Silicon carbide-silicon-graphite composite material and preparation method and application thereof
By generating nano-silicon and silicon carbide coating layers on the surface of graphite particles through the CVD method, a silicon carbide-silicon-graphite composite material is formed, which solves the problems of volume expansion of silicon materials and complex CVD process in lithium-ion batteries, and achieves high stability properties and electrochemical activity, extending battery life and simplifying the preparation process.
Patent Information
- Application Number
- CN202210330869.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-29
AI Technical Summary
The volume expansion of the silicon material in existing lithium-ion battery anode materials during the charge and discharge process leads to a reduction in capacity and a short cycle life. The process of preparing silicon-carbon composite materials by CVD is complicated, which limits its wide application.
By in-situ generating nano-silicon and silicon carbide coating layers on the surface of graphite particles through CVD method, a silicon carbide-silicon-graphite composite material is formed, which simplifies the process and improves the stability and electrochemical activity of the material. Silicon carbide is used as the coating. layer to enhance the material's strength.
It improves the stability and electrochemical activity of the composite material, extends the cycle life of the lithium-ion battery, simplifies the preparation process, reduces the production cost, and is suitable for industrial production.
Smart Images

Figure CN114824199B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a silicon-carbon composite material, specifically to a silicon carbide-silicon-graphite composite material, further relates to a method for preparing the silicon carbide-silicon-graphite composite material by using vapor deposition, and to an application of the silicon carbide-silicon-graphite composite material in a negative electrode material for a lithium ion battery, belonging to the technical field of preparing negative electrode materials for lithium ion batteries. Background Art
[0002] Lithium-ion batteries play an extremely important role in the field of portable electronic devices and electric vehicles because of their high capacity and good stability. With the progress and development of the industry, the demand for new power sources in society is increasing rapidly. Among the many lithium-ion battery negative electrode materials, compared with the traditional graphite negative electrode material (~372mAhg -1 ) Silicon material has a very high theoretical capacity (~4200mAhg -1 ) and a lower potential to lithium (<0.5V vs Li / Li + ), so silicon materials have excellent development prospects in the field of lithium batteries. However, silicon-based negative electrode materials will have serious volume expansion problems during the process of lithium insertion and extraction, resulting in a large reduction in the capacity of the negative electrode, making the cycle life of silicon materials as negative electrode materials short. At the same time, silicon materials have low conductivity as semiconductors. These properties are not conducive to the use of silicon materials in lithium-ion batteries.
[0003] In order to solve the problem of silicon materials in lithium-ion batteries, silicon materials are nano-sized and many nanostructured forms of silicon, such as nanoparticles, nanowires and nanotubes, are prepared to solve this problem and reduce the material failure caused by the expansion of silicon materials during charging and discharging. For the practical application of nano-silicon, it has been emphasized that it is a reasonable strategy to combine silicon materials with graphite to make carbon-silicon composite materials, rather than using silicon-based materials to achieve high energy density. Silicon materials with nano-sized structures can be prepared on the surface of graphite using the CVD method. At the same time, the nano-silicon materials prepared by the CVD method can control the growth size, morphology and content of silicon materials in the negative electrode materials. It is a very excellent method for preparing nano-silicon materials. However, these silicon-graphite composite materials have limited specific capacity and limited silicon content. Otherwise, excessive deposition of Si will cause the Si nanolayer on the graphite to thicken, resulting in accelerated degradation of the cycle performance and weakening of the advantages of nano-sized. At the same time, coating the silicon material can not only reduce the impact of the expansion of the silicon material, but also effectively reduce the specific surface area of the graphite, thereby reducing the lithium ion loss of the silicon-carbon composite negative electrode material during the first cycle.
[0004] Currently, most CVD preparations of silicon-carbon composite materials often require multiple steps, multiple heating and cooling processes, and multiple depositions of silicon and carbon sources must be changed to obtain the final product. The material preparation process is often too complicated, which is not conducive to the wider use of CVD preparations of silicon-carbon materials. The development of CVD preparations of silicon-carbon composite materials with simpler steps is of great significance to the application of silicon-based materials in lithium-ion batteries. Summary of the invention
[0005] In view of the defects of the prior art, the first object of the present invention is to provide a silicon carbide-silicon-graphite composite material, which uses graphite as a matrix material, and has nano-silicon and silicon carbide coating layers generated in situ on the graphite surface by a CVD method. The nano-silicon is evenly dispersed and has a high bonding strength with the graphite, which greatly improves the stability and electrochemical activity of the composite material. Silicon carbide is used as the coating layer, which has a higher coating thickness than the common amorphous carbon coating layer, and the thickness can reach 100 to 200 nm. The silicon carbide coating with a crystalline structure is more firm, which greatly improves the stability of the composite material.
[0006] The second object of the present invention is to provide a method for preparing a silicon carbide-silicon-graphite composite material. In the method, during the deposition of nano-silicon and silicon carbide coating layers, only one CVD process is required to complete the process, thereby simplifying the process and overcoming the defect that in the prior art of preparing silicon-carbon composite materials by CVD, multiple vapor deposition steps are often required to complete the deposition of different components. The complex deposition process limits the wide application of coated carbon-silicon composite materials.
[0007] The third object of the present invention is to provide an application of a silicon carbide-silicon-graphite composite material, which can be used as a lithium ion negative electrode material to obtain a lithium ion battery with high lithium storage capacity and good cycle stability.
[0008] In order to achieve the above technical objectives, the purpose of the present invention is to provide a method for preparing a silicon carbide-silicon-graphite composite material, which is to sequentially generate nano-silicon and silicon carbide layers on the surface of graphite particles or a composite of graphite particles and metal catalysts by chemical vapor deposition, and then remove the metal catalyst by high-temperature volatilization or acid washing to obtain the composite material.
[0009] The technical solution of the present invention combines metal catalysts with graphite particles, and generates silicon nanomaterials (which may be silicon nanoparticles or silicon nanofibers, etc.) in situ on the graphite surface by vapor deposition under the catalytic action of the metal catalyst, or directly deposits silicon nanofilms on the graphite particle surface without adding catalysts, and then deposits silicon carbide coating layers. The two deposits can be completed by a single CVD deposition process, and then the metal catalyst is removed by high-temperature volatilization to obtain a pure silicon carbide-silicon-graphite composite material. In the prior art, in the process of preparing silicon-carbon composite materials with a coating structure by vapor deposition, multiple vapor deposition steps are often required to complete the deposition process of different materials, and the complex deposition process limits the production process of coated carbon-silicon composite materials. The carbon-silicon composite material designed in the technical solution of the present invention uses graphite particles as carriers, nanosilicon as active substances, and silicon carbide as coating layers, and the generation process of nanosilicon and silicon carbide can be completed in the same CVD deposition system by simply adjusting the silicon-carbon atomic ratio and deposition temperature, thereby simplifying the preparation process of coated silicon-carbon composite materials.
[0010] As a preferred solution, the graphite particles and metal catalyst composite are obtained by wet mixing of metal catalyst and graphite particles. Generally speaking, metal catalyst and graphite particles can be mixed by dry method or wet method. Dry mixing is to directly mechanically mix graphite particles and metal catalyst, such as grinding, ball milling and the like. Wet mixing is mainly to dissolve the metal catalyst in a solvent, mix it with graphite particles during condensation, and dry it. Wet mixing is preferred, which can evenly load the metal catalyst on the surface of graphite particles.
[0011] As a preferred solution, the metal catalyst is a metal compound containing at least one of iron, nickel, copper and cobalt. The specific metal catalyst is a soluble salt of a metal such as iron, nickel, copper, cobalt, such as ferric chloride, nickel nitrate, copper sulfate, cobalt chloride, etc.
[0012] As a preferred solution, the graphite particles are artificial graphite and / or natural graphite, such as spherical graphite, flake graphite and expanded graphite.
[0013] As a preferred solution, the mass of the metal catalyst accounts for 1% to 10% of the total mass of the graphite particles and the metal catalyst composite. If the content of the metal catalyst is less than 1%, the amount of effective substances deposited on the surface of the graphite particles in situ will be reduced, and too much metal catalyst will reduce the electrode capacity of the graphite. More preferably, the mass of the metal catalyst accounts for 2% to 6% of the total mass of the graphite particles and the metal catalyst composite.
[0014] As a preferred solution, the chemical vapor deposition conditions for generating nano-silicon are: using one or more of silane, methylsilane, chlorosilane, and chloromethylsilane as the silicon source, the atmosphere is a hydrogen atmosphere, the temperature is 500-1100°C, and the time is 1-3 hours; the nano-silicon is silicon nanoparticles, silicon nanofilms, or silicon nanofibers. The morphology of the generated nano-silicon is related to the selected silicon source raw material and the deposition temperature and time and other conditions. For example, under the same deposition conditions, the higher the silicon-hydrogen ratio, the more likely it is to generate silicon nanofibers. For example, when the ratio of silicon atoms to hydrogen atoms is 1:2 during the vapor deposition process, silicon nanoparticles are mainly generated, and when the ratio of silicon atoms to hydrogen atoms is 2:1, silicon nanofibers are mainly generated. The silicon source is mainly a gaseous silicon-containing small molecule compound, specifically silane such as monosilane, disilane, etc., chlorosilane such as monochlorosilane, chloromethylsilane such as (chloromethyl) trimethylsilane
[0015] As a preferred solution, the chemical vapor deposition conditions for generating the silicon carbide layer are: using silane as the silicon source, using at least one of methane, ethane, propane, isopropane, butane, isobutane, ethylene, propylene, acetylene, and methane as the carbon source, or using at least one of methylsilane, chlorosilane, and chloromethylsilane as both the silicon source and the carbon source, the atmosphere is an inert atmosphere, the molar ratio of the silicon source to the carbon source is measured according to the molar ratio of silicon atoms to carbon atoms of not less than 1:2, the temperature is 600 to 1500°C, and the time is 0.5 to 3 hours. The vapor deposition pressure can be negative pressure, positive pressure or normal pressure. Generally, silicon-carbon composite materials use a carbon coating layer, but CVD deposits an amorphous carbon layer that does not form a stable carbon crystal structure, so it is difficult to form a thicker carbon coating layer on the surface of the tiny particles. The thickness of the carbon coating layer is often less than 100nm; and the silicon carbide coating can form a stable crystal structure during the deposition process to form a silicon carbide coating layer formed by the aggregation of tiny silicon carbide crystal particles one by one (as shown in the description Figure 2 d), so that silicon carbide can have a higher thickness, above 200nm. Inert atmosphere such as argon.
[0016] As a preferred solution, the conditions for high-temperature volatilization removal of metal catalysts are: temperature of 1500-2500° C. and time of 0.5-2 hours. Under the preferred conditions, efficient volatilization removal of metal catalysts can be achieved.
[0017] As a preferred solution, the conditions for acid washing to remove the metal catalyst are: washing with 0.1-2 mol / L dilute hydrochloric acid or dilute sulfuric acid.
[0018] As a preferred solution, the single layer thickness of the silicon carbide layer is 0.1-1.0 μm.
[0019] The invention also provides a silicon carbide-silicon-graphite composite material, which is obtained by the preparation method.
[0020] The silicon carbide-silicon-graphite composite material of the present invention uses graphite particles as a matrix material, and nano silicon and silicon carbide coating layers are in-situ generated on the surface of the graphite particles by a CVD method. The nano silicon is evenly dispersed on the surface of the graphite particles and has a high bonding strength with the graphite particles, which greatly improves the stability and electrochemical activity of the composite material. Compared with a common amorphous carbon coating layer, the silicon carbide is used as the coating layer, which has a higher coating thickness of 100 to 200 nm, or even more than 200 nm. The SiC coating layer with a crystal structure is more solid, which greatly improves the stability of the composite material.
[0021] The present invention also provides an application of a silicon carbide-silicon-graphite composite material, which is applied as a negative electrode material for a lithium-ion battery.
[0022] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0023] 1. In the silicon carbide-silicon-graphite composite material of the technical solution of the present invention, nano-silicon and graphite particles are in-situ composited by a chemical vapor deposition method, the nano-silicon is evenly dispersed, and the bonding strength between the nano-silicon and the graphite particles is high, which greatly improves the stability and electrochemical activity of the composite material. The in-situ generated silicon carbide layer is used as the coating layer. Compared with the common amorphous carbon coating layer, the silicon carbide coating layer has a higher coating thickness, which can reach 100 to 200 nm, and the SiC coating layer with a crystalline structure is more solid. The silicon carbide layer can effectively alleviate the volume effect brought by silicon in the cycle process, greatly improve the stability of the composite material, and help to improve the performance and service life of the battery.
[0024] 2. During the preparation of the silicon carbide-silicon-graphite composite material of the technical solution of the present invention, the effective substance nano-silicon and the silicon carbide coating layer can be produced in a single CVD deposition process, which reduces the heat loss in the production process and simplifies the preparation process of the coated silicon-carbon composite material.
[0025] 3. The preparation method of the silicon carbide-silicon-graphite composite material of the technical solution of the present invention has a simple process, low cost, and is easy to industrialize.
[0026] 4. The silicon carbide-silicon-graphite composite material of the technical solution of the present invention is prepared by a chemical vapor deposition method, and has the characteristics of controllable silicon size, morphology, and loading, and controllable silicon carbide coating thickness. It can be used to prepare silicon-carbon composite negative electrode materials with different performance requirements according to design needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1XRD patterns of pure graphite G, silicon-graphite composite material Si / G, silicon carbide-graphite composite material SiC@G, and silicon carbide-silicon-graphite composite material SiC@Si / G (Example 1).
[0028] Figure 2 It is a scanning electron microscope image; among them, a is pure graphite G, b is silicon carbide-graphite composite material SiC@G, c is silicon-graphite composite material Si / G, and d is silicon carbide-silicon-graphite composite material SiC@Si / G.
[0029] Figure 3 The cycling curves of lithium-ion batteries of pure graphite G, silicon-graphite composite material Si / G, silicon carbide-graphite composite material SiC@G and silicon carbide-silicon-graphite composite material SiC@Si / G were tested using CR2032 half-cell test with lithium metal as the counter electrode. DETAILED DESCRIPTION
[0030] The following embodiments are intended to further illustrate the present invention, but are not intended to limit the scope of protection of the claims of the present invention.
[0031] Example 1
[0032] 1. Weigh 50g of graphite powder and 2g of ferric chloride in an aqueous solution, dry it in a blast drying oven at 80℃ for 12h, grind it, and sieve it through 200 mesh. Place the above sample in a chemical vapor deposition furnace, use trichloromethylsilane as the silicon source, set the deposition atmosphere to hydrogen atmosphere, and deposit it at 800℃ under normal pressure for 1h to obtain a silicon nanofiber-graphite composite material.
[0033] 2. In the same vapor deposition furnace, the temperature was increased to 900°C, trichloromethylsilane was used as the silicon source and carbon source, argon was used as the carrier gas, and the deposition atmosphere was set to argon atmosphere. The deposition was performed for 0.5 h, and then the sample was placed in a high-temperature furnace for heat treatment at 1500°C for 0.5 h to remove trace elements to obtain a silicon carbide-silicon nanofiber-graphite composite material. The deposited sample was ground and washed three times with deionized water, filtered, and dried to obtain a silicon carbide-silicon nanofiber-graphite composite material (d).
[0034] The XRD pattern of the prepared silicon carbide-silicon-graphite composite material is as follows: Figure 1 As shown, compared with the diffraction peaks of the graphite substrate, the silicon carbide-silicon-graphite composite material has obviously more characteristic peaks of silicon and silicon carbide, which indicates the successful deposition of silicon and the successful coating of silicon carbide.
[0035] The scanning electron microscope image of the prepared silicon carbide-silicon-graphite composite material is shown in Figure 2 As shown, Figure 2 Figure a is an electron microscope image of a single graphite particle. Figure 2The sample c in the middle is obtained by silicon fiber deposition. The silicon fibers are densely and staggeredly distributed on the graphite surface. Figure 2 Figure b shows the morphology of the sample after being coated with silicon carbide. Figure 2 (d) in the middle is the sample morphology of silicon carbide-silicon-graphite composite material after silicon deposition and then silicon carbide deposition.
[0036] The negative electrode material is composed of a composite negative electrode material, conductive carbon black and adhesive PVDF in a ratio of 7:1:2. Lithium metal is used as the counter electrode. Celgard2400 polypropylene porous diaphragm is used. The electrolyte is 1 mol / L LiPF6 solution. The organic solvent is a mixture with a volume ratio of EC:DMC=1:1. A CR2032 half-cell test is prepared with a test current density of 100 mA / g.
[0037] The cycle performance curve of silicon carbide-silicon-graphite composite material is as follows Figure 3 As shown in the figure, the reversible specific capacity of graphite G after 100 cycles is 330 mAh / g, and the reversible specific capacity of silicon-silicon-graphite composite material after 100 cycles is 490 mAh / g, and the capacity hardly changes. This is because the growth of silicon nanofibers improves the lithium storage capacity of the material, and the coating of the silicon carbide layer improves the cycle stability of the composite material.
[0038] Comparative Example 1
[0039] 1. Weigh 50g of graphite powder and 2g of ferric chloride in an aqueous solution, dry it in a blast drying oven at 80℃ for 12h, grind it, and sieve it through 200 mesh. Place the above sample in a chemical vapor deposition furnace, use trichloromethylsilane as the silicon source, set the deposition atmosphere to hydrogen atmosphere, and deposit it at 800℃ under normal pressure for 1h to obtain a silicon nanofiber-graphite composite material.
[0040] 2. The sample without silicon carbide deposition was placed in a high-temperature furnace for heat treatment at 1500°C for 0.5h to remove trace elements to obtain a carbon-silicon composite material without silicon carbide deposition. The deposited sample was ground and washed three times with deionized water, filtered and dried to obtain a silicon nanofiber-graphite composite material (c).
[0041] The prepared silicon-carbon composite negative electrode material was assembled into a lithium battery according to Example 1. After 100 cycles, the specific capacity was only 327 mAh / g. Figure 3 As shown in the Si / G curve, the capacity of the carbon-silicon composite material coated with silicon carbide is greatly reduced after multiple cycles. This is because in the absence of a silicon carbide layer, the silicon material undergoes a drastic volume expansion and pulverization, leading to failure, and the overall capacity of the composite material decreases.
[0042] Comparative Example 2
[0043] 1. Weigh 50g of graphite powder and 2g of ferric chloride in an aqueous solution, dry in a forced air drying oven at 80°C for 12h, grind, and sieve through 200 mesh. Take the above sample and place it in a chemical vapor deposition furnace at a temperature of 900°C, use trichloromethylsilane as the silicon source and carbon source, use argon as the carrier gas, set the deposition atmosphere to an argon atmosphere, deposit for 0.5h, then place it in a high-temperature furnace for heat treatment at 1500°C for 0.5h, remove trace elements to prepare a silicon carbide-silicon nanofiber-graphite composite material, grind the deposited sample, wash it three times with deionized water, filter it, and dry it to prepare a silicon carbide-graphite composite material (b).
[0044] The prepared silicon carbide-graphite composite negative electrode material was assembled into a lithium battery according to Example 1. The capacity was 343 mAh / g in the first cycle and 330 mAh / g after 100 cycles. Figure 3 As shown in the SiC@G curve, the capacity has not changed significantly compared with the graphite substrate, indicating that the SiC coating will not affect the original capacity.
[0045] Example 2
[0046] 1. Weigh 50g of graphite powder and 2g of nickel nitrate, mix them in aqueous solution, dry them in a forced air drying oven at 80℃ for 12h, grind them, and sieve them through 200 mesh. Place the above sample in a chemical vapor deposition furnace, use silane as the silicon source, set the deposition atmosphere to hydrogen atmosphere, deposit at 600℃ for 0.5h, and the pressure is -0.1MPa to obtain a silicon nanoparticle-graphite composite material.
[0047] 2. Control the temperature of the chemical vapor deposition furnace to 600°C, add acetylene as the carbon source, use silane as the silicon source, adjust the ratio of carbon atoms to silicon atoms to 2:1, use argon as the carrier gas, set the deposition atmosphere to argon atmosphere, deposit for 1 hour, grind the deposited sample, wash it three times with deionized water, filter it, and dry it to prepare a silicon carbide-silicon nanoparticle-natural graphite composite material.
[0048] 3. The sample was then placed in a high-temperature furnace for heat treatment at 1500°C for 0.5h. After the sample cooled to room temperature, it was ground and washed three times with deionized water, filtered, dried, and trace elements were removed to prepare a silicon carbide-silicon nanoparticle-natural graphite composite material.
[0049] The prepared silicon carbide-silicon-natural graphite silicon-carbon composite negative electrode material was assembled into a lithium battery according to Example 1, with an initial discharge specific capacity of 980 mAh / g, and after 50 cycles, it still had a specific capacity of 560 mAh / g.
[0050] Example 3
[0051] 1. Weigh 50g of graphite powder, grind it, and sieve it through 200 mesh. Place the above sample in a chemical vapor deposition furnace, use silane as the silicon source, set the deposition atmosphere to hydrogen atmosphere, and deposit it at 600℃ under normal pressure for 0.5h, with a pressure of -0.1MPa, to obtain a silicon nanofilm-graphite composite material.
[0052] 2. Control the temperature of the chemical vapor deposition furnace to 600°C, add propylene as the carbon source, use silane as the silicon source, control the deposition atmosphere to be argon atmosphere, adjust the ratio of carbon atoms to silicon atoms to 2:1, deposit for 0.5h, grind the deposited sample, wash it three times with deionized water, filter it, and dry it to prepare a silicon carbide-silicon nanofilm-graphite composite material.
[0053] 3. The prepared silicon carbide-silicon nanofilm-graphite composite negative electrode material was assembled into a lithium battery according to Example 1, with an initial discharge specific capacity of 760 mAh / g and a capacity of 460 mAh / g after 50 cycles.
[0054] Example 4
[0055] 1. Weigh 50g of graphite powder and 2g of nickel nitrate, mix them in aqueous solution, dry them in a forced air drying oven at 80℃ for 12h, grind them, and sieve them through 200 mesh. Place the above sample in a chemical vapor deposition furnace, use silane as the silicon source, and deposit them at 700℃ for 0.5h to obtain a silicon nanofiber-graphite composite material.
[0056] 2. The temperature of the chemical vapor deposition furnace was controlled at 800°C, dichlorodimethylsilane was used as the carbon source and silicon source, the atmosphere was set to argon atmosphere, and the deposition was performed for 0.5 h. After the deposited sample was ground, it was washed three times with deionized water, filtered and dried to prepare a silicon carbide-silicon nanofiber-graphite composite material.
[0057] 3. The sample was then washed with 0.5 mol / L dilute hydrochloric acid solution to remove the catalyst, and then washed three times with deionized water, filtered, dried, and trace elements were removed to prepare a silicon carbide-silicon nanofiber-natural graphite composite material.
[0058] The prepared silicon carbide-silicon nanofiber-graphite composite negative electrode material was assembled into a lithium battery according to Example 1, and the initial discharge specific capacity was 856 mAh / g, and the capacity was 558 mAh / g after 50 cycles.
Claims
1. A method for preparing a silicon carbide-silicon-graphite composite material, characterized in that: Nano-silicon and silicon carbide layers are sequentially generated on the surface of the composite of graphite particles and metal catalysts by chemical vapor deposition, and then the metal catalysts are removed by high-temperature volatilization or acid washing. The chemical vapor deposition conditions for generating nano-silicon are: using one or more of silane, methylsilane, chlorosilane, and chloromethylsilane as silicon sources, hydrogen atmosphere, temperature of 500-1100° C., and time of 1-3 hours; the nano-silicon is silicon nanoparticles; the ratio of silicon atoms to hydrogen atoms is 1:2; The chemical vapor deposition conditions for generating the silicon carbide layer are: using silane as the silicon source, using at least one of methane, ethane, propane, isopropane, butane, isobutane, ethylene, propylene, and acetylene as the carbon source, or using at least one of methylsilane, chlorosilane, and chloromethylsilane as both the silicon source and the carbon source, the atmosphere is an inert atmosphere, the molar ratio of the silicon source to the carbon source is measured according to the molar ratio of silicon atoms to carbon atoms of not less than 1:2, the temperature is 600 to 1500° C., and the time is 0.5 to 3 hours; the conditions for high-temperature volatilization to remove the metal catalyst are: the temperature is 1500 to 2500° C., and the time is 0.5 to 2 hours; The graphite particles and metal catalyst composite is obtained by mixing the metal catalyst and the graphite particles through a wet method.
2. The method for preparing a silicon carbide-silicon-graphite composite material according to claim 1, characterized in that: The metal catalyst is a metal compound containing at least one of iron, nickel, copper and cobalt; The graphite particles are artificial graphite and / or natural graphite.
3. The method for preparing a silicon carbide-silicon-graphite composite material according to claim 1, characterized in that: The mass of the metal catalyst accounts for 1% to 10% of the total mass of the composite of graphite particles and the metal catalyst.
4. The method for preparing a silicon carbide-silicon-graphite composite material according to claim 1, characterized in that: The single layer thickness of the silicon carbide layer is 0.1-1.0 μm.
5. A silicon carbide-silicon-graphite composite material, characterized in that: Obtained by the preparation method according to any one of claims 1 to 4.
6. The use of a silicon carbide-silicon-graphite composite material according to claim 5, characterized in that: Used as negative electrode material for lithium-ion batteries.
Citation Information
Patent Citations
Carbon / silicon / carbon nano composite structure cathode material and preparation method thereof
CN102214817A
Composite material, preparation method, lithium ion battery negative electrode material containing composite material and lithium ion battery
CN111900353A
Silicon-natural graphite composite material, application and method for preparing silicon-natural graphite composite material through catalysis of trace harmless impurities
CN112234171A
Silicon carbide-coated hollow silicon material, preparation method thereof, and electrode and electrochemical device using silicon carbide-coated hollow silicon material
CN112242504A
Negative electrode material and preparation method thereof, negative electrode plate and lithium ion battery
CN113735127A