Composition and method for making green body or printed article using the same
Through the use of high-load particle compositions, the shear thickening behavior, stability and transparency problems in additive manufacturing are solved, efficient and low-cost production of complex components is achieved, and the quality and stability of green bodies and printed products are improved. sex.
Patent Information
- Application Number
- CN202080081973.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-27
- Filing Date
- 2020-11-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-11-24
AI Technical Summary
The curable compositions used in the existing additive manufacturing technology have problems such as shear thickening behavior, equipment failure, high cost, poor stability, low optical transparency and shrinkage, making it difficult to quickly produce glass and ceramic components with complex geometric morphology.
A composition containing high load particles (about 65% or higher) was developed, which is basically free of solvents, using photoinitiators, curing agents and organic binders, which reduces shear thickening behavior and improves particle stability. and curing rate compositions for printing green bodies and articles, achieving high-quality, low-cost, optically transparent manufacturing.
It achieves a reduction in additive manufacturing time and cost, improves the stability and optical transparency of the composition, reduces equipment damage and sintering and shrinkage, and improves the dimensional stability and strength of green bodies and printed products.
Smart Images

Figure CN114760953B_ABST
Abstract
Description
[0001] Related Applications Cross Reference
[0002] This application claims priority under 35 USC §119 to U.S. Provisional Application No. 62 / 941,155, filed on November 27, 2019, the contents of which are incorporated herein by reference in their entirety. Technical Field
[0003] The present disclosure relates generally to compositions and methods for making green bodies or printed articles using the same, and more particularly to compositions and methods for making green bodies containing particles or printed articles using the same. Background Art
[0004] It is known to use additive manufacturing (AM) techniques to form green bodies and / or printed articles. For example, AM can be used for rapid prototyping (RP) and / or manufacturing of specialty components. AM can include: stereolithography (SLA), three-dimensional (3D) printing, fused deposition modeling (FDM), solid free form manufacturing (SFF) and / or layered object manufacturing (LOM). AM methods can be controlled based on computer-aided (CAD) data. AM methods can include layer-by-layer deposition. AM can produce parts with complex geometries without the need for complex tools and with minimized production setup time.
[0005] The use of curable compositions in AM processes is known. Printing techniques include the methods described above as well as screen printing, flexographic printing, jet dispersion and / or inkjet printing. Printing techniques can deposit the composition in a predetermined pattern. When a printing technique is used to apply a curable material, the curable material can undergo a curing process.
[0006] However, AM of known curable compositions using shear thickening (e.g., thixotropy) can limit production rates and / or cause equipment failures (e.g., clogging, wear), which can increase the time and / or cost associated with AM. In addition, curable compositions comprising particles can have agglomeration problems, which can cause equipment failures. Similarly, curable compositions comprising particles may have poor particle wetting. In addition, curable compositions comprising particles can have limited stability (e.g., before precipitation and / or particle precipitation occurs), which increases the cost and / or complexity of AM. Curable compositions typically include solvents (e.g., protonated solvents, such as water) in combination with rheology modifiers (e.g., thickeners). Using solvents and / or thickeners can impair curing speed. In addition, using solvents and / or thickeners can reduce the quality of the resulting green body or printed product. For example, due to the capture of microbubbles, large pores are formed, and / or the incomplete removal of binders, thickeners and / or solvents, the green body or printed product may include poor optical transparency (e.g., not optically transparent). Furthermore, such compositions may result in excessive shrinkage during sintering and / or reduce the strength of the green body and / or printed article.
[0007] Alternatively, 3D glass- and ceramic-based parts can be manufactured through processes such as molding and pressing. These processes require special tools (e.g., molds), which can make it difficult to produce parts quickly. The more complex the geometry of the part, the longer and more expensive it will be to produce the part through traditional methods (e.g., molding and pressing). For short-run, complex glass- and ceramic-based parts, additive manufacturing can be an attractive option.
[0008] Therefore, there is a need to minimize (e.g., reduce, decrease, eliminate) the shear thickening behavior in the composition. In addition, there is also a need for a composition comprising an increased particle load (e.g., % by weight), the composition comprising a printable viscosity and confirming increased stability (e.g., sedimentation (settle) is reduced, sedimentation (sedimentation) is reduced). In addition, there is a need to reduce the time-consuming and / or cost-related AM using such compositions. In addition, there is a need for a composition that cures more quickly. In addition, there is a need for a composition that can produce a green body and / or printed product comprising good optical transparency. In addition, there is a need for a composition that can produce a green body and / or printed product comprising good dimensional stability. In addition, there is a need for a composition that can produce a printed product with reduced shrinkage and / or increased strength. Summary of the invention
[0009] Compositions and methods for making green bodies and / or printed articles using the same are described herein. The compositions of the present disclosure can reduce the time and / or cost associated with, for example, additive manufacturing to produce green bodies and / or printed articles. In addition, the compositions of the present disclosure can include highly loaded particles (e.g., about 65% by weight or higher) with good particle stability and / or wettability. The methods using the compositions of the present disclosure can additionally produce optically transparent green bodies and / or printed articles exhibiting good dimensional stability and / or mechanical strength.
[0010] The compositions of the embodiments of the present disclosure can reduce the time and / or cost associated with additive manufacturing, producing green bodies and / or producing printed products. Such compositions have reduced shear thickening behavior (e.g., shear thickening behavior decreases, or there is no shear thickening behavior), which can achieve increased processing speed and / or reduced equipment damage. Such compositions include good particle wetting, which can achieve an increase in composition stability (e.g., reducing and / or reducing precipitation (settle) and / or precipitation (sedimentation)). Such compositions can include printable viscosities (e.g., within the range of about 100 millipascals-seconds (mPa-s) to about 7000mPa-s), which are used for additive manufacturing even when the composition includes high-load (e.g., about 65% by weight or more) particles. Providing a composition that is substantially free of solvent can increase the solidification rate of the composition, which can reduce processing time. Providing a composition that is substantially free of solvent can reduce (e.g., reduce, eliminate) the use of rheology modifiers and increase composition homogeneity, which can improve the quality of the resulting green bodies and / or printed products. Providing a composition that is substantially free of solvent can increase the optical clarity of the resulting green body and / or printed article. Providing a composition comprising a high loading (e.g., about 65% by weight or more) of particles can reduce (e.g., reduce) the material cost associated with other components of the composition. Providing a composition comprising particles (the particles comprising an accessible surface area substantially comprising oxides) (e.g., a composition without a surface modification of the particles and / or a coupling agent) can reduce the cost of the composition.
[0011] The composition of the embodiment of the present disclosure can be used for the manufacturing method of green body and / or printed product. As discussed above, the method of the composition of the embodiment of the present disclosure can reduce the time and / or cost associated with such method. In addition, the method of the embodiment of the present disclosure can produce high-quality green body and / or printed product. Providing a composition comprising high-load (e.g., about 65% by weight or more) particles can increase the dimensional stability and / or strength of green body and / or printed product. Providing a composition comprising high-load (e.g., about 65% by weight or more) particles can reduce (e.g., reduce) the shrinkage associated with sintering to form printed products. Providing a composition comprising high-load (e.g., about 65% by weight or more) can increase the optical transparency of green body and / or printed product. Providing a composition comprising particles (the particles include an accessible surface area substantially comprising oxides) (e.g., a composition without a surface modification and / or coupling agent of particles) can increase the optical transparency of green body and / or printed product. Providing a composition substantially free of solvent can increase the dimensional stability and / or strength of green body and / or printed product. Providing a substantially solvent-free composition can reduce (eg, minimize) shrinkage associated with sintering to form a printed article. Providing a substantially solvent-free composition can increase the optical clarity of a green body and / or a printed article.
[0012] Some exemplary embodiments of the present disclosure are described below, and it is to be understood that any features of the various embodiments may be used alone or in combination with each other.
[0013] In some embodiments, the composition will include particles that account for 5% or more (% weight) of the composition. The composition will include a photoinitiator. The composition will include a curing agent that includes dipropylene glycol diacrylate. The composition will include a dispersant that includes a phosphate ester. The composition will include an organic binder that includes isobornyl methacrylate. The composition will be substantially free of solvent.
[0014] In other embodiments, the weight % of the particles will be about 65% or higher.
[0015] In other embodiments, the composition can include a viscosity range of about 100 millipascal-seconds (mPa-s) to about 7000 mP-s.
[0016] In some embodiments, the composition will include particles that will account for 65% or more (% weight) of the composition without solvent. The composition will include a photoinitiator. The composition will include a curing agent. The composition will include a dispersant. The composition will include an organic binder. The composition may include a viscosity range that can be about 100 millipascal-seconds (mPa-s) to about 7000 mP-s. The composition will be substantially free of solvent.
[0017] In other embodiments, the organic binder may include isobornyl methacrylate.
[0018] In other embodiments, the curing agent may include dipropylene glycol diacrylate.
[0019] In other embodiments, the dispersant may include a phosphate ester.
[0020] In even other embodiments, the viscosity may range from about 3,000 mPa-s to about 5,000 mP-s.
[0021] In other embodiments, the weight % of the particles may range from about 70 weight % to about 80 weight %.
[0022] In other embodiments, the particles may comprise a surface pH of about 9 or greater.
[0023] In even other embodiments, the surface pH of the particles may range from about 10 to about 12.
[0024] In other embodiments, the particles may include a median particle size range of about 3 microns to about 7 microns.
[0025] In other embodiments, the particles may include glass-based particles.
[0026] In other embodiments, the particles may include ceramic-based particles.
[0027] In other embodiments, the total weight % of the photoinitiator, curing agent, and dispersant ranges from about 1 weight % to about 15 weight %.
[0028] In other embodiments, the composition comprises a precipitation rating of 6 or greater after about 1 day.
[0029] In other embodiments, the organic binder may include one or more of an acrylate, an epoxide, or a urethane.
[0030] In other embodiments, the particles may include an accessible surface area substantially entirely comprised of oxide.
[0031] In some embodiments, a method of making a green body may include producing a composition. The composition may include particles that account for 5% or more (% weight) of the composition. The composition may include a photoinitiator. The composition may include a curing agent that may include dipropylene glycol diacrylate. The composition may include a dispersant that may include a phosphate ester. The composition may include an organic binder that includes isobornyl methacrylate. The composition may be substantially solvent-free. The method may include printing the green body using the composition. The method may include curing the green body.
[0032] In other embodiments, the weight % of the particles will be about 65% or higher.
[0033] In other embodiments, the composition can include a viscosity range of about 100 millipascal-seconds (mPa-s) to about 7000 mP-s.
[0034] In some embodiments, a method of making a green body may include producing a composition. The composition may include particles that account for 65% or more (% weight) of the composition. The composition may include a photoinitiator. The composition may include a curing agent. The composition may include a dispersant. The composition may include an organic binder. The composition may include a viscosity range that may be about 100 millipascal-seconds (mPa-s) to about 7000 mP-s. The composition may be substantially solvent-free. The method may include printing the green body with the composition. The method may include curing the green body.
[0035] In other embodiments, the green body may be optically transparent.
[0036] In some embodiments, a method of making a printed article may include producing a composition. The composition may include particles that account for 65% or more (% weight) of the composition. The composition may include a photoinitiator. The composition may include a curing agent. The composition may include a dispersant. The composition may include an organic binder. The composition may include a viscosity range that may be about 100 millipascal-seconds (mPa-s) to about 7000 mP-s. The composition may be substantially solvent-free. The method may include printing a green body using the composition. The method may include curing the composition. The method may include heating the cured green body to remove the organic binder to form a porous article. The method may include sintering the porous article to form a printed article.
[0037] In some embodiments, a method of making a printed article may include producing a composition. The composition may include particles that occupy 5% by weight or more (% weight) of the composition. The composition may include a photoinitiator. The composition may include a curing agent that may include dipropylene glycol diacrylate. The composition may include a dispersant that may include a phosphate ester. The composition may include an organic binder that includes isobornyl methacrylate. The composition may be substantially solvent-free. The method may include printing a green body using the composition. The method may include curing the green body. The method may include heating the cured green body to remove the organic binder to form a porous article. The method may include sintering the porous article to form a printed article.
[0038] In other embodiments, the weight % of the particles will be about 65% or more of the composition.
[0039] In other embodiments, the composition can include a viscosity range of about 100 millipascal-seconds (mPa-s) to about 7000 mP-s.
[0040] In other embodiments, the printed article may be optically clear.
[0041] In even other embodiments, the viscosity may range from about 3,000 mPa-s to about 5,000 mPa-s.
[0042] In other embodiments, the composition may include a photoinitiator, a curing agent, and a dispersant in an amount ranging from about 1 wt % to about 15 wt %.
[0043] In other embodiments, the particles may include glass-based particles.
[0044] In other embodiments, the particles may include ceramic-based particles.
[0045] In other embodiments, the weight % of the particles is from about 70% to about 80% by weight of the composition.
[0046] In other embodiments, the particles may include an accessible surface area that may be substantially entirely comprised of oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The above features and advantages and other features and advantages of the embodiments of the present disclosure will be better understood by reading the following detailed description with reference to the accompanying drawings, in which:
[0048] Figure 1 The flowchart of the present disclosure shows an exemplary method of implementing the present disclosure;
[0049] Figure 2Schematically showing the steps in the method of an embodiment of the present disclosure;
[0050] Figure 3 Schematically showing the steps in the method of an embodiment of the present disclosure;
[0051] Figure 4 Schematically showing the steps in the method of an embodiment of the present disclosure;
[0052] Figure 5 schematically showing steps in a method of an embodiment of the present disclosure; and
[0053] Figure 6 A printed article according to an embodiment of the present disclosure is schematically shown.
[0054] Throughout this disclosure, the drawings are used to emphasize certain aspects. Thus, unless otherwise explicitly stated, the relative sizes of the various regions, parts, and substrates shown in the drawings should be assumed to be proportional to their actual relative sizes. DETAILED DESCRIPTION
[0055] Embodiments will be described more fully herein with reference to the accompanying drawings, in which exemplary embodiments are shown. Whenever possible, the same reference numerals are used throughout the drawings to represent the same or similar parts. However, the claims may include many different aspects of various embodiments and should not be construed as being limited to the embodiments set forth herein.
[0056] Unless otherwise specified, the discussion of features of some embodiments may be equally applicable to corresponding features of any embodiment of the present disclosure. For example, throughout the present disclosure, the same part number may indicate that, in some embodiments, the features referred to are consistent with each other, and unless otherwise specified, the discussion of the features referred to in one embodiment may be equally applicable to the features referred to in any other embodiment of the present disclosure.
[0057] The compositions of embodiments of the present disclosure include particles. In some embodiments, the particles include glass-based particles. In some embodiments, the particles include ceramic-based particles.
[0058] As used herein, "glass-based" includes both glass and glass-ceramic, wherein the glass-ceramic has: one or more crystalline phases, and an amorphous residual glass phase. Glass-based materials cool or have cooled to become glass, glass-ceramic and / or become glass-ceramic materials after further processing. Glass-based materials (e.g., glass-based substrates) can include amorphous materials (e.g., glass) and optionally one or more crystalline materials (e.g., ceramics). Amorphous materials and glass-based materials can be strengthened. As used herein, the term "strengthened" can refer to materials that have been chemically strengthened by, for example, exchanging smaller ions in the substrate surface with larger ions, as discussed below. However, other strengthening methods known in the art can also be used, such as using thermal tempering or the mismatch of thermal expansion coefficients between substrate portions to produce compressive stress and central tension regions to form a strengthened substrate. Exemplary glass-based materials (which may be free of lithium oxide or contain lithium oxide) include soda-lime silicate glass, alkali aluminosilicate glass, alkali-containing borosilicate glass, alkali-containing aluminoborosilicate glass, alkali-containing phosphosilicate glass, and alkali-containing aluminophosphosilicate glass. In one or more embodiments, the glass-based material may include, in terms of mole percent (mol%), SiO2 from about 40 mol% to about 80%, Al2O3 from about 10 mol% to about 30 mol%, B2O3 from 0 mol% to about 10 mol%, ZrO2 from 0 mol% to about 5 mol%, P2O5 from 0 mol% to about 15 mol%, TiO2 from 0 mol% to about 2 mol%, R2O from 0 mol% to about 20 mol%, and RO from 0 mol% to about 15 mol%. As used herein, R2O refers to alkali metal oxides such as Li2O, Na2O, K2O, Rb2O, and Cs2O. As used herein, RO refers to MgO, CaO, SrO, BaO, and ZnO. In some embodiments, the glass-based substrate may also optionally include 0 mol % to about 2 mol % of each of the following: Na2SO4, NaCl, NaF, NaBr, K2SO4, KCl, KF, KBr, As2O3, Sb2O3, SnO2, Fe2O3, MnO, MnO2, MnO3, Mn2O3, Mn3O4, Mn2O7. "Glass-ceramics" include materials produced by controlled crystallization of glass. In some embodiments, the glass-ceramics have a crystallinity of about 1% to about 99%. Examples of suitable glass ceramics may include Li2O-Al2O3-SiO2 system (i.e., LAS system) glass ceramics, MgO-Al2O3-SiO2 system (i.e., MAS system) glass ceramics, ZnO×Al2O3×nSiO2 (i.e., ZAS system) and / or glass ceramics including a main crystalline phase containing β-quartz solid solution, β-spodumene, cordierite, petalite and / or lithium disilicate. The glass ceramic substrate may be strengthened using the strengthening process described herein.In one or more embodiments, the MAS system glass ceramic substrate can be strengthened in a Li2SO4 molten salt to generate 2Li. + Mg 2+ In some embodiments, a substrate comprising a glass-based substrate can be optically transparent.
[0059] As used herein, "ceramic-based" includes both ceramics and glass-ceramics, wherein the glass-ceramics have: one or more crystalline phases, and an amorphous residual glass phase. In some embodiments, a ceramic-based material can be formed by heating a glass-based material to form a ceramic (e.g., crystalline) portion. In other embodiments, the ceramic-based material may include one or more nucleating agents that promote the formation of a crystalline phase. In some embodiments, the ceramic-based material may include one or more oxides, nitrides, oxynitrides, carbides, borides, and / or silicides. Exemplary embodiments of ceramic oxides include zirconium oxide (ZrO2), zirconium oxide (ZrSiO4), alkali metal oxides (e.g., sodium oxide (Na2O)), alkaline earth metal oxides (e.g., magnesium oxide (MgO)), titanium dioxide (TiO2), hafnium oxide (Hf2O), yttrium oxide (Y2O3), iron oxide, beryllium oxide, vanadium oxide (VO2), fused silica, mullite (a mineral containing a combination of aluminum oxide and silicon dioxide), and spinel (MgAl2O4). Exemplary embodiments of ceramic nitrides include silicon nitride (Si3N4), aluminum nitride (AlN), gallium nitride (GaN), beryllium nitride (Be3N2), boron nitride (BN), tungsten nitride (WN), vanadium nitride, alkaline earth metal nitrides (e.g., magnesium nitride (Mg3N2)), nickel nitride, and tantalum nitride. Exemplary embodiments of oxynitride ceramics include silicon oxynitride, aluminum oxynitride, and SiAlON (a combination of aluminum oxide and silicon nitride, and may have a chemical formula such as Si 12-m-n Al m+n O n N 16-n 、Si 6-n Al n O n N 8-n or Si 2-n Al n O 1+n N 2-n, where m, n, and generated subscripts are all non-negative integers). Exemplary embodiments of carbides and carbon-containing ceramics include silicon carbide (SiC), tungsten carbide (WC), iron carbide, boron carbide (B4C), alkali metal carbides (e.g., lithium carbide (Li4C3)), alkaline earth metal carbides (e.g., magnesium carbide (Mg2C3)), and graphite. Exemplary embodiments of borides include chromium boride (CrB2), molybdenum boride (Mo2B5), tungsten boride (W2B5), iron boride, titanium boride, zirconium boride (ZrB2), hafnium boride (HfB2), vanadium boride (VB2), niobium boride (NbB2), and lanthanum boride (LaB6). Exemplary embodiments of silicides include molybdenum disilicide (MoSi2), tungsten disilicide (WSi2), titanium disilicide (TiSi2), nickel silicide (NiSi), alkaline earth silicides such as sodium silicide (NaSi), alkali metal silicides such as magnesium silicide (Mg2Si), hafnium disilicide (HfSi2), and platinum silicide (PtSi).
[0060] In some embodiments, the particles may be optically transparent. As used herein, "optically transparent" or "optically clear" means that the average transmittance in the wavelength range of 400nm to 700nm is 70% or greater through a 1.0 mm thick sheet of material. In some embodiments, an "optically transparent material" or "optically clear material" may have an average transmittance in the wavelength range of 400nm to 700nm of 75% or greater, 80% or greater, 85% or greater, or 90% or greater, 92% or greater, 94% or greater, 96% or greater through a 1.0 mm thick sheet of material. The average transmittance in the wavelength range of 400nm to 700nm is calculated by measuring the transmittance at integer wavelengths from about 400nm to about 700nm and averaging the measurements.
[0061] In some embodiments, the particles may occupy about 5% or more, about 50% or more, about 60% or more, about 70% or more, about 75% or more, about 80% or less, about 75% or less, or about 70% or less of the composition by weight (% wt). In even other embodiments, the particles may include a % wt % range of about 5% to about 80%, about 5% to about 75%, about 5% to about 70%, about 50% to about 80%, about 50% to about 75%, about 50% to about 70%, about 60% to about 80%, about 60% to about 75%, about 60% to about 70%, about 65% to about 80%, about 65% to about 75%, about 65% to about 70%, about 70% to about 80%, about 70% to about 75%, or any range or sub-range therebetween. Providing a high load of particles (e.g., about 65% by weight or more) may increase the dimensional stability and / or strength of the green body and / or printed article. In addition, providing high loadings of particles (e.g., about 65 wt % or more) can reduce (e.g., decrease) shrinkage associated with sintering to form a printed article. Providing high loadings of particles (e.g., about 65 wt % or more) can increase the optical clarity of the green body and / or printed article. Providing a composition comprising high loadings of particles (e.g., about 65 wt % or more) can reduce (e.g., decrease) material costs associated with other components of the composition.
[0062] In some embodiments, the particles may include a median particle size of about 1 micrometer (μm) or more, about 3 μm or more, about 5 μm or more, about 10 μm or less, about 7 μm or less, or about 5 μm or less. In even other embodiments, the particles may include a median particle size in the range of about 1 μm to about 10 μm, about 1 μm to about 7 μm, about 1 μm to about 5 μm, about 3 μm to about 10 μm, about 3 μm to about 7 μm, about 3 μm to about 5 μm, about 5 μm to about 10 μm, about 5 μm to about 7 μm, or any range or sub-range therebetween.
[0063] In some embodiments, the particles may include a surface pH. As used herein, the surface pH of the particles is measured as the pH of a mixture of 100 grams (g) of particles and 100 g of deionized water. In some embodiments, the surface pH of the particles may be about 9 or more, about 9.5 or more, about 10 or more, about 12 or more, about 15 or less, about 13 or less, about 12 or less, about 11 or less, or about 10 or less. In some embodiments, the surface pH of the particles may be in the range of about 9 to about 15, about 9 to about 13, about 9 to about 12, about 9 to about 11, about 9 to about 10, about 9.5 to about 13, about 9.5 to about 12, about 9.5 to about 11, about 9.5 to about 10, about 10 to about 15, about 10 to about 13, about 10 to about 12, about 10 to about 11, or any range or sub-range therebetween. Providing particles comprising an alkaline surface pH (eg, about 9 or higher) can increase the compatibility (eg, wetting of particles, stability of the composition) of components (eg, particles, curing agent, dispersant, binder) in the composition.
[0064] In some embodiments, the accessible surface area of the particles will be substantially completely oxides. In other embodiments, the accessible surface area of the particles will be completely oxides. As used herein, the accessible surface area of a particle is defined as the surface touched by a probe comprising a 100nm diameter. Atomic force microscopy (AFM), scanning electron microscopy (SEM) and / or cryogenic electron microscopy (cryo-EM) can be used to measure the accessible surface area. As used herein, when about 95% or more of the accessible surface area comprises non-oxides, the accessible surface area of the particles will be substantially completely oxides. As used herein, oxides include compounds comprising oxides and / or protonated oxides (e.g., alcohols). Exemplary embodiments of oxides include, but are not limited to, silicon dioxide (SiO2), zirconium oxide (ZrO2), zirconium oxide (ZrSiO4), alkali metal oxides (e.g., sodium oxide (Na2O)), alkaline earth metal oxides (e.g., magnesium oxide (MgO)), titanium dioxide (TiO2), hafnium oxide (Hf2O), and yttrium oxide (Y2O3). In some embodiments, the particles may not have undergone a surface modification reaction (e.g., a reaction with a silane coupling agent). Providing particles that include an accessible surface area that substantially includes an oxide (e.g., a composition without a surface modification and / or coupling agent for the particles) can reduce the cost of the composition. Providing a composition that includes particles that include an accessible surface area that substantially includes an oxide (e.g., a composition without a surface modification and / or coupling agent for the particles) can increase the optical transparency of the green body and / or printed article.
[0065] In some embodiments, the composition may include a photoinitiator. As used herein, a photoinitiator is a compound that is sensitive to one or more wavelengths, which reacts after absorbing light containing the one or more wavelengths to produce one or more free radicals or ionic species that initiate polymerization. In other embodiments, the photoinitiator may be sensitive to one or more wavelengths of ultraviolet (UV) light. Exemplary embodiments of UV light-sensitive photoinitiators include, but are not limited to, benzoin ethers, benzil ketals, dialkoxyacetophenones, hydroxyalkylphenones, aminoalkylphenones, acylphosphine oxides, thioxanthones, hydroxyalkyl ketones, and thioxanthanamine. In other embodiments, the photoinitiator may be sensitive to one or more wavelengths of visible light. Exemplary embodiments of photoinitiators sensitive to visible light include, but are not limited to, 5,7-diiodo-3-butoxy-6-fluoroalkane, bis(4-methoxybenzoyl)diethylgermanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 3-methyl-4-aza-6-helicene, and thiocyanine borate. In other embodiments, the photoinitiator may be sensitive to wavelengths at which other components of the composition are substantially transparent. As used herein, the condition for a compound (e.g., a component of a composition) to be substantially transparent at a predetermined wavelength is if, at the predetermined wavelength, a sheet of the compound having a thickness of 1.0 mm is transmitted through, it includes an average transmittance of 75% or more (e.g., 80% or more, 85% or more, or 90% or more, 92% or more, 94% or more, 96% or more). Providing a photoinitiator enables control of the curing activation of the composition. Providing a photoinitiator enables uniform curing of the composition. In other embodiments, the photoinitiator can generate one or more free radicals (e.g., free radicals). Exemplary embodiments of photoinitiators that generate one or more free radicals include: acetophenone, anisoin, anthraquinone, benzene, benzil, benzoin, benzoin ethyl ether, benzoin isobutyl ether, benzoin methyl ether, benzophenone, hydroxycyclohexyl phenyl ketone, 4-benzoylbiphenyl, camphorquinone, 2-chlorothioxanthene-9-one, bibezosuberenone, 2-,2-diethoxyacetophenone, dimethylbenzil, ferrocene, ethylanthraquinone, hydroxyacetophenone, hydroxybenzophenone, thioxanthene-9-one, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and phosphine oxide. Exemplary embodiments of photoinitiators that generate one or more ions include, but are not limited to, triaryl sulfone hexafluoroantimonate and bis (4-tert-butylphenyl) iodine perfluoro-1-butane sulfonate. Commercially available photoinitiators include, but are not limited to, the Irgacure product line from Ciba Specialty Chemical.
[0066] In some embodiments, the composition may include a curing agent. As used herein, a curing agent is a multifunctional monomer that promotes polymerization of a polymer comprising branched and / or crosslinked polymers when activated by a photoinitiator. In other embodiments, the curing agent may include a multifunctional (e.g., difunctional, trifunctional, tetrafunctional) acrylate compound (e.g., monomer). Exemplary embodiments of difunctional acrylate monomers include, but are not limited to, dipropylene glycol diacrylate (e.g., SR-508 (Sartomer)), propylene glycol dimethacrylate (e.g., SR-644 (Sartomer)), 1,6-hexanediol diacrylate (e.g., Miramer M200 (Miwon)), bisphenol A diacrylate (e.g., Miramer M2100 (Miwon)), tripropylene glycol diacrylate (TPGDA) (e.g., Photomer 4061 (IGM Resins)), neopentyl glycol diacrylate (e.g., Photomer 4127 (IGM Resins)), and 1,6-hexanediol ethoxylated diacrylate (e.g., Photomer 4369 (IGM Resins)). Exemplary embodiments of trifunctional acrylate monomers include trimethylolpropane trimethacrylate (TMPTMA (e.g., SR-350 (Sartomer), Photomer 2006 (IGM Resins)). Exemplary embodiments of tetrafunctional acrylate monomers include tetrafunctional amine-modified polyether acrylates (e.g., Photomer 5662 (IGM Resins)). In even other embodiments, the curing agent may include dipropylene glycol diacrylate. Providing a difunctional curing agent may facilitate substantially complete curing. Providing a difunctional acrylate curing agent may facilitate rapid curing, which may reduce the time associated with the manufacture of an article (e.g., a printed article, a green body). Providing one or more trifunctional and / or tetrafunctional curing agents (e.g., trifunctional and / or tetrafunctional curing agents) may facilitate hard curing, which may be characterized by good strength and / or dimensional stability of the cured green body.
[0067] In some embodiments, the composition may include a dispersant. As used herein, a dispersant is one or more compounds designed to increase the wetting and / or stability of particles. In other embodiments, a dispersant may include a phosphate ester. Exemplary embodiments of phosphate ester dispersants include BYK 180 (BYK-Gardner). Providing a dispersant may increase the wetting of particles, which may contribute to higher particle loadings (e.g., about 65% by weight or higher). Providing a dispersant may increase the stability of the composition (e.g., reduce deposition) and / or improve the flow properties of the composition (e.g., reduce shear thickening).
[0068] In some embodiments, the composition may include an organic binder. As used herein, an organic binder is a polymerizable unit, which is not a curing agent, and the monofunctional monomers included therein can act as end caps for the polymer. In other embodiments, the organic binder may include monofunctional monomers, monofunctional oligomers, and / or multifunctional oligomers. In other embodiments, the organic binder may include acrylates, epoxides, and / or carbamates. Exemplary embodiments of acrylates include: monofunctional acrylate monomers, difunctional acrylate oligomers, trifunctional acrylate oligomers, and tetrafunctional acrylate oligomers. Exemplary embodiments of monofunctional acrylate monomers include, but are not limited to: isobornyl methacrylate (e.g., Photomer 2012 (IGM Resins)) and phenoxyethyl acrylate (e.g., Photomer 4035 (IGM Resins)). Exemplary embodiments of tetrafunctional acrylate oligomers include Photomer5429 (IGM Resins). Exemplary embodiments of epoxides include, but are not limited to, bisphenol-based epoxy resins, phenolic-based epoxides, cycloaliphatic-based epoxides, and glycidylamine-based epoxides. Exemplary embodiments of carbamates include polyester carbamate resins (e.g., N3D-I150 (Sartomer)). In some embodiments, the organic binder may include isobornyl methacrylate. In other embodiments, the organic binder may include acrylate oligomers. In even other embodiments, the organic binder may include monofunctional acrylates (e.g., isobornyl methacrylate) and polyurethane resins (e.g., N3D-I150 (Sartomer)). Providing an organic binder may reduce the time consuming of curing the composition because the organic binder may include partially polymerized oligomers. Providing an organic binder having substantially the same chemical properties (e.g., functionality) as the curing agent may contribute to the compatibility and stability of the composition. Providing an organic binder (e.g., a multifunctional oligomer) comprising a monofunctional monomer and a resin can provide controlled polymerization with good stability, good flow properties (e.g., a viscosity range of 100 mPa-s to 7000 mPa-s with reduced or no shear thickening), and dimensional stability of the composition after it is printed but before it is cured.
[0069] In some embodiments, the composition may be substantially free of solvent. In other embodiments, the composition may be free of solvent. In even other embodiments, the composition may be completely free of solvent. As used herein, the condition that the composition is completely free of solvent is: if it contains only components that precipitate in the curing reaction and / or it contains only components that are considered to be based on particles, photoinitiators, curing agents, organic binders or dispersants discussed above. As used herein, the condition that the composition is free of solvent is: if it contains 99.5% by weight or more of components that precipitate in the curing reaction and / or it contains 99.5% by weight or more of components that are considered to be based on particles, photoinitiators, curing agents, organic binders or dispersants discussed above. As used herein, the condition that the composition is substantially free of solvent is: if it contains 98% by weight or more of components that precipitate in the curing reaction and / or it contains 98% by weight or more of components that are considered to be based on particles, photoinitiators, curing agents, organic binders or dispersants discussed above. For example, water and octanol are considered to be solvents. The solvent may include one or more of a polar solvent (e.g., water, alcohol, acetate, acetone, formic acid, dimethylformamide, acetonitrile, dimethyl sulfone, nitromethane, propylene carbonate, poly(ether ether ketone)) or a non-polar solvent (e.g., pentane, 1,4-dioxane, chloroform, dichloromethane, diethyl ether, hexane, heptane, benzene, toluene, xylene). For example, a composition comprising up to 0.5% by weight of a solvent is considered to be substantially solvent-free and solvent-free. Similarly, a composition that does not contain a solvent is considered to be substantially solvent-free, solvent-free, and completely solvent-free. Providing a composition that is substantially solvent-free (e.g., completely solvent-free) can increase the curing rate of the composition, which can reduce processing time. Providing a composition that is substantially solvent-free (e.g., completely solvent-free) can reduce (e.g., reduce, eliminate) the use of rheology modifiers and increase composition homogeneity, which can improve the quality of the resulting green body and / or printed article. Providing a substantially solvent-free composition (eg, completely solvent-free) can increase the optical clarity of the resulting green body and / or printed article.
[0070] In some embodiments, the composition can include a viscosity of about 10 millipascal-seconds (mPa-s) or more, about 50 mPa-s or more, about 100 mPa-s or more, about 300 mPa-s or more, about 500 mPa-s or more, about 1,000 mPa-s or more, about 3,000 mPa-s or more, about 10,000 mPa-s or less, about 7,000 mPa-s or less, about 5,000 mPa-s or less, about 2,000 mPa-s or less, or about 1,000 mPa-s or less. In some embodiments, the composition can include a viscosity range of about 10 mPa-s to about 10,000 mPa-s, about 10 mPa-s, to about 7,000 mPa-s, about 10 mPa-s to about 5,000 mPa-s, about 10 mPa-s to about 2,000 mPa-s, about 10 mPa-s to about 1,000 mPa-s, about 100 mPa-s to about 10,000 mPa-s, about 100 mPa-s to about 7,000 mPa-s, about 100 mPa-s to about 5,000 mPa-s, about 100 mPa-s to about 10,000 mPa-s a-s to about 2,000 mPa-s, about 100 mPa-s to about 1,000 mPa-s, about 300 mPa-s to about 10,000 mPa-s, about 300 mPa-s to about 7,000 mPa-s, about 300 mPa-s to about 5,000 mPa-s, about 300 mPa-s to about 2,000 mPa-s, about 300 mPa-s to about 1,000 mPa-s , about 500 mPa-s to about 10,000 mPa-s, about 500 mPa-s to about 7,000 mPa-s, about 500 mPa-s to about 5,000 mPa-s, about 500 mPa-s to about 2,000 mPa-s, about 500 mPa-s to about 1,000 mPa-s, about 1,000 mPa-s to about 10,000 mPa-s, about 1,000 mPa-s To about 7,000 mPa-s, about 1,000 mPa-s to about 5,000 mPa-s, about 1,000 mPa-s to about 2,000 mPa-s, about 3,000 mPa-s to about 10,000 mPa-s, about 3,000 mPa-s to about 7,000 mPa-s, about 3,000 mPa-s to about 5,000 mPa-s, or any range or sub-range therebetween.
[0071] As used herein, the viscosity of the composition is measured at 25°C using a rotational rheometer (e.g., RheolabQC of Anton Par). The viscosity can be measured in the following shear rate range: from about 0.01 1 / s to about 1,000 1 / s, from about 0.1 1 / s to about 500 1 / s, from about 5 1 / s to about 200 1 / s, from about 10 1 / s to about 100 1 / s, from about 20 1 / s to about 50 1 / s, or any range or sub-range therebetween. In some embodiments, at 0.01 1 / s, the composition may include a viscosity falling within one or more of the viscosity ranges specified above. In other embodiments, the composition may include a viscosity averaged at a shear rate measurement of 10 logarithmic intervals within one or more of the viscosity ranges specified above. In even other embodiments, the composition may include a viscosity measured at a shear rate of 10 logarithmic intervals that all fall within one or more of the viscosity ranges specified above. In other embodiments, the composition can include minimal shear thickening, for example, the ratio of the viscosity measured at a shear rate of 100 1 / s to the viscosity at a shear rate of 0.01 1 / s can be about 10 or less, about 5 or less, about 2 or less, or about 1 or less. Providing a composition with reduced shear thickening behavior (e.g., decreased shear thickening behavior, or no shear thickening behavior) can achieve increased processing speeds and / or reduced equipment damage.
[0072] In some embodiments, the composition may include a sedimentation rating. As used herein, the sedimentation rating is measured according to ASTM D869, wherein, after waiting for a predetermined amount of time, a square-end blade scraper is dropped into the composition in the container and graded in the range of 0 to 10. A sedimentation rating of 10 corresponds to a perfect suspension, wherein no significant change occurs relative to the initial state of the composition. A sedimentation rating of 8 corresponds to a composition with slight sediment on the scraper. A sedimentation rating of 6 corresponds to a composition containing certain lumps, resistance encountered when the scraper moves sideways, and a significant deposit on the scraper. A sedimentation rating of 4 corresponds to such a composition, wherein the scraper does not fall to the bottom of the container under its own gravity, and the scraper is difficult to move sideways. As used herein, for a composition that is considered to be stable for a predetermined time interval, the composition is required to have a sedimentation rating of 6 or higher at the predetermined time interval. In other embodiments, the composition may include a sedimentation rating of 6 or higher after waiting for about 1 day. In even other embodiments, the composition may include a sedimentation rating of 8 or higher after waiting for about 1 day. In even other embodiments, the composition may include a sedimentation rating of 6 or higher after waiting for about 3 days. In other embodiments, the composition can include a precipitation rating of 8 or higher after waiting about 3 days. In other embodiments, the composition can include a precipitation rating of 6 or higher after waiting about 7 days.
[0073] Will refer to Figure 2-3 as well as Figure 1 An embodiment of a method for manufacturing a green body according to an embodiment of the present disclosure is discussed in the flowchart in FIG.
[0074] In the first step 101 of the method for making the green body 207, the method can start with providing a composition. In some embodiments, the composition can be obtained by purchasing the composition or any other means. In some embodiments, the composition can be provided by generating the composition. In other embodiments, generating the composition can include mixing particles with a photoinitiator, a curing agent, and an organic binder. In even other embodiments, the particles can occupy the following % weight % of the composition: about 5% or more, about 50% or more, about 60% or more, about 70% or more, about 75% or more, about 80% or less, about 75% or less, or about 70% or less. In even other embodiments, the particles may include a % weight of the composition in the range of about 5% to about 80%, about 5% to about 75%, about 5% to about 70%, about 50% to about 80%, about 50% to about 75%, about 50% to about 70%, about 60% to about 80%, about 60% to about 75%, about 60% to about 70%, about 65% to about 80%, about 65% to about 75%, about 65% to about 70%, about 70% to about 80%, about 70% to about 75%, or any range or sub-range therebetween. In even other embodiments, the particles may include glass-based particles. In even other embodiments, the particles may include ceramic-based particles. In even other embodiments, the particles may include a median particle size of about 1 μm or more, about 3 μm or more, about 5 μm or more, about 10 μm or less, about 7 μm or less, or about 5 μm or less. In even other embodiments, the particles may include a median particle size in the range of about 1 μm to about 10 μm, about 1 μm to about 7 μm, about 1 μm to about 5 μm, about 3 μm to about 10 μm, about 3 μm to about 7 μm, about 3 μm to about 5 μm, about 5 μm to about 10 μm, about 5 μm to about 7 μm, or any range or sub-range therebetween. In even other embodiments, glass-based particles and / or ceramic-based particles may be formed by glass-based samples or glass-based sample layers, which may be provided by various strip forming processes, such as slot drawing, down drawing, fusion down drawing, up drawing, roller pressing, redrawing or float. In even other embodiments, a predetermined particle size (e.g., median particle size, particle size distribution) may be obtained by ball milling the particles. In even other embodiments, the curing agent may include dipropylene glycol diacrylate. In even other embodiments, the dispersant may include a phosphate ester. In even other embodiments, the organic binder may include one or more of an acrylate, an epoxide, and / or a urethane. In even other embodiments, the composition may be substantially free of solvent. In other embodiments, the composition may be completely free of solvent.In even other embodiments, the particles may be mixed with an already formed mixture of two or more of a photoinitiator, a curing agent, a dispersant, and a binder. In some embodiments, the composition may include a viscosity of about 10 millipascal-seconds (mPa-s) or more, about 50 mPa-s or more, about 100 mPa-s or more, about 300 mPa-s or more, about 500 mPa-s or more, about 1,000 mPa-s or more, about 3,000 mPa-s or more, about 10,000 mPa-s or less, about 7,000 mPa-s or less, about 5,000 mPa-s or less, about 2,000 mPa-s or less, or about 1,000 mPa-s or less. In some embodiments, the composition may include a viscosity range of about 10 mPa-s to about 10,000 mPa-s, about 10 mPa-s, to about 7,000 mPa-s, about 10 mPa-s to about 5,000 mPa-s, about 10 mPa-s to about 2,000 mPa-s, about 10 mPa-s to about 1,000 mPa-s, about 100 mPa-s to about 10,000 mPa-s, about 100 mPa-s to about 7,000 mPa-s, about 100 mPa-s to about 5,000 mPa-s, about 100 mPa-s to about 10,000 mPa-s a-s to about 2,000 mPa-s, about 100 mPa-s to about 1,000 mPa-s, about 300 mPa-s to about 10,000 mPa-s, about 300 mPa-s to about 7,000 mPa-s, about 300 mPa-s to about 5,000 mPa-s, about 300 mPa-s to about 2,000 mPa-s, about 300 mPa-s to about 1,000 mPa-s , about 500 mPa-s to about 10,000 mPa-s, about 500 mPa-s to about 7,000 mPa-s, about 500 mPa-s to about 5,000 mPa-s, about 500 mPa-s to about 2,000 mPa-s, about 500 mPa-s to about 1,000 mPa-s, about 1,000 mPa-s to about 10,000 mPa-s, about 1,000 mPa-s To about 7,000 mPa-s, about 1,000 mPa-s to about 5,000 mPa-s, about 1,000 mPa-s to about 2,000 mPa-s, about 3,000 mPa-s to about 10,000 mPa-s, about 3,000 mPa-s to about 7,000 mPa-s, about 3,000 mPa-s to about 5,000 mPa-s, or any range or sub-range therebetween.
[0075] After step 101, the method may proceed to step 103, which includes printing a green body 207 using the composition 205. In some embodiments, Figure 2As shown, printing with composition 205 to obtain green body 207 may include using printing device 201. In some embodiments, printing device 201 may include container 203. In some embodiments, as shown, printing with composition 205 to obtain green body 207 may include depositing composition 205 by pouring composition 205 from container 203 to form green body 207. In some embodiments, the container may include a printer box, a beaker, a pipette (e.g., a micropipette), a syringe, or a catheter (e.g., a hose). In some embodiments, printing device 201 may include a workbench 209. In some embodiments, as shown, green body 207 may be deposited onto workbench 209. In other embodiments, as shown, workbench 209 may be displaceable in a first direction 211. In other embodiments, as shown, workbench 209 may be displaceable in a second direction 213. In even other embodiments, as shown, workbench 209 may be displaceable in a first direction 211 and a second direction 213 perpendicular to first direction 211. In other embodiments, although not shown, the workbench may be displaceable in a third direction that is perpendicular to both the first direction and the second direction. In some embodiments, although not shown, the movement of the workbench in one or more directions may be coordinated with the deposition of the composition by a controller (e.g., a computer numerical controller (CNC) (e.g., according to a CAD design). In some embodiments, a layer of the composition may be deposited (e.g., including a thickness range of about 10 μm to about 1 mm). In other embodiments, multiple layers may be deposited in sequence to form a green body by building up a green body with multiple layers deposited. It is to be understood that the printing device 201 may include a top-down SLA printer, a bottom-up DLP, or any other printing device known in the art.
[0076] After step 103, the method may proceed to step 105, which includes curing the green body 207. Figure 3As shown, curing of green body 207 may include emitting a light beam from light source 301. In some embodiments, light source 301 may include a laser, a light emitting diode (LED), and / or an organic light emitting diode. In other embodiments, the laser may include a gas laser, an excimer laser, a dye laser, or a solid-state laser. Exemplary embodiments of gas lasers include: helium, neon, argon, krypton, xenon, helium neon (HeNe), xenon neon (XeNe), carbon dioxide (CO2), carbon monoxide (CO), copper (Cu) vapor, gold (Au) vapor, cadmium (Cd) vapor, ammonia, hydrogen fluoride (HF), and deuterium fluoride (DF). Exemplary embodiments of excimer lasers include chlorine, fluorine, iodine, or nitrous oxide (N2O) in an inert environment containing argon (Ar), krypton (Kr), xenon (Xe), or a combination thereof. Exemplary embodiments of dye lasers include those using organic dyes, such as: rhodamine, fluorescein, coumarin, stilbene, umbelliferone, tetraene, or malachite green dissolved in a liquid solvent. Exemplary embodiments of solid-state lasers include crystal lasers, fiber lasers, and laser diodes. Crystal-based lasers include a host crystal doped with a lanthanide or transition metal. Exemplary embodiments of host crystals include: yttrium aluminum garnet (YAG), yttrium lithium fluoride (YLF), yttrium othoaluminate (YAL), yttrium scandium gallium garnet (YSSG), lithium aluminum hexafluoride (LiSAF), lithium calcium aluminum hexafluoride (LiCAF), zinc selenide (ZnSe), zinc sulfide (ZnS), ruby, forsterite, and sapphire. Exemplary embodiments of dopants include: neodymium (Nd), titanium (Ti), chromium (Cr), cobalt (Co), iron (Fe), erbium (Er), holmium (Ho), thulium (Tm), ytterbium (Yb), dysprosium (Dy), cerium (Ce), gadolinium (Gd), samarium (Sm), and terbium (Tb). Exemplary embodiments of solid state crystals include: ruby, alexandrite, chromium fluoride, forsterite, lithium fluoride (LiF), sodium chloride (NaCl), potassium chloride (KCl), and rubidium chloride (RbCl). The laser diode may include a heterojunction or PIN diode, having three or more materials for the p-type, intrinsic, and n-type semiconductor layers, respectively. Exemplary embodiments of laser diodes include: AlGaInP, AlGaAs, InGaN, InGaAs, InGaAsP, InGaAsN, InGaAsNSb, GaInP, GaAlAs, GaInAsSb, and lead (Pb) salts. Due to their size, adjustable output power, and ability to operate at room temperature (i.e., about 20°C to about 25°C), some laser diodes may represent exemplary embodiments.
[0077] In some embodiments, the light source 301 can be configured to emit a light beam containing ultraviolet (UV) wavelengths or visible light wavelengths. In other embodiments, the wavelength of the light beam can be in the following range: about 10nm to about 400nm, about 100nm to about 400nm, about 200nm to about 400nm, about 10nm to about 300nm, about 100nm to about 300nm, about 200nm to about 300nm, about 10nm to about 200nm, about 100nm to about 200nm, or any range or sub-range therebetween. In other embodiments, the operating wavelength range can be in the following light wavelength range: about 315nm to about 400nm, about 280nm to about 315nm, about 100nm to about 280nm, or 122nm to about 200nm. In other embodiments, the wavelength of the light beam can be in the range of about 300 nanometers (nm) to about 1000 nm, about 350 nm to about 900 nm, about 400 to about 800 nm, about 500 nm to about 700 nm, or any range or sub-range therebetween. In even other embodiments, the wavelength of the light beam can be about 365 nm, about 415 nm, or about 590 nm. In other embodiments, the wavelength of the light beam can correspond to a wavelength to which the photoinitiator is sensitive.
[0078] After step 105, the method may proceed to step 113, which includes the end of the manufacturing process of the green body 207. In some embodiments, the method of manufacturing the green body 207 may proceed in sequence along steps 101, 103, 105, and 113, as described above. In other embodiments, arrow 102 may correspond to going directly from step 103 to step 113, such as when no curing of the green body has occurred. In some embodiments, arrow 106 may correspond to going from step 105 to step 103, such as when a layer of the composition 205 is deposited (e.g., printed) as part of the green body 207 before printing another layer of the composition 205. In other embodiments, the cycle of printing a layer (e.g., step 103) and then curing the layer (e.g., step 105) may be repeated until the green body is fully printed (e.g., proceeding to step 113). It is to be understood that the above variations may be combined in some embodiments.
[0079] Will refer to Figure 2-6 as well as Figure 1 Other embodiments of the method for manufacturing a printed article of the present disclosure are discussed in the flowchart in FIG. Figure 6 6. A method of manufacturing a printed article 601 is shown. For example, the method may include a first step 101 of producing a composition 205. The first step 101 may be performed as described above with reference to step 101 of manufacturing a green body 207.
[0080] After step 101, the method for manufacturing the printed article 601 may proceed to step 103, which includes printing the green body 207 using the composition 205. Figure 2 Step 103 is performed as shown in step 103 of manufacturing green body 207.
[0081] After step 103, the method may proceed to step 105, which includes curing the green body 207. Figure 3 Step 105 is performed as shown in step 105 of manufacturing green body 207.
[0082] After step 105, the method may proceed to step 107, which includes heating the solidified green body 207 to remove the organic binder to form the porous article 503. In some embodiments, Figure 4As shown, heating the cured green body 207 may include placing the cured green body 207 in an oven 401 and then heating the cured green body 207 in the oven 401 to form the porous article 503. In some embodiments, substantially all of the organic binder may be removed by heating the cured green body 207. In other embodiments, all of the organic binder may be removed by heating the cured green body 207. In other embodiments, the cured green body 207 may be heated to a temperature of about 250° C. or more, about 350° C. or more, about 400° C. or more, about 1000° C. or less, about 800° C. or less, or about 600° C. or less. In other embodiments, the cured green body 207 can be heated to a temperature in the range of about 250°C to about 1000°C, about 250°C to about 800°C, about 250°C to about 600°C, about 350°C to about 1000°C, about 350°C to about 800°C, about 350°C to about 600°C, about 400°C to about 1000°C, about 400°C to about 800°C, about 400°C to about 600°C, or any range or sub-range therebetween. In other embodiments, the cured green body 207 can be heated to a temperature in one or more of the ranges specified above for a time of about 20 minutes or more, about 1 hour or more, about 3 hours or more, about 8 hours or more, about 24 hours or less, about 16 hours or less, or about 8 hours or less. In other embodiments, the cured green body 207 can be heated to a temperature within one or more of the ranges specified above for a time ranging from about 20 minutes to about 24 hours, about 20 minutes to about 16 hours, about 20 minutes to about 8 hours, about 1 hour to about 24 hours, about 1 hour to about 24 hours, about 1 hour to about 16 hours, about 1 hour to about 8 hours, about 3 hours to about 24 hours, about 3 hours to about 16 hours, about 3 hours to about 8 hours, about 8 hours to about 24 hours, about 8 hours to about 16 hours, or any range or sub-range therebetween. In some embodiments, a plurality of pores 505 corresponding to the spaces occupied by the organic components of the composition (e.g., photoinitiator, curing agent, dispersant, organic binder, and cured polymeric product) are formed in the porous article 503.
[0083] After step 107, the method may proceed to step 109, which includes sintering the porous article 503 to form a printed article 601. In some embodiments, Figure 5 As shown, sintering the porous product 503 may include: placing the porous product 503 in a sintering oven 501, and then heating the porous product 503 in the sintering oven 501 to sinter the porous product 503 into a printed product 601, as shown in FIG. Figure 6As shown. In some embodiments, sintering can include a process of agglomerating (e.g., directly bonding to each other) particles into a solid (e.g., a ceramic article, a printed article) by heating without completely liquefying the particles so that the crystal structure of the particles is in an agglomerate. In other embodiments, sintering can include heating the porous article 503 to a temperature of about 500°C or more, about 1000°C or more, about 1400°C or more, about 2000°C or more, about 3200°C or less, about 3000°C or less, about 2500°C or less, or about 2000°C or less. In other embodiments, sintering can include heating the porous article 503 to a temperature in the range of about 500°C to about 3200°C, about 500°C to about 3000°C, about 500°C to about 2500°C, about 1000°C to about 3200°C, about 1000°C to about 3000°C, about 1000°C to about 2500°C, about 1400°C to about 3200°C, about 1400°C to about 3000°C, about 1400°C to about 2500°C, about 1400°C to about 2000°C, about 2000°C to about 3200°C, about 2000°C to about 3000°C, about 2000°C to about 2500°C, or any range or sub-range therebetween. In other embodiments, sintering may include heating the porous article 503 to a temperature within one or more of the ranges specified above for a time period of about 20 minutes or more, about 1 hour or more, about 3 hours or more, about 8 hours or more, about 24 hours or less, about 16 hours or less, or about 8 hours or less. In other embodiments, sintering may include heating the porous article 503 to a temperature within one or more of the ranges specified above for a time period of about 20 minutes to about 24 hours, about 20 minutes to about 16 hours, about 20 minutes to about 8 hours, about 1 hour to about 24 hours, about 1 hour to about 24 hours, about 1 hour to about 16 hours, about 1 hour to about 8 hours, about 3 hours to about 24 hours, about 3 hours to about 16 hours, about 3 hours to about 8 hours, about 8 hours to about 24 hours, about 8 hours to about 16 hours, or any range or sub-range therebetween. In some embodiments, sintering may reduce (e.g., reduce, eliminate) the size and / or number of pores 505 in the porous article 503. In some embodiments, sintering is associated with about 10% or less, about 8% or less, about 5% or less, about 2% or less, about 1% or less, about 1% or more, about 1% or more, about 2% or more, or about 5% or more shrinkage of the porous article 503. In some embodiments, sintering is associated with shrinkage of the porous article 503 of about 1% to about 10%, about 1% to about 8%, about 1% to about 5%, about 1% to about 2%, about 2% to about 10%, about 2% to about 8%, about 2% to about 5%, about 5% to about 10%, about 5% to about 8%, or any range or sub-range therebetween.
[0084] After step 109, the method can proceed to step 111, which includes the end of the manufacturing process of the printed article 601. In some embodiments, the method of manufacturing the printed article 601 can proceed along steps 101, 103, 105, 107, 109, and 111, as described above. In some embodiments, arrow 106 can correspond to going from step 105 to step 103, such as when a layer of composition 205 is deposited (e.g., printed) as part of the green body 207 before printing another layer of composition 205. In other embodiments, the cycle of printing a layer (e.g., step 103) and then curing the layer (e.g., step 105) can be repeated until the green body is fully printed (e.g., proceeding to step 107). In some embodiments, arrow 108 can correspond to going from step 107 to step 111, wherein the printed article produced by the method includes as Figure 5 The porous article 503 is shown as not having been sintered but may optionally be sintered later. It will be appreciated that the above variations may be combined in some embodiments.
[0085] Example
[0086] Various embodiments are further illustrated by the following examples. Table 1 is used to demonstrate the compatibility of the curing agent and organic binder with particles (using Corning Gorilla Glass as an example). Table 2 is used to demonstrate the wetting of particles and unexpected benefits using a composition comprising isobornyl acrylate, isobornyl methacrylate, dipropylene glycol diacrylate, BYK 180 and an acrylate organic binder and particles (using particles comprising Corning Gorilla Glass as an example).
[0087] Table 1 presents 31 different curing agents or binders mixed with an equal amount of Corning Gorilla glass particles containing a median particle size of 5 μm. Photomer products are purchased from IGM Resins. SR, N3D and Sartomer products are purchased from Sartomer. Miramer products are purchased from Miwon. The initial reactivity and precipitation of the mixture are graded. The initial reactivity is rated on a scale of 0 to 10, where 0 corresponds to no reactivity and 10 is the most reactive (e.g., bubbling, odor, color change, opacity change). As described above, the precipitation rating is measured according to ASTM D869 with a waiting time of 2 days between mixing and measuring. As described above, the precipitation is rated on a scale of 0 to 10, where 0 corresponds to the worst precipitation and 10 corresponds to no precipitation. Acceptable components have an initial reactivity of 2 or less and a precipitation rating of 6 or more.
[0088] Table 1: Initial reactivity and precipitation ratings of components with particles
[0089]
[0090]
[0091] Example AK includes an unacceptable reactivity rating and the worst precipitation rating. Example LQ includes an unacceptable reactivity rating but includes an acceptable precipitation rating. Example R includes an acceptable reactivity rating but includes an unacceptable precipitation rating. Examples S-EE include both an acceptable reactivity rating and an acceptable precipitation rating. Considering that Examples A-EE all include acrylate- or methacrylate-based compounds, the acceptable performance of Examples S-EE is unexpected given the unacceptable performance of Example AR and the functional similarity of the compounds.
[0092] Table 2 presents 7 compositions containing Corning Gorilla Glass with a median particle size of 5 μm, such that the glass particles account for 75% by weight of the composition. The mixtures were rated based on whether they could be printed as SLA additive manufacturing process parts. In addition, the evaluation of wetting, flow and / or curing was recorded. Example 1 had only minimal wetting, which made it semi-solid and not printable by SLA. Examples 2-5 could not be printed by SLA, had poor flowability and were shear thickening. Example 6, in which Sartomer 508 was omitted, could not be printed by SLA, did not cure properly, and only partially wetted the glass particles. It can be seen that only Example 7 is printable by SLA. Example 7 contains Byk 180, Photomer 2021 and Sartomer 508. Example 7 has good flow properties, good wetting of the glass particles, and good curing. Example 7 demonstrates the unexpected benefit of wetting and printability of the 75% particle containing Byk 180, Photomer 2021, and Sartomer 508 in view of the unprintable Examples 1-6.
[0093] Table 2: Performance of the compositions
[0094]
[0095] The composition provided by the present disclosure above can reduce the time-consuming and / or cost associated with additive manufacturing, production of green bodies and / or printed products. In addition, the composition of the present disclosure can include high-load particles (e.g., about 65% by weight or higher), with good particle stability and / or wettability. Such compositions have reduced shear thickening behavior (e.g., shear thickening behavior decreases, or there is no shear thickening behavior), which can achieve increased processing speed and / or reduced equipment damage. Such compositions include good particle wetting, which can achieve an increase in composition stability (e.g., reduction and / or reduction of precipitation (settle) and / or precipitation (sedimentation)). Such compositions can include printable viscosity (e.g., about 100 millipascals-seconds (mPa-s) in the range of about 7000mPa-s), which is even used for additive manufacturing when the composition includes high-load (e.g., about 65% by weight or more) particles. Providing a composition substantially free of solvent can increase the solidification rate of the composition, which can reduce processing time. Providing a composition that is substantially free of solvents can reduce (e.g., reduce, eliminate) the use of rheology modifiers and increase composition homogeneity, which can improve the quality of the resulting green body and / or printed article. Providing a composition that is substantially free of solvents can increase the optical clarity of the resulting green body and / or printed article. Providing a composition that includes high loadings (e.g., about 65% by weight or more) of particles can reduce (e.g., reduce) the material costs associated with other components of the composition. Providing a composition that includes particles that include an accessible surface area that substantially includes oxides (e.g., a composition that does not have a surface modification of the particles and / or a coupling agent) can reduce the cost of the composition.
[0096] In addition, the above-described method can additionally produce optically transparent green bodies and / or printed products that exhibit good dimensional stability and / or mechanical strength. The composition of the present disclosure embodiment can be used for the manufacturing method of green bodies and / or printed products. As discussed above, the method using the composition of the present disclosure embodiment can reduce the time-consuming and / or cost associated with such methods. In addition, the method of the present disclosure embodiment can produce high-quality green bodies and / or printed products. Providing a composition comprising high-load (e.g., about 65% by weight or more) particles can increase the dimensional stability and / or strength of green bodies and / or printed products. Providing a composition comprising high-load (e.g., about 65% by weight or more) particles can reduce (e.g., reduce) the shrinkage associated with the sintering of the formed printed products. Providing a composition comprising high-load (e.g., about 65% by weight or more) particles can increase the optical transparency of green bodies and / or printed products. Providing a composition comprising particles (the particles comprising an accessible surface area substantially comprising oxides) (e.g., a composition without a surface modification of the particles and / or a coupling agent) can increase the optical clarity of a green body and / or a printed article. Providing a composition substantially free of solvents can increase the dimensional stability and / or strength of a green body and / or a printed article. Providing a composition substantially free of solvents can reduce (e.g., decrease) shrinkage associated with sintering to form a printed article. Providing a composition substantially free of solvents can increase the optical clarity of a green body and / or a printed article.
[0097] As used herein, the term "controller" may include all devices, apparatuses, and machines for processing data, including, for example, a programmable processor, a computer, a computer numerical control controller, or a plurality of processors or computers. In addition to hardware, the processor may also include coding that generates an execution environment for the computer program in question, such as coding that constitutes processor firmware, a protocol stack, a database management system, an operating system, or a combination of one or more of them. In some embodiments, a controller may be included and / or executed in a digital circuit or computer software, firmware, or hardware, including the structure disclosed in this specification and its structural equivalent form, or a combination of one or more of them. The embodiments of the controller described herein may be used as one or more computer program products, such as one or more modules of computer program instructions encoded on a tangible program carrier, for executing a data processing device or controlling the operation of a data processing device. The tangible program carrier may be a computer-readable medium. The computer-readable medium may be a machine-readable storage device, a machine-readable storage substrate, a storage device, or a combination of one or more of them. A computer program (also referred to as a program, software, software application, script or coding) can be written in any form of programming language, including an assembly or compiled language or a declarative or procedural language, and it can be configured in any form, including as a stand-alone program or as a module, component, subroutine or other unit suitable for use in a computer environment. A computer program does not necessarily correspond to a file in a file system. A program can be stored in a portion of a file that loads other programs or data (e.g., one or more scripts stored in a markup language document), in a single file dedicated to the program in question, or in multiple parallel files (e.g., a file storing one or more modules, subroutines or partial coding). A computer program can be used to execute on one or more computers, which are located in one place or distributed in multiple places and interconnected by a communication network. The processes described herein can be performed by one or more programmable processors, which execute one or more computer programs to perform functions by operating on input data and generating output. Processes and logic flows can be performed by devices, and can be performed as special purpose logic circuits, such as FPGAs (field programmable gate arrays) or ASICs (application specific integrated circuits), which are just examples. Processors suitable for executing computer programs include, for example, general-purpose microprocessors and special-purpose microprocessors, and any one or more processors of any type of digital calculator. In general, a processor receives instructions and data from a read-only memory or a random access memory or both. The essential elements of a computer are a processor for executing instructions and one or more data storage devices for storing instructions and data.Typically, a computer will also include receiving data from and / or transferring data to one or more large storage devices, or being operatively connected to them for storing data, the one or more large storage devices being, for example, magnetic disks, magneto-optical disks, or optical disks. However, a computer does not necessarily require such devices. In addition, a computer may be embedded in another device, such as a mobile phone, a personal digital assistant (PDA), which are just examples. Computer-readable media suitable for storing computer program instructions and data include: all forms of data storage, including non-volatile memory, media and storage devices, including, for example, semiconductor storage devices such as EPROM, EEPROM and flash memory devices; magnetic disks, such as internal hard disks or removable disks; magneto-optical disks; and CD-ROM and DVD-ROM disks. The processor and memory may be implemented by special purpose logic circuits or incorporated therein. In order to provide interaction with a user, the embodiments described herein may be implemented on a computer having a display device such as a CRT (cathode ray tube) or LCD (liquid crystal display) monitor for displaying information to the user, as well as a keyboard and a pointing device such as a mouse or trackball or a touch screen by which the user can provide input to the computer. Other types of devices may also be used to provide interaction with the user, such as accepting input from the user in any form, including voice input, speech input or tactile input. The embodiments described herein may be performed in a computer system, the computer system including a back-end component such as a data server, or including a middleware component such as an application server, or including a front-end component such as a client computer with a graphical user interface or an Internet browser, through which the user can interact with the practice of the subject described herein, or any combination of one or more of such back-end, middle or front-end components. The components of the system may be interconnected by digital data communication of any form or medium such as a communication network. The embodiments of the communication network include a local area network ("LAN") or a wide area network ("WAN"), such as the Internet. The computer system may include a client and a server. The client and the server are generally far apart and usually interact through a communication network. The relationship between the client and the server is generated according to a computer program running on the respective computer and having a client-server relationship with each other.
[0098] Directional terms used herein, such as up, down, left, right, front, back, top, and bottom, are only used with reference to the drawings and are not intended to represent absolute orientations.
[0099] It will be understood that the various embodiments disclosed may relate to specific features, elements or steps described with a particular embodiment. It will also be understood that although specific features, elements or steps are described in conjunction with one embodiment, different embodiments may be interchanged or combined with each other in various combinations or permutations not shown.
[0100] It is also to be understood that the terms "the," "an," or "an" as used herein mean "at least one" and should not be limited to "only one" unless expressly specified to the contrary. Thus, for example, reference to "a" component includes embodiments having two or more such components unless the context clearly indicates otherwise. Similarly, "plurality" is intended to mean "more than one."
[0101] As used herein, the term "about" indicates that the amount, size, formulation, parameter and other variables and characteristics are not and need not be exact, but may be approximate and / or larger or smaller as needed, reflecting tolerances, conversion factors, rounding and measurement errors, etc., as well as other factors known to those skilled in the art. Herein, the range can be expressed as starting from "about" another specific value and / or ending at "about" another specific value. When expressing such a range, the embodiment includes starting from a specific value and / or ending at another specific value. Similarly, when the numerical value is expressed as an approximate value with the antecedent "about", it should be understood that the specific numerical value constitutes another embodiment. Whether or not the numerical value or the endpoint of the range of this specification is stated "about", the numerical value or the endpoint of the range is intended to include two embodiments: one modified with "about" and one not modified with "about". It should also be understood that the endpoint values of each range are meaningful when they are related to another endpoint value and when they are not related to another endpoint value.
[0102] Unless otherwise indicated, the terms "substantially," "substantially," and variations thereof as used herein are intended to mean that the described feature and value or description is equal or approximately the same. For example, a "substantially planar" surface is intended to mean a planar or approximately planar surface. Additionally, as defined above, "substantially similar" is intended to mean that two values are equal or approximately equal. In some embodiments, "substantially similar" can mean that the values differ from each other by within about 10%, such as within about 5%, or within about 2%.
[0103] Unless otherwise expressly stated, it is not intended that any method described herein be construed as requiring that its steps be performed in a specific order. Therefore, when a method claim does not actually state that its steps follow a certain order or it does not specifically indicate in any other way in the claims or description that the steps are limited to a specific order, it is not intended to imply any particular order.
[0104] Although the transitional term "comprising" may be used to disclose various features, elements, or steps of a particular embodiment, it is to be understood that this implies alternative embodiments including those that may be described using the transitional terms "consisting of," "consisting essentially of." Thus, for example, implicit alternative embodiments for a device comprising A+B+C include embodiments in which the device consists of A+B+C and embodiments in which the device consists essentially of A+B+C. As used herein, unless otherwise indicated, the terms "comprising" and "including" and variations thereof should be understood to be synonymous and open ended.
[0105] The above-described embodiments and features of those embodiments are exemplary and may be provided alone or in any combination with any one or more features of the other embodiments provided herein without departing from the scope of the present disclosure.
[0106] It is obvious to those skilled in the art that various modifications and changes can be made to the present disclosure without departing from the scope and spirit of the present disclosure. Therefore, the present disclosure covers modifications and changes to the embodiments herein as long as they fall within the scope of the appended claims and their equivalents.
Claims
1. A composition comprising: comprising 5% by weight or more of particles; Photoinitiator; a curing agent comprising dipropylene glycol diacrylate; a dispersant comprising a phosphate ester; and an organic binder comprising isobornyl methacrylate, in, The composition is substantially free of solvent.
2. The composition according to claim 1, wherein The weight % of the particles is 65% or higher.
3. The composition according to any one of claims 1 to 2, wherein The composition includes a viscosity range of 100 mPa-s to 7000 mPa-s.
4. A composition comprising: comprising 65% by weight or more of particles; Photoinitiator; Curing agent; Dispersants; as well as Organic binders, Wherein, the composition comprises a viscosity range of 100 mPa-s to 7000 mPa-s, and the composition is substantially free of solvent.
5. The composition according to claim 4, wherein The organic binder includes isobornyl methacrylate.
6. The composition according to claim 4, wherein Curing agents include dipropylene glycol diacrylate.
7. The composition of claim 4, wherein Dispersants include phosphate esters.
8. The composition of claim 4, wherein The viscosity range is 3,000 mPa-s to 5000 mPa-s.
9. The composition of claim 4, wherein The weight % of the particles ranges from 70 weight % to 80 weight %.
10. The composition according to claim 4, wherein The particles include a surface pH of 9 or greater.
11. The composition according to claim 10, wherein The surface pH of the particles ranged from 10 to 12.
12. The composition of claim 4, wherein The particles comprised a median particle size range of 3 microns to 7 microns.
13. The composition of claim 4, wherein The particles include glass-based particles.
14. The composition of claim 4, wherein The particles include ceramic based particles.
15. The composition of any one of claims 4 to 14, wherein The photoinitiator, curing agent and dispersant comprise a total weight % ranging from 1 wt% to 15 wt%.
16. The composition of any one of claims 4 to 14, wherein The composition comprises a precipitation rating of 6 or higher after 1 day.
17. The composition of any one of claims 4 to 14, wherein The composition also includes an organic binder comprising one or more of: an acrylate, an epoxide, or a urethane.
18. The composition of any one of claims 4 to 14, wherein The particles include an accessible surface area substantially entirely comprised of oxide.
19. A method of making a green body, comprising: A composition is produced comprising: comprising 5% by weight or more of particles; Photoinitiator; a curing agent comprising dipropylene glycol diacrylate; a dispersant comprising a phosphate ester; and an organic binder comprising isobornyl methacrylate; and printing a green body using the composition; and The green body is solidified. wherein the composition is substantially free of solvent.
20. The method of claim 19, wherein: The weight % of the particles is 65% or higher.
21. The method of claim 19 or 20, wherein: The composition includes a viscosity range of 100 mPa-s to 7000 mPa-s.
22. A method of making a green body, comprising: A composition is produced comprising: comprising 65% by weight or more of particles; Photoinitiator; Curing agent; Dispersants; as well as Organic binders; printing a green body using the composition; as well as The green body is solidified. Wherein, the composition comprises a viscosity range of 100 mPa-s to 7000 mPa-s, and the composition is substantially free of solvent.
23. The method of any one of claims 19, 20 and 22, wherein: The green body is optically clear.
24. A method of manufacturing a printed article, comprising: A composition is produced comprising: comprising 65% by weight or more of particles; Photoinitiator; Curing agent; Dispersants; as well as Organic binders; printing a green body using the composition; curing the green body by causing ultraviolet light or visible light to impinge on the green body; heating the solidified green body to remove the organic binder to form a porous article; as well as Sintering the porous article to form a printed article, Wherein, the viscosity ranges from 100 mPa-s to 7000 mPa-s, and the composition is substantially free of solvent.
25. A method of manufacturing a printed article, comprising: A composition is produced comprising: comprising 5% by weight or more of particles; Photoinitiator; a curing agent comprising dipropylene glycol diacrylate; a dispersant comprising a phosphate ester; and an organic binder comprising isobornyl methacrylate; printing a green body using the composition; curing the green body by causing ultraviolet light or visible light to impinge on the green body; heating the solidified green body to remove the organic binder to form a porous article; and Sintering the porous article to form a printed article, wherein the composition is substantially free of solvent.
26. The method of claim 25, wherein: The weight % of the particles is 65% or higher.
27. The method of claim 25 or 26, wherein: The composition includes a viscosity range of 100 mPa-s to 7000 mPa-s.
28. The method of claim 27, wherein: Printed articles are optically clear.
29. The method of claim 27, wherein: The viscosity range is 3,000 mPa-s to 5000 mPa-s.
30. The method of claim 27, wherein: The photoinitiator, curing agent and dispersant comprise a total weight % ranging from 1 wt% to 15 wt%.
31. The method of claim 27, wherein: The particles include glass-based particles.
32. The method of claim 27, wherein: The particles include ceramic based particles.
33. The method of claim 27, wherein: The weight % of the particles ranges from 70 weight % to 80 weight %.
34. The method of claim 27, wherein: The particles include an accessible surface area substantially entirely comprised of oxide.