Antioxidant blends for emulsion polymerized rubber
By using a stable combination of phosphite, amine and phenolic antioxidants in the elastomer, the problems of Mooney viscosity and color stability of the elastomer under temperature fluctuation conditions are solved, and higher storage stability and service life.
Patent Information
- Application Number
- CN202080038313.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technology has difficulty in maintaining the Mooney viscosity stability and color invariance of elastomers over long periods of time or under temperature fluctuations, resulting in performance degradation during storage and use.
The use of a stable composition containing phosphites, amines and phenolic antioxidants synergistically significantly improves the Mooney viscosity retention and color stability of elastomers during thermal aging.
The Mooney viscosity fluctuation is less than 30% and the yellowness index value is reduced within six days at 100°C, which significantly improves the storage stability and service life of the elastomer.
Smart Images

Figure BDA0003369794060000021 
Figure BDA0003369794060000051 
Figure BDA0003369794060000052
Abstract
Description
[0001] This application claims priority to UK Patent Application No. GB1907363.4, filed on 24 May 2019, which is incorporated herein by reference in its entirety.
[0002] This invention relates to stabilizing compositions. More specifically, but not exclusively, this invention relates to stabilizing compositions for stabilizing polymers, particularly stabilizing elastomers such as rubber and / or butadiene-based elastomers.
[0003] Polymers are used in a wide variety of applications. Elastomers are a class of polymers with diverse structures, properties, and applications. They all exhibit a degree of viscoelasticity and can be made from natural or synthetic polymers. Elastomers are used in many applications such as tires, pipes, gaskets, and seals due to their unique properties, such as high elasticity, durability, and high strength.
[0004] Elastomers are prone to physical and visual degradation over time, leading to poorer performance and reduced service life. Factors such as exposure to heat, oxygen, ozone, and radiation (e.g., light) can cause elastomer degradation and result in significant changes in their mechanical properties; for example, softening or hardening of the elastomer. Therefore, the viscosity of rubber can change significantly with degradation. Most commonly, the elastomer structure degrades through chain scission and / or cross-linking. Undesirable odors, discoloration, and fading of elastomers due to degradation can also be observed.
[0005] Polybutadiene and its copolymers containing fewer active double bonds are more susceptible to degradation due to chain crosslinking. Elastomers with larger groups or electron-donating groups, such as natural rubber, polyisoprene, and isobutylene isoprene rubber, are more prone to degradation via chain scission.
[0006] Mooney viscosity is widely used to assess the ability of elastomers to flow and retain their shape. It is important to ensure that the Mooney viscosity does not drift or fluctuate over long periods to ensure the elastomer's properties are maintained.
[0007] Therefore, it is important to maintain the Mooney viscosity of the elastomer material to minimize the degradation effects of chain scission and / or crosslinking. Elastomer discoloration due to degradation can also be observed; therefore, minimizing color changes is also crucial.
[0008] For many elastomer applications, it is desirable for elastomers to retain certain properties during storage, handling, and subsequent application. More specifically, it is desirable for elastomers to maintain their melt flow properties, Mooney viscosity, and good color stability during storage, even during prolonged or repeated exposure to temperature fluctuations.
[0009] To help maintain elastomer properties such as Mooney viscosity (M at 100°C) L(1+4) and color stability (according to the yellowness index), it is known to add different types of additives to elastomers, in particular, it is known to add antioxidants.
[0010] US9309379 describes a composition comprising a biodegradable emulsion crude rubber, synthetic latex or natural rubber latex and a stabilizer comprising a mixture selected from a specific group consisting of alkyl thiomethylphenol compounds and styrene diphenylamine.
[0011] US4489099 describes a chewing gum rubber composition (gum base) that uses dilauryl thiodipropionate and at least one ingredient selected from tert-butylhydroquinone (TBHQ) and vitamin E as an antioxidant stabilizer system.
[0012] EP2980146 describes an elastomeric composite material comprising a diene-based elastomer containing an antioxidant. The antioxidant comprises a combination of tri(nonylphenyl) phosphite (TNPP) and tetramethylethylenediamine (TMEDA), wherein the weight ratio of TNPP to TMEDA ranges from 4 / 1 to 50 / 1. Furthermore, rubber compositions comprising this elastomeric composite material, articles comprising this elastomeric composite material or rubber composition such as tires, and methods of manufacturing are disclosed.
[0013] EP2159264 describes an acrylic rubber composition and a vulcanized rubber that ensures the heat resistance of the vulcanized rubber, particularly with minimal change in elongation at break (EB) and hardness under heating conditions. An acrylic rubber composition comprises a carboxyl-containing acrylic rubber and, per 100 parts by weight of the carboxyl-containing acrylic rubber, 10 to 100 parts by weight of carbon black, 0.1 to 15 parts by weight of at least one primary antioxidant selected from amine antioxidants and phenolic antioxidants, and 0.1 to 15 parts by weight of at least one secondary antioxidant selected from phosphorus antioxidants and sulfur antioxidants.
[0014] WO2015114131 discusses compositions for stabilizing organic polymers, especially natural or synthetic rubber, against oxidative degradation and damage, comprising a) poly(dicyclopentadiene-co-p-cresol) (Formula I); b) a sterically hindered phenol of Formula II; and c) an alkylthiophenol of Formula III.
[0015]
[0016] WO2018041649 describes a liquid antioxidant composition for raw rubber comprising: a) 5% to 30% by weight of at least one aromatic amine antioxidant; b) 20% to 70% by weight of at least one hindered phenolic antioxidant; c) 0% to 40% by weight of at least one phosphite antioxidant; and d) 20% to 40% by weight of at least one solvent having a boiling point above 185°C and a freezing point below -10°C at 101.325 kPa, wherein the weight percentages of components a), b), c), or d) are based on the total weight of the antioxidant composition, wherein the mixture of components a), b), and c) is liquid at 25°C and 101.325 kPa.
[0017] WO2007050991 describes a composition comprising: an antioxidant; and at least one additive selected from the group consisting of: phosphorus stabilizers, acid stabilizers, and co-stabilizers.
[0018] GB2322374 describes a composition comprising: an organic material subjected to oxidation, heat or light-induced degradation; at least one compound of the benzofuran-2-one type; at least one compound selected from organophosphites or phosphonites; at least one compound selected from phenolic antioxidants; and at least one compound selected from sterically hindered amines.
[0019] JP2018070747 describes a polyolefin resin material stabilized with phenolic antioxidants, phosphorus-based antioxidants and hindered amine light stabilizers.
[0020] JP2003012900 describes a composition comprising an aromatic amine-based antioxidant, a hindered phenolic antioxidant, a sulfur-based antioxidant, and a phosphorus-based antioxidant.
[0021] US20070254990 describes a pipe coating resin composition with an oxidation induction time of more than five minutes, wherein the composition comprises: a thermoplastic ethylene-α-olefin copolymer composition having a melt index of 1 to 10 g / 10 min as determined by ASTM D1238 and a molecular weight distribution of 2.0 to 3.0; and an antioxidant system comprising 250 to 2500 ppm of hindered phenol, an auxiliary antioxidant for phosphorus (III) compounds, and a hindered amine light stabilizer.
[0022] There has been a long-standing industrial need for improved stable compositions that do not suffer from discoloration, Mooney viscosity changes, and undesirable odors, especially when exposed to temperature fluctuations during long or repeated storage periods.
[0023] According to a first aspect of the present invention, a stabilizing composition for an elastomer is provided, comprising:
[0024] a. A first stabilizing component, comprising at least one phosphite antioxidant;
[0025] b. A second stabilizing component comprising at least one amine antioxidant; and
[0026] c. A third stabilizing component, which contains at least one phenolic antioxidant.
[0027] The inventors of this invention have surprisingly discovered that, compared with compositions conventionally used in the art, the stabilizing compositions according to the invention result in excellent property retention and are very effective in stabilizing articles made of elastomers, particularly butadiene-based elastomers.
[0028] The elastomer may be butadiene-based. In this document, "butadiene-based" means that the elastomer contains butadiene or butadiene derivatives such as chloroprene as the monomeric basic unit. For example, the elastomer may contain polybutadiene (BR), nitrile rubber (NBR), styrene-butadiene (SBR), polychloroprene (CR), and / or a compatible mixture of two or more of these.
[0029] It has been unexpectedly found that elastomer materials containing the stabilizing composition of the present invention outperform industrial benchmarks in terms of Mooney viscosity retention and color performance, compared to 4,6-bis(octylthiomethyl)-o-cresol (LOWINOX). TM (520-CAS110553-27-0) The stable composition exhibits the same properties as the elastomeric material and has a lower overall odor. Therefore, the stable composition of the present invention can be used in place of conventional additives.
[0030] Without being bound by theory, it is believed that the antioxidants of the present invention exhibit synergistic effects on stabilized compositions or articles, such as elastomeric materials and articles made therefrom. Such synergistic blends are important in significantly improving Mooney viscosity retention and color retention during thermal aging, as well as providing a lower initial color.
[0031] The stabilizing composition of the present invention, when added to an elastomer, may cause the Mooney viscosity (measured according to ASTM D1646) of the elastomer to fluctuate less during six days of thermal aging at 100°C than the Mooney viscosity fluctuation of the same elastomer to which an equal weight / weight amount of the same stabilizing composition without any amine components has been added.
[0032] This accelerated thermal aging test uses high temperatures (100°C) to simulate several months of different storage and transportation conditions. It is a widely accepted standard quality control test for elastomers. This accelerated thermal aging test is used to predict the long-term thermal stability and storage stability of elastomers.
[0033] The maximum percentage fluctuation (measured as the percentage difference between the initial Mooney viscosity and the measured highest and / or lowest Mooney viscosity) may cause the elastomer's viscosity (measured according to ASTM D1646) to fluctuate by less than 30%, less than 25%, less than 20%, less than 16%, or less than 10% over a six-day period.
[0034] The stable composition of the present invention, when added to an elastomer, can make the initial yellowness index value (day 0) of the elastomer (measured according to ASTM E313) less than about 15, less than about 10, and less than about 8.
[0035] The stable composition of the present invention, when added to an elastomer, can reduce the yellowness index value (measured according to ASTM E313) of the elastomer to less than 45, less than 40, less than 37, less than 35, and less than 30 after four days.
[0036] In the following paragraphs, the product name AMINOX is used. TM ANOX TM BLE TM DURAZONE TM FLEXZONE TM LOWINOX TM ,NAUGALUBE TM NAUGARD TM NAUGAWHITE TM NOVAZONE TM OCTAMINE TM WESTON TM The specified compounds are available from USAA, LLC, 4 Mountainview Terrace, Suite 200, Danbury, CT06810.
[0037] Phosphite antioxidants can be liquids under environmental conditions. Amine antioxidants can also be liquids under environmental conditions. Preferably, both phosphite antioxidants and amine antioxidants are liquids under environmental conditions. However, in some cases, it is possible to produce a stable composition according to the invention that is liquid under environmental conditions by blending a liquid phosphite antioxidant with a solid amine antioxidant.
[0038] It is also possible to produce a stable composition according to the invention that is liquid under ambient conditions by blending a solid phosphite antioxidant with a liquid amine antioxidant.
[0039] "Environmental conditions" refers to a temperature preferably 50°C or lower, more preferably 30°C or lower, and most preferably 25°C or lower, and an atmospheric pressure of 101.325 kPa. For example, "environmental conditions" can refer to a temperature of 25°C and an atmospheric pressure of 101.325 kPa.
[0040] Preferably, the stable composition is a liquid under ambient conditions.
[0041] As described above, the phosphite antioxidants provided in the stabilizing compositions of the present invention are selected such that the stabilizing compositions are liquid under ambient conditions. This is often achieved by selecting a single phosphite antioxidant component that is itself liquid under ambient conditions.
[0042] Phosphite antioxidants may include organic phosphite antioxidants.
[0043] Phosphite antioxidants may include triaryl phosphites, trialkyl phosphites, and / or alkylaryl phosphites.
[0044] Phosphite antioxidants may include triaryl phosphites, optionally triphenyl phosphites.
[0045] Phosphite antioxidants may include one or more triaryl phosphites of formula I:
[0046]
[0047] Where R1, R2, and R3 are independently selected alkylated aryl groups of formula II:
[0048]
[0049] R4, R5, and R6 are independently selected from hydrogen and C1 to C6. 20 Alkyl, provided that at least one of R4, R5 and R6 is not hydrogen.
[0050] R4, R5, and R6 can be independently selected from hydrogen and C1 to C6. 10 Alkyl, provided that at least one of R4, R5 and R6 is not hydrogen.
[0051] R4, R5 and R6 may be independently selected from hydrogen and C1 to C6 alkyl groups, provided that at least one of R4, R5 and R6 is not hydrogen.
[0052] C1 to C6 alkyl groups may be selected from methyl, ethyl, propyl, butyl, pentyl, hexyl and / or their isomers, such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, tert-pentyl and / or neopentyl.
[0053] At least one of R4, R5 and R6 may be selected from tert-butyl and / or tert-pentyl.
[0054] One or more triaryl phosphites may have the structure of formula (III):
[0055]
[0056] R7, R8, and R9 are independently selected from methyl and ethyl groups, and n is 0, 1, 2, or 3.
[0057] One or more triaryl phosphites may be independently selected from tris(4-tert-butylphenyl) phosphite; tris(2,4-di-tert-butylphenyl) phosphite; bis(4-tert-butylphenyl)-2,4-di-tert-butylphenyl phosphite; bis(2,4-di-tert-butylphenyl)-4-tert-butylphenyl phosphite; tris(4-tert-pentylphenyl) phosphite; tris(2,4-di-tert-pentylphenyl) phosphite; bis(4-tert-pentylphenyl)-2,4-di-tert-pentylphenyl phosphite; bis(2,4-di-tert-pentylphenyl)-4-tert-pentylphenyl phosphite; and / or blends thereof.
[0058] One or more triaryl phosphites may be independently selected from tris(4-tert-pentylphenyl) phosphite; tris(2,4-di-tert-pentylphenyl) phosphite; bis(4-tert-pentylphenyl)-2,4-di-tert-pentylphenyl phosphite; bis(2,4-di-tert-pentylphenyl)-4-tert-pentylphenyl phosphite; and / or blends thereof.
[0059] Phosphite antioxidants may comprise blends of triaryl phosphites as described above. Preferably, the phosphite antioxidant comprises a blend of at least two, at least three, or at least four different triaryl phosphites.
[0060] A particularly preferred phosphite antioxidant according to the invention comprises a mixture of 2,4-bis(1,1-dimethylpropyl)phenyl phosphite and 4-(1,1-dimethylpropyl)phenyl phosphite (WESTO). TM 705-CAS 939402-02-5).
[0061] The inventors of this invention have discovered that certain advantages are achieved when phosphite antioxidants contain one or more triaryl phosphites. Specifically, it has been found that triaryl phosphites are much more stable and less prone to hydrolysis when combined with elastomers and under elastomer processing conditions compared to other known phosphite antioxidants, particularly alkylaryl phosphites such as tetra-C12-15-alkyl(propane-2,2-diylbis(4,1-phenylene))bis(phosphite) (CAS 96152-48-6). In WO2018041649, the key component of the antioxidant composition is the solvent, which is used to ensure that the antioxidant, especially the phosphite antioxidant, does not hydrolyze during the preparation of raw rubber. In contrast, the stable compositions of this invention are stable under elastomer processing conditions and can therefore be formulated in the absence of any solvent.
[0062] Phosphite antioxidants can be antioxidants that do not contain nonylphenyl groups.
[0063] Phosphite antioxidants may include trialkyl phosphites, such as DOVERPHOS TM LGP-11 (e.g., available from Dover Chemicals).
[0064] Phosphite antioxidants may include alkyl aryl phosphites, such as tri(tetranyl) phosphite (WESTON). TM TTDP-CAS 25488-25-3).
[0065] As a specific and non-limiting example, a phosphite antioxidant may, for example, comprise one or more of the following: a mixture of 2,4-bis(1,1-dimethylpropyl)phenyl phosphite and 4-(1,1-dimethylpropyl)phenyl phosphite (WESTON). TM 705 (CAS 939402-02-5); Tris(nonylphenyl) phosphite (WESTON) TM TNPP (CAS 26523-78-4); Tridecyl phosphite (WESTON) TM TTDP-CAS 25488-25-3); Trilauryl phosphite (WESTON) TM TLP-CAS 3076-63-9); Triisodecyl phosphite (WESTON) TM TDP-CAS 25448-25-3); Phenyl diisodecyl phosphite (WESTON) TM PDDP-CAS25550-98-5); Diphenylisodecyl phosphite (WESTON) TMDPDP (CAS 26544-23-0); Triisooctyl phosphite (TOP-CAS 25103-12-52); Tris(2-ethylhexyl) phosphite (CAS 78-42-2); Mixed 2-ethylhexylphenyl phosphite (WESTON) TM EHDP-CAS15647-8-2); Tris(dipropylene glycol) phosphite (WESTON) TM 430-CAS 36788-39-3); Poly(4,4'-isopropylidene diol) C12-15 alcohol phosphite (WESTON) TM 439-CAS96152-48-6); Polymerized liquid phosphite (DOVERPHOS) TM LGP-11, for example, available from Dover Chemicals; 4,4'-butylene-bis(3-methyl-6-tert-butylphenyl)alkyl (C13) ester of phosphite; and / or a compatible mixture of two or more thereof.
[0066] Phosphite antioxidants may comprise a mixture of 2,4-bis(1,1-dimethylpropyl)phenyl phosphite and 4-(1,1-dimethylpropyl)phenyl phosphite (WESTON) TM 705-CAS939402-02-5) and / or tridecyl phosphite (WESTON) TM TTDP-CAS25488-25-3).
[0067] Phosphite antioxidants may comprise a mixture of 2,4-bis(1,1-dimethylpropyl)phenyl phosphite and 4-(1,1-dimethylpropyl)phenyl phosphite (WESTON). TM 705-CAS939402-02-5).
[0068] The phosphite antioxidant may be present in amounts of about 20% to about 95% by weight of the stabilizing composition, about 25% to about 90% by weight of the stabilizing composition, about 30% to about 85% by weight of the stabilizing composition, about 35% to about 70% by weight of the stabilizing composition, or about 50% to about 65% by weight of the stabilizing composition.
[0069] Preferably, the phosphite antioxidant is present in an amount greater than about 40% by weight of the stable composition. For example, the phosphite antioxidant may be present in an amount greater than about 40% by weight of the stable composition up to about 60% by weight, about 65% by weight, about 70% by weight, about 75% by weight, about 80% by weight, about 85% by weight, about 90% by weight, or about 95% by weight.
[0070] The phosphite antioxidant may be present in amounts of about 41 wt%, about 42 wt%, about 45 wt%, or about 50 wt% to about 60 wt%, about 65 wt%, about 70 wt%, about 75 wt%, about 80 wt%, about 85 wt%, about 90 wt%, or about 95 wt% of the stabilizing composition. For example, phosphites may be present in amounts of about 42 wt% to about 75 wt%, about 45 wt% to about 70 wt%, or about 50 wt% to about 65 wt% of the stabilizing composition.
[0071] Phosphite antioxidants can be liquid at 50°C or lower, optionally 30°C or lower, optionally 25°C or lower, and at atmospheric pressure (101.325 kPa). Phosphite antioxidants can also be liquid at 25°C and atmospheric pressure (101.325 kPa).
[0072] The stabilizing component (b) contains one or more amine antioxidants.
[0073] As a specific and non-limiting example, amine antioxidants may, for example, contain 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (NAUGARD). TM 445-CAS 10081-67-1); mixed butylated diphenylamine and octylated diphenylamine (NAUGARD) TM PS30 (CAS 68411-46-1); Octyl diphenylamine (OCTAMINE) TM -CAS 101-67-7); Nonyl diphenylamine (NAUGALUBE) TM 438L-CAS 122-39-4); Polymerized 1,2-dihydro-2,2,4-trimethylquinoline (NAUGARD) TM Q-CAS26780-96-1); N,N-bis-(1,4-dimethylpentyl)-p-phenylenediamine (FLEXZONE) TM 4L-CAS3081-14-9); Acetone diphenylamine (AMINOX) TM -CAS 68412-48-6); the reaction product of diphenylamine and acetone (BLE) TM -CAS 112-39-4); 1,4-phenylenediamine, N,N'-mixed phenyl and tolyl derivatives (NOVAZONE) TM AS-CAS 68953-84-4); the reaction product of N-phenylaniline and 2,4,4-trimethylpentene (IRGANOX) TM 5057-CAS 68411-46-1 (e.g., available from BASF); N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (SANTOFLEX)TM 6PPD-CAS 793-24-8 (e.g., available from Eastman); N,N'-diphenyl-p-phenylenediamine (DPPD-CAS 74-31-7); N-isopropyl-N'-phenyl-1,4-phenylenediamine (IPPD-CAS 101-72-4); 2,4,6-tris-(N-1,4-dimethylpentyl-p-phenylenediamine)-1,3,5-triazine (DURAZONE) TM 37-CAS 121246-28-4); N,N'-bis(1,4-dimethylpentyl)-p-phenylenediamine (SANTOFLEX) TM 77PD-CAS 3081-14-9 (e.g., available from Eastman); and / or a compatible mixture of two or more of them.
[0074] Amine antioxidants may include 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (NAUGARD) TM 445-CAS10081-67-1) and / or mixtures of butylated diphenylamine and octylated diphenylamine (NAUGARD) TM PS30-CAS 68411-46-1).
[0075] Amine antioxidants may contain a mixture of butylated diphenylamine and octylated diphenylamine (NAUGARD). TM PS30-CAS68411-46-1).
[0076] Mixed butylated diphenylamine and octylated diphenylamine (NAUGARD) TM PS30 (CAS 68411-46-1) is a liquid amine antioxidant that is particularly helpful in producing liquid blends according to the invention.
[0077] The amine antioxidant may be present in amounts of about 1% to about 40% by weight of the stabilizing composition, about 1% to about 30% by weight of the stabilizing composition, about 5% to about 25% by weight of the stabilizing composition, or about 7% to about 20% by weight of the stabilizing composition.
[0078] Amine antioxidants can be secondary amines.
[0079] Amine antioxidants can be aromatic amines.
[0080] Amine antioxidants may have the general formula -R-NH-R', optionally, wherein the R and / or R' groups are aromatic. R and R' may be the same or different.
[0081] Amine antioxidants may have the general formula R-NH-R'-NH-R, optionally, wherein R' is aromatic and / or the R group is aromatic and / or alkyl. R and R' may be the same or different.
[0082] Amine antioxidants may contain at least one aromatic group, or at least two aromatic groups.
[0083] Amine antioxidants may consist of a single compound or a blend of two or more compounds.
[0084] Amine antioxidants may have a total nitrogen content of at least 3.5% or at least 4% by weight.
[0085] The stabilizing component (c) contains one or more phenolic antioxidants.
[0086] Phenolic antioxidants may consist of a single compound or a blend of two or more compounds.
[0087] Phenolic antioxidants can be optionally replaced.
[0088] Phenolic antioxidants may include semi-hindered and / or hindered phenolic antioxidants.
[0089] Phenolic antioxidants can include hindered phenolic antioxidants.
[0090] In this specification, "hindered" preferably means that the phenolic antioxidant contains substituted hydrocarbon groups at two positions adjacent to the phenolic -OH group, each of which is branched at the C1 position relative to the C1 and / or C2 position of the aromatic ring, preferably at the C1 position.
[0091] In this specification, "semi-hindered" preferably means that the phenolic antioxidant contains at least one substituted hydrocarbon group adjacent to the phenolic -OH group, and only one or each of the substituted groups is branched at the C1 and / or C2 position relative to the aromatic ring, preferably at the C1 position.
[0092] Phenolic antioxidants may contain phenolic groups that are substituted, preferably twice, and preferably substituted at the ortho position of the -OH group in the phenol.
[0093] Substituents on the phenolic group, or each substituent, may contain an alkyl group, optionally a branched alkyl group, optionally a tert-butyl group.
[0094] Phenolic antioxidants can be further substituted at the meta and para positions of the -OH group in phenol.
[0095] Phenolic antioxidants can contain multiple phenolic groups.
[0096] As specific and non-limiting examples, phenolic antioxidants may include: C13-C15 straight-chain and branched alkyl esters of 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate (ANOX). TM 1315-CAS171090-93-0); 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl ester (ANOX) TM PP18 (CAS 2082-79-3); 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate isooctyl ester (NAUGARD) TM PS48 (CAS 125643-61-0); Methyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate (CAS 6386-38-5); Pentaerythritol tetra(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (ANOX) TM 20-CAS 6683-19-8); Butylated hydroxytoluene (BHT-CAS128-37-0); Butylated hydroxyethylbenzene (BHEB-CAS4130-42-1); Butylated octylphenol (ANOX) TM T-CAS 12674-05-4); Styrified phenol (NAUGARD) TM SP-CAS61788-44-1); Styrified p-cresol (NAUGARD) TM 431-CAS 1817-68-1); 3,5-bis(1,1-dimethyl-ethyl)-4-hydroxyphenylpropionic acid C7-C9 branched alkyl ester (IRGANOX) TM 1135-CAS 125643-61-0 (e.g., available from BASF); 2,2-Methylenebis(6-nonyl-p-cresol) (NAUGAWHITE) TM -CAS 7786-17-6); 4-sec-butyl-2,6-di-tert-butylphenol (CAS 17540-75-9); 2-tert-butyl-4,6-dimethylphenol (LOWINOX) TM 624-CAS1879-09-0); Mixed tert-butylated phenols (ISONOX) TM133-CAS 60083-44-5 (e.g., available from SI Group Corporation, 2750 Balltown Road, Schenectady, NY 12301, US)); 4,4'-methylenebis(2,6-di-tert-butylphenol) (CAS 118-82-1); methyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (PP-CAS 6386-38-5); 2,4-dimethyl-6-(1-methylpentadecanyl)phenol (CAS 134701-20-5); and / or compatible mixtures of two or more thereof.
[0097] Phenolic antioxidants may include C13-C15 straight-chain and branched alkyl esters of 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate (ANOX). TM 1315-CAS 171090-93-0) and / or isooctyl 3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate (NAUGARD) TM PS48-CAS 125643-61-0).
[0098] The phenolic antioxidant may be present in amounts of about 5% to about 70% by weight of the stabilizing composition, about 10% to about 60% by weight of the stabilizing composition, about 15% to about 55% by weight of the stabilizing composition, about 20% to about 50% by weight of the stabilizing composition, or about 20% to about 40% by weight of the stabilizing composition.
[0099] Phenolic antioxidants may be selected to be liquid at a temperature of 50°C or lower, optionally 30°C or lower, optionally 25°C or lower, and at atmospheric pressure (101.325 kPa). Phenolic antioxidants may be liquid at 25°C and at atmospheric pressure (101.325 kPa).
[0100] The ratio of phosphite antioxidants to amine antioxidants to phenolic antioxidants in the stable composition may be: (about 35 to about 70): (about 1 to about 30): (about 15 to about 35); (about 45 to about 65): (about 5 to about 25): (about 15 to about 30); or (about 50 to about 65): (about 7 to about 20): (about 20 to about 30).
[0101] Other antioxidants, such as hydroxylamine or its precursors, lactone radical scavengers, acrylate radical scavengers, UV absorbers and / or chelating agents, may be included in the stable composition.
[0102] The stabilizing compositions according to the invention are particularly effective in stabilizing elastomeric materials. Elastomer materials can be stabilized to resist degradation induced by, for example, oxidation, heat, and / or radiation (e.g., light).
[0103] The stabilizing composition according to the invention may additionally contain a fourth stabilizing component, which contains at least one sulfur-containing antioxidant.
[0104] For example, a stable composition may contain:
[0105] a. A first stabilizing component, comprising at least one phosphite antioxidant;
[0106] b. A second stabilizing component comprising at least one amine antioxidant; and
[0107] c. A third stabilizing component, comprising at least one phenolic antioxidant; optionally,
[0108] d. The fourth stabilizing component, which contains at least one sulfur-containing antioxidant.
[0109] Sulfur-containing antioxidants may contain one or more thioether groups.
[0110] Sulfur-containing antioxidants may contain one or more thioester groups.
[0111] Sulfur-containing antioxidants may include sulfur-containing phenolic antioxidants.
[0112] Sulfur-containing antioxidants can be liquids under environmental conditions.
[0113] As specific and non-limiting examples, sulfur-containing antioxidants may include: 4,6-bis(octylthiomethyl)-o-cresol (LOWINOX) TM 520-CAS 110553-27-0); 2,2'-Thiodiethylidene bis[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate](ANOX) TM 70-CAS 41484-35-9); dilaurate thiodipropionate (NAUGARD) TM DLTDP (CAS 123-28-4); Distearate thiodipropionate (NAUGARD) TM DSTSP-CAS 693-36-7); di(tetrazolium)thiopropionate (NAUGARD) TM DTDTDP (CAS 10595-72-9); Pentaerythritol tetra(β-lauryl thiopropionate) (NAUGARD) TM 412S-CAS 29598-76-3); 2,4-bis(dodecylthiomethyl)-6-methylphenol (IRGANOX) TM 1726-CAS110675-26-8 (e.g., available from BASF); and / or a compatible mixture of two or more thereof.
[0114] Sulfur-containing antioxidants may include 4,6-bis(octylthiomethyl)-o-cresol (LOWINOX) TM 520-CAS 110553-27-0) and / or di(tetrazolium) thiodipropionate (NAUGARD) TM DTDTDP-CAS 10595-72-9).
[0115] The sulfur-containing antioxidant may be present in amounts of about 0% to about 50% by weight of the stabilizing composition, about 1% to about 40% by weight of the stabilizing composition, about 2% to about 30% by weight of the stabilizing composition, about 2% to about 20% by weight of the stabilizing composition, or about 2% to about 10% by weight of the stabilizing composition.
[0116] The ratio of phosphite antioxidants to amine antioxidants to phenolic antioxidants to sulfur-containing antioxidants in a stable composition can be:
[0117] (about 35 to about 70): (about 1 to about 30): (about 15 to about 35): (about 0 to about 20);
[0118] (about 45 to about 65): (about 5 to about 25): (about 15 to about 30): (about 1 to about 15); or
[0119] (about 50 to about 65): (about 7 to about 20): (about 20 to about 30): (about 1 to about 5).
[0120] According to a second aspect of the invention, the stabilizing composition is provided for use in stabilizing elastomeric materials.
[0121] Elastomers are amorphous polymers with a glass transition temperature lower than ambient temperature, preferably lower than their service temperature. Due to their low glass transition temperature, elastomers possess excellent viscoelastic properties such as high elasticity and excellent impact resistance.
[0122] Elastomers can be thermoplastic or thermosetting, vulcanized or unvulcanized.
[0123] Elastomer materials may include blends of natural rubber, synthetic rubber, and / or plastics with elastomers such as high-impact polystyrene (HIPS) or acrylonitrile butadiene styrene (ABS).
[0124] Elastomers can be butadiene-based. As mentioned above, in this context, "butadiene-based" means that the elastomer contains butadiene or butadiene derivatives such as chloroprene as the monomeric basic unit. For example, the elastomer may contain polybutadiene (BR), nitrile rubber (NBR), styrene-butadiene (SBR), polychloroprene (CR), and / or compatible mixtures of two or more of them.
[0125] According to a third aspect of the present invention, a stabilized elastomer composition is provided, comprising:
[0126] a. Elastomer materials
[0127] b. The stable composition according to the invention.
[0128] Stabilized elastomer compositions can be used to stabilize elastomer materials such as rubber.
[0129] Rubber may include natural rubber, synthetic rubber, and / or combinations thereof.
[0130] Elastomer materials can be products of emulsion polymerization or solution polymerization.
[0131] After incorporating the aforementioned stabilizers for final use, the elastomer material may or may not be cross-linked.
[0132] The stabilized elastomer composition may further comprise any material suitable for combination with the elastomer material and the stabilized composition of the present invention.
[0133] As specific and non-limiting examples, elastomers may include natural polyisoprene (cis-1,4-polyisoprene, natural rubber (NR)); goutabo rubber (trans-1,4-polyisoprene); synthetic polyisoprene; polybutadiene (butadiene rubber (BR)); polychloroprene (CR); butyl rubber (a copolymer of isobutylene and isoprene, IIR); halogenated butyl rubber; styrene-butadiene (a copolymer of styrene and butadiene, SBR); nitrile butadiene rubber (Buna-N rubber (NBR)); hydrogenated nitrile butadiene rubber (HNBR) and / or compatible mixtures of two or more thereof.
[0134] The elastomer may be derived from emulsion polymerization of at least one of styrene-butadiene (SBR); nitrile rubber (NBR); polybutadiene (BR); and polychloroprene (CR).
[0135] The elastomer may contain butadiene as one of the structural units. Other suitable structural unit comonomers may be styrene, acrylonitrile, ethylene, or propylene.
[0136] Elastomers can be used with different catalyst systems, including metallocene.
[0137] The present invention also relates to useful articles comprising the stabilized elastomer compositions described herein.
[0138] The stable composition according to the invention can be added to an elastomeric material in amounts of about 0.01 to about 5% by weight, about 0.05 to about 3% by weight, about 0.1 to about 2% by weight, or about 0.2 to about 1% by weight.
[0139] This percentage of the stabilized composition is important in providing the necessary protection for the stabilized elastomer composition during storage and transportation. Storage-stable compositions require minimal change in Mooney viscosity during long storage periods, such as up to one year at 40°C.
[0140] The stabilizing composition may be added during or after polymerization.
[0141] Preferably, the stabilizing composition is added after polymerization.
[0142] According to a fourth aspect of the present invention, a method for stabilizing articles made of elastomeric materials is provided, comprising incorporating or applying the stabilizing composition of the present invention into or to the elastomeric material.
[0143] For the avoidance of doubt, all features relating to the stable compositions of the present invention also relate, where appropriate, to stabilized elastomer compositions, stabilized articles, and methods of stabilizing articles, and vice versa.
[0144] The invention will now be described in more detail with reference to the following non-limiting embodiments. Example
[0145] Table 1 provides a summary of the details of the different stabilizing components used in the stabilized compositions. In the following text, the stabilizing components will be simply referred to by the names given in the “Abbreviation” column.
[0146]
[0147]
[0148] Key points of Table 1:
[0149] Component A: Phosphite Antioxidant
[0150] Component B amine antioxidants
[0151] Component C: Phenolic antioxidants
[0152] Component D: Sulfur-containing antioxidant
[0153] It will be obvious to technicians that certain materials (e.g., LOWINOX) TM 520-CAS 110553-27-0) may belong to one or more of component categories A, B, C, and D that are defined as essential components of the present invention. LOWINOX TM 520 can therefore be considered as component C and / or component D according to the present invention.
[0154] Table 2 shows the various stabilized compositions prepared. The percentages shown in the table are by weight of the total stabilized composition, and the dosage of the stabilized composition is in parts per hundred parts of rubber (phr).
[0155]
[0156] Examples A, B, C, and D are comparative examples without any amine components, with Example D representing an industrial standard. Examples 1 to 10 are based on the present invention.
[0157] Sample preparation
[0158] Antioxidant blends were prepared according to the compositions outlined in Table 2. The antioxidant blends (approximately 60 g) used in each embodiment were melted and mixed together. The mixtures were then heated to 70°C and oleic acid was added and mixed together. A KOH solution (13.3% by weight) (approximately 48 g) was then slowly added to the mixture while stirring at high speed to ensure homogeneous mixing and emulsion formation. The mixing speed was then reduced, and approximately 152 g of hot deionized water was added. The resulting antioxidant emulsion had a solids content of approximately 20% by weight.
[0159] Examples demonstrate the stability that can be obtained by using various stabilizing compositions in ESBR.
[0160] Antioxidant emulsion was added to ESBR latex. After stirring, the ESBR latex sample was coagulated using a standard hydrochloric acid coagulation system. More specifically, the sample was coagulated with 2% calcium chloride. The latex was then dropped into a 2% calcium chloride solution, and the rubber was transferred to fresh water. The rubber was washed three times under pressure. The rubber was then dried in a vacuum oven at 50°C for 16 hours. It was then subjected to HAAKE at 105°C. TM Use an internal mixer for 2 minutes to remove any residual water. Use a two-roll mill to make the elastomer more uniform.
[0161] The elastomer was oven aged at 100°C, and measurements were recorded every 24 hours for 4 days (yellowness index) and 6 days (Mounney viscosity).
[0162] Test conditions
[0163] Color stability
[0164] First, the sample was placed in a compression mold at 100°C for 5 minutes, resulting in an ESBR sheet 1 mm thick. Color change was measured using a colorimeter with the yellowness index (YI). Approximately 4 grams of elastomer were used for each YI measurement. YI values were taken at 0 hours and every 24 hours thereafter, measured as defined in ASTM E313. The average of five measurements was taken. A lower YI value indicates less color change in the composition. The results are shown in Table 3.
[0165] Table 3
[0166]
[0167] Stable compositions A and B represent comparative examples without the use of amine antioxidants. Example D represents an industry benchmark, including L520.
[0168] The results show that the ESBR samples stabilized with the stabilizing compositions according to the present invention (Examples 1-6) exhibited less discoloration than the industry standard.
[0169] ESBR samples stabilized with the stable composition according to the invention showed a lower initial yellowness index on day 0 and a lower yellowness index value on day 4.
[0170] Therefore, ESBR samples using the stable composition according to the invention provide better color retention, allowing for longer storage without color change.
[0171] Mooney viscosity
[0172] For each embodiment described above, approximately 20 g of sample was taken for Mooney viscosity testing. Mooney viscosity was measured using the standard method ASTM D1646(1+4)T 100°C. Mooney viscosity values were taken at 0 hours and every 24 hours thereafter.
[0173]
[0174] *The day ESBR begins to crosslink. When degradation via crosslinking predominates compared to chain scission, an overall increase in Mooney viscosity is expected. ESBR degradation is primarily dominated by crosslinking.
[0175] The elastomer structure degrades primarily through two distinct degradation mechanisms: chain scission and crosslinking. Chain scission typically occurs earlier in the degradation process and may lead to a decrease in Mooney viscosity. Crosslinking typically occurs later in the process and results in an increase in Mooney viscosity. Theoretically, Example 8 exhibited higher initial chain scission compared to the comparative examples, but subsequently showed relatively lower Mooney viscosity fluctuations, as observed from day 2 to day 6.
[0176] Small fluctuations in Mooney viscosity over time indicate the structural integrity of the elastomer and show minimal degradation.
[0177] Embodiments of the present invention exhibit superior Mooney viscosity at equivalent loads compared to comparative embodiments, and are equivalent to or superior to comparative embodiments at lower load levels.
[0178] Therefore, the embodiments comprising the stabilizing compositions according to the invention exhibit significantly superior Mooney viscosity retention and outperform comparative embodiments A to D. These stabilizing compositions will have better storage stability and better retention of physical properties.
[0179] The embodiments of the present invention exhibited a lower degree of Mooney viscosity fluctuation from day 0 to day 6. The results show that the maximum percentage fluctuation of the embodiments of the present invention was significantly lower than that of the comparative embodiments.
[0180] Therefore, the embodiments comprising the stabilizing composition according to the invention clearly demonstrate greater Mooney viscosity retention and less Mooney viscosity drift, and outperform comparative embodiments A to D.
[0181] Mooney viscosity tests were performed on samples from Examples 9 and 10. Mooney viscosity values were measured using the standard method ASTM D1646(1+4)T 100°C. Mooney viscosity values were taken at 0 hours and subsequently at 12, 24, 36, and 72 hours.
[0182]
[0183] Examples 9 and 10 both comprise stable compositions according to the invention. Example 10 shows a fairly low degree of Mooney viscosity fluctuation over 0 to 72 hours.
[0184] The results show that adding component D to the stabilizing composition significantly improves stability and reduces Mooney viscosity fluctuations. Therefore, the example (Example 10) containing the four-component stabilizing composition according to the invention clearly demonstrates greater Mooney viscosity retention and less Mooney viscosity drift. This stabilizing composition will have better storage stability and better retention of physical properties.
[0185] Elastomer converters generally standardize the processing conditions of elastomers for mass production; therefore, drift in Mooney viscosity will lead to fluctuations in the properties of the final product and result in inconsistent quality. This is undesirable.
[0186] Accelerated thermal aging tests simulate changes in Mooney viscosity under various storage and transportation conditions. This provides elastomer manufacturers with an indication of how stable their elastomers will be.
[0187] Therefore, when using the stable composition according to the invention, the increased stability and reduced Mooney viscosity fluctuations are beneficial to customers and result in greater consistency in product quality.
Claims
1. A stabilizing composition for an elastomer, comprising: a. a first stabilizing component comprising at least one phosphite antioxidant; wherein the phosphite antioxidant comprises a triaryl phosphite, optionally the triaryl phosphite is triphenyl phosphite; and optionally, wherein the phosphite antioxidant is a nonylphenyl-free antioxidant; b. a second stabilizing component comprising at least one aminic antioxidant; wherein the aminic antioxidant comprises at least one aromatic group; and c. a third stabilizing component comprising at least one phenolic antioxidant; wherein the phosphite antioxidant is present in an amount greater than 40% by weight of the stabilized composition; wherein the stable composition is a liquid composition at a temperature of 50°C or less and at atmospheric pressure, i.e., 101.325 kPa; and wherein the stable composition is formulated in the absence of any solvent.
2. The stabilized composition of claim 1, wherein the phosphite antioxidant comprises at least two different triaryl phosphites.
3. The stable composition according to claim 2, wherein the at least two different triaryl phosphites each have a structure of formula (III), Where R 7 , R 8 and R 9 are independently selected from methyl and ethyl groups, and n is 0, 1, 2 or 3.
4. The stabilizing composition of claim 3, wherein the at least two different triaryl phosphites are tris(4-tert-amylphenyl) phosphite; tris(2,4-di-tert-amylphenyl) phosphite; bis(4-tert-amylphenyl)-2,4-di-tert-amylphenyl phosphite; bis(2,4-di-tert-amylphenyl)-4-tert-amylphenyl phosphite; or mixtures thereof.
5. The stabilizing composition of claim 1, which, when added to an elastomer, causes the Mooney viscosity of the elastomer, as measured in accordance with ASTM D1646, to fluctuate less during six days of heat aging at 100°C than the Mooney viscosity of the same elastomer to which an equivalent weight / weight amount of the same stabilizing composition in the absence of any amine component has been added.
6. The stabilizing composition of any one of claims 1 to 5, further comprising a fourth stabilizing component comprising at least one sulfur-containing antioxidant.
7. The stable composition of claim 1, wherein the phenolic antioxidant comprises a hindered phenolic antioxidant.
8. The stable composition of claim 1, wherein the phenolic antioxidant is present in the stable composition in an amount of 5% to 70% by weight of the stable composition.
9. The stabilized composition of claim 1, wherein the phosphite antioxidant is a liquid at a temperature of 50°C or less and at atmospheric pressure, i.e., 101.325 kPa.
10. The stable composition of claim 1, wherein the aminic antioxidant is a secondary amine.
11. The stabilizing composition according to claim 1, wherein the amine antioxidant comprises 4,4'-bis(α,α-dimethylbenzyl)diphenylamine) and / or a mixed butylated diphenylamine, octylated diphenylamine.
12. The stabilized composition of claim 1, wherein the aminic antioxidant is present in the stabilized composition in an amount of 1 wt% to 40 wt% of the stabilized composition.
13. The stabilized composition of claim 1, wherein the ratio of phosphite antioxidant to amine antioxidant to phenolic antioxidant is: (35 to 70):(1 to 30):(15 to 35).
14. The stabilizing composition according to claim 6, wherein the ratio of the phosphite antioxidant to the amine antioxidant to the phenolic antioxidant to the sulfur-containing antioxidant in the stabilizing composition is: (35 to 70):(1 to 30):(15 to 35):(0 to 20).
15. The stable composition according to claim 1, which is a liquid composition at a temperature of 30°C or less and at atmospheric pressure, i.e., 101.325 kPa.
16. The stabilizing composition of claim 1, which, when added to an elastomer, causes the Mooney viscosity of the elastomer, measured according to ASTM D1646, to have a maximum fluctuation of less than 30% over a six day period.
17. The stabilizing composition of claim 1, which, when added to an elastomer, causes the elastomer to have a yellowness index value of less than 45 after four days as measured according to ASTM E313.
18. Use of the stabilizing composition according to any one of claims 1 to 17 for stabilizing elastomeric materials.
19. A stabilized elastomeric composition comprising: a. Elastomer materials b. A stable composition according to any one of claims 1 to 17.
20. The stabilized elastomeric composition according to claim 19, wherein the elastomeric material comprises natural rubber and / or synthetic rubber; and / or The elastomeric material is a product of emulsion polymerization.
21. The stabilized elastomeric composition of claim 19, wherein the elastomeric material comprises a butadiene-based elastomer.
22. The stabilized elastomeric composition of claim 21, wherein the butadiene-based elastomer comprises at least one of styrene-butadiene, polybutadiene, nitrile rubber, or polychloroprene.
23. The stabilized elastomeric composition of claim 19, wherein the stabilizing composition is added to the elastomeric material in an amount of 0.01 to 5% weight / weight.
24. A useful article comprising the stabilized elastomeric composition of any one of claims 19 to 23.
25. A method for stabilizing an article made of an elastomeric material, comprising incorporating or applying the stabilizing composition of any one of claims 1 to 17 to the elastomeric material.
Citation Information
Patent Citations
Acrylic rubber composition, vulcanized rubber therefrom and use thereof
EP2159264A1
Elastomer containing combination of tris(nonyl phenyl) phosphite and tetramethylethylenediamine, preparation and compositions and articles of manufacture thereof
EP2980146A1
Stabilising composition
GB201907363D0
Stabilizer mixture for organic materials
GB2322374A
Polyester elastomer resin composition for blow molding
JP2003012900A