Method for preparing solar cell, solar cell and power generation device
By forming a phosphosilicate glass layer during the preparation process of solar cells and using laser doping technology, the problem of difficult control of the sintering temperature is solved, and solar cell preparation with high efficiency and high yield is achieved.
Patent Information
- Application Number
- CN202210294324.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-03-24
AI Technical Summary
During the preparation process of solar cells, the sintering temperature is difficult to solve the problems of under-burning and over-burning at the same time, resulting in reduced efficiency and yield of solar cells.
By forming a phosphorus-silicate glass layer on the surface of the silicon wafer, and using laser doping technology to diffuse phosphorus atoms into the doping layer, a silicon wafer with a high phosphorus content is formed, thereby ensuring that the gap between the metal gate line and the silicon wafer is ensured under lower temperature sintering conditions. good ohmic contact.
It improves the efficiency and yield of solar cells, overcomes the contradiction between high-temperature and low-temperature sintering, enhances the passivation effect of hydrogen, and reduces the damage to silicon wafers caused by high-temperature sintering.
Smart Images

Figure CN114823304B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a method for preparing a solar cell, a solar cell and a power generation device. Background Art
[0002] Solar cells are semiconductor components that use the photovoltaic effect to convert light energy into electrical energy. Solar energy is an inexhaustible clean energy source and has therefore received widespread attention.
[0003] PERC (Passivated Emitter and Rear Cell), or passivated emitter and rear cell technology, is considered to be a very cost-effective technology for preparing solar cells. PERC technology refers to adding a dielectric passivation layer to the back of the solar cell, which can reduce the recombination of surface carriers and thus improve conversion efficiency.
[0004] Screen sintering is an indispensable step in the preparation process of PERC cells. Specifically, the surface of solar cells is usually provided with a grid electrode for extracting carriers. Sintering is to melt the grid wire at high temperature, melt the metal and silicon in the grid wire, and etch the silicon nitride film on the surface of the silicon wafer into the silicon matrix, forming a uniform and good ohmic contact on the back electrode, back electric field, positive electrode and silicon substrate. After the printing of the cell, a good sintering environment can not only form a dense structure and have good electrode current collection and conductivity, but also the hydrogen in the silicon nitride dielectric film on the surface of the cell is released during high temperature treatment and diffused into the silicon wafer, which can not only passivate the dangling bonds at the interface of the silicon material, but also passivate deeply into the silicon material, thereby ensuring the efficiency and yield of the cell.
[0005] In the actual production process, when the sintering temperature is low, there is under-firing. When under-firing, the metal paste cannot fully penetrate the silicon nitride dielectric film into the silicon wafer, and cannot form a good ohmic contact, resulting in a decrease in the yield and efficiency of the solar cell. When the sintering temperature is high, over-firing will occur. When over-firing, the metal components of the gate line are likely to enter the junction area, causing a partial short circuit; and aluminum metal will also melt into silicon and form an aluminum-silicon alloy layer, causing the cell to fail. The hydrogen in the silicon nitride thin layer will also escape from the silicon, weakening the passivation effect of hydrogen on the silicon wafer, which will also lead to a decrease in the yield and efficiency of the solar cell. The above two situations contradict each other. It is difficult to solve the above two problems at the same time in the actual preparation process, which limits the improvement of the efficiency of solar cell products. Summary of the invention
[0006] Based on this, in order to overcome the contradiction existing in the sintering temperature to a certain extent, it is necessary to provide a method for preparing a solar cell, and correspondingly, to provide a solar cell and a power generation device.
[0007] According to one embodiment of the present invention, a method for preparing a solar cell comprises the following steps:
[0008] Placing a P-type doped silicon wafer in a reaction chamber to form an N-type doped layer on the surface of the silicon wafer;
[0009] Introducing a phosphorus source into the reaction chamber, controlling the flow rate of the phosphorus source to be 1200 sccm to 1500 sccm, so that the phosphorus source reacts with the silicon wafer to form a phosphorus-silicate glass layer on the surface of the N-type doped layer;
[0010] Doping the portion of the silicon wafer used for screen-printing the gate electrode with laser so that the phosphorus atoms in the phosphorus-silicate glass layer at the laser-doped portion diffuse into the N-type doping layer;
[0011] The phosphorus silicon glass layer is removed, and a gate line electrode is formed at a position on the surface of the silicon wafer for screen printing the gate line electrode, and a sintering process is performed.
[0012] In one of the embodiments, in the step of forming the phosphosilicate glass layer, the temperature in the reaction chamber is controlled to be 780° C. to 820° C., and the reaction time is controlled to be 12 min to 16 min.
[0013] In one of the embodiments, in the step of forming the phosphosilicate glass layer, an oxygen source with a flow rate of 300 sccm to 500 sccm is introduced into the reaction chamber.
[0014] In one embodiment, the phosphorus source is selected from phosphorus oxychloride.
[0015] In one of the embodiments, during sintering, the sintering temperature is controlled to be 760°C to 800°C.
[0016] In one of the embodiments, in the step of laser doping the silicon wafer, the power of the laser is controlled to be 15W to 35W.
[0017] In one of the embodiments, during the process of forming the N-type doping layer, a phosphorus source is first introduced into the reaction chamber for pre-deposition, and then a high-temperature push-junction treatment is performed at a temperature of 840°C to 880°C, and then a low-temperature push-junction treatment is performed at a temperature of 780°C to 820°C.
[0018] In one of the embodiments, during the process of forming the N-type doping layer, the flow rate of the introduced phosphorus source is 600 sccm to 800 sccm.
[0019] Furthermore, a solar cell is provided, which is prepared by the method for preparing a solar cell according to any of the above embodiments.
[0020] A power generation device comprises the solar cell as described in any one of the above embodiments.
[0021] The method for preparing a solar cell provided by the present invention has the following beneficial effects. The method for preparing a solar cell adopts a specific diffusion process, so that the phosphorus content of the phosphorus silicon glass layer on the surface of the silicon wafer is increased, and the phosphorus content in the silicon wafer under the grid line is increased, which is conducive to forming a good ohmic contact between the metal grid line electrode and the silicon wafer. This enables the metal slurry to form a good ohmic contact with the silicon wafer even if a relatively low temperature sintering process is adopted, thereby overcoming the contradiction that there will be problems in both high temperature sintering and low temperature sintering. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of the variation of the surface concentration of phosphorus element in the silicon wafers of Example 1 and Comparative Example 1 with the junction depth. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are provided herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the technical field of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items. "More than" used herein includes two and more than two items. "Above a certain number" used herein should be understood as a certain number and a range greater than a certain number.
[0025] According to one embodiment of the present invention, a method for preparing a solar cell comprises the following steps:
[0026] Placing a P-type doped silicon wafer in a reaction chamber to form an N-type doped layer on the surface of the silicon wafer;
[0027] Introducing a phosphorus source into the reaction chamber, controlling the flow rate of the phosphorus source to be 1200 sccm to 1500 sccm, and heating the silicon wafer to form a phosphorus silicon glass layer on the surface of the N-type doped layer;
[0028] Doping the portion of the silicon wafer used for screen-printing the gate electrode with laser so that the phosphorus atoms in the phosphorus-silicate glass layer at the laser-doped portion diffuse into the N-type doping layer;
[0029] The phosphorus silicon glass layer is removed, and a gate line electrode is formed at a position on the surface of the silicon wafer for screen printing the gate line electrode, and a sintering process is performed.
[0030] The method for preparing the solar cell in the above embodiment can be implemented in a specific manner including the following steps S1 to S4.
[0031] Step S1, placing a P-type doped silicon wafer in a reaction chamber, and forming an N-type doped layer on the surface of the P-type doped silicon wafer.
[0032] It can be understood that pure silicon is an intrinsic semiconductor, in which the number of electrons and holes should be the same. P-type doped silicon wafers are silicon wafers doped with acceptor impurities. Acceptor impurities can provide hole carriers to the silicon wafer, making the holes in the silicon wafer majority carriers. P-type doped silicon wafers can be selected from boron doped silicon wafers.
[0033] In one specific example, the P-type doped silicon wafer is a texturing silicon wafer. Texturing refers to forming a pyramid-shaped microstructure on the surface of the silicon wafer through processes such as alkali polishing to enhance the silicon wafer's ability to absorb light.
[0034] In one specific example, after placing the P-type doped silicon wafer in the reaction chamber, the reaction chamber may be preheated to control the temperature of the chamber to be heated to 660° C. to 860° C. After the preheating is completed, the temperature of the reaction chamber is maintained, and the reaction chamber is evacuated to a pressure of 50 Pa to 150 Pa.
[0035] In one specific example, before forming the N-type doped layer, an oxygen source is introduced to pre-oxidize the silicon wafer. Optionally, the flow rate of the oxygen source is 600 sccm. The main purpose of pre-oxidation is to grow a dense silicon dioxide layer of corresponding thickness at different positions of the silicon wafer to alleviate the problem that the silicon wafer block resistance is high in the center and low around.
[0036] In one specific example, after oxidation, pre-deposition can be performed on the surface of the silicon wafer to form an N-type doped layer. Specifically, in the process of forming the N-type doped layer, a phosphorus source is first introduced into the reaction chamber for pre-deposition, and then a high-temperature push-junction treatment is performed at a temperature of 840°C to 880°C, and then a low-temperature push-junction treatment is performed at a temperature of 780°C to 820°C. Among them, in the process of pre-deposition, the temperature in the reaction chamber can be first controlled to be maintained at 760°C to 800°C, the pressure can be maintained at 90Pa to 110Pa, and a phosphorus source is introduced for pre-deposition, and the flow rate of the phosphorus source is 600 to 800sccm. Further, after 4 minutes of deposition, the main function of the pre-deposition is to deposit a layer of phosphorus on the surface of the silicon wafer. The main purpose of the high-temperature push-junction treatment is to redistribute the phosphorus on the surface of the silicon wafer, so that the phosphorus deposited on the surface diffuses into the interior of the silicon wafer, and the low-temperature push-junction can make the phosphorus more evenly distributed in the silicon wafer. It can be understood that the N-type doped layer is formed on the surface of the original silicon wafer and forms a PN junction with the P-type silicon wafer below.
[0037] Step S2, introducing a phosphorus source into the reaction chamber, controlling the flow rate of the phosphorus source to be 1200 sccm to 1500 sccm, and heating the silicon wafer to form a phosphosilicate glass (PSG) layer on the surface of the N-type doped layer.
[0038] It can be understood that the flow rate of the phosphorus source in this step is significantly higher than that in the previous step. This is mainly because phosphorus atoms need to be diffused into the silicon substrate when preparing the PN junction, and this step is to form a phosphosilicate glass layer with a required high phosphorus content on the surface of the silicon wafer to prepare for subsequent laser doping and further silk-screen sintering. When forming the required phosphosilicate glass layer, there are requirements for the flow rate of the phosphorus source. If the flow rate of the phosphorus source is lower than 1200 sccm, the phosphorus concentration in the formed phosphosilicate glass layer cannot meet the requirements, and then the subsequent laser doping and further silk-screen sintering are difficult to obtain the required technical effects.
[0039] It is understood that the silicon wafer needs to be heated when forming the phosphosilicate glass layer to promote the reaction between the phosphorus source and the silicon wafer. In one specific example, in order to work together with the flow rate of the phosphorus source to save preparation time as much as possible while maintaining the concentration of phosphorus in the phosphosilicate glass layer, in the step of forming the phosphosilicate glass layer, the temperature in the reaction chamber can also be controlled to be 800°C to 820°C. Furthermore, the reaction time can also be controlled to be 12min to 16min.
[0040] In one specific example, in the step of forming the phosphosilicate glass layer, an oxygen source with a flow rate of 300 sccm to 500 sccm is introduced into the reaction chamber.
[0041] In one specific example, the phosphorus source can be selected from phosphorus oxychloride.
[0042] In one specific example, after the phosphosilicate glass layer is formed, the silicon wafer can be further oxidized to remove impurities. Specifically, after the phosphosilicate glass layer is formed, 1000 sccm to 1200 sccm of oxygen is introduced to form silicon dioxide, which plays a role in gettingtering impurities, and the phosphosilicate glass layer is used to adsorb and fix sodium, potassium and other ions, and these harmful ions are removed while the phosphosilicate glass layer is subsequently removed.
[0043] Furthermore, after the oxidation treatment, nitrogen gas may be introduced into the reaction chamber to a normal pressure state, and then the silicon wafer may be taken out of the reaction chamber for use.
[0044] Step S3, using laser to dope the silicon wafer to diffuse the phosphorus atoms in the phosphorus-silicate glass layer into the N-type doping layer.
[0045] Step S3 is the operation of laser doping. Laser doping uses the thermal effect of laser to melt the surface of the silicon wafer, so that the phosphorus atoms in the phosphorus silicon glass covering the top of the emitter enter the surface of the silicon wafer. The diffusion coefficient of phosphorus atoms in liquid silicon is several orders of magnitude higher than that in solid silicon. After solidification, the doped phosphorus atoms replace the silicon atoms to form a heavily doped layer.
[0046] In one specific example, the laser doped portion mainly corresponds to the position of the subsequent gate electrode. Therefore, laser doping does not need to laser dope the entire surface of the silicon wafer. In one specific example, the laser doping is performed on the surface of the silicon wafer at a preset position for screen printing the gate electrode.
[0047] There are also the following problems with laser doping on the surface of silicon wafers. Normally, a lower laser power cannot achieve the effect of heavy doping, resulting in poor ohmic contact between the emitter and the subsequently formed metal grid electrode. Therefore, in traditional technology, a higher power laser is usually selected to perform laser doping on the surface of the silicon wafer to obtain the effect of heavy doping. However, a higher laser power will destroy the velvet structure of the silicon wafer, which will further reduce the efficiency of the solar cell. In this embodiment, due to the adoption of a specific process for preparing the phosphosilicate glass layer, the phosphorus content in the phosphosilicate glass layer is effectively increased, which is more conducive to the formation of heavy doping, and the dense and sufficient phosphosilicate glass layer can protect the laser pulse from bombarding the surface of the silicon wafer, reduce velvet damage, reduce dangling bonds and dislocation defects, reduce the recombination of the cell surface, and increase the minority carrier lifetime, thereby improving the yield.
[0048] Furthermore, the above process for preparing the phosphorus silicon glass layer can also appropriately reduce the power of laser doping, reducing the damage to the velvet structure, which is equivalent to improving the efficiency of solar cells based on traditional technology. In one specific example, in the step of laser doping a silicon wafer by laser doping, the power of the laser is controlled to be 15W to 35W to reduce the damage caused by laser doping to the velvet structure on the surface of the silicon wafer.
[0049] Furthermore, in one specific example, during the process of laser doping and engraving the auxiliary grid and the anti-break grid, the frequency of the laser is 200kHz to 240kHz. Furthermore, the power factor of the laser can be set to 230kHz to 270kHz.
[0050] Step S4, removing the phosphosilicate glass layer, forming a gate electrode on the laser-doped portion of the surface of the silicon wafer, and performing a sintering process.
[0051] The method for removing the phosphosilicate glass layer may be alkali treatment, and the alkali treatment may be selected from the alkali polishing method commonly used in the traditional technology.
[0052] The gate electrode may be formed by screen printing a metal paste to form the gate electrode, which usually needs to be sintered after screen printing so that the metal paste penetrates the silicon nitride dielectric film and enters the silicon wafer to form a good ohmic contact.
[0053] The process in step S2 can increase the phosphorus content in the phosphorus silicon glass layer, so that the sintering temperature of the screen-printed gate electrode can be effectively reduced in this step. In one specific example, during the sintering process, the sintering temperature can be controlled to be 760°C to 800°C. Further, the sintering temperature can be controlled to be 760°C to 790°C. Further, the sintering temperature can be controlled to be 760°C to 780°C.
[0054] Through the above embodiments, it can be understood that the method for preparing a solar cell provided by the present invention has the following beneficial effects. A specific diffusion process is used in the method for preparing a solar cell, which increases the phosphorus content of the phosphorus-silicon glass layer on the surface of the silicon wafer, and increases the phosphorus content in the silicon wafer under the grid line, which is conducive to forming a good ohmic contact between the metal grid line electrode and the silicon wafer. This enables the metal slurry to form a good ohmic contact with the silicon wafer even if a relatively low temperature sintering process is used, thereby overcoming the contradiction that there will be problems in both high temperature sintering and low temperature sintering.
[0055] Furthermore, the above-mentioned manufacturing steps of phosphosilicate glass with increased phosphorus content combined with sintering at a lower temperature can not only overcome the ohmic contact problem existing in low-temperature sintering, but also help to improve the passivation effect of hydrogen atoms in silicon wafers, reduce the amplification of defects in silicon wafers caused by high-temperature sintering, and ultimately achieve the purpose of improving the efficiency of solar cells and improving product quality.
[0056] Furthermore, the above-mentioned step of manufacturing phosphosilicate glass with increased phosphorus content can also be combined with the step of heavy doping with lower laser power, by making use of the characteristics of the phosphosilicate glass layer with high phosphorus content to achieve the use of lower laser power. At the same time, combined with the protective effect of the dense phosphosilicate glass layer, the velvet damage on the silicon wafer surface caused by the laser doping process can be reduced, thereby avoiding the performance degradation caused by this process.
[0057] In order to make it easier to understand and implement the present invention, the following more specific and detailed embodiments and comparative examples are provided as references. Through the description and performance results of the following specific embodiments and comparative examples, the embodiments of the present invention and their advantages will also be apparent.
[0058] Unless otherwise specified, the raw materials used in the following examples can be purchased from the market.
[0059] In addition, in the actual preparation process, the actual thickness of each layer may be slightly different from the tested thickness, but it does not affect the implementation of the comparative examples and embodiments.
[0060] Example 1: Preparation of a silicon wafer having a phosphosilicate glass layer with a high phosphorus content
[0061] (1) The textured silicon wafer is placed into a reaction furnace tube, and the furnace tube is heated to 760°C ± 100°C;
[0062] (2) The temperature of each temperature zone is maintained at 760±100℃ and vacuumed to 50Pa-150Pa;
[0063] (3) The temperature of each temperature zone is maintained at 760±100℃, and the vacuum is evacuated to 50Pa-150Pa. The vacuum is stopped and the furnace tube is leak-checked;
[0064] (4) Pre-oxidation: The temperature of each temperature zone is maintained at 760±100°C, the pressure in the reaction furnace tube is maintained at 100±10Pa, oxygen is passed through for oxidation, the time is controlled at 3min, and the oxygen flow rate is 600sccm;
[0065] (5) Pre-deposition: After oxidation, the temperature of each temperature zone is maintained at 770±20°C, the pressure is maintained at 100±10Pa, oxygen and phosphorus oxychloride are passed, the oxygen flow rate is 600sccm, the flow rate of phosphorus oxychloride is 600sccm~800sccm, and the time of this step is 4min; then each temperature zone is raised by 10°C, the gas flow rate is kept unchanged, and deposition is continued for 4min;
[0066] (6) The temperature in each temperature zone is maintained at 860±20℃, and high temperature pushing is performed for 10 minutes, and then the temperature is maintained for 2.5 minutes;
[0067] (7) The temperature in each temperature zone is maintained at 800±20℃, cooled and pushed for 15 minutes, and then maintained at the temperature for 6 minutes;
[0068] (8) Maintaining the temperature at 800±20° C., introducing 1300 sccm of phosphorus oxychloride and 400 sccm of oxygen for 10 min to form a PSG layer with a high phosphorus content;
[0069] (9) The temperature of each temperature zone is maintained at 800±20°C, and 1000sccm of oxygen is introduced for oxidation;
[0070] (10) After oxidation, fill with nitrogen at 2500 sccm to normal pressure; and remove the silicon wafer.
[0071] Comparative Example 1: Preparation of silicon wafer with low phosphorus content phosphosilicate glass layer
[0072] (1) The textured silicon wafer is placed into a reaction furnace tube, and the furnace tube is heated to 760°C ± 100°C;
[0073] (2) The temperature of each temperature zone is maintained at 760±100℃ and vacuumed to 50Pa-150Pa;
[0074] (3) The temperature of each temperature zone is maintained at 760±100℃, and the vacuum is evacuated to 50Pa-150Pa. The vacuum is stopped and the furnace tube is leak-checked;
[0075] (4) Pre-oxidation: The temperature of each temperature zone is maintained at 760±100°C, the pressure in the reaction furnace tube is maintained at 100±10Pa, oxygen is passed through for oxidation, the time is controlled at 3min, and the oxygen flow rate is 600sccm;
[0076] (5) Pre-deposition: After oxidation, the temperature of each temperature zone is maintained at 770±20°C, the pressure is maintained at 100±10Pa, oxygen and phosphorus oxychloride are passed, the oxygen flow rate is 600sccm, the flow rate of phosphorus oxychloride is 600sccm~800sccm, and the time of this step is 4min; then each temperature zone is raised by 10°C, the gas flow rate is kept unchanged, and deposition is continued for 4min;
[0077] (6) The temperature in each temperature zone is maintained at 860±20℃, and high temperature pushing is performed for 10 minutes, and then the temperature is maintained for 2.5 minutes;
[0078] (7) The temperature in each temperature zone is maintained at 800±20℃, cooled and pushed for 15 minutes, and then maintained at the temperature for 6 minutes;
[0079] (8) Maintaining the temperature at 800±20° C., introducing 800 sccm of phosphorus oxychloride and 400 sccm of oxygen for 10 min to form a PSG layer;
[0080] (9) The temperature of each temperature zone is maintained at 800±20°C, and 1000sccm of oxygen is introduced for oxidation;
[0081] (10) After oxidation, fill with nitrogen at 2500 sccm to normal pressure; and remove the silicon wafer.
[0082] The silicon wafers prepared in Example 1 and Comparative Example 1 were characterized to test the relationship between the surface concentration of phosphorus and the junction depth. The results are as follows: Figure 1 .
[0083] Figure 1 The relationship between the surface concentration of phosphorus in a silicon wafer and the junction depth is shown in FIG. Figure 1 The inflection point 1 is the highest point, usually located at a depth of 10nm, and usually indicates the surface concentration of doping. 20 / cm 3 -10 21 / cm 3 The surface doping concentration of Example 1 is greater than the surface doping concentration of Comparative Example 1.
[0084] More importantly, Figure 1 The inflection point 2 in the figure is a mutation point. The concentration gradient at the inflection point 2 directly affects the effect of subsequent gate electrode sintering. The inflection point 2 of comparative example 1 is a mutation point, the slope of the curve changes significantly, the concentration gradient is large, and the sintering process is more difficult. The slope of the curve of embodiment 1 changes more gently, the concentration gradient is small, and the sintering process is easier to carry out, so the required temperature is also lower.
[0085] Inflection point 3 indicates the location of the PN junction. The abscissa of inflection point 3 is the junction depth, which is generally between 0.25μm and 0.40μm. A deeper diffusion junction can prevent the gate electrode metal from penetrating into the junction area and reduce the probability of introducing the electrode metal energy level into the bandgap. It can not only make the electrode and the silicon wafer in good contact, but also appropriately relax the strict requirements for temperature and time control during the junction. The ordinate of inflection point 3 indicates the effective doping situation. When the effective doping is more, the open circuit voltage and short circuit current can be increased.
[0086] Example 2
[0087] The sample of Example 1 was treated as follows:
[0088] (1) The preset gate line position on the surface of the silicon wafer is doped with laser, so that the phosphorus in the PSG diffuses into the surface of the silicon wafer. The laser power is set at 25 W, the frequency of the laser engraving parameters of the graphic sub-gate and the anti-break gate is set at 220 kHz, and the energy factor value is set at 250 kHz;
[0089] (2) Screen-printing the grid electrode and sintering it, with the sintering temperature set at 780°C.
[0090] Comparative Example 2
[0091] Take the sample of Comparative Example 1 and process it as follows:
[0092] (1) The preset gate line position on the surface of the silicon wafer is doped with laser, so that the phosphorus in the PSG diffuses into the surface of the silicon wafer. The laser power is set at 25 W, the frequency of the laser engraving parameters of the graphic sub-gate and the anti-break gate is set at 220 kHz, and the energy factor value is set at 250 kHz;
[0093] (2) Screen-printing the grid electrode and sintering it, with the sintering temperature set at 840°C.
[0094] Comparative Example 3
[0095] Take the sample of Comparative Example 1 and process it as follows:
[0096] (1) The preset gate line position on the surface of the silicon wafer is doped with laser, so that the phosphorus in the PSG diffuses into the surface of the silicon wafer. The laser power is set at 25 W, the frequency of the laser engraving parameters of the graphic sub-gate and the anti-break gate is set at 220 kHz, and the energy factor value is set at 250 kHz;
[0097] (2) Screen-printing the grid electrode and sintering it, with the sintering temperature set at 780°C.
[0098] Comparative Example 4
[0099] The sample of Example 1 was treated as follows:
[0100] (1) The preset gate line position on the surface of the silicon wafer is doped with laser, so that the phosphorus in the PSG diffuses into the surface of the silicon wafer. The laser power is set at 25 W, the frequency of the laser engraving parameters of the graphic sub-gate and the anti-break gate is set at 220 kHz, and the energy factor value is set at 250 kHz;
[0101] (2) Screen-printing the grid electrode and sintering it, with the sintering temperature set at 780°C.
[0102] The solar cells prepared in the above-mentioned Example 2 and Comparative Examples 2 to 4 were characterized to obtain their efficiency data, and the results can be seen in Table 2.
[0103] Table 2: Comparison of battery efficiency data of Example 2 and Comparative Examples 2 to 4
[0104]
[0105] It can be seen from the data in Table 2 that compared with Comparative Example 2 using the method used in the traditional production line, the efficiency of Example 2 can be improved by 0.036%, mainly reflected in the short-circuit current gain of 0.009A, the fill factor gain of 0.07%, and the pass rate increase of 0.59%. This is mainly because Example 2 adopts a specific method for preparing the phosphorus silicon glass layer, so that the subsequent screen printing sintering steps can be carried out at a lower temperature, which is conducive to the silver paste shaping of the gate electrode, and the ohmic contact is good, which is conducive to improving the short-circuit current and fill factor, which is consistent with the theoretical analysis.
[0106] Furthermore, the yield test was performed on Example 2 and Comparative Example 2, and the specific test results are shown in Table 3.
[0107] Table 3: Comparison of battery yield data of Example 2 and Comparative Example 2
[0108]
[0109] It can be seen from the data in Table 3 that the yield of the battery cell of Example 2 is 0.56% higher than that of Comparative Example 2, which is mainly reflected in foggy blackening, dirtiness and graphite boat marks. This may be mainly due to the fact that the process of Example 2 helps to reduce the escape of hydrogen ions during the sintering process and improve the protection and passivation effect of the silicon nitride film.
[0110] Furthermore, an ORT test (Ongoing Reliability test, i.e., product reliability test or product continuity test) was performed on the battery cells of Example 2 and Comparative Example 2. The results are shown in Table 4.
[0111] Table 4: Comparison of battery ORT test data of Example 2 and Comparative Example 2
[0112]
[0113]
[0114] As can be seen from Table 4, the results of the front silver tensile test, back silver tensile test data, and curvature test data of Example 2 and Comparative Example 2 all show OK. At the same time, the curvature of Example 2 is better than that of Comparative Example 2. Since the thermal expansion coefficient of the silicon wafer is different from that of the aluminum layer in contact with the back, the shrinkage of the aluminum layer after sintering will cause the silicon wafer to deform, which is called silicon wafer warpage. The thinner the silicon wafer and the thicker the aluminum layer, the greater the distortion of the silicon wafer, causing the curvature of the cell to exceed the predetermined specified requirements. The lower electric shock sintering temperature will not cause damage to the silicon wafer, and it will slow down the shrinkage of the aluminum paste on the back, reduce the warpage of the solar cell, improve the yield rate, and increase the service life of the cell, which is conducive to the development of thinner silicon wafer technology in the future.
[0115] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0116] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a solar cell, characterized in that: The steps include: Placing a P-type doped silicon wafer in a reaction chamber to form an N-type doped layer on the surface of the silicon wafer; Introducing a phosphorus source into the reaction chamber, controlling the flow rate of the phosphorus source to be 1200 sccm to 1500 sccm, so that the phosphorus source reacts with the silicon wafer to form a phosphorus-silicate glass layer on the surface of the N-type doped layer; Doping the portion of the silicon wafer used for screen-printing the gate electrode with laser so that the phosphorus atoms in the phosphorus-silicate glass layer at the laser-doped portion diffuse into the N-type doping layer; The phosphorus silicon glass layer is removed, and a gate electrode is formed on the surface of the silicon wafer at a position for screen printing the gate electrode, and a sintering treatment is performed. During the sintering, the sintering temperature is controlled to be 760° C. to 800° C.
2. The method for preparing a solar cell according to claim 1, characterized in that: In the step of forming the phosphosilicate glass layer, the temperature in the reaction chamber is controlled to be 780° C. to 820° C., and the reaction time is controlled to be 12 min to 16 min.
3. The method for preparing a solar cell according to claim 1, characterized in that: In the step of forming the phosphosilicate glass layer, an oxygen source with a flow rate of 300 sccm to 500 sccm is introduced into the reaction chamber.
4. The method for preparing a solar cell according to any one of claims 1 to 3, characterized in that: The phosphorus source is selected from phosphorus oxychloride.
5. The method for preparing a solar cell according to any one of claims 1 to 3, characterized in that: After forming the phosphosilicate glass layer, the method further includes: introducing 1000 sccm to 1200 sccm of oxygen into the reaction chamber.
6. The method for preparing a solar cell according to any one of claims 1 to 3, characterized in that: In the step of laser doping the silicon wafer, the power of the laser is controlled to be 15W to 35W.
7. The method for preparing a solar cell according to any one of claims 1 to 3, characterized in that: In the process of forming the N-type doping layer, a phosphorus source is first introduced into the reaction chamber for pre-deposition, and then a high-temperature push-junction treatment is performed at a temperature of 840°C to 880°C, and then a low-temperature push-junction treatment is performed at a temperature of 780°C to 820°C.
8. The method for preparing a solar cell according to claim 7, characterized in that: In the process of forming the N-type doping layer, the flow rate of the introduced phosphorus source is 600 sccm to 800 sccm.
9. A solar cell, characterized in that: The solar cell is prepared by the method for preparing the solar cell according to any one of claims 1 to 8.
10. A power generation device, characterized in that: Comprising the solar cell as claimed in claim 9.
Citation Information
Patent Citations
Diffusion process of silicon-wafer laser doping SE
CN107394012A
Regional layered deposition diffusion process
CN110164759A
Novel alkaline polishing selective emitter process technology
CN110473938A
Lightly-doped substrate, substrate with selective emitter, and solar cell and preparation method and application thereof
CN112038438A
Manufacturing method of selective emitter
CN113594303A