Electrolytic copper foil

By increasing the ratio of vertically long columnar crystals in the electrolytic copper foil, the problem of high tensile strength and poor flexibility of the electrolytic copper foil after annealing is solved, achieving both high flexibility and smoothness, and is suitable for the needs of flexible substrates.

CN114901873BActive Publication Date: 2024-10-15MITSUI MINING & SMELTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180007696.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-30
Filing Date
2021-01-14
Publication Date
2024-10-15
Estimated Expiration
2041-01-14

AI Technical Summary

Technical Problem

The existing electrolytic copper foil has high tensile strength and poor flexibility after annealing, making it difficult to balance smoothness and softness. It is especially difficult to control under the high flexibility requirements after annealing at 180°C.

Method used

By increasing the proportion of elongated columnar crystals that extend elongatedly along the foil thickness direction based on electron backscatter diffraction (EBSD) cross-sectional analysis, ensuring that the microscopic unevenness and softness of the copper grains meet specific conditions, thereby manufacturing Electrolytic copper foil with high flexibility and smoothness.

Benefits of technology

It is realized that the electrolytic copper foil annealed at 180°C has significantly low tensile strength and high flexibility, taking into account smoothness and softness, and is suitable for the needs of flexible substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114901873B_ABST
    Figure CN114901873B_ABST
Patent Text Reader

Abstract

Provided is an electrolytic copper foil having high smoothness and high flexibility suitable for flexible substrates (especially high flexibility after annealing at 180°C for 1 hour). The electrolytic copper foil has a microscopic roughness ten-point height Rz of 0.1 μm or more and 2.0 μm or less on at least one surface, and when the electrolytic copper foil is cross-sectionally analyzed by electron backscatter diffraction (EBSD), the ratio of the area occupied by copper crystal grains that satisfy all of the following conditions in the area of ​​the observation field occupied by the copper crystal grains is 63% or more: i) oriented along (101); ii) the aspect ratio is 0.500 or less; iii) when the angle between the normal line of the electrode surface of the electrolytic copper foil and the major axis of the copper crystal grain is θ (°), |sinθ| is 0.001 or more and 0.707 or less; and iv) the minor axis length when the crystal is approximated by an ellipse is 0.38 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolytic copper foil, in particular to an electrolytic copper foil for a flexible substrate. Background Art

[0002] As electrolytic copper foil for printed circuit boards, copper foil that contains as little chlorine as possible (hereinafter referred to as chlorine-free copper foil) is known. For example, Patent Document 1 (Japanese Patent Publication No. 2006-52441) discloses a copper foil in which the Cl content in an untreated copper foil is less than 30 ppm. In addition, Patent Document 2 (Japanese Patent Publication No. 7-268678) discloses an electrolytic copper foil, wherein each peak value of the X-ray diffraction intensity of the (111) plane and the (220) plane of the copper foil measured from the electrolysis-finished surface side satisfies the prescribed conditions, and discloses that the electrolytic copper foil is manufactured using a copper electrolyte solution in which the lead ion concentration is controlled to be less than 3 ppm, the tin ion concentration is controlled to be less than 6 ppm, the chlorine ion concentration is controlled to be less than 2 ppm, the silicon ion concentration is controlled to be less than 15 ppm, the calcium ion concentration is controlled to be less than 30 ppm, and the arsenic ion concentration is controlled to be less than 7 ppm.

[0003] It is also known that a technique has been attempted to improve the properties of existing chlorine-free copper foil by adding a trace amount of chloride ions to the copper plating solution during foil making. For example, Patent Document 3 (Japanese Patent Publication No. 2018-178261) discloses an electrolytic copper foil having (a) a brightness L* value of 75 to 90 on the side not subjected to roughening treatment based on the L*a*b colorimetric system, and (b) a tensile strength of 40 kgf / mm 2 Above and 55kgf / mm 2 Hereinafter, it is preferred that the percentage of low angle grain boundaries (LAGB) measured by electron backscatter diffraction (EBSD) is less than 7.0%. The document states that in the initial copper plating process, a plating solution having a chloride ion concentration of 10 ppm, 15 ppm or 20 ppm and a 60 A / dm 2 、70A / dm 2 or 80A / dm 2 The current density is used to manufacture electrolytic copper foil.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2006-52441

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 7-268678

[0008] Patent Document 3: Japanese Patent Application Publication No. 2018-178261 Summary of the invention

[0009] Unlike copper foil for rigid substrates, copper foil for flexible substrates is required to have flexibility that allows it to be bent freely by external force. Although there are chlorine-free copper foils with a certain degree of smoothness and flexibility, further improvement in smoothness and flexibility is required. Copper foil generally has the property that the tensile strength is reduced and the flexibility is increased by annealing, but compared with rolled copper foil, electrolytic copper foil has a tendency to have a higher tensile strength after annealing (for example, at 180°C for 1 hour), that is, poor flexibility. Therefore, an electrolytic copper foil with significantly lower tensile strength (that is, high flexibility) after annealing is desired. However, it is difficult to control the tensile strength of the electrolytic copper foil with a low roughness surface with a microscopic roughness ten-point height Rz of more than 0.1μm and less than 2.0μm after annealing, and it is currently difficult to balance smoothness and flexibility.

[0010] The present inventors have obtained the following insight: by increasing the ratio of longitudinal columnar crystals (hereinafter referred to as longitudinal crystals) that are specified by cross-sectional analysis based on electron backscatter diffraction (EBSD) and that extend elongatedly in the foil thickness direction, it is possible to provide an electrolytic copper foil having a high degree of smoothness with a microscopic roughness ten-point height Rz of not less than 0.1 μm and not more than 2.0 μm, and exhibiting high flexibility suitable for flexible substrates (especially high flexibility after annealing at 180°C for 1 hour).

[0011] Therefore, an object of the present invention is to provide an electrolytic copper foil having high smoothness and exhibiting high flexibility suitable for a flexible substrate (particularly high flexibility after annealing at 180° C. for 1 hour).

[0012] According to one aspect of the present invention, there is provided an electrolytic copper foil having at least one surface having a microscopic roughness ten-point height Rz of 0.1 μm or more and 2.0 μm or less,

[0013] When the electrolytic copper foil is subjected to cross-sectional analysis by electron backscatter diffraction (EBSD), the ratio of the area occupied by copper crystal grains satisfying all of the following conditions in the area of ​​the observation field occupied by copper crystal grains is 63% or more:

[0014] i) along the (101) orientation;

[0015] ii) The aspect ratio is less than 0.500;

[0016] iii) when the angle between the normal line of the electrode surface of the electrolytic copper foil and the major axis of the copper crystal grain is θ (°), |sinθ| is greater than or equal to 0.001 and less than or equal to 0.707; and

[0017] iv) The minor axis length of the crystal when an ellipse approximation is performed is 0.38 μm or less.

[0018] According to another aspect of the present invention, there is provided a flexible substrate including the above-mentioned electrolytic copper foil. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a graph showing the relationship between the longitudinal crystal ratio and the post-heat tensile strength of the electrolytic copper foils obtained in Examples 1 to 11.

[0020] Figure 2 The cross-sectional EBSD images (IQ+IPF images (ND direction) of the electrolytic copper foils obtained in Examples 1 to 11. DETAILED DESCRIPTION

[0021] definition

[0022] In this specification, the "electrode surface" of the electrolytic copper foil refers to the surface on the side in contact with the cathode when the electrolytic copper foil is manufactured. In addition, in this specification, the "precipitation surface" of the electrolytic copper foil refers to the surface on the side where the electrolytic copper is gradually precipitated when the electrolytic copper foil is manufactured, that is, the surface on the side not in contact with the cathode.

[0023] Electrolytic copper foil

[0024] The copper foil of the present invention is an electrolytic copper foil. The ten-point height Rz of the microscopic roughness of at least one surface of the electrolytic copper foil is greater than 0.1 μm and less than 2.0 μm. Moreover, when the electrolytic copper foil is cross-sectionally analyzed by electron backscatter diffraction (EBSD), the ratio of the area occupied by copper grains that meet all the following conditions in the area of ​​the observation field occupied by the copper grains is greater than 63%: i) along the (101) orientation, ii) the aspect ratio is less than 0.500, iii) when the angle between the normal line of the electrode surface of the electrolytic copper foil and the long axis of the copper grain is set to θ (°), |sinθ| is greater than 0.001 and less than 0.707; and iv) the short axis length when the crystal is approximated by an ellipse is less than 0.38 μm. In this way, by increasing the ratio of longitudinal columnar crystals (hereinafter referred to as longitudinal crystals) that are specific and extend slenderly in the foil thickness direction and are analyzed based on EBSD, it is possible to provide an electrolytic copper foil having a high degree of smoothness with a microscopic roughness ten-point height Rz of not less than 0.1 μm and not more than 2.0 μm and exhibiting high flexibility suitable for flexible substrates (especially high flexibility after annealing at 180°C for 1 hour).

[0025] As mentioned above, copper foil generally has the property that the tensile strength is reduced and the flexibility is increased by annealing, but the electrolytic copper foil tends to have a higher tensile strength after annealing (for example, at 180°C for 1 hour) than the rolled copper foil. Therefore, it is desirable to have an electrolytic copper foil with a significantly lower tensile strength (i.e., high flexibility) after annealing. However, it is difficult to control the tensile strength of the electrolytic copper foil with a low roughness surface having a microscopic roughness ten-point height Rz of more than 0.1μm and less than 2.0μm after annealing, and it is currently difficult to balance smoothness and flexibility. In this regard, according to the electrolytic copper foil of the present invention, it is possible to achieve a good balance between smoothness and flexibility.

[0026] The ten-point height Rz of the microscopic roughness of at least one surface of the electrolytic copper foil is preferably 0.1 μm or more and 2.0 μm or less, more preferably 0.3 μm or more and 2.0 μm or less, further preferably 0.3 μm or more and 1.8 μm or less, particularly preferably 0.6 μm or more and 1.5 μm or less, and most preferably 0.6 μm or more and 1.2 μm or less. In this way, the electrolytic copper foil with a low roughness surface has the advantage of having few fracture starting points. It should be noted that the "ten-point height Rz of microscopic roughness" in this specification is measured in accordance with JIS-B0601:1982, which is equivalent to Rzjis in JIS-B0601:2001.

[0027] It is also preferred that both sides of the electrolytic copper foil have a microscopic roughness ten-point height Rz within the above range. That is, the microscopic roughness ten-point height Rz of both sides of the electrolytic copper foil is preferably 0.1 μm or more and 2.0 μm or less, more preferably 0.3 μm or more and 2.0 μm or less, further preferably 0.3 μm or more and 1.8 μm or less, particularly preferably 0.6 μm or more and 1.5 μm or less, and most preferably 0.6 μm or more and 1.2 μm or less. In this way, the electrolytic copper foil with low roughness surfaces on both sides has the advantage of having fewer fracture starting points.

[0028] The tensile strength of the electrolytic copper foil under normal conditions without annealing is preferably 56 kgf / mm 2 Above and below 65kgf / mm 2 , more preferably 57kgf / mm 2 Above and 64kgf / mm 2 Below, more preferably 59kgf / mm 2 Above and 64kgf / mm 2 Below, most preferably 60kgf / mm 2 Above and 64kgf / mm 2 In addition, the tensile strength of the electrolytic copper foil after annealing at 180°C for 1 hour is preferably 15 kgf / mm 2 Above and below 25kgf / mm 2 , more preferably 15kgf / mm2 Above and 24.5kgf / mm 2 Below, more preferably 16kgf / mm 2 Above and 24.5kgf / mm 2 Below, particularly preferably 16kgf / mm 2 Above and 24kgf / mm 2 If it is within the above range, when the electrolytic copper foil is subjected to a heat history based on annealing (for example, at 180°C for 1 hour), high flexibility suitable for flexible substrates can be exerted. The tensile strength of the normal state without annealing and the tensile strength after annealing are both measured at room temperature (for example, 25°C) in accordance with IPC-TM-650.

[0029] When evaluating the cross section of the electrolytic copper foil of the present invention, the ratio of the longitudinal columnar crystals (hereinafter referred to as longitudinal crystals) extending slenderly in the foil thickness direction is high. The microstructure rich in the longitudinal crystals is beneficial to both the smoothness of the microscopic roughness ten-point height Rz of 0.1 μm or more and 2.0 μm or less and the high flexibility suitable for flexible substrates (especially the high flexibility after annealing at 180°C for 1 hour). Moreover, when analyzing the cross section of the electrolytic copper foil by electron backscatter diffraction (EBSD), the longitudinal crystals can specifically meet the following conditions:

[0030] i) along the (101) orientation;

[0031] ii) The aspect ratio is less than 0.500;

[0032] iii) when the angle between the normal line of the electrode surface of the electrolytic copper foil and the major axis of the copper crystal grain is θ (°), |sinθ| is greater than or equal to 0.001 and less than or equal to 0.707; and

[0033] iv) The minor axis length of the crystal when an ellipse approximation is performed is 0.38 μm or less.

[0034] Specifically, when the electrolytic copper foil of the present invention is cross-sectionally analyzed by EBSD, the ratio of the area occupied by the copper grains that meet all the conditions of i) to iv) in the area of ​​the observation field (e.g., width 10μm×height 28μm) occupied by the copper grains (i.e., the longitudinal crystal ratio) is 63% or more, more preferably 63% or more and 90% or less, further preferably 63% or more and 85% or less, particularly preferably 63% or more and 80% or less, and most preferably 63% or more and 75% or less. If it is within this range, the smoothness of the microscopic roughness ten-point height Rz of 0.1μm or more and 2.0μm or less and the high flexibility suitable for flexible substrates (especially the high flexibility after annealing at 180°C for 1 hour) can be achieved. At this time, as the observation field in EBSD, a rectangular area of ​​width×height that satisfies the conditions shown in Table 1 is specified.

[0035] [Table 1]

[0036] Table 1

[0037]

[0038] It should be noted that when the width in the EBSD observation field of view is specific, the reason for using a position deviated by 3 μm in the thickness direction from the electrode surface of the copper foil as the reference position P0 (i.e., excluding the area from the electrode surface of the copper foil to 3 μm in the thickness direction from the field of view) is to exclude the surface area on the side where the copper grains are relatively or excessively fine due to the influence of the cathode (especially its structure) used in the manufacture of the electrolytic copper foil, thereby ensuring an EBSD observation field of view that more representatively reflects the main part of the thickness direction of the copper foil.

[0039] EBSD analysis can be performed as follows: the electrolytic copper foil is subjected to cross-section polishing (CP) processing to form a ground cross section, and an EBSD device (SUPRA55VP, manufactured by Carl Zeiss AG) is used to perform EBSD analysis of the ground cross section on the observation field of width × height shown in Table 1 under SEM conditions of Vacc. = 20 kV, Apt. = 60 μm, HC mode, Tilt = 70° and Scan Phase = Cu.

[0040] The determination of the longitudinal crystal ratio based on the EBSD image can be performed through the following steps.

[0041] One extraction based on condition i):

[0042] The EBSD image of the observation field was analyzed using EBSD analysis software (OIM Analysis 7, manufactured by TSL Solutions Co., Ltd.) to extract crystals oriented along (h, k, l) = (1, 0, 1) (for detailed setting conditions, refer to the examples described later). In this way, the crystal grain region satisfying the condition i) above was extracted.

[0043] Secondary extraction based on conditions ii), iii) and iv):

[0044] From the data obtained from the first extraction, it can be seen that all crystals that satisfy the aspect ratio of 0.500 or less, the major axis slope |sinθ| of 0.001 or more and 0.707 or less, and the minor axis length of 0.38 μm or less when the grain is approximated by an ellipse (refer to the embodiment described later for detailed setting conditions) are further extracted to obtain the value (μm) of the sum of these areas. 2 ) is taken as the area of ​​the longitudinal grain. In this way, the grain region satisfying the above conditions ii), iii) and iv) is extracted.

[0045] Calculation of the longitudinal crystal ratio:

[0046] The area S of the longitudinal grain obtained by secondary extraction VC (μm 2 ) and the area of ​​the observation field S OA (μm 2 ), according to 100×S VC / S OA The ratio of the area occupied by the longitudinal grains to the area occupied by the copper grains was calculated by the formula as the longitudinal crystal ratio (%) (for setting conditions, refer to the examples described later).

[0047] The thickness of the electrolytic copper foil is not particularly limited, but is preferably 5 μm to 35 μm, more preferably 7 μm to 35 μm, further preferably 9 μm to 18 μm, and particularly preferably 12 μm to 18 μm.

[0048] Preferably, the electrolytic copper foil is subjected to surface treatment on one side or both sides. The surface treatment may be a surface treatment commonly performed on the electrolytic copper foil. As preferred examples of surface treatment, roughening treatment, rust prevention treatment (e.g., galvanizing treatment, zinc-nickel alloy treatment and other galvanizing alloy treatments), silane coupling agent treatment and the like may be cited. In addition, the electrolytic copper foil may be provided in the form of a copper foil with a carrier.

[0049] Manufacturing method

[0050] The electrolytic copper foil of the present invention can be manufactured in the following manner: using a copper electrolyte (aqueous solution) having a copper (Cu) concentration, a sulfuric acid (H2S04) concentration, and a chlorine (Cl) concentration shown in Table 2, maintaining the bath temperature (temperature of the aqueous solution) shown in Table 2, and performing electrolytic precipitation at the current density shown in Table 2, thereby manufacturing the electrolytic copper foil of the present invention. That is, by satisfying the conditions of the copper electrolyte composition, bath temperature, and current density, a cross-sectional structure having a longitudinal crystal ratio of 63% or more can be achieved, and as a result, an electrolytic copper foil having a microscopic roughness ten-point height Rz of 0.1 μm or more and 2.0 μm or less on the precipitation surface (or both the precipitation surface and the electrode surface) and exhibiting high flexibility suitable for flexible substrates (especially high flexibility after annealing at 180°C for 1 hour) can be manufactured. As shown in Table 2, the copper electrolyte used in the manufacturing method is preferably a chlorine-free electrolyte that contains as little chlorine as possible.

[0051] [Table 2]

[0052] Table 2

[0053]

[0054] Example

[0055] The present invention will be described in more detail based on the following examples.

[0056] Examples 1 to 11

[0057] (1) Manufacturing of electrolytic copper foil

[0058] A sulfuric acid copper sulfate solution (without chlorine added) with the composition shown in Table 4 was used as the copper electrolyte, a titanium plate electrode (surface roughness Ra = 0.19 μm, in accordance with JIS-B0601: 1982) was used as the cathode, and a DSA (dimensional stability anode) was used as the anode. Electrolysis was carried out at the bath temperature and current density shown in Table 4 to obtain an electrolytic copper foil with a thickness of 18 μm.

[0059] (2) Evaluation of Electrolytic Copper Foil

[0060] The obtained electrolytic copper foil was subjected to measurement of microscopic roughness ten-point height Rz, cross-sectional analysis by EBSD, and measurement of tensile strength as follows.

[0061] <Measurement of Ten-Point Height Rz of Microscopic Roughness>

[0062] The microscopic roughness ten-point height Rz (equivalent to Rzjis in JIS-B0601:2001) of the deposited surface of the electrolytic copper foil was measured using a surface roughness measuring machine (Surfcorder SE-30H, manufactured by Kosaka Laboratory Co., Ltd.) in accordance with JIS-B0601:1982 under the conditions of λc: 0.8 μm, reference length: 0.8 mm, and conveying speed: 0.1 mm / s. The results are shown in Table 4.

[0063] <Longitudinal crystal ratio / EBSD cross-section analysis>

[0064] Four electrolytic copper foil samples were overlapped and bonded with an adhesive (LOCTITE (registered trademark), manufactured by Henkel Japan Ltd.), and then an ultraviolet curing resin was applied to the sample surface as a protective layer. After the entire sample was coated with carbon, a wide argon ion beam cross-section processing (cross-section polisher (CP) (registered trademark), manufactured by JEOL Ltd.) (acceleration voltage: 5 kV) was performed for 3 hours to obtain a polished cross section for EBSD measurement. During EBSD observation, carbon coating (1 flash) was performed. An EBSD device (a device equipped with an EBSD measuring device (Pegasus, AMETEK, Inc.) on a FE-SEM device (SUPRA55VP, manufactured by Carl Zeiss AG)) was used to perform EBSD analysis of the polished cross section under the SEM conditions of Vacc. = 20 kV, Apt. = 60 μm, HC mode, Tilt = 70° and Scan Phase = Cu. The observation field in EBSD is set to (according to the conditions shown in Table 1 above) 10 μm in width × 28 μm in height. In the EBSD image of the observation field, the area occupied by the copper grains that meet all the following conditions (hereinafter referred to as the area of ​​the longitudinal grains) is determined through the following primary extraction and secondary extraction:

[0065] i) along the (101) orientation;

[0066] ii) The aspect ratio is less than 0.500;

[0067] iii) when the angle between the normal line of the electrode surface of the electrolytic copper foil and the major axis of the copper crystal grain is θ (°), |sinθ| is greater than or equal to 0.001 and less than or equal to 0.707; and

[0068] iv) The minor axis length of the crystal when an ellipse approximation is performed is 0.38 μm or less.

[0069] One extraction based on condition i)

[0070] The EBSD image of the observation field was analyzed using EBSD analysis software (OIM Analysis 7, manufactured by TSL Solutions Co., Ltd.), and crystals oriented along (hkl) = (101) were extracted. Specifically, in the screen of OIM Analysis 7, [(h, k, l) = (1, 0, 1)] was selected in [Property] of [All Data] under [Crystal Orientation], and the value of [Deviation] was set to less than 60, and (h, k, l) = (1, 0, 1) was selected in [Orientation Deviation], and the value of [Deviation] was set to less than 12, and [Gain Data], that is, particle data, was extracted. At this time, the setting conditions of OIM Analysis 7 were set as follows.

[0071] PCO[Copper,0.000,45.000,90.000]<60

[0072] AND PCD[Copper,1,0,1,0,0,1]<12

[0073] Secondary extraction based on conditions ii), iii) and iv)

[0074] From the data extracted as described above, all crystals satisfying the aspect ratio of 0.500 or less, the major axis slope |sinθ| of 0.001 or more and 0.707 or less, and the minor axis length of 0.38 μm or less when the crystal grains are approximated by an ellipse are further extracted, and the value obtained by adding these areas (μm 2 That is, the setting conditions of OIM Analysis 7 are set as shown in Table 3.

[0075] [Table 3]

[0076] Table 3

[0077]

[0078] ※θ<=45 and θ>=135

[0079] Calculation of the longitudinal crystal ratio:

[0080] The area S of the longitudinal grains obtained after the first extraction and the second extraction is used. VC (μm 2 ) and the area of ​​the observation field S OA (μm 2 ), according to 100×S VC / S OA The ratio of the area occupied by the longitudinal grains to the area occupied by the copper grains was calculated as the longitudinal crystal ratio (%). The results are shown in Table 4.

[0081] <Determination of normal tensile strength>

[0082] The electrolytic copper foil sample without annealing was cut into a size of 10 mm × 100 mm to obtain a test piece. The test piece was installed in a measuring device (AGI-1KNM1, manufactured by Shimadzu Corporation) and the tensile strength (tensile strength) of the normal state was measured at room temperature (about 25°C) according to IPC-TM-650 under the conditions of tensile speed: 50 mm / min and full-scale test force: 50N. The results are shown in Table 4.

[0083] <Determination of tensile strength after heating>

[0084] The electrolytic copper foil sample annealed at 180°C for 1 hour was cut into a size of 10 mm x 100 mm to obtain a test piece. The test piece was used to measure the tensile strength under the same conditions as the normal tensile strength measurement described above, and the post-heat tensile strength was measured. The results are shown in Table 4.

[0085] [Table 4]

[0086] Table 4

[0087]

[0088] * Shows a comparative example.

Claims

1. An electrolytic copper foil, wherein at least one surface of the electrolytic copper foil has a microscopic roughness ten-point height Rz of 0.1 μm or more and 2.0 μm or less, When the electrolytic copper foil is subjected to cross-sectional analysis by electron backscatter diffraction (EBSD), the ratio of the area occupied by copper crystal grains satisfying all of the following conditions in the area of ​​the observation field occupied by copper crystal grains is 63% or more: i) along the (101) orientation; ii) The aspect ratio is less than 0.500; iii) when the angle between the normal line of the electrode surface of the electrolytic copper foil and the major axis of the copper crystal grain is θ (°), |sinθ| is greater than or equal to 0.001 and less than or equal to 0.707; and iv) the minor axis length of the crystal when the ellipse is approximated is less than 0.38 μm, The observation field of view refers to a rectangular area of ​​width × height that meets the following conditions: The width is the distance E1-E0 in the copper foil thickness direction from the visual field end E0 to the visual field end E1 on the opposite side of the precipitation surface closest to the copper foil, when the maximum range of the visual field filled with copper crystals is narrowed to one visual field from the visual field end E0, which is 3 μm away from the electrode surface of the copper foil in the thickness direction. The height is 28 μm in the copper foil surface direction.

2. The electrolytic copper foil according to claim 1, wherein The microscopic roughness ten-point height Rz of both surfaces of the electrolytic copper foil is 0.1 μm or more and 2.0 μm or less.

3. The electrolytic copper foil according to claim 1 or 2, wherein: After annealing at 180°C for 1 hour, the tensile strength measured according to IPC-TM-650 is 15 kgf / mm 2 Above and below 25kgf / mm 2 .

4. The electrolytic copper foil according to claim 1 or 2, wherein: Under normal conditions without annealing, the tensile strength measured according to IPC-TM-650 is 56kgf / mm 2 Above and below 65kgf / mm 2 . 5 . A flexible substrate comprising the electrolytic copper foil according to claim 1 .