainder is deionized water.
[0273] Preparation 13
[0274] Formulation 13 is a dispersion prepared by the general method described above, which is 35% cottonwood biochar, 30% styrene / maleic anhydride copolymer dispersant, 2.5% ethylene glycol emulsion defoamer, 3.0% octanoyl hydroxamic acid preservative, and the remainder is deionized water.
[0275] Preparation 14
[0276] Preparation 14 is a dispersion prepared by the general method described above, which is 15% elm biochar, 20% sorbitan monolaurate dispersant, 8% microfibrillated cellulose anticoagulant, 0.3% modified fatty acid-based defoamer, and the remainder is deionized water.
[0277] Preparation 15
[0278] Formulation 15 is a dispersion prepared by the general method described above. The formulation is 43% Japanese cedar biochar, 47% nitrogen-grafted polymer dispersant, 0.5% oil-based defoamer, 1.0% o-phthalaldehyde preservative, and the remainder is deionized water.
[0279] Preparation 16
[0280] Formulation 16 is a dispersion prepared by the general method described above, which is 30% poplar biochar, 25% sodium lignin sulfonate dispersant, 5% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is deionized water.
[0281] Preparation 17
[0282] Formulation 17 is a dispersion prepared by the general method described above. The formulation is 20% pine tree biochar, 15% controlled radical polymerized acrylate block copolymer dispersant, 5% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is non-deionized water.
[0283] Preparation 18
[0284] Formulation 18 is a dispersion prepared by the general method described above. The formulation is 65% cedar biochar, 15% polyurethane-based dispersant, 10% microfibrillated cellulose anticoagulant, 0.5% oil-silica-based defoamer, and the remainder is deionized water.
[0285] Preparation 19
[0286] Formulation 19 is a dispersion prepared by the general method described above. The formulation is 55% cottonwood biochar, 20% ethoxylated fatty acid ester dispersant, 10% microfibrillated cellulose, 0.6% silicone-based defoamer, and the remainder is deionized water.
[0287] Preparation 20
[0288] Formulation 20 is a dispersion prepared by the general method described above. The formulation is 42% hickory biochar, 20% sorbitan monolaurate dispersant, 10% microfibrillated cellulose, 0.6% oil-wax based defoamer, and the remainder is deionized water.
[0289] Preparation 21
[0290] Formulation 21 is a dispersion prepared by the general method described above, which is 70% poplar biochar, 15% butyl acetate dispersant, 2% microfibrillated cellulose anticoagulant, 0.5% oil-based defoamer, 0.1% propyl gallate preservative, and the remainder is deionized water.
[0291] Preparation 22
[0292] Formulation 22 is a dispersion prepared by the general method described above, which is 54% elm biochar, 20% butyl acetate dispersant, 10% microfibrillated cellulose, 2.0% oil-based defoamer, and the remainder is deionized water.
[0293] Preparation 23
[0294] Formulation 23 is a dispersion prepared by the general method described above, which is 46% elm biochar, 40% polyether phosphate dispersant, 10% microfibrillated cellulose, 0.8% oil-wax defoamer, and the remainder is deionized water.
[0295] Preparation 24
[0296] Formulation 24 is a dispersion prepared by the general method described above. The formulation was 43% hemlock biochar, 15% alkanol-amine dispersant, 6% microfibrillated cellulose, and the remainder was deionized water.
[0297] Preparation 25
[0298] Formulation 25 is a dispersion prepared by the general method described above. The formulation is 23% cottonwood biochar, 20% glyceryl monostearate dispersant, 5% microfibrillated cellulose, 2.0% oil-based defoamer, and the remainder is deionized water.
[0299] Preparation 26
[0300] Formulation 26 is a dispersion prepared by the general method described above, which is 25% of Acer truncatum biochar, 20% of styrene / maleic anhydride copolymer dispersant, 8% of microfibrillated cellulose, 0.05% of an oil-based defoamer, and the remainder is deionized water.
[0301] Preparation 27
[0302] Formulation 27 is a dispersion prepared by the general method described above. The formulation is 14% paulownia biochar, 40% polyvinyl acetate dispersant, 6% microfibrillated cellulose, 0.8% silicone-based defoamer, and the remainder is deionized water.
[0303] Preparation 28
[0304] Formulation 28 is a dispersion prepared by the general method described above. The formulation is 41% hickory biochar, 40% quaternary ammonium salt dispersant, 7% microfibrillated cellulose, 2.5% oil-based defoamer, and the remainder is deionized water.
[0305] Preparation 29
[0306] Formulation 29 is a dispersion prepared by the general method described above. The formulation is 60% pine biochar, 24% benzyl methacrylate terpolymer dispersant, 8% microfibrillated cellulose, 0.5% oil-based defoamer, and the remainder is deionized water.
[0307] Preparation 30
[0308] Formulation 30 is a dispersion prepared by the general method described above. The formulation is 63% birch biochar, 24% fatty acid calcium dispersant, 13% microfibrillated cellulose, 0.5% oil-wax based defoamer, and the remainder is deionized water.
[0309] Preparation 31
[0310] Preparation 31 is a dispersion prepared by the general method described above, which is 45% fir biochar, 24% quaternary ammonium salt dispersant, 14% microfibrillated cellulose, and the rest is solvent.
[0311] Preparation 32
[0312] Formulation 32 is a dispersion prepared by the general method described above. The formulation is 23% fir biochar, 35% polyurethane-based dispersant, 14% microfibrillated cellulose, 0.7% oil-based defoamer, and the remainder is deionized water.
[0313] Preparation 33
[0314] Formulation 33 is a dispersion prepared by the general method described above. The formulation is 40% hemlock biochar, 15% polycarboxylic acid dispersant, 17% microfibrillated cellulose, 0.7% silicone-based defoamer, and the remainder is deionized water.
[0315] Preparation 34
[0316] Formulation 34 is a dispersion prepared by the general method described above. The formulation is 43% larch biochar, 15% potassium polyacrylate dispersant, 0.09% silicone defoamer, and the remainder is deionized water.
[0317] Preparation 35
[0318] Formulation 35 is a dispersion prepared by the general method described above. The formulation is 61% Japanese cedar biochar, 10% hydroxyethyl methylcellulose dispersant, 10% microfibrillated cellulose, 0.8% oil-based defoamer, and the remainder is deionized water.
[0319] Preparation 36
[0320] Formulation 36 is a dispersion prepared by the general method described above. The formulation is 52% Paulownia biochar, 10% saponified vegetable oil dispersant, 10% microfibrillated cellulose, 0.9% oil-based defoamer, and the remainder is deionized water.
[0321] Preparation 37
[0322] Formulation 37 is a dispersion prepared by the general method described above. The formulation is 53% coffee pulp biochar, 20% 2-amino-2methyl-1-propanol dispersant, 10% microfibrillated cellulose, 0.7% silicone defoamer, and the remainder is deionized water.
[0323] Preparation 38
[0324] Formulation 38 is a dispersion prepared by the general method described above, which is 41% Japanese cedar biochar, 30% polyethylene wax dispersant, 15% microfibrillated cellulose, 0.9% ethylene glycol emulsion defoamer, and the remainder is deionized water.
[0325] Preparation 39
[0326] Formulation 39 is a dispersion prepared by the general method described above. This formulation is 46% sycamore biochar, 20% ethoxylated linear fatty alcohol dispersant, 15% microfibrillated cellulose, 0.8% oil-wax defoamer, and the remainder is deionized water.
[0327] Preparation 40
[0328] Formulation 40 is a dispersion prepared by the general method described above. The formulation is 45% red laurel biochar, 10% alkyl polyamine dispersant, 15% microfibrillated cellulose, 0.9% oil-silica defoamer, and the remainder is deionized water.
[0329] Preparation 41
[0330] Formulation 41 is a dispersion prepared by the general method described above. This formulation is 40% red laurel biochar, 20% alkyd resin dispersant, 20% microfibrillated cellulose, 1.0% oil-silica based defoamer, and the remainder is deionized water.
[0331] Preparation 42
[0332] Formulation 42 is a dispersion prepared by the general method described above, which is 35% elm biochar, 30% monofunctional oil-alkylene oxide block copolymer dispersant, 20% microfibrillated cellulose, and the remainder is deionized water.
[0333] Preparation 43
[0334] Formulation 43 is a dispersion prepared by the general method described above, which is 40% elm biochar, 25% methacrylic acid dispersant, 10% microfibrillated cellulose, 0.5% polyether-based defoamer, and the remainder is deionized water.
[0335] Preparation 44
[0336] Formulation 44 is a dispersion prepared by the general method described above, which is 40% elm biochar, 25% stearic acid dispersant, 10% microfibrillated cellulose, 0.5 modified fatty acid-based defoamer, and the remainder is deionized water.
[0337] Preparation 45
[0338] Formulation 45 is a dispersion prepared by the general method described above, which is 40% elm biochar, 25% anionic polyether sulfate dispersant, 10% microfibrillated cellulose, 0.5% silicone-based defoamer, and the remainder is deionized water.
[0339] Preparation 46
[0340] Formulation 46 is a dispersion prepared by the general method described above, which is 40% elm biochar, 25% cationic polyacrylate and phosphate dispersant, 10% microfibrillated cellulose, 0.5% silicone defoamer, and the remainder is deionized water.
[0341] Preparation 47
[0342] Formulation 47 is a dispersion prepared by the general method described above. The formulation is 40% ash biochar, 40% ethoxylated fatty acid ester dispersant, 15% microfibrillated cellulose anticoagulant, and the remainder is deionized water.
[0343] Preparation 48
[0344] Formulation 48 is a dispersion prepared by the general method described above. This formulation is 40% ash biochar, 40% butyl acetate dispersant, 0.5% silicone-based defoamer, 0.1% kaison preservative, and the remainder is deionized water.
[0345] Preparation 49
[0346] Formulation 49 is a dispersion prepared by the general method described above, which is 23% elm biochar, 57% nitrogen-grafted polymer dispersant, 10% microfibrillated cellulose anticoagulant, 0.3% oil-based defoamer, 0.005% octanoyl hydroxamic acid preservative, and the remainder is deionized water.
[0347] Preparation 50
[0348] Formulation 50 is a dispersion prepared by the general method described above, which is 65% birch biochar, 25% fatty acid calcium dispersant, 5% microfibrillated cellulose anticoagulant, 0.75% oil-silica based defoamer, 0.09% peracetic acid preservative, and the remainder is deionized water.
[0349] Characterization of formulations
[0350] Scanning Electron Microscope (SEM) and Scanning Transmission Electron Microscopy (STEM) Imaging
[0351] like Figure 1A , 1B , 2A and 2B, some embodiments of the pigment dispersion compositions with carbonaceous particles derived from biochar as disclosed herein were imaged on SEM micrographs using a "sputtering process". The sputtering process is a specific form of scanning electron microscopy (SEM). It is typically used to reconstruct the topography of a sample and provide an image thereof. For Figure 1A , 1B, 2A and 2B, the dispersion sample is dried on an imaging substrate. Because the SEM uses electrons to produce the image, the sample must be conductive. Therefore, in the sputtering process, a thin layer of metal is applied to the dried particles before the sample is imaged. This is sputtering. Typically, a Leica EM SCD005 sputter coater or equivalent is used. For Figure 1A , 1B , 2A and 2B, the sputtering of the metal layer was performed with a current of 60 mA for 25 seconds. The thickness of the sputtered film is typically in the range of 2-20 nm.
[0352] Produced using Nova NANOSEM 45 Figure 1A , 1B , 2A and 2B. SEM uses a focused electron beam with a voltage of about 5 kV and an emission current that can be varied between 80-140 μA. The beam reacts with the sample and one or more detectors collect the resulting electrons to form an image. For the sputtering process, a SED Everhart-Thornley detector (ETD) is typically used as a detector. Imaging is performed under vacuum so that nothing interferes with the electrons in the beam. Pictures obtained with the sputtering process are opaque.
[0353] Figure 1A and 1B A random sample of biochar-derived particulate matter imaged from a first biochar pigment dispersion composition according to Formulation 16 is shown, Figure 2A and 2B A random sample of biochar-derived particulate matter imaged from a second biochar pigment dispersion composition according to Formulation 17 is shown. Figure 1B In the figure, two representative particles are indicated by surrounding oval circles, where the particle in the upper right portion of the image has a diameter of 46.62 nm, and the more representative particles in the lower right portion of the image have a diameter of 40.80 nm. Figure 2B In the image, two representative particles are represented by the surrounding oval circles, with the particle in the middle right portion of the image having a diameter of 53.45 nm and the more numerous particles in the lower right portion of the image having a diameter of 64.11 nm. The microscopist noted that Figure 1A , 1B , 2A and 2B show that each dispersion is monodisperse or nearly monodisperse, meaning that the particles appear to be all about the same size. The diameter of the microparticles from the first biochar pigment dispersion is between 40nm and 50nm, and the diameter of the microparticles from the second biochar dispersion is between 50nm and 65nm.
[0354] Figure 3 , 4, 5 and 6 are STEM images of random samples of pigment particles, wherein at least 95% by number of the particles or at least 100 particles have a diameter in the range between 15 nm and 25 nm. Figure 3 and 4 is a STEM image of biochar particles collected from Preparation 16. Figure 5 and 6 is a STEM image of biochar particles collected from Preparation 17.
[0355] Some embodiments of pigment dispersion compositions having carbonaceous particles derived from biochar as disclosed herein were imaged on STEM micrographs, referred to herein as "STEM processes". Figure 3 and Figure 4 Some embodiments of pigment dispersion compositions having carbonaceous particles derived from biochar as disclosed herein were imaged using the "Lacey STEM process" as defined herein. Figure 5 and Figure 6 An example image from a Lacey STEM process is depicted in . As defined herein, the Lacey STEM process is a specific form of Scanning Transmission Electron Microscopy (STEM). STEM is a technique used to provide images of thin samples of materials. An electron beam passes through the sample, giving very little information about the surface and more information about the shape and structure of the particles. In the Lacey STEM process, a FEI Nova NanoSEM 450 scanning electron microscope or equivalent instrument is used with a STEM bright field and dark field (DF) (BF DF) high angle annular dark field (HAADF) detector.
[0356] In the Lacey STEM process, a droplet of the diluted dispersion is added on top of a Lacey carbon transmission electron microscopy (TEM) film. The diluent is typically water if the dispersion is miscible in water, otherwise it is typically acetone. The Lacey structure explains Figure 5 and Figure 6 The dispersion was diluted enough so that when the image was scanned, there were not many particles on the web. The naturally formed clusters were evident due to the dilution process on the Lacey web substrate. Surprisingly, the particles had a very high structure after grinding. In contrast, the branches in the liquid dispersion of petroleum carbon black are referred to as "transient structure" and this structure is typically broken up by grinding. Characterization of many of the dispersion embodiments disclosed herein was performed based on the methods and images produced by the Lacey STEM process. Other imaging processes, such as sputtering processes, do not account for the naturally formed cluster characteristics.
[0357] The FEI Nova NanoSEM 450 electron microscope is able to take STEM and SEM images simultaneously. When taking a picture with an image in "STEM mode", two detectors are used simultaneously. This is why it is possible to acquire images of the same object in both modes. The screen is split and images are presented from both detectors. When the image in one mode moves, the image in the other mode moves with it. To obtain a good resolution of the image, the instrument is zoomed in for fine focus, and then the instrument is zoomed out to about an integer magnification, so that the clarity is even better at this magnification. The brightness and contrast of the image are adjusted as needed. The adjustments are then paused so that the image can be saved.
[0358] A monodisperse dispersion is one in which the variation in particle size is very small, forming a narrow (unimodal) distribution around a mean value.
[0359] Figure 3 , 4 , 5 and 6 are STEM images of random samples of pigment particles, wherein at least 95% of the particles by number or at least 100 particles have a diameter in the range between 15 nm and 25 nm. The STEM images show that Formulations 16 and 17 form nearly monodisperse particles. Figure 3 and Figure 4 is a STEM image of the biochar particles used in Formulation 16. Figure 5 and Figure 6 is a Lacey STEM image of the biochar particles used in Formulation 17.
[0360] Figure 7 and 8 is a scanning electron microscope image of a plant charcoal raw material that can be used to make a Figure 1A and 1B A feedstock of submicron carbon particles of the type depicted. Figure 7 The plant charcoal raw material described in the invention is used in preparation 17, Figure 8 The plant charcoal raw material depicted in was used in preparation 16.
[0361] Laser scattering
[0362] Laser scattering measurements on liquid dispersions were performed using the following "LDA protocol":
[0363] (a) The dispersion sample was diluted with water to a concentration of 0.0010 vol. %.
[0364] (b) Analyze the samples using a Malvern Mastersizer 2000 laser diffraction particle size analyzer or equivalent.
[0365] (c) The size range is set to: 0.020μm to 2000μm.
[0366] (d) The sample is analyzed using Mie scattering to analyze the light intensity distribution pattern.
[0367] The particle distribution of Formulation 11 was observed to be as follows: D10 130 nm, D50 333 nm, D90 534 nm. The particle distribution of Formulation 12 was observed to be as follows: D10 250 nm, D50 605 nm, D90 750 nm. It should be noted that the particle size indicated by the laser diffraction number is usually higher than the particle size calculated from the STEM image because the laser diffraction number accounts for the entire particle cluster and particle chain. The STEM image shows the individual particle size.
[0368] Surface area determination
[0369] The surface area is measured by static pressure gas adsorption, also known as specific surface area analysis (static volume method) by gas physical adsorption. The surface of the sample is prepared by heating the sample to 90 ° C for 0.5 hours under vacuum in the first round of degassing. In the subsequent second round of degassing, the sample is heated to 200 ° C for 3 hours under vacuum. The sample is then exposed to nitrogen, and a certain amount of gas is adsorbed to the surface of the particles. The amount of adsorbed gas is measured at different relative pressures. The surface area is calculated using the following Brunauer-Emmett-Teller (BET) equation.
[0370]
[0371] A series of three relative pressure data points were collected on a Micromeritics Tristar II 3020 instrument.
[0372] The surface area of the particles in Formulation 11 was observed to be 375 m 2 g -1 The surface area of the particles in Formulation 12 was observed to be 745 m 2 g -1 .
[0373] Raman spectroscopy
[0374] Raman spectroscopy can be used as a method to identify different carbon phases within carbonaceous materials. For example, Raman spectroscopy can be used to distinguish between several types of carbon, such as diamond, graphite, and diamond-like carbon. The Raman spectra of nanocrystalline and amorphous carbon are dominated by D (D for disorder) and G (G for graphite) peaks with different intensities, positions, and bandwidths. -1 The G band at 1350 cm corresponds to the symmetric E mode in graphite-like materials, while the -1 The D band at φ originates from the confinement of graphite domain size caused by grain boundaries or defects.
[0375] Raman spectroscopic analysis of two representative biochar samples disclosed herein is as follows: Raman measurements were performed with a "LabRam" spectrometer equipped with a "BX40 Olympus" microscope in backscattering geometry (180°). An Ar+ ion laser (514.5 nm wavelength) and a 1800 gr / mm grating were used in these measurements.
[0376] Three spectra at random spots were obtained from each sample. Sample 1 is shown in Fig.10 and 11 (Spectra 1, 2 and 3 and baseline corrected spectra 1-b, 2-b and 3-b). Sample 1 is a random sample of pigment particles collected from Formulation 16. Sample 2 is also shown in Fig.10 and 11 (Spectra 4, 5, and 6 and baseline corrected spectra 4-b, 5-b, and 6-b). Sample 2 is a random sample of pigment particles collected from Formulation 17.
[0377] The original spectra were baseline corrected and analyzed using sp 2 D(1350cm -1 ) and G(1590cm -1 The data of these bands: position, width (full width at half maximum), intensity (peak area) and peak height are shown in Table 2.
[0378] Table 2
[0379]
[0380]
[0381] Two formulas are found in the literature for calculating the grain size of graphitic carbon.
[0382] Use intensity ratio I D / I G , TUINSTRA and KOENIG (1970) proposed a formula for calculating the grain size of graphite carbon:
[0383]
[0384] We call it the TK model. This model can only be applied to pure sp from graphite to nanographite samples. 2 Carbon, of which L a For each Raman measurement, the L determined by the TK formula is reported in Table 1 a (nm) TK The mean value with standard deviation is given for each sample.
[0385] ColorLab Analysis
[0386] Almost no black pigment is completely black. Most black pigments have a slight hue (color). A perfect black sample absorbs all wavelengths of light and reflects no hue. Laboratory color space testing can be used to analyze the hue of a black pigment. While most black pigments are not "perfect," it is assumed that they are dark enough to prevent most incident light from reaching the detector. The hue of samples of the pigment dispersion formulations of the embodiments disclosed herein including carbonaceous particulate matter derived from biochar was tested according to the following "Black Pigment Color Analysis Protocol."
[0387] Dilute the sample in white suspension:
[0388] 2% Hydroxypropyl methylcellulose (to slow separation)
[0389] 4% TiO2 (to provide a white background)
[0390] The balance was deionized water.
[0391] The dilution was semi-quantitative, where 10-14 mg of pigment was added to 10 g of white suspension.
[0392] The sample was mixed thoroughly and placed in a 10 mm disposable (PS) cuvette.
[0393] The white suspension was run as a blank standard and the samples were read against it, so the value reported is the difference.
[0394] Use a Hunter Instruments UltraScan PRO or equivalent with the following settings:
[0395] CIELab / D65 / 10Deg / Sphere / RSEX / 0.190" / 10mm PS Cuvette
[0396] Analysis of five representative dispersants prepared according to the techniques disclosed herein was performed using the black pigment color analysis protocol.
[0397] Table 3 gives the values in tabular form.
[0398] Table 3
[0399] ID L* a* b* dL* <![CDATA[TiO2 blank]]> 84.99 -0.16 0.69 84.99 Sample 1 51.9 -0.41 0.16 -33.09 Sample 2 57.97 -0.36 0.84 -27.02 Sample 3 52.48 -0.34 0.87 -32.52 Sample 4 48.97 -0.24 1.22 -36.02 Sample 5 60.84 0.04 2.17 -24.15
[0400] Fig.12 A graph showing a graphical representation of the detected colors as plotted in the CIE Lab color space is shown. It should be noted that the distance of the sample from the origin is an indication of the magnitude of the color measured, however, the dilution procedure has not been refined to give quantitative results and errors of up to about 50% are expected.
[0401] Dynamic light scattering submicron particle size distribution
[0402] Dynamic light scattering (DLS) is a technique that can be used to determine the size distribution curve of small particles in suspension. The following DLS protocol was used to determine the particle size characteristics of particulate material in a dispersion formulation including carbonaceous particulate matter derived from biochar as disclosed herein.
[0403] (a) A sample of the dispersion was prepared by diluting in deionized water.
[0404] (b) Malvern Zetasizer Nano Z DLS or equivalent particle analyzer is used to analyze the samples.
[0405] (c) Set to a backscattering angle of 173° at 25°C.
[0406] Each of the two samples of submicron particles is measured using the DLS scheme. Sample A (1-3) is a random sample of pigment particles collected from preparation 16. Sample B (1-3) is a random sample of pigment particles collected from preparation 17. Use dynamic light scattering based on intensity and based on polystyrene latex with a refractive index of 1.590 and an absorptivity of 0.010 as a standard to measure. Even if the material used is not exactly polystyrene, the material is often used as a reference in polymer science at nanoscale. It should be noted that the particle size represented by the DLS number is usually larger than the particle size calculated from the STEM image, because the DLS number explains the entire particle cluster and chain-like grape-like morphology. The STEM image shows a single particle size. The results of DLS measurement are shown in Table 4 below.
[0407] Table 4
[0408]
[0409] The data from three measurements for each of the two formulations are shown in Tables 5-10 below. Figures 13 to 18 The data in Tables 5-10 are plotted separately.
[0410] Table 5 - Sample A1
[0411]
[0412]
[0413] Table 6 - Sample A2
[0414]
[0415] Table 7 - Sample A3
[0416]
[0417]
[0418] Table 8 - Sample B1
[0419]
[0420] Table 9 - Sample B2
[0421]
[0422]
[0423] Table 10 - Sample B3
[0424]
[0425] Dispersant Identification
[0426] Dispersants and surfactants have been tested to identify suitable candidates. Technical requirements are to produce a stable fluid-based dispersion in which the particles do not settle to the bottom of the container; the dispersion does not "break" when diluted in water or solvent; the dispersion does not gel during or after manufacturing; the dispersion remains fluid and viscous during manufacturing; the dispersion does not separate from the water or solvent after manufacturing; and the dispersant and formulation facilitate achieving submicron particle size during manufacturing.
[0427] To obtain the most environmentally friendly composition, preferred dispersants are selected to be petroleum-free, low petroleum-based, or petroleum-derived; have as much biorenewable content as possible; have zero to low VOC content, and be non-toxic to aquatic life, ecology, and human health.
[0428] Specific dispersants work better with specific carbons, and dispersions may work better for specific applications. Adding a defoamer helps keep the viscosity low for manufacturing. Also, adding an anticoagulant to prevent the pigment particles from settling in the dispersion when stored may be beneficial.
[0429] In one embodiment, the pigment is made from pulverized wood biochar. It is compatible with dispersants made from modified, structured or unstructured acrylic or acrylate polymers or copolymers having pigment affinity groups. The acrylic copolymers are branched or comb-shaped and create a matrix around the pigment particles, keeping them suspended in solution. The pigment is also compatible with hydroxyl-functional carboxylates having pigment affinity groups.
[0430] In a second embodiment, the pigment is made from pulverized wood biochar. It is compatible with sodium lignin sulfonate or lignin sulfonic acid, a sodium salt-based dispersant, and a hydroxy-functional carboxylic acid ester with pigment-affinic groups.
[0431] Both the first and second example dispersions are compatible with biorenewable rapeseed oil as a defoaming agent.
[0432] It has been found that the use of unstructured or structured acrylic polymer or copolymer dispersants or unstructured or structured acrylate polymer or copolymer dispersants or sodium lignin sulfonate or sodium lignin sulfonate salt-based dispersants can enhance the jetness of vegetable charcoal pigments. y .
[0433] It should be understood that the compositions described herein may also be free of dispersants. In other words, the present disclosure also relates to a pigment preparation comprising carbonaceous particulate matter derived from biochar and a grinding fluid, and is free of dispersants.
[0434] It is contemplated that the pigment preparation may be provided as a carbonaceous particulate matter derived from biochar, having the following characteristics:
[0435] A random sample of carbonaceous particles imaged on a two-dimensional scanning transmission electron micrograph obtained from the sputtering process at a magnification of at least 50,000 times shows that the particles are spherical in shape;
[0436] A random sample of the carbonaceous particulate matter imaged on a scanning transmission electron micrograph 2D micrograph from a Lacey STEM process at a magnification of at least 50,000 times shows a circularity of the particles greater than about 0.8 with a standard deviation of less than about 30% of the circularity;
[0437] A random sample of carbonaceous particles imaged on scanning transmission electron micrographs from a Lacey STEM process at a magnification of at least 50,000 times showed that the particles had smooth surfaces;
[0438] A random sample of carbonaceous particles imaged on scanning transmission electron microscopy 2D micrographs from the Lacey STEM process at a magnification of at least 50,000 times showed that the carbonaceous particles had a chain-like grape-bunch-like morphology;
[0439] A random sample of the carbonaceous particulate matter exhibits particles having diameters less than about 100 nm, or less than about 80 nm, or less than about 60 nm, with a standard deviation of less than 25% of the mean diameter, as calculated from spatial measurements of a random sample of the particles imaged on two-dimensional micrographs from a Lacey STEM process at a magnification of at least 50,000 times, with a standard deviation of less than 25% of the mean diameter;
[0440] a random sample of the carbonaceous particulate matter exhibits an average diameter of the particles in the range of about 10 nm to about 100 nm, or in the range of about 10 nm to about 80 nm, or in the range of 10 nm to 60 nm, with a standard deviation of less than 25% of the average diameter as calculated from spatial measurements of a random sample of the particles imaged on scanning transmission electron micrographs from a Lacey STEM process at a magnification of at least 50,000 times;
[0441] A random sample of the carbonaceous particulate material exhibits a circularity of the particles of at least about 0.8 or at least about 0.75 with a standard deviation of less than 30% of the circularity, the circularity being calculated from spatial measurements of the random sample of the particles imaged on a scanning transmission electron micrograph two-dimensional micrograph from a Lacey STEM process at a magnification of at least 50,000 times;
[0442] A random sample of carbonaceous particulate matter shows a surface area of carbonaceous particulate matter, as measured by static volumetric gas physisorption, of greater than or equal to about 300 m 2 g -1 .
[0443] Although preferred embodiments of the present invention have been shown and described herein, it will be apparent to those skilled in the art that these embodiments are provided by way of example only. Without departing from the present invention, those skilled in the art will now appreciate that many variations, changes and substitutions are possible. It should be understood that various alternatives to the embodiments of the present invention described herein can be used to implement the present invention. The following claims are intended to define the scope of the present invention, and thus encompass methods and structures and their equivalents within the scope of these claims.
Claims
1. Use of a pigment dispersion formulation as a grinding base in a mill to reduce the size of carbonaceous particulates derived from biochar to submicron size, the pigment dispersion formulation comprising a combination of carbonaceous particulates derived from biochar, a dispersant, microfibrillated cellulose and a grinding fluid.
2. The use according to claim 1, wherein The average size of a random sample of the carbonaceous particles ranges between 118 nm and 171 nm and the polydispersity index ranges between 0.05% and 0.15% of the average size as measured by dynamic light scattering.
3. The use according to claim 2, wherein The particles of the carbonaceous particulate matter have an average diameter less than 100 nm with a standard deviation less than 25% of the average diameter calculated from spatial measurements of a random sample of the particles imaged on two-dimensional micrographs from a Lacey STEM process at a magnification of at least 50,000 times.
4. The use according to claim 1, wherein The concentration of polycyclic aromatic hydrocarbons (PAH) in the biochar is lower than 10 mg / kg.
5. The use according to claim 4, wherein The polycyclic aromatic hydrocarbons (PAH) in the biochar were undetectable.
6. The use according to claim 2, wherein: Analysis of random samples of particles of the carbonaceous particulate matter imaged on scanning transmission electron micrographs at a magnification of at least 50,000 times from the sputtering process showed that the particles were spherical in shape.
7. The use according to claim 2, wherein: A random sample of particles of the carbonaceous particulate matter imaged on a scanning transmission electron micrograph 2D micrograph from a Lacey STEM process at a magnification of at least 50,000 times showed that the particles had a smooth surface.
8. The use according to claim 2, wherein Under laser excitation at a wavelength of 514.5 nm using a 1800 gr / mm grating, the formulation exhibited a G position at 1580 cm -1 and 1605cm -1 and Raman spectra with I(D) / I(G) ratios between 2.49 and 3.
07.
9. The use according to claim 1, wherein The surface area of the particles of the carbonaceous particulate matter as measured by static volumetric gas physisorption is greater than or equal to 300 m 2 g -1 .
10. The use according to claim 2, wherein: The blackness My is greater than 250.
11. The use according to claim 2, wherein: The blackness Mc is greater than 250.
12. The use according to claim 2, wherein: The tinting strength is greater than or equal to 94%.
13. The use according to claim 1, wherein The color fastness is 8.
14. Use of a pigment dispersion formulation as a grinding base in a mill to reduce the size of carbonaceous particulates derived from biochar to submicron size, the pigment dispersion formulation comprising carbonaceous particulates derived from biochar, a 100% active dispersant, microfibrillated cellulose and a combination of an activator / support.
15. The use according to claim 14, wherein The average size of a random sample of the carbonaceous particles ranges between 118 nm and 171 nm and the polydispersity index ranges between 0.05% and 0.15% of the average size as measured by dynamic light scattering.
16. The use according to claim 15, wherein The particles of the carbonaceous particulate matter have an average diameter less than 100 nm with a standard deviation less than 25% of the average diameter calculated from spatial measurements of a random sample of the particles imaged on two-dimensional micrographs from a Lacey STEM process at a magnification of at least 50,000 times.
17. The use according to claim 14, wherein The concentration of polycyclic aromatic hydrocarbons (PAH) in the biochar is less than 10 mg / kg.
18. The use according to claim 17, wherein The polycyclic aromatic hydrocarbons (PAH) in the biochar were undetectable.
19. The use according to claim 15, wherein Analysis of random samples of particles of the carbonaceous particulate matter imaged on scanning transmission electron micrographs 2D micrographs from the sputtering process at a magnification of at least 50,000 times showed that the particles were spherical in shape.
20. The use according to claim 15, wherein A random sample of particles of the carbonaceous particulate matter imaged on a scanning transmission electron micrograph 2D micrograph from a Lacey STEM process at a magnification of at least 50,000 times showed that the particles had a smooth surface.
21. The use according to claim 15, wherein Under laser excitation at a wavelength of 514.5 nm using a 1800 gr / mm grating, the formulation exhibited a G position at 1580 cm -1 and 1605cm -1 and Raman spectra with I(D) / I(G) ratios between 2.49 and 3.
07.
22. The use according to claim 14, wherein The surface area of the particles of the carbonaceous particulate matter as measured by static volumetric gas physisorption is greater than or equal to 300 m 2 g -1 .
23. The use according to claim 15, wherein The blackness My is greater than 250.
24. The use according to claim 15, wherein The blackness Mc is greater than 250.
25. The use according to claim 15, wherein The tinting strength is greater than or equal to 94%.
26. The use according to claim 14, wherein The color fastness is 8.