Stacked III-V semiconductor diodes

By designing the structure of high n-type and high p-type doping layers and low-doping drift regions in III-V semiconductor diodes, combined with GaAs materials and epitaxial growth technology, the problems of diode turn-off voltage and capacitance in the existing technology are solved , realizing high-performance GaAs power diodes.

CN114914290BActive Publication Date: 2024-10-293 5 POWER ELECTRONICS GMBH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202210116254.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-07
Publication Date
2024-10-29
Estimated Expiration
2042-02-07

AI Technical Summary

Technical Problem

Existing III-V semiconductor diodes have problems with turn-off voltage and capacitance under high voltage, and have large reverse recovery charges, which affects their performance.

Method used

A stacked III-V semiconductor diode is designed, which includes a highly n-type doped cathode layer, a highly p-type doped anode layer and a low-doped drift region. The drift region is composed of low n-type doping and The drift layer composition of low p-type doping, dopant concentration gradient design to achieve high blocking voltage and low capacitance, combined with GaAs material and epitaxial growth technology, optimizes the structure and doping distribution of the diode.

Benefits of technology

It achieves a blocking voltage higher than 1100V and a small on-resistance, reduces the reverse recovery charge, improves the diode's withstand voltage strength and switching speed, and creates a high-performance GaAs power diode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114914290B_ABST
    Figure CN114914290B_ABST
Patent Text Reader

Abstract

A stacked III-V semiconductor diode comprising GaAs or consisting of GaAs comprises a highly n-type doped cathode layer, a highly p-type doped anode layer and a drift region arranged between the cathode layer and the anode layer, wherein the drift region comprises a low n-type doped drift layer and a low p-type doped drift layer, the n-type doped drift layer is arranged between the p-type doped drift layer and the cathode layer, the two drift layers each having a layer thickness of at least 5 μm and having a maximum of 8·10 15 cm ‑3 The dopant concentration maximum values ​​of the two drift layers have a ratio of 0.1 to 10 to each other, and the ratio of the layer thickness of the n-doped drift layer to the layer thickness of the p-doped drift layer is between 0.5 and 3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a stacked III-V semiconductor diode, which comprises GaAs or is composed of GaAs. The stacked III-V semiconductor diode has a highly n-type doped cathode layer, a highly p-type doped anode layer and a drift region arranged between the cathode layer and the anode layer. Background Art

[0002] A high-voltage-resistant semiconductor diode p made of gallium arsenide is known from the German Ashkinazi "GaAs Power Devices", ISBN 965-7094-19-4, pages 8 and 9. + -nn + structure.

[0003] Other stacked III-V semiconductor diodes are known from EP 3 321 971 B1 and EP 3 321 970 B1, wherein the semiconductor diode has an additional intermediate layer between the drift region and the cathode or anode. Other semiconductor components are known from EP 3321 971 B1, DE 10 2016 111 844 A1, JP H06-314 801A and DE 10 2018 000 395 A1.

[0004] Against this background, the object of the present invention is to specify a device which expands the prior art. Summary of the invention

[0005] This object is achieved by a stacked III-V semiconductor diode according to the invention. Advantageous embodiments of the invention are described below.

[0006] In the subject matter of the present invention, a stacked III-V semiconductor diode is provided, which includes GaAs or consists of GaAs, and the III-V semiconductor diode has a highly n-type doped cathode layer, a highly p-type doped anode layer and a drift region arranged between the cathode layer and the anode layer.

[0007] The drift region has a low n-type doped drift layer and a low p-type doped drift layer, wherein the n-type doped drift layer is arranged between the p-type doped drift layer and the cathode layer.

[0008] The two drift layers each have a layer thickness of at least 5 μm and a maximum of 8·10 15 cm -3 The maximum dopant concentration.

[0009] The dopant concentration maximum values ​​of the two drift layers have a ratio of 0.1 to 10 to each other.

[0010] The ratio of the layer thickness of the n-doped drift layer to the layer thickness of the p-doped drift layer is between 0.5 and 3.

[0011] It can be understood that all semiconductor layers of the semiconductor diode composed of GaAs or including GaAs, ie, in particular, the cathode layer, the anode layer and the drift region, respectively consist of GaAs or at least include GaAs.

[0012] In other words, each semiconductor layer of the III-V semiconductor diode has at least the elements Ga and As.

[0013] The semiconductor layer is preferably produced by epitaxy. In one embodiment, the cathode layer or the anode layer can be formed from the substrate layer. Preferably, further III-V semiconductor layers are grown epitaxially on the substrate layer in order to form a III-V semiconductor diode.

[0014] Alternatively, the III-V semiconductor diode comprises at least one semiconductor bond. In this case, the surfaces of two GaAs semiconductor wafers or GaAs wafers are bonded together.

[0015] The doping of the corresponding GaAs semiconductor layer is preferably introduced during the epitaxy. The epitaxy is preferably carried out by means of MOVPE and / or LPE.

[0016] In one configuration, the doping is carried out by means of ion implantation in addition to after the epitaxial growth or alternatively instead of introduction during the epitaxial growth.

[0017] Furthermore, it is understood that the semiconductor diode preferably has further layers made of other materials, in particular metallic connection contact layers, which consist, for example, completely or partially of metal, for example gold, or of a metal alloy, and are produced, for example, by electron beam evaporation or by sputtering.

[0018] At least the region of the cathode layer and of the anode layer adjoining the connecting contact layer preferably has a high dopant concentration in order to form a contact that is as low-ohmic as possible and to keep the series resistance or the power loss of the semiconductor diode as low as possible.

[0019] The drift zone is characterized by a total width of at least 10 μm. Preferably, the total width is at least 20 μm or at least 40 μm or at least 60 μm. The total width is divided into weakly p-doped and weakly n-doped regions or layers.

[0020] The ratio of the layer thicknesses of the two drift layers is selected such that the thickness of the n-doped drift layer is at least half the thickness of the p-doped drift layer or such that the thickness of the n-doped drift layer is at most three times the thickness of the p-doped drift layer.

[0021] The respective dopant concentrations of the two drift layers are each as low as possible in a region adjacent to the other drift layer and may rise slightly in a direction pointing away from the other drift layer. In one embodiment, the rise is implemented by means of one or more steps.

[0022] Thus, a pn junction is constructed within the drift region and in a region with a very low dopant concentration.

[0023] Due to a wide drift zone composed of two differently low-doped layers, diodes with particularly high blocking voltages of more than 1100 V or even more than 1200 V can be realized and diodes with low on-resistance and particularly low capacitance per unit area can be produced.

[0024] In one embodiment, isoelectric or equivalent centers are embedded in the p-doped drift layer and / or the anode layer in order to increase the switching speed, that is to say the changeover between reverse and forward. The isoelectric or equivalent centers represent impurity complexes. They are energetically low and significantly reduce the service life of the charge carriers, ie they are scavenged by the charge carriers, in particular during reverse operation.

[0025] In one embodiment, the isoelectric center comprises N and / or Zn-0 and / or Mn and / or an element from the Group III main group and / or an element from the Group V main group.

[0026] In another extended scenario, the concentration of isoelectric centers is 5·10 11 cm -3 and 8.10 14 cm -3 In the range of 5-10 12 cm -3 and 1.10 14 cm -3 In the range of 1·10 13 cm -3 and 8.1013 cm -3 The concentration of the isoelectric center is preferably 1 / 1000 to 1 / 10, or 1 / 100 to 1 / 20 of the dopant concentration of the corresponding region of the drift layer or the anode layer.

[0027] In particular, GaAs power diodes with a reverse recovery charge of up to 80 nC per 1 mm diode area can be produced.

[0028] In one embodiment, the layer thickness of the n-doped drift layer is greater than the layer thickness of the p-doped drift layer. In another embodiment, the n-doped drift layer and / or the p-doped drift layer has a layer thickness of at least 20 μm or at least 40 μm. The particularly high layer thickness of the two drift layers can in particular achieve an improved voltage resistance of the diode.

[0029] In one configuration, the n-doped drift layer has a dopant concentration profile along the layer thickness which increases in the direction toward the cathode layer to a dopant concentration maximum.

[0030] The slow reduction of the dopant concentration of the n-doped drift layer in the direction of the p-doped drift layer makes it possible in particular to achieve very low dopant concentrations and to produce controlled and reproducible pn junctions.

[0031] In another alternative embodiment, the p-doped drift layer has a doping concentration profile along the layer thickness which increases in the direction toward the anode layer to a doping concentration maximum. As already explained, this increase can also be achieved by means of a step-like, ie, stair-like, The process of change is carried out.

[0032] In an alternative embodiment, the rising dopant concentration variation process is configured to be linear or concave or convex. The convex rise follows a Gaussian curve, for example, and the concave rise follows an exponential function, for example. It is understood that the concentration variation process is always below 8·10 15 cm -3 The maximum doping.

[0033] In another embodiment, the dopant concentration profile of the n-doped drift layer and / or the p-doped drift layer has one or more steps along the layer thickness. In an alternative embodiment, one step or more steps or each step has convex sides or concave sides or linear sides.

[0034] In another embodiment, the dopant concentration variation process of the two drift layers decreases to less than 3·10 in the direction toward the other drift layer. 15 cm-3 or less than 6.10 14 cm -3 or less than 3.10 14 cm -3 or less than 2.10 14 cm -3 The value of .

[0035] In one embodiment, the dopant concentration along at least 80% of the thickness of the n-doped drift layer and / or the p-doped drift layer is greater than 5·10 13 cm -3 .

[0036] In another embodiment, the cathode layer has at least 1·10 18 cm -3 Or at least 5.10 18 cm -3 Or at least 8.10 18 cm -3 of dopant concentration.

[0037] In another embodiment, the anode layer has at least 1·10 17 cm -3 Or at least 5.10 17 cm -3 Or at least 8.10 18 cm -3 Low doping enables improved diode turn-off behavior and reduced reverse recovery charge.

[0038] It is understood that, in particular in the region of the cathode and anode layers adjacent to the metallic connecting contacts, the highest possible dopant concentration should be achieved in order to keep the series resistance of the diode as low as possible or to produce the lowest possible ohmic contacts.

[0039] In another configuration, the cathode layer and / or the anode layer has a layer thickness of at least 2 μm or at least 5 μm or at least 20 μm. Small layer thicknesses make it easier to keep the series resistance of the diode small.

[0040] In another embodiment, the cathode layer and / or the anode layer comprises a first section having a constant dopant concentration variation and a second section arranged between the first section and the drift region, the second section having a dopant concentration variation that rises linearly and / or rises concavely and / or rises in a step-like manner in the direction toward the first section. Preferably, the step-like dopant concentration region comprises or consists of one step or two steps or three steps.

[0041] The second layer section enables in particular a transition in the structured dopant concentration ( ): from a low level in the region of the drift zone to a significantly higher level in a second section of the anode layer and / or cathode layer.

[0042] In one embodiment, during the course of the doping profile, the second layer section has at least one step or exactly one step or at least two steps or exactly two steps.

[0043] In a further embodiment, in the case of a single step, on the upper side of the step the dopant concentration is 2 times, 5 times or 8 times the dopant concentration of the drift layer adjoining the second region.

[0044] By using a gradual or stepwise rise in the transition region, abrupt transitions (i.e., avoiding 8.10 15 cm -3 The dopant concentration of the diode is increased to the dopant concentration of the first section), which significantly improves the turn-off behavior of the diode.

[0045] In a first embodiment, the second section has a layer thickness of at least 0.5 μm and at most 10 μm. Preferably, the second section of the cathode layer has a layer thickness of 3 μm to 5 μm, and the second section of the anode layer preferably has a layer thickness of 2 μm to 4 μm.

[0046] In another embodiment, the cathode layer or the anode layer is formed as a substrate. A typical layer thickness of the cathode layer or the anode layer formed as a substrate is 100 μm to 250 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The invention is explained in detail below with reference to the drawings. In this case, parts of the same type are marked with the same reference numerals. The embodiments shown are highly schematic, i.e. the spacings and the lateral and vertical extensions are not to scale and - unless otherwise indicated - do not have any derivable geometrical relationships with one another. It is shown therein:

[0048] Figure 1 A diagram showing a first embodiment of a stacked III-V semiconductor diode,

[0049] Figure 2 A view showing a second embodiment of a stacked III-V semiconductor diode,

[0050] Figure 3 A view showing a third embodiment of a stacked III-V semiconductor diode,

[0051] Figure 4FIG. 2 shows a dopant concentration variation along a stacked III-V semiconductor diode in another embodiment.

[0052] Figure 5 Another embodiment of a dopant concentration profile along a stacked II-V semiconductor diode is shown. DETAILED DESCRIPTION

[0053] Figure 1 The image shows a view of a first embodiment of a stacked III-V semiconductor diode 10, which has GaAs or consists of GaAs. The highly n-doped substrate layer forms a cathode layer 12, on which a total thickness D is arranged. D A drift region 14 is formed, after which a layer having a thickness D A A highly p-type doped anode layer 16 is provided.

[0054] The drift region 14 is divided into a layer having a layer thickness D adjacent to the cathode layer 12. n A weakly n-doped drift layer 14.1 and a layer thickness D arranged between the n-doped drift layer 14.1 and the anode layer 16 p A weakly p-doped drift layer 14.2.

[0055] Accordingly, the cathode layer 12 formed from the substrate has a slightly greater layer thickness D of 50 μm to 250 μm. K The dopant concentration of the cathode layer is preferably at least 8·10 18 cm -3 , and is constant or at least substantially constant along the layer thickness.

[0056] The further layers are preferably produced epitaxially on the cathode layer 12. The doping can be produced during or after the epitaxy by ion implantation. The layer thickness D of the n-doped drift layer 14.1 is 100 Å. n The dopant concentration increases from a maximum of 8·10 μm in the direction toward the p-doped drift layer 14 . 2 . 15 cm -3 The highest preferred is 2.10 15 cm -3 The maximum dopant concentration is reduced.

[0057] Layer thickness D of the p-doped drift layer 14 . 2 p The layer thickness D of the p-doped drift layer 14.2 is at least 5 μm, preferably at least 20 μm. p The layer thickness D of the drift layer 14 . 1 , which is preferably n-doped, is nThe dopant concentration of the p-doped drift layer 14.2 increases in the direction toward the anode layer 16 to at least 1·10 17 cm -3 Or at least 1.10 18 cm -3 The maximum dopant concentration.

[0058] exist Figure 2 Another embodiment is shown in the image of FIG. Figure 1 The difference between the images.

[0059] The stacked III-V semiconductor diode 10 has a cathode layer 12, which includes a 18 cm -3 , preferably at least 8.10 18 cm -3 The first section 12.1 of constant dopant concentration and comprises a second section 12.2. The second section 12.2 is arranged between the first section 12.1 and the drift zone 14 and has a relatively small layer thickness D of 0.5 μm to 10 μm, preferably 3 μm to 5 μm. K2 .

[0060] The second layer section is used to configure the transition of the dopant concentration from the highly doped first section 12.1 of the cathode layer to the low n-doped drift layer 14.1. For this purpose, the second section 12.2 has a rising dopant concentration variation from a dopant concentration minimum to a dopant concentration maximum in the direction of the first section 12.1. The dopant concentration variation is linearly or concavely or convexly constructed, or is stepped with one step or multiple steps. Preferably, the side surfaces of one step or multiple steps or all steps are convexly or concavely or linearly constructed.

[0061] In a first embodiment, the dopant concentration maximum of the second section 12.2 corresponds to the dopant concentration of the first section 12.1, and the dopant concentration minimum of the second section 12.2 corresponds to the dopant concentration maximum of the n-doped drift zone. In other embodiments, a dopant concentration jump is formed at the boundary surface between the first and second sections 12.1, 12.2 and / or between the second section 12.2 and the drift zone 14, wherein the dopant concentration jump is smaller due to the dopant concentration profile of the second section 12.2 compared to an embodiment of the semiconductor diode 10 without the second cathode section 12.2 (geringer ).

[0062] exist Figure 3 Another embodiment is shown in the image of FIG. Figure 2The difference between the images.

[0063] The stacked III-V semiconductor diode 10 comprises an anode layer 16, wherein the anode layer comprises a first section 16.1 and a second section 16.2, wherein the first section has a thickness of at least 1·10 17 cm -3 The second section has a constant dopant concentration of 1.5 μm, the second section having a dopant concentration profile that increases in the direction of the first section 16 . 1 and a layer thickness D of 0.5 μm to 10 μm, preferably 2 μm to 4 μm. A2 .

[0064] Like the second section 12.2 of the cathode layer 12, the second section 16.2 of the anode layer 16 is used to configure the transition of the dopant concentration. The dopant concentration variation of the second section 16.2 is linear, concave or convex, or stepped with one or more steps. In the step-shaped variation, the side surfaces of one or more steps or all steps are preferably convex, concave or linear.

[0065] In another embodiment (not shown here), the stacked III-V semiconductor diode 10 has the above-described anode layer 16 with two sections 16 . 1 and 16 . 2 and Figure 1 The drift layer 14 of the first exemplary embodiment (ie without the second section 12 . 2 ) is shown in FIG.

[0066] exist Figure 4 Another embodiment is shown in the image of FIG. Figure 1 The difference between the images.

[0067] exist Figure 4 , a stacked III-V semiconductor diode 10 having a structure corresponding to Figure 1 In an alternative embodiment, the dopant concentration profile of the n-doped drift layer 14 . 1 extends convexly, concavely, or linearly in the direction of the cathode layer 12 .

[0068] In alternative embodiments, the dopant concentration profile of the p-doped drift layer 14 . 2 runs constantly or rises in the direction of the anode layer 16 , wherein the rise is designed to be stepped, convex, linear or concave.

[0069] In a first embodiment, the convex rise of the n-doped and / or p-doped drift layer 14 . 1 or 14 . 2 is embodied in a Gaussian manner.

[0070] Alternatively, in one embodiment, the concave rise of the n-doped and / or p-doped drift layer 14 . 1 or 14 . 2 follows an exponential curve.

[0071] exist Figure 5 Another embodiment is shown in the image of FIG. Figure 3 The difference between the images.

[0072] exist Figure 5 , different dopant concentration variations along a stacked III-V semiconductor diode 10 are shown by way of example.

[0073] The dopant concentration profile begins with a constant, high dopant concentration of the n-type dopant in the first section 12.1 of the cathode layer 12, followed by a dopant concentration drop in the second section 12.2 of the cathode layer, wherein the drop is convex and begins at the dopant concentration level of the first section 12.2 or at a significantly lower level.

[0074] Subsequently, the dopant concentration in the n-doped drift layer 14 . 1 decreases further. The decrease is performed slowly, with or without steps.

[0075] A dopant change occurs between the n-doped drift layer 14 . 1 and the p-doped drift layer 14 . 2 , wherein the p-doped drift layer 14 . 2 has a constant, linearly increasing or stepped p-dopant concentration in the exemplary embodiment shown.

[0076] In the second section 16.2 of the anode layer 16 adjoining the drift zone, the dopant concentration of the p-type dopant increases in a step-like manner over a plurality of rectangularly shaped steps. The first section 16.1 of the adjoining anode layer 16 has at least 1·10 17 cm -3 A constant dopant concentration level.

[0077] Additionally, the anode layer 16 has a third section 16.3 following the first section 16.1, so that the first section 16.1 is arranged between the second section 16.2 and the third section 16.3. The third section 16.3 has a higher dopant concentration than the first section 16.1, preferably at least 5·10 18 cm -3 Or at least 1.10 19 cm -3 of a constant dopant concentration.

Claims

1. A stacked III-V semiconductor diode (10), comprising GaAs or consisting of GaAs, and having: - a highly n-doped cathode layer (12), - a highly p-doped anode layer (16), and - a drift region (14), which is arranged between the cathode layer (12) and the anode layer (16), - the drift region (14) comprises a drift layer (14.1) with low n-type doping and a drift layer (14.2) with low p-type doping, - the low n-type doped drift layer (14.1) is arranged between the low p-type doped drift layer (14.2) and the cathode layer (12), It is characterized in that The two drift layers (14.1, 14.2) each have a layer thickness (D n , D p ) and along the corresponding layer thickness (D n , D p ) has a maximum of 8.10 15 cm -3 The maximum dopant concentration is - the dopant concentration maxima of the two drift layers (14.1, 14.2) have a ratio of 0.1 to 10 to one another, and, - the layer thickness (D n ) and the layer thickness (D p ) is between 0.5 and 3. The anode layer (16) comprises a first section (12.1, 16.1) and a second section (12.2, 16.2), wherein the second section is arranged between the first section (12.1, 16.1) and the drift region (14), the first section having a constant dopant concentration variation process, and the second section having a dopant concentration variation process that rises in a step-like manner in a direction toward the first section (12.1, 16.1).

2. The stacked III-V semiconductor diode (10) according to claim 1, characterized in that: The layer thickness (D n ) is greater than the layer thickness (D p ).

3. The stacked III-V semiconductor diode (10) according to claim 1 or 2, characterized in that: The low n-doped drift layer (14.1) and / or the low p-doped drift layer (14.2) has a layer thickness (D n , D p ).

4. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that: The low n-doped drift layer (14.1) has a thickness (D n ) has a dopant concentration variation process that rises in the direction toward the cathode layer (12) to the maximum dopant concentration.

5. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that The low p-type doped drift layer (14.2) has a thickness (D p ) has a dopant concentration variation process that rises to a maximum dopant concentration in a direction toward the anode layer (16).

6. The stacked III-V semiconductor diode (10) according to claim 4 or 5, characterized in that: The rising dopant concentration profile is designed to be linear and / or concave and / or convex and / or the rising dopant concentration profile comprises a plurality of steps.

7. The stacked III-V semiconductor diode (10) according to claim 4 or 5, characterized in that: The dopant concentration of the low n-doped drift layer (14.1) and / or the low p-doped drift layer (14.2) varies along the layer thickness (D n , D p ) has one or more steps.

8. The stacked III-V semiconductor diode (10) according to claim 7, characterized in that: The step, or the steps, or each step may have convex sides, or concave sides, or linear sides.

9. The stacked III-V semiconductor diode (10) according to any one of claims 4 to 8, characterized in that: The dopant concentration variation process of the two drift layers (14.1, 14.2) decreases to less than 9·10 in the direction toward the other drift layer (14.1, 14.2). 14 cm -3 , or less than 6·10 14 cm -3 , or less than 3·10 14 cm -3 , or less than 2·10 14 cm -3 The value of .

10. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that The cathode layer (12) and / or the anode layer (16) has at least 1·10 17 cm -3 , or at least 5.10 18 cm -3 , or at least 8.10 18 cm -3 of dopant concentration.

11. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that The cathode layer (12) and / or the anode layer (16) has a layer thickness (D) of at least 2 μm or at least 5 μm or at least 20 μm. K , D A ).

12. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that The cathode layer (12) comprises a first section (12.1, 16.1) and a second section (12.2, 16.2), wherein the second section is arranged between the first section (12.1, 16.1) and the drift region (14), the first section having a constant dopant concentration variation process, and the second section having a dopant concentration variation process that rises linearly and / or rises concavely and / or rises in a step-like manner in a direction toward the first section (12.1, 16.1).

13. The stacked III-V semiconductor diode (10) according to claim 12, characterized in that: The second section (12.2, 16.2) has a layer thickness (D) of at least 0.5 μm and at most 10 μm, at least 2 μm and at most 4 μm. K2 , D A2 ).

14. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that The cathode layer (12) or the anode layer (16) is designed as a substrate.

15. The stacked III-V semiconductor diode (10) according to any one of the preceding claims, characterized in that Isoelectric or isovalent centers are present in the low p-doped drift layer and / or the anode layer in order to increase the switching speed.

Citation Information

Patent Citations

  • Power semiconductor device

    DE102016111844A1

  • Stacked III-V semiconductor diode

    DE102018000395A1

  • Iii-v semiconductor diode

    EP3321970B1

  • Iii-v semiconductor diode

    EP3321971B1

  • Semiconductor device and manufacture thereof

    JP1994314801A