Ionium salt initiator, treatment-free heat-sensitive plate precursor and treatment-free heat-sensitive plate containing the same, and application thereof
By using the macromolecular iodonium salt of double bonds as initiators, the surface migration and residue problems of onium salt initiators in the imaging layer of the treatment-free heat-sensitive plate are solved, and the initiation efficiency and image quality are improved, and better results are achieved. print resistance.
Patent Information
- Application Number
- CN202210432509.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-14
- Filing Date
- 2022-04-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-23
AI Technical Summary
Onium salt initiators have surface migration and residual problems in the imaging layer of the heat-sensitive plate without treatment, affecting the initiation efficiency and image quality.
A macromolecular iodonium salt containing double bonds is used as an initiator. The iodonium salt has carbon, nitrogen or oxygen atoms at the para-position position of the two benzene rings and contains double bond olefin groups at the end to increase the iodonium salt. steric hindrance and crosslinking reaction with thermally sensitive resin and crosslinkable prepolymer during laser imaging to reduce the production of small molecules.
It effectively reduces the surface migration of iodonium salt in the imaging layer, improves the initiation efficiency and the performance of the process-free thermal version, and improves image quality and print resistance.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithography, and in particular relates to an iodonium salt initiator, a treatment-free thermosensitive plate precursor and a treatment-free thermosensitive plate containing the same, and applications thereof. Background Art
[0002] Computer-to-plate technology (CTP technology) is widely used in modern printing. Common CTP plates are divided into photosensitive CTP plates and thermal CTP plates.
[0003] Thermal CTP plate (thermal plate for short) is an offset printing plate that uses infrared laser for imaging. Thermal plates are widely used because they can be operated in bright rooms and have high imaging quality.
[0004] The printing industry is an environmentally unfriendly and highly polluting industry, especially the waste developer produced during the printing process, which causes great harm to the environment. Therefore, the printing industry around the world is advocating the implementation of green printing technology. Green printing technology refers to the use of environmentally friendly materials and process technologies to reduce the pollution generated during the printing process. Developing green and environmentally friendly printing plates is the top priority in the development of green printing.
[0005] Thermal plate technology is constantly improving and developing, and thermal plate materials are also being updated. One of the directions of technological development is to explore green printing technology and develop environmentally friendly, process-free thermal plates.
[0006] There are many technical routes for processing-free thermal plates, which can be divided into thermal ablation technology, phase change technology, hot melt technology, etc. Thermal ablation technology refers to the use of infrared laser energy to ablate the oleophilic coating, exposing the hydrophilic surface of the aluminum plate to form a hydrophilic area; phase change technology refers to the use of laser energy to convert the polymer into hydrophilic and oleophilic, thereby separating ink and water; hot melt technology refers to the use of laser energy to melt the thermoplastic polymer particles dispersed in the cross-linked hydrophilic layer, changing from hydrophilic to hydrophobic and oleophilic.
[0007] There are two types of unprocessed thermal plates: (1) Direct-on-press unprocessed thermal plates. After the plate is imaged, it can be directly put on the press and developed and printed under the action of the printing press fountain solution; (2) Low-chemical development type unprocessed thermal plates. After the plate is exposed and imaged on the platemaking machine, no chemical developer is required. It can be developed by washing with clean water and then printed on the press.
[0008] The development of process-free thermal plates, especially the development of process-free thermal plate precursors, is a hot topic in the world today. The process-free thermal plate precursor refers to the precursor for manufacturing process-free thermal plates, and generally refers to the necessary materials and technologies required before manufacturing process-free thermal plates.
[0009] Technology for developing processing-free heat-sensitive plate precursors: WO2013 / 032780 discloses a lithographic printing plate precursor for on-press development; EP0980754 introduces a decarboxylation technology to achieve hydrophilic-hydrophobic conversion; WO94 / 23954 introduces a hot-melt micro-gel technology; US4004924 introduces a mixture of thermoplastic hydrophobic particles and hydrophilic binders; EP 2006-5-2406114475.4 introduces a hot-melt thermoplastic particle; US2005-8-3 11 / 196,124 introduces a one-dimensional linear structure hydrophilic adhesive; US 2006-7-27 11 / 494,235 introduces a printing plate precursor containing a hydrophilic group and an esterified allyl group, etc.
[0010] At present, there are many technologies used in the treatment-free thermal plates. One of the mainstream technologies is to use the heat of the laser to act on the initiator, which triggers the chemical reaction of the thermal layer to achieve laser imaging. Among them, onium salt initiators are widely used in the laser imaging system of treatment-free thermal plates.
[0011] In the process of continuous development and improvement of treatment-free thermal plate technology, technicians have found that the onium salt initiators used in the laser imaging system of treatment-free thermal plates have the following urgent problems to be solved: 1. The surface migration problem of onium salt initiators in the imaging layer. The surface migration problem of onium salt initiators in the imaging layer directly affects the initiation efficiency, resulting in insufficient deep initiation, unrealistic image dot restoration, and loose coating. 2. The small molecules produced by the onium salt initiators after laser decomposition damage the imaging layer. The above problems are particularly obvious in treatment-free thermal plates containing discrete particles in the imaging layer.
[0012] The purpose of the present invention is to solve the surface migration and residue problems of the onium salt initiator in the imaging layer, improve the initiation efficiency, and further enhance the performance of the treatment-free thermal sensitive plate. Summary of the invention
[0013] In order to solve the above problems, the present invention provides an iodonium salt initiator and a treatment-free thermosensitive plate precursor and a treatment-free thermosensitive plate and applications thereof. The iodonium salt initiator has at least one olefin group containing carbon, nitrogen or oxygen atoms and a double bond at the end of two para positions of two benzene rings. The olefin group can increase the steric hindrance of the iodonium salt. At the same time, the olefin group can participate in the cross-linking reaction of the imaging layer during laser imaging, reducing the damage of the imaging layer to the small molecules generated by the decomposition of the iodonium salt. The iodonium salt initiator can effectively solve the surface migration and residue problems of the onium salt initiator in the imaging layer in the prior art, and can improve the performance of the treatment-free thermosensitive plate, especially the treatment-free thermosensitive plate containing discrete particles.
[0014] The object of the present invention is achieved in the following manner:
[0015] The iodonium salt initiator described in the present invention is a cationic initiator, specifically a macromolecular iodonium salt containing a double bond, having the following structure:
[0016]
[0017] in:
[0018] R1 and R2 are H, or an alkyl group of 1 to 12 carbon atoms, or an olefin group containing carbon, oxygen or nitrogen atoms and a double bond at the terminal, and at least one of R1 and R2 is an olefin group containing carbon, nitrogen or oxygen atoms and a double bond at the terminal,
[0019] R3, R4, R5, and R6 are independently H or an alkyl group of 1 to 12 carbon atoms;
[0020] X - is an acid anion, preferably, X - It is a hexafluorophosphate anion, a hexafluoroantimonate anion or a tetrafluoroborate anion.
[0021] A treatment-free thermal plate precursor comprises a carrier and an imaging layer, wherein the imaging layer comprises a hydrophilic thermal sensitive resin, a cross-linkable prepolymer, a thermal initiator and an infrared absorber; the thermal initiator is the iodonium salt initiator of the above structure provided in the present application.
[0022] The iodonium salt initiator provided by the invention is a macromolecular iodonium salt containing a double bond, wherein at least one of the two para positions of two benzene rings is an olefin group containing a carbon, nitrogen or oxygen atom and a double bond at the end, and the olefin group can increase the steric hindrance of the iodonium salt, improve the compatibility of the iodonium salt with a heat-sensitive resin and a cross-linkable prepolymer, reduce the surface migration of the iodonium salt in an imaging layer, and improve the initiation efficiency; during laser imaging, the double bond contained in the residual end of the iodonium salt can undergo a cross-linking reaction with the heat-sensitive resin and the cross-linked prepolymer, and reduce the damage to the imaging layer caused by the generation of small molecules; and at the same time, substituents can be set at the four meta positions of the two benzene rings to increase the steric hindrance of the iodonium salt, further reduce the surface migration of the iodonium salt in the imaging layer, improve the initiation efficiency, and further achieve the purpose of improving the performance of the treatment-free heat-sensitive plate. DETAILED DESCRIPTION
[0023] The iodonium salt initiator described in the present invention is a cationic initiator, specifically a macromolecular iodonium salt containing a double bond, having the following structure:
[0024]
[0025] in:
[0026] R1 and R2 are H, or an alkyl group of 1 to 12 carbon atoms, or an olefin group containing carbon, oxygen or nitrogen atoms and a double bond at the terminal, and at least one of R1 and R2 is an olefin group containing carbon, nitrogen or oxygen atoms and a double bond at the terminal,
[0027] R3, R4, R5, and R6 are independently H or an alkyl group of 1 to 12 carbon atoms;
[0028] X - is an acid anion, preferably, X - It is a hexafluorophosphate anion, a hexafluoroantimonate anion or a tetrafluoroborate anion.
[0029] A treatment-free thermal plate precursor comprises a carrier and an imaging layer, wherein the imaging layer comprises a hydrophilic thermal sensitive resin, a cross-linkable prepolymer, a thermal initiator and an infrared absorber; the thermal initiator is the iodonium salt initiator of the above structure provided in the present application.
[0030] The iodonium salt initiator of the structure of the present application can undergo homolytic and heterolytic cleavage under the action of laser heat, and can simultaneously generate free radicals and electrophilic proton acids, so that the heat-sensitive resin and the cross-linkable prepolymer undergo free radical polymerization and cationic polymerization, thereby achieving laser imaging.
[0031] X of the iodonium salt of the present invention - The onium salt counter ion includes an acid anion, such as a chloride ion or other halogen anion, a sulfate, a p-toluenesulfonate, a hexafluorophosphate, a hexafluoroantimonate, a tetrafluoroarsenate, etc. The onium salt counter ion of the present invention is preferably a hexafluorophosphate, a hexafluoroantimonate, a tetrafluoroarsenate.
[0032] The specific examples of the macromolecular iodonium salt (code D) having the structure of the present invention include the following (but not limited to):
[0033] D1:
[0034]
[0035] D2:
[0036]
[0037] D3:
[0038]
[0039] D4:
[0040]
[0041] D5
[0042]
[0043] D6:
[0044]
[0045] D7
[0046]
[0047] D8:
[0048]
[0049] D9:
[0050]
[0051] D10:
[0052]
[0053] D11:
[0054]
[0055] D12:
[0056]
[0057] D13:
[0058]
[0059] D14
[0060]
[0061] D15
[0062]
[0063] D16
[0064]
[0065] D17:
[0066]
[0067] D18
[0068]
[0069] D19
[0070]
[0071] D20
[0072]
[0073] D21
[0074]
[0075] D22:
[0076] D23:
[0077]
[0078] The thermal initiator in the imaging layer accounts for 1-10% by weight of the total solid content of the composition.
[0079] The hydrophilic heat-sensitive resin in the imaging layer is described below:
[0080] The imaging layer of the unprocessed thermal plate requires a polymer resin, specifically, a polymer film-forming resin with functional groups. The hydrophilic thermal resin in the imaging layer of the present invention is a functional film-forming resin. In addition to having film-forming properties, which can ensure that the coating liquid of the imaging layer forms a film and adheres to the carrier after drying, this polymer resin also has the special functions of being hydrophilic and thermally sensitive.
[0081] The hydrophilic thermosensitive resin in the treatment-free thermosensitive plate precursor of the present invention is a polyolefin resin having a side chain containing a hydrophilic group and an epoxy group. Furthermore, the hydrophilic thermosensitive resin in the treatment-free thermosensitive plate precursor of the present invention is a polyolefin resin having at least a polyether acrylate or acrylamide hydrophilic copolymer unit and an epoxy acrylate copolymer unit in the copolymer chain.
[0082] As the main resin in the imaging layer of the treatment-free thermal plate, it must first have hydrophilicity. During laser imaging, the uncrosslinked part can be simply pre-cleaned with water or water containing gum, or cleaned under the action of the fountain solution during machine printing to expose the hydrophilic plate base. After the laser heat effect, the crosslinked imaging part forms a three-dimensional network structure due to the crosslinking of the hydrophilic resin and the prepolymer, and the polarity and solubility of the resin change from hydrophilic to hydrophobic. The best way to achieve water solubility of the resin is to directly select a vinyl monomer with a hydrophilic side group as the copolymer unit of the resin. The hydrophilic side groups include carboxyl, hydroxyl, phosphoric acid, sulfonic acid, amino, amide, ether, etc. The hydrophilic thermosensitive resin of the present invention uses a branched polyether or amide group as the hydrophilic group, that is, the hydrophilic thermosensitive resin contains at least a polyether acrylate or acrylamide hydrophilic copolymer unit on the copolymer chain. The hydrophilic copolymer units of polyether acrylate or acrylamide give the hydrophilic thermosensitive resin good self-emulsification, which can make the hydrophilic thermosensitive resin form nano-micron thermoplastic particles. At the same time, the polyether group and acrylamide have good solvent resistance and can resist the erosion of the imaging layer by the monomers in the UV ink.
[0083] In addition, as the main resin in the imaging layer of the treatment-free thermal plate, the resin preferably contains a heat-sensitive group to facilitate thermal imaging. Such imaging groups can be double bonds that can undergo free radical polymerization or epoxy groups that can undergo cationic polymerization, etc. The hydrophilic thermal resin of the present invention contains a heat-sensitive group, and an epoxy group that can undergo cationic polymerization is selected as the photosensitive group, so the resin structural unit contains an epoxy acrylate copolymer unit, and epoxy acrylic monomers such as glycidyl methacrylate and 3,4-epoxycyclohexyl methacrylate can be preferred. Further, epoxy acrylic monomers containing cyclohexyl groups, such as 3,4-epoxycyclohexyl methacrylate, can be preferred. Cyclohexyl groups can have better rigidity, and the epoxy groups on the cyclohexyl groups have very high cationic polymerization activity.
[0084] Finally, as the main resin in the imaging layer of the treatment-free thermal plate, the comprehensive properties of the resin, such as rigidity and ink affinity, need to be considered. When the resin is in the form of nano-micron particles and used as an adhesive for the chemical-free thermal plate, the resin preferably contains a thermoplastic structural unit, which is conducive to laser hot-melt film formation. The hydrophilic thermal resin of the present invention preferably has a styrene structural unit. As is known to all, the styrene structural unit has good thermoplasticity and a high glass transition temperature. Styrene copolymers as adhesives for chemical-free thermal CTP plates have the advantages that the heated part is easier to melt, the molecules are arranged more closely, the thermal image part is more solid, and the printing durability of the plate can be increased.
[0085] The hydrophilic thermosensitive resin in the imaging layer of the treatment-free thermal plate can be in the form of a solid, a solution or an emulsion, etc. It is preferably in the form of discrete particles. During thermal imaging, the laser can cause the temperature of the thermoplastic polymer particles in the discrete particle state to undergo agglutination reaction, and the exposed area changes from hydrophilic to hydrophobic and lipophilic.
[0086] The hydrophilic thermosensitive resin of the present invention is synthesized by solution or emulsion copolymerization, and the copolymerization reaction can be random copolymerization or block copolymerization, preferably random copolymerization. The initiator of the polymerization includes peroxides such as di-tert-butyl peroxide, benzoyl peroxide, persulfates such as potassium persulfate, ammonium persulfate, azo compounds such as azobisisobutyronitrile, etc., and the copolymerization method is preferably emulsion polymerization.
[0087] The reaction solvents that can be used include water, alcohols, ketones, esters, ethers and the like or mixtures thereof. The copolymerization temperature is preferably 40-100°C, and optimally 60-90°C.
[0088] The treatment-free heat-sensitive plate precursor of the present invention, wherein the hydrophilic heat-sensitive resin can be preferably a polyolefin resin obtained by copolymerization of styrene, polyethylene glycol acrylate (molecular weight of 2000), isopropyl acrylamide and 3,4-epoxycyclohexyl methacrylate, and the copolymerized units in the hydrophilic heat-sensitive resin are calculated by weight percentage, styrene accounts for 30-70%, polyethylene glycol methyl ether methacrylate (number average molecular weight Mn=2000) accounts for 5-20%, isopropyl acrylamide accounts for 5-20%, and 3,4-epoxycyclohexyl methacrylate accounts for 10-30%. The state is discrete particles with a particle size of 50-200nm.
[0089] The hydrophilic thermosensitive resin in the imaging layer accounts for 40-80% of the total solid content of the composition by weight.
[0090] The cross-linkable prepolymers in the imaging layer are described below:
[0091] The crosslinkable prepolymer in the imaging layer can be a monomer capable of free radical polymerization or a monomer capable of cationic polymerization, etc. The monomer capable of free radical polymerization is generally an acrylic monomer containing a double bond, and the monomer capable of cationic polymerization is generally a monomer containing an epoxy group. The crosslinkable prepolymer in the imaging layer of the present invention is a multifunctional acrylic monomer or a multifunctional polyurethane acrylic monomer, where multifunctionality means that it contains multiple double bonds. Multifunctional acrylic monomers such as 1,6-hexanediol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, trimethylolpropane triacrylate, hydroxypropyl glyceryl triacrylate, hydroxyethyl trimethylolpropane triacrylate, polyethylene glycol dimethacrylate, dipentaerythritol hexaacrylate, etc.; multifunctional polyurethane acrylic monomers are condensation products of isocyanates and multifunctional acrylates, such as condensation products of isocyanates with hydroxyethyl acrylate and pentaerythritol triacrylate, etc.; or are condensation products of double-bond-containing isocyanates such as methacryloyloxyisocyanate and polyhydroxy compounds such as pentaerythritol.
[0092] The cross-linkable prepolymer in the imaging layer accounts for 10-50% of the total solid content of the composition by weight.
[0093] The infrared absorbers in the imaging layer are described below:
[0094] The infrared absorber in the imaging layer of the present invention mainly plays the role of energy transfer. The heat of the infrared laser transfers the laser energy to the thermal initiator through the infrared absorber. The thermal initiator is cracked to generate active groups to make the hydrophilic thermosensitive resin and the cross-linkable prepolymer undergo three-dimensional network polymerization to achieve thermal imaging. The maximum absorption wavelength range of the infrared absorber is 750-1100nm, and it is selected from carbon black, azo dyes, triarylamine dyes, indolium dyes, oxocyanol dyes, cyanine dyes, merocyanine dyes, indocyanine dyes, phthalocyanine dyes, polythiophene dyes, pyrazoline azo dyes, oxazine dyes, naphthoquinone dyes, anthraquinone dyes, quinone imine dyes, methine dyes, porphyrin dyes, etc. In order to improve the platemaking contrast, it is beneficial for the printing operator to check the plate with the naked eye to detect the image defects of the printing plate, and at the same time, it is beneficial for modern highly intelligent printing machines to realize automatic intelligent plate loading through the automatic positioning and recognition of the cross-line images at the four corners of the plate. The selected infrared absorber can be an infrared absorber with a color change function, and the presentation of high-contrast images is achieved through laser cracking. The infrared absorber in the imaging layer of the present invention is preferably a cyanine dye of 750-850 nm.
[0095] The infrared absorber in the imaging layer of the present invention accounts for 1-10% by weight of the total solid content of the composition.
[0096] The carrier in the process-free heat-sensitive plate precursor of the present invention is described in detail below.
[0097] The imaging layer of the present invention needs to be coated on a carrier, and the carrier includes a metal substrate such as a steel substrate, a copper substrate, an aluminum substrate, etc. The carrier selected in the present invention is an aluminum substrate that has been roughened by electrolysis and anodized.
[0098] The aluminum substrate is made by electrolytic roughening, and the average center line roughness is 0.3-0.6um. An aluminum substrate with more than 99% aluminum, 0.1%-0.5% iron, 0.03%-0.3% silicon, 0.003%-0.03% copper, and 0.01%-0.1% titanium is used. The electrolytic roughening electrolyte can be an aqueous solution of acid, alkali or salt. First, place the aluminum plate in an aqueous solution of 1%-30% sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, etc., and chemically corrode it at a temperature of 20-80°C for 5-250 seconds. Then neutralize it in 10%-30% nitric acid or sulfuric acid at a temperature of 20-70°C to remove the ash. At a temperature of 10-60°C, use a rectangular wave, a mezzanine wave or a sine wave with alternating positive and negative polarity at 5-100A / dm 2 The aluminum substrate treated by electrolytic roughening and anodizing is then anodized. Anodizing is usually carried out by sulfuric acid method, with the concentration of sulfuric acid being 5-30% and the current density being 1-15A / dm 2 The oxidation temperature is 20-60°C and the oxidation time is 5-250 seconds to form 1-10g / m2 The aluminum substrate treated by electrolytic roughening and anodizing can be sealed or not. A variety of methods can be used to seal 50-80% of the volume of the oxide film micropores. For example, a coating thickness of 3mg / m 2 Polyvinylphosphonic acid seals the micropores of the oxide film.
[0099] The process-free thermal plate precursor of the present invention can be used to manufacture process-free thermal plates, and the process of manufacturing the process-free thermal plates includes at least carrier treatment and imaging layer coating. A protective layer can be coated or not. A protective layer is coated on the imaging layer to reduce the inhibitory effect of oxygen on the performance of the thermal plate imaging layer, and the imaging layer is not polluted or scratched by the external environment. The protective layer can be made of a water-soluble polymer compound with relatively good crystallinity, such as polyvinyl alcohol, polyvinyl pyrrolidone, hydroxypropyl cellulose, gelatin, gum arabic, polyacrylic acid and other water-soluble polymers.
[0100] When the unprocessed heat-sensitive plate is manufactured using the unprocessed heat-sensitive plate precursor of the present invention, other necessary additives may be added, such as solvents, room temperature thermal polymerization inhibitors, surfactants, layer colorants, etc. The solvent is mainly used to prepare the heat-sensitive coating photosensitive liquid from the heat-sensitive composition, including: alcohols, ketones, esters, ethers, amides, aromatic solvents, ethylene dichloride, tetrahydrofuran, etc. The solvent can be used in pure or mixed forms; the room temperature thermal polymerization inhibitor is to prevent the plate from polymerizing at room temperature and improve the room temperature stability of the plate. Thermal polymerization inhibitors include: hydroquinone, nitroxide piperidinol, p-methoxyphenol, di-tert-butyl-p-cresol, pyrogallol, tert-butyl catechol, benzoquinone, 4,4'-thiobis-(3-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-16-tert-butylphenol), and primary cerium salt of N-nitrosophenylhydroxylamine, etc. The addition of layer colorants is to increase the image density of the thermal plate after platemaking, which is convenient for visual inspection or image analysis of the thermal plate after platemaking. Analytical measuring equipment is used to measure the properties of the plate, which include: methyl violet, ethyl violet, crystal violet, crystal violet, Victoria blue, oil green, oil blue, oil yellow, rhodamine B, methyl violet, malachite green, methylene blue, triazines, etc.; surfactants need to be added to the coating, and non-ionic surfactants, amphoteric surfactants, silicon-containing surfactants, fluorine-containing surfactants, etc. can be selected, such as betaines, stearic acid glyceryl esters, sorbic acid palm oil esters, polysiloxanes, and polyfluoroalkyl ethers.
[0101] The process-free heat-sensitive plate prepared using the process-free heat-sensitive plate precursor of the present invention is usually coated by a technique known in the art (eg, knife coating, blade coating, strip coating, roller coating, press coating, etc.).
[0102] The process-free thermal plate made by using the process-free thermal plate precursor of the present invention is scanned and exposed by a thermal CTP plate-making machine, and then washed and developed with water or directly mounted on a printing machine and developed and printed with a fountain solution of the printing machine.
[0103] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that this embodiment is only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Technical personnel skilled in the art can make some non-essential improvements and adjustments based on the above-mentioned contents of the present invention.
[0104] The following are synthesis examples of the present invention, but the present invention is not limited to the following examples.
[0105] Part 1: Examples of initiator synthesis (D1-D23 were all synthesized by Lucky Huaguang, and the following is the basic synthesis route).
[0106] The main raw materials can be obtained from the following companies: sodium borate tetrahydrate, ammonium chloride, potassium iodate, and barium chloride are from Shanghai Bailingwei Technology, concentrated sulfuric acid (mass fraction 98%), acetic acid, acetic anhydride, cyclohexanone, and methanol are from Kaifeng Reagent Co., Ltd., 4-N(allyl)-3,5-diisopropyliodobenzene and 3,5-dimethyl-4-tert-butyl-p-iodobenzene are from Shenyang Chemical Research Institute, N-(ethyl acrylate)-2,6-dimethyl-benzoic acid, (hydroxypropyl methacrylate substituted) isopropyl-2,6-dimethylbenzene and N-(acryloyloxy)-2,6-dimethylbenzene are from Lucky Huaguang, potassium hexafluorophosphate, potassium tetrafluoroborate, and potassium hexafluoroantimonate are from Tianjin Bodi Chemical Co., Ltd., and ether and petroleum ether are from Tianjin Chemical Reagent Plant No. 2.
[0107] Examples of the synthesis of asymmetric macromolecular iodonium salts:
[0108] Synthesis of iodonium salt D13:
[0109] In a 500 ml four-necked flask equipped with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection, add 23 g of sodium borate tetrahydrate, 40 g of acetic acid and 60 g of acetic anhydride, stir at 30 ° C for 1.5 hours, then add 58.2 g of 3,5-dimethyl-4-tert-butyl-p-iodobenzene, stir at 40 ° C for 1.5 hours, then cool to 0 ° C, and then add 43.4 g N-(Ethyl acrylate)-2,6-dimethyl-benzoic acid, control the temperature below 5°C, add a mixture of 30ml of concentrated sulfuric acid and 30ml of acetic acid, raise the temperature to 15°C and stir for 24 hours, pour the reaction solution into ice water and stir for 0.5 hour, extract with petroleum ether 3 times, then slowly add 1000ml of 20% ammonium chloride aqueous solution by mass fraction to the aqueous phase, precipitate solid, filter, wash with deionized water, and vacuum dry, then dissolve the obtained solid in methanol, add 30g of potassium fluoroborate and react for 2 hours, deionize the reaction solution in 1000ml of deionized water, collect the precipitated solid by filtration, wash with deionized water, and vacuum dry to obtain the target product D13.
[0110] Synthesis of iodonium salt D16:
[0111] In a 500 ml four-necked flask equipped with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection, add 23 g of sodium borate tetrahydrate, 40 g of acetic acid and 60 g of acetic anhydride, stir at 30 ° C for 1.5 hours, then add 43.4 g of 4-N (allyl) -3,5-diisopropyl iodobenzene, stir at 40 ° C for 1.5 hours, then cool to 0 ° C, and then add 53 g N-(ethyl acrylate)-2,6-dimethyl-benzoic acid, control the temperature below 5°C, add a mixture of 30ml of concentrated sulfuric acid and 30ml of acetic acid, raise the temperature to 15°C and stir for 24 hours, pour the reaction solution into ice water and stir for 0.5 hour, extract with petroleum ether 3 times, then slowly add 1000ml of 20% ammonium chloride aqueous solution to the aqueous phase, precipitate solid, filter, wash with deionized water, and vacuum dry, then dissolve the obtained solid in methanol, slowly drop 400ml of 10% potassium hexafluorophosphate aqueous solution, filter and collect the precipitated solid, wash with deionized water, and vacuum dry to obtain the target product D16.
[0112] Symmetrical macromolecular iodonium salt synthesis example:
[0113] Synthesis of iodonium salt D17:
[0114] In a 500ml four-necked flask equipped with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection device, 47.1g of potassium iodate, 78g of N-(ethyl acrylate)-2,6-dimethyl-benzoic acid, 200ml of glacial acetic acid and 100ml of acetic anhydride were added, and stirred in an ice-water bath. A mixture of 40ml of concentrated sulfuric acid and 60ml of acetic acid was slowly added dropwise, and the mixture was reacted for 6 hours. The mixture was then heated to 15°C and stirred for 24 hours. The insoluble matter was filtered out, and a mixture of 500g of ether and 500g of water was added. The aqueous phase was taken, and extracted twice with 200ml of ether. The aqueous phase was taken, diluted to 1000ml with deionized water, and 400ml of a 10% potassium hexafluorophosphate aqueous solution was slowly added dropwise. The precipitated solid was collected by filtration, washed twice with deionized water and ether alternately, and dried in vacuo to obtain the target product D17.
[0115] Synthesis of iodonium salt D19:
[0116] In a 1000ml four-necked flask equipped with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection device, add 47.1g potassium iodate, 78g 2,6-dimethyl-N-(ethyl acrylate)-benzoic acid, 21g barium chloride, 200ml glacial acetic acid, 100ml acetic anhydride, and stir in an ice-water bath. Slowly drop a mixture of 40ml concentrated sulfuric acid and 60ml acetic acid, react for 6 hours, then raise the temperature to 15°C and stir for 24 hours, filter out insoluble matter, add 200ml cyclohexanone and 40g potassium hexafluoroantimonate, react for 2 hours, drop the reaction solution into 1000ml deionized water, collect the precipitated solid by filtration, wash twice with deionized water, and vacuum dry to obtain the target product D19.
[0117] Referring to the above basic synthetic route, macromolecular iodonium salts D1-D23 were synthesized.
[0118] Part II: Examples of synthesis of hydrophilic thermosensitive resins (No. A1-A22).
[0119] The main raw materials can be obtained from the following companies: styrene St, isopropyl acrylamide IPAM, and isopropyl alcohol are from Shanghai Bailingwei Technology; polyethylene glycol methyl ether methacrylate PEGMA (number average molecular weight Mn=2000) is from Merck Chemical Sigma-Adrich; 3,4-epoxycyclohexyl methacrylate CMA is from Mitsubishi Rayon Chemical Co., Ltd. of Japan; methyl ethyl ketone MEK: Lanzhou Petrochemical, azobisisobutyl cyanide AIBN: Tianjin Fuchen Chemical Reagent.
[0120] Hydrophilic thermosensitive resin A1: Add 75g of deionized water and 250g of isopropanol to a 500ml four-necked flask with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection device, heat to 80°C and start dripping the following mixed solution: 30g (30 wt%) styrene St, 20g (20 wt%) polyethylene glycol methyl ether methacrylate PEGMA (number average molecular weight Mn=2000), 20g (20 wt%) isopropyl acrylamide IPAM, 30g (30 wt%) 3,4-epoxycyclohexyl methacrylate, 1g azobisisobutyronitrile, drip for 60 minutes, then react at 80°C for 8 hours, add 0.51g of azobisisobutyronitrile and continue to react for 8 hours, then cool down to terminate the reaction, and the particle size is 50nm. The reaction stock solution is used directly according to the solid content.
[0121] According to the copolymer unit ratio given in Table 1 and referring to the synthesis process of hydrophilic thermosensitive resin A1, the amount of water and alcohol and the dropping time were adjusted to synthesize hydrophilic thermosensitive resins A1-A22 with different copolymer unit ratios and particle sizes. The particle sizes are shown in Table 1.
[0122] Comparative Example of Synthesis of the Hydrophilic Thermosensitive Resin of the Present Invention Hydrophilic Thermosensitive Resin:
[0123] According to Agfa patent EP 2006-5-24 06114475.4, Agfa polymer F is synthesized. The polymer does not contain hydrophilic groups. The polymer structure is:
[0124]
[0125] Basic operation: add 75g of deionized water, 250g of isopropanol, and 5g of sodium dodecyl sulfate to a 1000ml four-necked flask with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection device, and add 60g (60 weight%) of St (styrene), 40g (40 weight%) of AN (acrylonitrile), and 0.7g of AIBN (azobisisobutyronitrile) dropwise at 80°C for 0.5 hour. After reacting for 7.5 hours, add 0.3g of AIBN (azobisisobutyronitrile) and continue to react for another 12 hours before ending.
[0126] According to Kodak patent US2005-8-3 11 / 196, Kodak polymer K was synthesized. The polymer contains polyether hydrophilic groups but no epoxy groups. The polymer structure is:
[0127]
[0128] Basic operation: add 75g of deionized water and 250g of n-propanol to a 1000ml four-necked flask with temperature control heating, mechanical stirring, condensation reflux and nitrogen protection device, and add 20g (20 weight%) of St (styrene), 70g (70 weight%) of AN (acrylonitrile), 10g (10 weight%) of PEGMA (polyethoxy methacrylate) and AIBN (azobisisobutyronitrile) dropwise at 80°C for 0.5 hour. After reacting for 7.5 hours, add 0.3g of AIBN (azobisisobutyronitrile) and continue to react for another 12 hours before ending.
[0129] Example 1
[0130] Preparation of the plate base: A1050 rolled aluminum plate with a purity of 99.5% and a thickness of 0.3 mm was etched in a 5% sodium hydroxide aqueous solution at 70°C for 20 seconds, rinsed with running water, and immediately neutralized with a 1% nitric acid aqueous solution. Then, in a 1% hydrochloric acid aqueous solution, a sinusoidal alternating current of 50 A / dm was used at 40°C. 2 The surface was electrolytically roughened for 16 seconds at a current density of 15A / dm, then neutralized with a 5% sodium hydroxide aqueous solution at 40°C for 10 seconds and washed with water. Finally, a 20% sulfuric acid aqueous solution was used at 30°C at a current density of 15A / dm 2 The current density was 20 seconds for anodization and then washed with water. The holes were sealed with a 5% sodium silicate aqueous solution at 80°C for 18 seconds, washed with water and dried. The average center line roughness of the plate obtained was 0.5 μm and the oxide film weight was 3.0 g / dm 2 .
[0131] Imaging layer raw materials: Infrared absorbers that meet the requirements of the present invention can be obtained from Dye Chemical or Merck. The infrared absorber (IR820) in the example is Merck product Sigma-Adrich 543365, chemical name: 2-[2-[2-chloro-3-[[1,3-dihydro-1,1-dimethyl-3-(4-sulfonic acid butyl)-2H-benzo[e]indol-2-ylidene]-ethylidene]-1-cyclohexene-1-yl]-vinyl]-1,1-dimethyl-3-(4-sulfonic acid butyl)-1H-benzo[e]indolium hydroxide inner salt; multifunctional acrylate: S R399 is dipentaerythritol pentaacrylate, from Sartomer; multifunctional polyurethane acrylate: PU100 is polyurethane acrylate, which is a condensation product of Covestro's Desmodurn100, hydroxyethyl acrylate and pentaerythritol triacrylate, obtained from Shenyang Chemical Research Institute; surfactant BYK306 comes from BYK; 1-methoxy-2-propanol comes from Union Carbide Chemical; polyvinyl alcohol PVA-205 comes from Kuraray Co., Ltd. of Japan; polyvinyl pyrrolidone PVP K30 comes from BASF of Germany; emulsifier OP-10 comes from Hamm of Germany.
[0132] Imaging layer raw materials (specific raw materials and amounts are shown in Table 2):
[0133] Hydrophilic thermosensitive resin
[0134] Cross-linkable prepolymer
[0135] Thermal initiator
[0136] Infrared absorber (IR820)
[0137] The above raw materials were added with 0.5g of surfactant BYK306 and 700g of 1-methoxy-2-propanol to prepare an imaging layer coating solution, which was extruded onto the hydrophilized substrate and dried at 100°C for 60 seconds to obtain 15mg / dm 2 Dry weight of coating.
[0138] The following protective layer was extrusion coated on the imaging layer and then dried at 110°C for 60 seconds. 2 Dry weight of coating.
[0139] Protective layer formula:
[0140]
[0141] Different thermal plates were prepared using the same process as above: the necessary additives such as the plate base, protective layer, solvent, etc. remained unchanged, and the imaging layer formula was changed according to the data given in Table 2 to prepare Examples 1-22 and Comparative Example thermal plates 1-12, and their properties are listed in Table 3 below.
[0142] Test and analysis of plate materials:
[0143] Initial: refers to when the plate is just manufactured;
[0144] Forced aging: simulate the natural storage state in a forced way;
[0145] 1. Initial sensitivity: The sensitivity is characterized by the laser energy value required for imaging. If the initiation efficiency of the newly produced plate is low, the energy required for laser imaging is higher. All the newly produced plates mentioned above are placed on a Kodak Thermal CTP platemaking machine at 5mJ / cm 2 The progressive amount is between 80-200mJ / cm 2 The plate was exposed within an energy range of , and the initial sensitivity of the plate was measured according to the Pantone LIVE color digital workflow. Its performance is listed in Table 3 below.
[0146] 2. Initial dot quality: Dot quality is characterized by whether 1-99% of the dots can be restored after laser imaging. For example, 1-99% means that 1% to 99% of the dots can be restored, which is the best value. 2-98% means that only 2-98% of the dots can be restored, and 1% and 99% of the dots cannot be restored, which is slightly worse, and so on. The lower the initiation efficiency of the newly produced plate, the higher the 1-100% dots cannot be completely restored. All the above plates were exposed on the Kodak Quansheng thermal CTP platemaking machine with the best sensitivity energy, and the initial dot restoration value of the image was measured according to the PantoneLIVE color digital workflow. Its performance is listed in the following Table 3.
[0147] 3. Forced aging sensitivity: Forced aging is to simulate the changes of thermal plates during the shelf life under natural storage conditions. All the above plates are placed in a standard thermal plate product packaging box and forced to age for 5 days in an aging box at 40°C and 80% humidity. Then, the plate was aged on a Kodak Thermal CTP platemaker at 5mJ / cm 2 The progressive amount is between 80-200mJ / cm 2 The plate was exposed within an energy range and the sensitivity was measured according to the Pantone LIVE color digital workflow. The performance is listed in Table 3 below.
[0148] 4. Forced aging dot quality: All the above plates are placed in a standard thermal plate product box, forced to age for 5 days in an aging box at 40°C and 80% humidity, and then exposed on a Kodak Thermal CTP platemaking machine with the energy of the best sensitivity. According to the PantoneLIVE color digital workflow, the image dot reproduction value is measured. Its performance is listed in Table 3 below.
[0149] 5. Migration rating: Place all the above plates into a standard thermal plate product box and force age them in an aging box at 40°C and 80% humidity for 7 days. The thermal initiator migrates to the surface of the plate, and there will be a difference in appearance compared to the newly made sensitive plate. Use X.rite Pantone eXact scanning spectrophotometer to analyze and rate the apparent quality of the thermal plate according to the Pantone LIVE color digital workflow to obtain the migration value, which is scored on a 10-point scale, with 10 points being the worst and 1 point being the best.
[0150] 6. Printing run: If the iodonium salt initiation efficiency is low and the imaging layer is not fully cured, the printing run of the plate will be reduced; in addition, if the iodonium salt migrates on the surface of the imaging layer, laser exposure will also produce small molecules to break the imaging layer structure, which will also greatly reduce the printing run of the plate. The total number of normal prints printed by the thermal plate was tested using a Heidelberg-XL754C printing press, and its performance is listed in Table 3 below.
[0151] The detection application results in Table 3 show that, compared with other treatment-free plates, the heat-sensitive plate manufactured by the treatment-free heat-sensitive plate precursor of the present invention has excellent imaging performance, stability and printing durability. This is because the thermal initiator in the treatment-free heat-sensitive plate precursor of the present invention is a macromolecular iodonium salt containing a double bond, and at least one of the two para positions of the two benzene rings is an olefin group containing a carbon, nitrogen or oxygen atom and a double bond at the end. The olefin group can increase the steric hindrance of the iodonium salt, improve the compatibility of the iodonium salt with the heat-sensitive resin and the cross-linkable prepolymer, reduce the surface migration of the iodonium salt in the imaging layer, and improve the initiation efficiency; during laser imaging, the double bond contained in the iodonium salt residue can react with the heat-sensitive resin and the cross-linked prepolymer, reducing the damage to the heat-sensitive coating caused by small molecules; at the same time, substituents can be set at the four meta positions of the two benzene rings to increase the steric hindrance of the iodonium salt, reduce the surface migration of the iodonium salt in the imaging layer, improve the initiation efficiency, and achieve the purpose of improving the performance of the treatment-free heat-sensitive plate.
[0152] Table 1 Hydrophilic thermosensitive resin synthesis weight percentage feed and particle size table
[0153]
[0154]
[0155] Table 2 Feeding table of imaging layer of plate materials in the embodiment and comparative example (unit: g)
[0156]
[0157]
[0158]
[0159] Table 3 Plate application performance table
[0160]
[0161]
[0162] The above description is only a preferred embodiment of the present invention, but the protection scope of the present invention is not limited thereto. It should be pointed out that for those skilled in the art and any technician familiar with the technical field, without departing from the overall concept of the present invention, the technical solution and the inventive concept of the present invention are equivalently replaced or changed, and several changes and improvements are made, which should also be regarded as the protection scope of the present invention.
Claims
1. An iodonium salt initiator, characterized in that: The iodonium salt initiator is one of the following structures: D2: D3: D4: D5 D8: D10: D11: D12: D13: D15 D16 D17: D18 D19 D21 D22: D23: 。 2. A process-free thermal plate precursor, comprising a carrier and an imaging layer, characterized in that: The imaging layer comprises a hydrophilic thermosensitive resin, a cross-linkable prepolymer, a thermal initiator and an infrared absorber; the thermal initiator is the iodonium salt initiator described in claim 1.
3. The process-free heat-sensitive plate precursor according to claim 2, characterized in that: In the imaging layer, by weight percentage, the hydrophilic thermosensitive resin accounts for 40-80% of the total solid content of the composition, the cross-linkable prepolymer accounts for 10-50% of the total solid content of the composition, the thermal initiator accounts for 1-10% of the total solid content of the composition, and the infrared absorber accounts for 1-10% of the total solid content of the composition.
4. The process-free thermal plate precursor according to claim 2, characterized in that: A protective layer is also provided on the imaging layer.
5. The process-free heat-sensitive plate precursor according to any one of claims 2 to 4, characterized in that: The hydrophilic thermosensitive resin is a polyolefin resin with a branched chain containing a hydrophilic group and an epoxy group; the cross-linkable prepolymer is a multifunctional acrylic monomer or a multifunctional polyurethane acrylic monomer.
6. The process-free heat-sensitive plate precursor according to claim 5, characterized in that: The hydrophilic thermosensitive resin is a polyolefin resin containing at least a polyether acrylate or acrylamide hydrophilic copolymer unit and an epoxy acrylate copolymer unit in the copolymer chain.
7. The process-free heat-sensitive plate precursor according to claim 5, characterized in that: The hydrophilic thermosensitive resin is a polyolefin resin obtained by copolymerizing styrene, polyethylene glycol methyl ether methacrylate with a number average molecular weight Mn=2000, isopropyl acrylamide and 3,4-epoxycyclohexyl methacrylate; calculated by weight percentage, styrene accounts for 30-70%, polyethylene glycol methyl ether methacrylate with a number average molecular weight Mn=2000 accounts for 5-20%, isopropyl acrylamide accounts for 5-20%, and 3,4-epoxycyclohexyl methacrylate accounts for 10-30%.
8. The process-free heat-sensitive plate precursor according to claim 2, characterized in that: The hydrophilic thermosensitive resin is in the form of discrete particles with a particle size of 50-200 nm.
9. The process-free thermal plate precursor according to claim 2, characterized in that: The infrared absorber is a cyanine dye with an absorption peak at 750-850nm, and the carrier is an aluminum plate substrate that has been subjected to electrolytic roughening and anodizing treatment.
10. A treatment-free thermal plate, characterized in that: The method is prepared from the processing-free heat-sensitive plate precursor described in any one of claims 2 to 9.
11. The use of the treatment-free thermal plate according to claim 10, characterized in that: After the thermal plate is scanned and exposed by a thermal CTP plate-making machine, it is washed with water and developed before being mounted on a printing press for printing or directly mounted on a printing press for development and printing with a printing press fountain solution.
Citation Information
Patent Citations
Thermorecording
US4004924A
Lithographic printing original plate and method for producing the same
WO1994023954A1
Lithographic printing plate precursors for on-press development
WO2013032780A1
Processless thermal sensitive plate used for direct printing on printer
CN105372935A
Heat-sensitive resin, environment-friendly heat-sensitive plate and preparation method of environment-friendly heat-sensitive plate
CN113912772A