A multi-element doped sodium ion battery positive electrode material and its preparation method and application
By doping the sodium-ion battery cathode material Na3V2(PO4)3 with manganese, silicon and transition metals, the problem of insufficient energy density and electrochemical performance has been solved, and the performance of the sodium-ion battery has been significantly improved, making it suitable for large-scale applications. Scale energy storage systems.
Patent Information
- Application Number
- CN202210461978.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-04-28
AI Technical Summary
Existing sodium-ion battery cathode materials have deficiencies in energy density, electrochemical performance, and cycle performance, which limit their application in large-scale energy storage systems.
By doping the Na3V2(PO4)3 structure with multiple elements of manganese, silicon and transition metals, NazMnwVyMu(PO4)3-x(SiO4)x is formed, maintaining the three-dimensional framework structure and improving energy density and electrochemical performance.
It achieves higher energy density, better electrochemical performance and better cycle performance, significantly improves the discharge specific capacity and cycle life of sodium-ion batteries, and is suitable for large-scale industrial production.
Smart Images

Figure HDA0003620690020000011 
Figure HDA0003620690020000012 
Figure HDA0003620690020000013
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion battery electrode materials, and in particular to a multi-element doped sodium ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] With the continuous use of non-renewable energy, the energy crisis has made renewable energy (such as wind energy, tidal energy, solar energy, etc.) more and more valued. Since renewable energy itself is uncontrollable and unadjustable, energy storage plays a key role in the utilization of these energy sources. Rechargeable batteries are the representative technology of energy storage. After decades of development, lithium-ion batteries have been widely used, making it possible to reduce the consumption of fossil fuels. However, due to the limited lithium resources and the scarcity of heavy metal elements such as cobalt and nickel commonly used in lithium-ion batteries, their application in large-scale energy storage will be limited.
[0003] As we all know, the reserves of sodium in the earth's crust are relatively abundant and widely distributed. At the same time, sodium and lithium have similar physical and chemical properties and similar extraction / insertion mechanisms. Therefore, the research and development of sodium-ion batteries is expected to alleviate the problem of limited development of energy storage batteries caused by the shortage of lithium resources to a certain extent. In addition to the advantages of abundant resources, low cost, and wide distribution, sodium-ion batteries have greater safety advantages compared to lithium-ion batteries. The thermal runaway temperature of sodium batteries is higher than that of lithium batteries, and they are more easily passivated and oxidized, and are not prone to flammability, which is the main disadvantage of lithium batteries. Therefore, sodium-ion batteries have great potential for industrialization.
[0004] In sodium-ion batteries, cathode materials are the bottleneck for improving their energy density and power output, so it is necessary to vigorously develop advanced cathode materials. Na3V2(PO4)3 with sodium superionic conductor (NASICON) structure has the advantages of excellent structural stability, high redox potential, good thermal stability, large theoretical energy density and open three-dimensional framework structure. However, due to the Na + The large ionic radius and slow diffusion kinetics rate have greatly restricted the energy density, electrochemical properties and cycle performance of the material, limiting its further practical application, especially in large-scale energy storage systems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a multi-element doped sodium ion battery positive electrode material and its preparation method and application in view of the shortcomings of the existing sodium ion battery positive electrode materials, and to dope and modify Na3V2(PO4)3 with NASICON structure by using manganese, silicon and transition metals, with manganese doping at the V position, transition metal doping at the V position and silicon doping at the P position, so that the material has higher energy density and better electrochemical performance and cycle performance while maintaining an excellent three-dimensional framework structure.
[0006] In order to solve the technical problem proposed by the present invention, the present invention provides a multi-element doped sodium ion battery positive electrode material, the composition of the material is Na z Mn w V y M u (PO4) 3-x (SiO4) x ; Wherein, M is a transition metal, 0≤x≤0.5, 0.5≤y≤2, 0.01≤w≤1, 0≤u≤1, 3≤z≤4, x and u are not 0 at the same time, and the algebraic sum of the valences of each element is zero.
[0007] In the above scheme, the transition metal is Zr 4+ , Nb 5+ ,La 3+ 、Ce 3+ 、Ti 4+ Cr 3+ , Fe 3+ One of them.
[0008] The present invention also provides a method for preparing a multi-element doped sodium ion battery positive electrode material, which specifically comprises the following steps:
[0009] (1) Mixing: weighing a sodium source, a vanadium source, a phosphorus source, a manganese source, a silicon source, a transition metal source, and a complexing agent according to a molar ratio of sodium:vanadium:phosphorus:manganese:silicon:transition metal of z:y:(3-x):w:x:u, and mixing them together in water to prepare a precursor solution;
[0010] (2) Drying: Drying the precursor solution in one stage until it forms a gel, and then drying the gel product in a second stage to obtain a precursor;
[0011] (3) Grinding: Grinding the precursor to prepare precursor powder;
[0012] (4) Sintering: The precursor powder is pre-sintered in an inert protective atmosphere and then sintered to obtain the final product, the sodium ion battery positive electrode material.
[0013] In the above scheme, the sodium source is one or more of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, sodium carbonate, sodium bicarbonate, etc.; the vanadium source is one or more of ammonium metavanadate, sodium metavanadate, vanadium acetylacetonate, etc.; the phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, etc.
[0014] In the above scheme, the manganese source is one or more of manganese acetate, manganese nitrate, manganese oxalate dihydrate, manganese carbonate, manganese dihydrogen phosphate, etc.; the silicon source is one or more of silicon acetate, hexamethylcyclotrisiloxane, tetraethyl orthosilicate, etc.; the transition metal source is one or more of zirconium nitrate, zirconium acetate, zirconium acetylacetonate, hydrated niobium oxalate, sodium niobate, lanthanum nitrate, lanthanum oxalate, lanthanum acetate, lanthanum carbonate, ammonium cerium nitrate, cerium nitrate, cerium oxalate, cerium carbonate, tetrabutyl titanate, chromium acetate, chromium nitrate, ferric nitrate, ferric oxalate, ferric citrate, etc.
[0015] In the above scheme, the complexing agent is one or more of oxalic acid, ascorbic acid, citric acid monohydrate, malic acid and the like.
[0016] In the above scheme, the molar amount of the complexing agent in the precursor solution is 1-2 times the sum of the molar amounts of vanadium, manganese and transition metals, and the mass fraction of the solute in the precursor solution is 10-25%.
[0017] In the above scheme, both the first-stage drying and the second-stage drying are normal pressure drying; the drying temperature of the first-stage drying is 75-95°C, and the drying time is 3-4h; the drying temperature of the second-stage drying is 120-180°C, and the drying time is 3-4h.
[0018] In the above scheme, the grinding time is 20-60 minutes, and the grinding makes the precursor powder particle size uniform.
[0019] In the above scheme, the heating rate of pre-sintering is 3-10℃ / min, and after heating to 350-450℃, it is kept warm for 3-4h; the heating rate of sintering is 3-10℃ / min, and after heating to 500-850℃, it is kept warm for 5-15h.
[0020] In the above scheme, the inert protective atmosphere is one or more of argon, nitrogen, hydrogen argon, helium, etc.
[0021] The present invention also provides an application of a multi-element doped sodium ion battery positive electrode material in a sodium ion battery, and the specific method is as follows:
[0022] Multi-element doped sodium ion battery cathode material Na z Mn w V y M u (PO4) 3-x (SiO4) xIt is made into a sodium ion button battery by using sodium metal as the positive electrode, sodium metal as the negative electrode, and glass fiber as the separator, and assembling the negative electrode shell, negative electrode, separator, electrolyte, positive electrode, gasket, shrapnel, and positive electrode shell in the order of the negative electrode shell.
[0023] In the above scheme, the electrolyte is prepared by dissolving a sodium salt and an additive in a solvent, the sodium salt is sodium perchlorate, the additive is fluoroethylene carbonate (FEC), the solvent is ethylene carbonate (EC) and polycarbonate (PC) in a volume ratio of 1:1, the concentration of the sodium salt in the electrolyte is 1 mol / L, and the amount of the additive added is 5% of the total mass of the sodium salt and the solvent.
[0024] The present invention performs doping modification on Na3V2(PO4)3, and doping with different elements has different effects: ① when V in the material is replaced by Mn, the main structure of the material will not be damaged, and a higher voltage and energy density can be obtained in the electrochemical reaction. At the same time, since V is a toxic rare metal, Mn is non-toxic and its resources are far more abundant than V, after Mn replaces V, the safety of the material is also improved, and the cost of the material is significantly reduced; ② doping transition metals M with different valence states and radii at the V position is beneficial to supporting the crystal framework, and the Mn-O bond, MO bond, Mn-M bond and their spatial configuration are changed through the "Coulomb effect" between ions, thereby increasing the disorder of Mn-O6, inhibiting the Jahn-Taylor distortion caused by Mn, and improving the electrochemical performance and cycle performance of the material; ③ introducing Si with a larger ionic radius at the P position to increase the unit cell volume and the bottleneck area of ion transmission, and improving Na through the "spatial effect". + Transport performance, and due to Si 4+ Replace P 5+ , increasing the Na + The concentration achieves charge balance, allowing the material to achieve smaller particle size and better cycle performance.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention uses manganese, silicon and transition metal to dope and modify Na3V2(PO4)3. Manganese doping at the V position improves the energy density of the material, transition metal doping at the V position improves the electrochemical performance and cycle performance of the material, and silicon doping at the P position improves the Na + Transport properties and cycling performance of materials, multi-element doped sodium ion battery cathode materials Na z Mn w V y M u (PO4) 3-x (SiO4) xIt has higher energy density, better electrochemical properties and cycle performance. Compared with the undoped sodium-ion battery positive electrode material Na3V2(PO4)3, it shows higher discharge specific capacity, better cycle life and more stable high-rate performance, and has good application prospects in sodium-ion batteries and energy storage.
[0027] (2) The present invention first prepares a precursor by a sol-gel method, and then grinds and sinters it to prepare a multi-element doped sodium ion battery positive electrode material. The preparation method has a short process and is easy to operate. In the preparation process, a part of the vanadium source is replaced by a manganese source and a transition metal source, thereby reducing the use of toxic metals, improving the safety of the material and reducing the cost. The obtained Na z Mn w V y M u (PO4) 3-x (SiO4) x It still maintains the excellent three-dimensional framework structure of Na3V2(PO4)3, has good structural stability, strengthens the stability of the framework during the charging and discharging process, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the XRD diagram of Na3V2(PO4)3 obtained in Comparative Example 1 of the present invention.
[0029] Figure 2 This is the constant current cycle diagram of Na3V2(PO4)3 obtained in Comparative Example 1 of the present invention.
[0030] Figure 3 This is the rate performance diagram of Na3V2(PO4)3 obtained in Comparative Example 1 of the present invention.
[0031] Figure 4 The Na obtained in Example 1 of the present invention 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 XRD pattern of .
[0032] Figure 5 The Na obtained in Example 1 of the present invention 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 The charge and discharge performance diagram.
[0033] Figure 6 The Na obtained in Example 1 of the present invention 3.3 Mn 0.1 V 1.9 (PO4) 2.8(SiO4) 0.2 Constant current cycle diagram.
[0034] Figure 7 The Na obtained in Example 1 of the present invention 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 Rate performance diagram.
[0035] Figure 8 The Na4MnV obtained in Example 2 of the present invention 0.95 Zr 0.05 (PO4) 2.95 (SiO4) 0.05 XRD pattern of .
[0036] Fig. 9 The Na4MnV obtained in Example 2 of the present invention 0.95 Zr 0.05 (PO4) 2.95 (SiO4) 0.05 SEM image of .
[0037] Fig.10 The Na4MnV obtained in Example 3 of the present invention 0.9 La 0.1 XRD pattern of (PO4)3.
[0038] Fig.11 The Na4MnV obtained in Example 4 of the present invention 0.8 La 0.2 XRD pattern of (PO4)3. DETAILED DESCRIPTION
[0039] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0040] Comparative Example 1
[0041] A sodium ion battery positive electrode material, the composition of which is Na3V2(PO4)3, and the preparation method comprises the following steps:
[0042] (1) Mixing: 0.4972 g CH3COONa, 0.4726 g NH4VO3, 0.6971 g NH4H2PO4 and 1.6896 g C6H8O7 were mixed together in 30 mL of deionized water to prepare a precursor solution;
[0043] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 80°C and dried for 3.5 hours to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 120°C and dried for 4 hours to obtain a light green fluffy porous solid, i.e., the precursor.
[0044] (3) Grinding: Grind the precursor for 25 minutes to prepare a precursor powder with uniform particle size;
[0045] (4) Sintering: The precursor powder is placed in a muffle furnace, and under argon protection conditions, the temperature is increased to 350°C at a heating rate of 3°C / min, and then kept at this temperature for 3 hours for pre-sintering. The temperature is then increased to 850°C at a heating rate of 3°C / min, and then kept at this temperature for 7 hours. The mixture is cooled to obtain the final product Na3V2(PO4)3.
[0046] Figure 1 This is the XRD diagram of Na3V2(PO4)3 obtained in this comparative example. It can be seen from the figure that the diffraction peaks of the material are narrow and sharp, and the positions and relative intensities of the diffraction peaks are basically consistent with the Na3V2(PO4)3 standard card, indicating that the material has been successfully prepared and has good crystallinity.
[0047] Figure 2 This is the constant current cycle diagram of Na3V2(PO4)3 obtained in this comparative example. It can be seen from the figure that the first discharge capacity of the material at a current density of 0.2C is 88mAh / g. After 40 cycles, the discharge capacity is 51mAh / g, and the capacity retention rate is only 57.9%.
[0048] Figure 3 This is the rate performance diagram of Na3V2(PO4)3 obtained in this comparative example. It can be seen from the figure that at current densities of 0.5C, 1C, 2C, and 5C, the discharge specific capacity of the material decreases significantly with the increase of current density, and the high-rate performance of the material is average.
[0049] Example 1
[0050] A sodium ion battery positive electrode material, comprising Na 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 , the preparation method comprises the following steps:
[0051] (1) Mixing: 1.0937 g CH3COONa, 2.6736 g C 15 H 21 O6V, 1.2883g NH4H2PO4, 0.1014gMnN2O6·4H2O, 0.17g C8H 12O4Si and 2.1134 g C6H8O6 were mixed together in 30 mL of deionized water to prepare a precursor solution;
[0052] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 90°C and dried for 3 h to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 150°C and dried for 3 h to obtain a light grayish yellow fluffy porous solid, i.e., the precursor.
[0053] (3) Grinding: Grind the precursor for 30 min to prepare a precursor powder with uniform particle size;
[0054] (4) Sintering: The precursor powder was placed in a muffle furnace, and under argon protection, the temperature was raised to 400°C at a heating rate of 5°C / min, and then kept at this temperature for 3.5 hours for pre-sintering. The temperature was then raised to 550°C at a heating rate of 5°C / min, and then kept at this temperature for 14 hours. The final product Na 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 .
[0055] Figure 4 The Na obtained in this example 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 The XRD diagram shows that the diffraction peaks of the material are narrow and sharp, indicating that the material has good crystallinity. The positions and relative intensities of the diffraction peaks are compared with the Na3V2(PO4)3 standard card, and it is found that the XRD spectrum shifts to a low angle after doping, which is due to the addition of Mn ions. 2+ With Si 4+ The radius is greater than V 3+ With P 5+ The radius of Mn increases the unit cell volume of the material. 2+ With Si 4+ The incorporation of Si does not change the original NASICON structure, but 4+ Successfully incorporated P 5+ The sites bring good structural stability to the sample and strengthen the stability of the framework during the charging and discharging process.
[0056] Figure 5 The Na obtained in this example 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2The charge and discharge performance diagram shows that the first discharge specific capacity of the material at 0.5C, 1C, 2C and 5C are 83.4mAh / g, 82.8, 80.8mAh / g and 73.7mAh / g respectively, and it has a high initial discharge specific capacity at different rates.
[0057] Figure 6 The Na obtained in this example 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 From the constant current cycle diagram, it can be seen that the first discharge capacity of the material at a current density of 0.2C is 94.9mAh / g. After 40 cycles, the discharge capacity is 92.7mAh / g, and the capacity retention rate is as high as 98.98%, indicating that the material has a high discharge capacity and good cycle stability.
[0058] Figure 7 The Na obtained in this example 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 The rate performance diagram shows that at current densities of 0.5C, 1C, 2C, and 5C, there is no obvious difference in the discharge specific capacity of the material. Even at a larger current density, it has an ideal discharge specific capacity, indicating that the material has good performance at high rates.
[0059] In summary, multi-element doped sodium ion battery cathode materials Na 3.3 Mn 0.1 V 1.9 (PO4) 2.8 (SiO4) 0.2 Compared with the undoped sodium-ion battery positive electrode material Na3V2(PO4)3, it exhibits higher discharge specific capacity, better cycle life and more stable high-rate performance, indicating that after doping, it has higher energy density and better electrochemical and cycle performance.
[0060] Example 2
[0061] A sodium ion battery positive electrode material, comprising Na4MnV 0.95 Zr 0.05 (PO4) 2.95 (SiO4) 0.05 , the preparation method comprises the following steps:
[0062] (1) Mix 1.3091 g CH3COONa, 0.4633 g NaVO3, 1.3721 g NH4H2PO4, 0.4601 g MnCO3, 0.0425 g C8H 12 O4Si, 0.0864 g Zr(NO3)4·5H2O, and 0.7275 g C2H2O4 were mixed together in 30 mL of deionized water to prepare a precursor solution;
[0063] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 75°C and dried for 4 hours to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 180°C and dried for 3 hours to obtain a light grayish yellow fluffy porous solid, i.e., the precursor.
[0064] (3) Grinding: Grind the precursor for 40 min to prepare a precursor powder with uniform particle size;
[0065] (4) Sintering: The precursor powder was placed in a muffle furnace, and under argon protection, the temperature was raised to 350°C at a heating rate of 8°C / min, and then kept at this temperature for 4 hours for pre-sintering. The temperature was then raised to 750°C at a heating rate of 8°C / min, and then kept at this temperature for 11 hours. The final product, Na4MnV 0.95 Zr 0.05 (PO4) 2.95 (SiO4) 0.05 .
[0066] Figure 8 The Na4MnV obtained in this example 0.95 Zr 0.05 (PO4) 2.95 (SiO4) 0.05 The XRD diagram shows that the diffraction peaks of the material are narrow and sharp, indicating that the material has good crystallinity. The positions and relative intensities of the diffraction peaks are compared with the Na4MnV(PO4)3 standard card, and it is found that the XRD spectrum shifts to a low angle after doping. The original NASICON structure of the material has not changed, but the unit cell volume has increased. 2+ 、Zr 4+ and Si 4+ The incorporation of further improves the structural stability of the material.
[0067] Fig. 9 The Na4MnV obtained in this example 0.95 Zr 0.05 (PO4) 2.95 (SiO4) 0.05 From the SEM image, it can be seen that the material has good crystallinity and the particle size is about 3-8μm.
[0068] Example 3
[0069] A sodium ion battery positive electrode material, comprising Na4MnV 0.9 La 0.1 (PO4)3, the preparation method comprises the following steps:
[0070] (1) Mixing: 0.3314 g CH3COONa, 0.4261 g NH4VO3, 1.454 g NaH2PO4, 0.9906 g (CH3COO)2Mn·4H2O, 0.1739 g La(NO3)3·6H2O and 1.6091 g C4H6O5 were mixed in 30 mL of deionized water to prepare a precursor solution;
[0071] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 85°C and dried for 4 hours to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 160°C and dried for 3 hours to obtain a light grayish yellow fluffy porous solid, i.e., the precursor.
[0072] (3) Grinding: Grind the precursor for 25 minutes to prepare a precursor powder with uniform particle size;
[0073] (4) Sintering: The precursor powder was placed in a muffle furnace, and under the protection of hydrogen and argon, the temperature was raised to 350°C at a heating rate of 5°C / min, and then kept at this temperature for 3 hours for pre-sintering. Then, the temperature was raised to 600°C at a heating rate of 5°C / min, and then kept at this temperature for 15 hours. The final product, Na4MnV 0.9 La 0.1 (PO4)3.
[0074] Fig.10 The Na4MnV obtained in this example 0.9 La 0.1 The XRD pattern of (PO4)3 shows that the diffraction peaks of the material are narrow and sharp, indicating that the material has good crystallinity. The positions and relative intensities of the diffraction peaks are compared with the Na4MnV(PO4)3 standard card, and it is found that the XRD pattern shifts to a low angle after doping. The original NASICON structure of the material has not changed, but the unit cell volume has increased. 2+ and La 3+ The incorporation of further improves the structural stability of the material.
[0075] Example 4
[0076] A sodium ion battery positive electrode material, comprising Na4MnV 0.8 La 0.2 (PO4)3, the preparation method comprises the following steps:
[0077] (1) Mixing: 0.3314 g CH3COONa, 0.3781 g NH4VO3, 1.454 g NaH2PO4, 0.9906 g (CH3COO)2Mn·4H2O, 0.3464 g La(NO3)3·6H2O and 1.6091 g C4H6O5 were mixed in 30 mL of deionized water to prepare a precursor solution;
[0078] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 85°C and dried for 4 hours to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 160°C and dried for 3 hours to obtain a light grayish yellow fluffy porous solid, i.e., the precursor.
[0079] (3) Grinding: Grind the precursor for 25 minutes to prepare a precursor powder with uniform particle size;
[0080] (4) Sintering: The precursor powder was placed in a muffle furnace, and under the protection of hydrogen and argon, the temperature was raised to 350°C at a heating rate of 5°C / min, and then kept at this temperature for 3 hours for pre-sintering. Then, the temperature was raised to 600°C at a heating rate of 5°C / min, and then kept at this temperature for 15 hours. The final product, Na4MnV 0.8 La 0.2 (PO4)3.
[0081] Fig.11 The Na4MnV obtained in this example 0.8 La 0.2 The XRD pattern of (PO4)3 shows that the diffraction peaks of the material are narrow and sharp, indicating that the material has good crystallinity. The positions and relative intensities of the diffraction peaks are compared with the Na4MnV(PO4)3 standard card, and it is found that the XRD pattern shifts to a low angle after doping. The original NASICON structure of the material has not changed, but the unit cell volume has increased. 2+ and La 3+ The incorporation of further improves the structural stability of the material.
[0082] Example 5
[0083] A sodium ion battery positive electrode material, comprising Na4MnV 0.9 Ce 0.1 (PO4)3, the preparation method comprises the following steps:
[0084] (1) Mixing: 1.3135 g CH3COONa, 0.4261 g NH4VO3, 1.5847 g (NH4)2HPO4, 0.991 g (CH3COO)2Mn·4H2O, 0.1753 g Ce(NO3)3·6H2O and 2.5273 g C6H8O7 were mixed in 30 mL of deionized water to prepare a precursor solution;
[0085] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 80°C and dried for 3.5 hours to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 150°C and dried for 3.5 hours to obtain a light grayish yellow fluffy porous solid, i.e., the precursor.
[0086] (3) Grinding: Grind the precursor for 20 min to prepare a precursor powder with uniform particle size;
[0087] (4) Sintering: The precursor powder was placed in a muffle furnace, and under nitrogen protection, the temperature was raised to 450°C at a heating rate of 3°C / min, and then kept at this temperature for 4 hours for pre-sintering. The temperature was then raised to 650°C at a heating rate of 3°C / min, and then kept at this temperature for 12 hours. The final product, Na4MnV 0.9 Ce 0.1 (PO4)3.
[0088] Example 6
[0089] A sodium ion battery positive electrode material, comprising Na 3.8 MnV 0.9 Nb 0.1 (PO4)3, the preparation method comprises the following steps:
[0090] (1) Mixing: 1.2268 g CH3COONa, 1.2925 g C 15 H 21 O6V, 0.4647 g NH4H2PO4, 1.1513 g MnH4P2O8·2H2O, 0.0659 g NaNbO3 and 1.6091 g C4H6O5 were mixed together in 30 mL of deionized water to prepare a precursor solution;
[0091] (2) Drying: The precursor solution is placed in a constant temperature water bath, heated to 90°C and dried for 3 h to form a blue gel-like semi-solid. The gel-like semi-solid is then placed in a drying oven, heated to 120°C and dried for 4 h to obtain a light grayish yellow fluffy porous solid, i.e., the precursor.
[0092] (3) Grinding: Grind the precursor for 30 minutes to prepare a precursor powder with uniform particle size;
[0093] (4) Sintering: The precursor powder was placed in a muffle furnace, and under helium protection, the temperature was raised to 400°C at a heating rate of 6°C / min, and then kept at this temperature for 3.5 hours for pre-sintering. The temperature was then raised to 800°C at a heating rate of 3°C / min, and then kept at this temperature for 8 hours. The final product Na 3.8 MnV 0.9 Nb 0.1 (PO4)3.
[0094] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.
Claims
1. A multi-element doped sodium ion battery positive electrode material, characterized in that: The composition of the positive electrode material is Na z Mn w V y (PO4) 3-x (SiO4) x ; Among them, 0.2≤x≤0.5, 0.5≤y≤2, 0.01≤w≤1, 3≤z≤4, and the algebraic sum of the valences of each element is zero; The method for preparing the positive electrode material comprises the following steps: (1) Mixing: weigh a sodium source, a vanadium source, a phosphorus source, a manganese source, a silicon source, and a complexing agent according to a molar ratio of sodium, vanadium, phosphorus, manganese, and silicon of z:y:(3-x):w:x, and mix them together in water to prepare a precursor solution; The mass fraction of the solute in the precursor solution is 10-25%, wherein the complexing agent is one or more of oxalic acid, ascorbic acid, citric acid monohydrate, and malic acid, and the molar amount of the complexing agent is 1-2 times the sum of the molar amounts of vanadium and manganese; (2) Drying: Drying the precursor solution in one stage until it forms a gel, and then drying the gel product in a second stage to obtain a precursor; (3) Grinding: Grinding the precursor to make precursor powder; (4) Sintering: The precursor powder is pre-sintered in an inert protective atmosphere and then sintered to obtain the final product, the sodium ion battery positive electrode material.
2. A method for preparing a multi-element doped sodium ion battery positive electrode material as claimed in claim 1, characterized in that: The steps include: (1) Mixing: weigh a sodium source, a vanadium source, a phosphorus source, a manganese source, a silicon source, and a complexing agent according to a molar ratio of sodium, vanadium, phosphorus, manganese, and silicon of z:y:(3-x):w:x, and mix them together in water to prepare a precursor solution; The mass fraction of the solute in the precursor solution is 10-25%, wherein the complexing agent is one or more of oxalic acid, ascorbic acid, citric acid monohydrate, and malic acid, and the molar amount of the complexing agent is 1-2 times the sum of the molar amounts of vanadium and manganese; (2) Drying: Drying the precursor solution in one stage until it forms a gel, and then drying the gel product in a second stage to obtain a precursor; (3) Grinding: Grinding the precursor to make precursor powder; (4) Sintering: The precursor powder is pre-sintered in an inert protective atmosphere and then sintered to obtain the final product, the sodium ion battery positive electrode material.
3. The method for preparing a multi-element doped sodium ion battery positive electrode material according to claim 2, characterized in that: The sodium source is one or more of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, sodium carbonate, and sodium bicarbonate; the vanadium source is one or more of ammonium metavanadate, sodium metavanadate, and vanadium acetylacetonate; the phosphorus source is one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, and sodium phosphate; the manganese source is one or more of manganese acetate, manganese nitrate, manganese oxalate dihydrate, manganese carbonate, and manganese dihydrogen phosphate; the silicon source is one or more of silicon acetate and tetraethyl orthosilicate.
4. The method for preparing a multi-element doped sodium ion battery positive electrode material according to claim 2, characterized in that: Both the first stage drying and the second stage drying are performed at normal pressure; the drying temperature of the first stage drying is 75-95°C, and the drying time is 3-4h; the drying temperature of the second stage drying is 120-180°C, and the drying time is 3-4h.
5. The method for preparing a multi-element doped sodium ion battery positive electrode material according to claim 2, characterized in that: The heating rate of pre-sintering is 3-10℃ / min. After heating to 350-450℃, keep warm for 3-4h. The heating rate of sintering is 3-10℃ / min. After heating to 500-850℃, keep warm for 5-15h.
6. The method for preparing a multi-element doped sodium ion battery positive electrode material according to claim 2, characterized in that: The inert protective atmosphere is one or more of argon, nitrogen and helium.
7. Use of the multi-element doped sodium ion battery positive electrode material as claimed in claim 1 in a sodium ion battery.
Citation Information
Patent Citations
Positive electrode material for transition metal-doped sodium ion battery and preparation and application thereof
CN109755565A
Carbon-coated vanadium titanium manganese sodium phosphate microspheres as well as preparation method and application thereof
CN113764662A
Manganese-rich phosphate positive electrode material and preparation method and application thereof
CN113929069A