Hydrogenation catalyst carrier and preparation method thereof, hydrogenation catalyst and preparation method thereof
By impregnating the γ-Al2O3 support with an organic modifier to adjust the surface properties and form ordered adsorption centers, the problem of poor dispersion of active metals was solved, the activity and synergistic effect of the hydrogenation catalyst were improved, and better hydrogenation performance was achieved.
Patent Information
- Application Number
- CN202110200368.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-02-23
AI Technical Summary
In existing supported hydrogenation catalysts, the poor dispersion of active metals leads to uneven catalyst activity, which affects their hydrogenation activity.
Organic modifiers, such as 3,5-difluorobenzoylhydrazine and 4-amino-2-fluoropyridine, are impregnated on γ-Al2O3 supports to adjust the surface properties of the support, form ordered adsorption centers, promote the localization and loading of active metals, and avoid disordered aggregation.
It improves the loading order of active metals, enhances the hydrogenation activity and synergistic effect of the catalyst, and improves the hydrodesulfurization, denitrification and aromatic saturation activity of the catalyst.
Smart Images

Figure CN114950459B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalysts, and relates to a supported hydrogenation catalyst carrier and a preparation method thereof, a hydrogenation catalyst and a preparation method thereof. Background Art
[0002] For traditional supported non-precious metal hydrogenation catalysts, the active metal accounts for about 15-35% of the total weight of the catalyst, and the active metal components are usually a combination of two or more. The synergistic effect between the active metal components has an important influence on the improvement of catalyst performance. The degree of dispersion of the active metal on the carrier surface plays a decisive role in the synergistic effect between the active metal components.
[0003] In the process of active metal impregnation, traditional supported hydrogenation catalysts often have random deposition of active components, resulting in uneven distribution of metal atoms of different sizes along the radial direction of the carrier. Smaller atoms tend to deposit more inside the carrier and less outside. Larger atoms tend to deposit more outside the carrier and less inside, which affects the activity of the catalyst.
[0004] In order to improve catalyst performance, improving catalyst preparation methods and enhancing the dispersion of active metals has become an important direction in the research and development of new catalysts.
[0005] CN1552795A discloses a method for preparing an impregnation liquid for a hydrogenation catalyst, in which ultrasonic waves are used in the preparation process of the metal impregnation liquid, so that the impregnation liquid has the characteristics of low viscosity and good stability. However, this method is not effective for impregnation solutions with low metal content, and due to the effect of ultrasonic waves, metal components tend to migrate into the micropores of the carrier, reducing the metal content of the metal components on the mesoporous surface of the carrier, reducing the number of active metal components on the mesoporous surface, and being unfavorable to the reaction of reactant molecules on the catalyst surface.
[0006] CN1552794A discloses an impregnation solution for hydrogenation catalyst and its preparation method. In this method, the metal component is first dissolved in water, and then an organic carboxylic acid is added to form a stable complex with the main metal, so that the metal impregnation solution has the characteristics of good stability and low viscosity. However, under conventional calcination conditions, this method is prone to partially coking the organic carboxylic acid on the catalyst surface, thereby reducing the number of active metal centers.
[0007] CN 85103891 describes a method for preparing a hydrogenation conversion catalyst. The method is to add a phosphorus-containing substance and a soluble amine compound to an impregnation solution, respectively, mix the two solutions together for impregnation, and adjust the pH value and temperature of the impregnation solution during the impregnation process. The process conditions for preparing the catalyst by this method are complex, and ammonia gas is released during the dissolution of ammonium hydroxide, which is harmful to the environment. The denitrification effect is not obvious, and it is not easy to be industrialized.
[0008] Chinese patent CN 101590416A describes a method for preparing a molybdenum-nickel hydrogenation catalyst. The method adopts two steps of kneading and impregnation to prepare the catalyst. First, in the presence of nitric acid, molybdenum oxide, titanium-containing compounds, phosphorus-containing compounds and aluminum oxide are kneaded, extruded, dried and roasted to obtain an aluminum oxide molded product containing titanium, phosphorus and molybdenum, and then impregnated with a nickel-containing phosphoric acid solution. After drying and roasting, a molybdenum-nickel hydrogenation catalyst is obtained. Chinese patent CN 1052501A discloses a method for preparing a hydrogenation catalyst. In order to improve the activity of the catalyst, the method adds additives P, F, and B to the impregnation solution containing Co-W-Mo trimetallics, impregnates by a segmented impregnation method, and obtains a finished catalyst after drying and roasting. The above method is subjected to high-temperature roasting after impregnation with the loaded active metal. The interaction between the active metal component and the carrier is strong, which affects the sulfurization effect of the catalyst, and also causes some active metal components to aggregate, affecting the dispersion of the active metal, and thus affecting the activity of the catalyst.
[0009] Japanese patent JP 04~166231 describes a method for preparing a hydrogenation catalyst. The method adopts step-by-step impregnation, wherein the carrier is first impregnated with a phosphorus-containing active metal component solution, and then dried at room temperature to 200°C. After drying, the impregnated carrier is contacted with a polyhydroxy compound solution, and then dried below 200°C to obtain a finished catalyst. U.S. Patent US6281333 discloses a method for preparing a hydrogenation treatment catalyst. The carrier is loaded with an active metal impregnation solution containing organic volatile components, and the catalyst is obtained without calcination. In the above-mentioned catalyst preparation process, an organic additive is added to the impregnation solution to increase the viscosity of the impregnation solution, which is not conducive to the dispersion of the active metal on the carrier surface. Moreover, the catalyst particles after impregnation are easy to stick together, and there is a clumping phenomenon. There is a metal precipitation phenomenon on the catalyst surface after drying, which affects the high dispersion of the active component on the carrier surface and has an adverse effect on the activity of the catalyst. Chinese patent CN99113281.5 discloses a distillate oil hydrorefining catalyst and its preparation method. The catalyst uses alumina or silicon-containing alumina as a carrier, W, Mo, and Ni as three metals as active components, and phosphoric acid is added as an additive. By adopting a segmented impregnation method, the metal distribution on the catalyst is made more uniform, and the hydrogenation and denitrification activity of the catalyst is greatly improved. Chinese patent CN200910012488.9 provides a method for preparing a hydroprocessing catalyst, which uses an impregnation liquid prepared by a conventional method to prepare a hydroprocessing catalyst. The impregnation liquid is highly acidic, which has a serious destructive effect on the specific surface area and pore volume of the catalyst, and after the catalyst is calcined at high temperature, the active components are prone to aggregate on the surface of the carrier, affecting the reaction activity. Chinese patent CN101089132A discloses a hydrodesulfurization catalyst with four active components of W-Mo-Ni-Co. The method uses a specific ratio of W-Mo-Ni-Co-P active components and impregnates them into an alumina carrier through a saturated co-impregnation technology. However, the loading amount of the active components is limited and it is impossible to provide more total active metals. During the impregnation process, the action of phosphorus and the surface groups of the carrier will weaken the adsorption of the active components on the carrier, making the metal components easily agglomerated, reducing the dispersion of the active components in the catalyst, and weakening the catalyst activity.
[0010] In general, the main problem that needs to be solved to improve the performance of petroleum fraction hydrogenation catalysts is how to improve the dispersion of metals in the process of preparing catalysts by supporting metal components on carriers, and reduce the decrease in specific surface area and pore volume caused by the blockage of carrier pores by metal components. To solve this problem, it is necessary to develop new methods for supporting active metal components on catalysts. Summary of the invention
[0011] The main purpose of the present invention is to provide a hydrogenation catalyst carrier and a preparation method thereof, a hydrogenation catalyst and a preparation method thereof, so as to overcome the defects of poor dispersibility of active components of supported hydrogenation catalysts and poor hydrogenation activity of hydrogenation catalysts in the prior art.
[0012] In order to achieve the above object, the present invention provides a method for preparing a hydrogenation catalyst carrier, comprising γ-Al 2 O 3 The carrier is impregnated with a modifier solution and dried to obtain a hydrogenation catalyst carrier;
[0013] The modifier solution includes an organic modifier, and the organic modifier includes one or more of 3,5-difluorobenzohydrazide, 4-amino-2-fluoropyridine, heptafluorobutyric anhydride, 4-vinylphenylboric acid, 2-aminoethyl diphenylborate and 4-carboxyphenylboric acid.
[0014] The method for preparing the hydrogenation catalyst carrier of the present invention, wherein the γ-Al 2 O 3 The preparation of the carrier includes: kneading an aluminum-containing precursor, a binder, a peptizing agent and water, and then extruding, drying and calcining to obtain γ-Al 2 O 3 carrier.
[0015] The method for preparing the hydrogenation catalyst carrier of the present invention, wherein the γ-Al 2 O 3 A modification aid is added during the preparation of the carrier, and the modification aid includes one or more of a B-containing compound, a Zr-containing compound, a Si-containing compound, a P-containing compound, and a Ti-containing compound.
[0016] The method for preparing a hydrogenation catalyst carrier of the present invention, wherein the mass content of the organic modifier as fluorine in the hydrogenation catalyst carrier is 0.62-12.5% and / or the mass content of the organic modifier as boron in the hydrogenation catalyst carrier is 0.25-10%.
[0017] The method for preparing the hydrogenation catalyst carrier of the present invention, wherein the γ-Al 2 O 3 The drying temperature after the carrier is impregnated with the modifier solution is 100°C to 120°C, and the drying time is 2h to 14h; the γ-Al 2 O 3 The drying temperature in the preparation process of the carrier is 100° C. to 120° C., and the drying time is 2 h to 14 h.
[0018] In order to achieve the above object, the present invention provides a hydrogenation catalyst carrier, which is obtained by the above-mentioned preparation method of the hydrogenation catalyst carrier.
[0019] In order to achieve the above object, the present invention provides a hydrogenation catalyst, which includes a carrier and an active component. The carrier is the above hydrogenation catalyst carrier, and the active component is one or more of Ni, Co, W and Mo.
[0020] The hydrogenation catalyst of the present invention, wherein the mass content of fluorine in the organic modifier is 0.5-10% of the hydrogenation catalyst and / or the mass content of boron in the organic modifier is 0.2-8% of the hydrogenation catalyst; and / or the mass content of the active component in terms of metal is 15-35% of the hydrogenation catalyst.
[0021] In order to achieve the above-mentioned object, the present invention provides a method for preparing a hydrogenation catalyst, comprising impregnating the above-mentioned hydrogenation catalyst carrier with an impregnation liquid including an active component precursor, and drying and calcining to obtain a hydrogenation catalyst; the active component precursor is one or more of a Ni precursor, a Co precursor, a W precursor and a Mo precursor.
[0022] Beneficial effects of the present invention:
[0023] Before the active metal is impregnated into the hydrogenation catalyst carrier of the present invention, the organic modifier is first impregnated to adjust the surface properties of the carrier and form a plurality of orderly arranged adsorption centers, so as to promote the positioning loading of the active metal atoms subsequently loaded, greatly improve the orderliness of the active metal loading, avoid the problem of low metal utilization rate caused by disordered stacking and inability to fully exert the synergistic effect, and thus make the catalyst of the present invention have better hydrogenation activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 XRD spectra of catalysts impregnated with different organic modifiers and containing different active metal systems.
[0025] Figure 2 The H of the catalyst prepared by impregnation with organic modifier and the catalyst prepared without impregnation with organic modifier 2 -TPR comparison spectra.
[0026] Figure 3 Comparative DRUVS spectra of the catalyst prepared by impregnation with organic modifier and the catalyst prepared without impregnation with organic modifier. DETAILED DESCRIPTION
[0027] The following is a detailed description of the embodiments of the present invention. The embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and processes are given. However, the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments where specific conditions are not specified are usually based on conventional conditions.
[0028] The present invention provides a method for preparing a hydrogenation catalyst carrier, comprising γ-Al 2 O 3 The carrier is impregnated with a modifier solution and dried to obtain a hydrogenation catalyst carrier;
[0029] The modifier solution includes an organic modifier, and the organic modifier includes one or more of 3,5-difluorobenzohydrazide, 4-amino-2-fluoropyridine, heptafluorobutyric anhydride, 4-vinylphenylboric acid, 2-aminoethyl diphenylborate and 4-carboxyphenylboric acid.
[0030] Before the active metal is impregnated into the hydrogenation catalyst carrier of the present invention, the organic modifier is first impregnated to adjust the surface properties of the carrier and form a plurality of orderly arranged adsorption centers, so as to promote the positioning loading of the active metal atoms subsequently loaded, greatly improve the orderliness of the active metal loading, avoid the problem of low metal utilization rate caused by disordered stacking and inability to fully exert the synergistic effect, and thus make the catalyst of the present invention have better hydrogenation activity.
[0031] The present invention does not particularly limit γ-Al 2 O 3 The source of the carrier can be commercially available γ-Al 2 O 3 In one embodiment, the present invention provides a γ-Al 2 O 3 The preparation method of the carrier comprises kneading an aluminum-containing precursor, a binder, a peptizing agent and water, and then extruding, drying and calcining to obtain a γ-Al 2 O 3 In another embodiment, the aluminum-containing precursor is pseudo-boehmite, and the binder is sesbania powder, but the present invention is not limited thereto. In another embodiment, the drying temperature is 100-120°C, the drying time is 2h to 14h, and the calcination temperature is 500-700°C, but the present invention is not limited thereto.
[0032] In one embodiment, γ-Al 2 O 3 A modification aid is also added during the preparation of the carrier, and the modification aid includes one or more of a B-containing compound, a Zr-containing compound, a Si-containing compound, a P-containing compound, and a Ti-containing compound. In another embodiment, the present invention provides a γ-Al 2 O 3 The preparation of the carrier is as follows: an aluminum-containing precursor, a modification aid, a binder, a peptizing agent and water are kneaded, and then extruded, dried and calcined to obtain γ-Al 2 O 3 carrier.
[0033] In one embodiment, the B compound contained in the modification aid of the present invention may be boric acid, sodium borate, potassium borate, the Zr compound contained may be zirconium tetrachloride, zirconium dioxide, zirconium silicate, the Si compound contained may be silica sol, sodium silicate, the P compound contained may be phosphoric acid, sodium dihydrogen phosphate, potassium dihydrogen phosphate, and the Ti compound contained may be titanic acid and titanium dioxide.
[0034] The present invention does not particularly limit the content of the modifier in the modifier solution. In one embodiment, the mass content of the modifier in the modifier solution of the present invention is 25-50%. In another embodiment, concentrated phosphoric acid, nitric acid, hydrochloric acid, etc. are also added to the modifier solution. In another embodiment, the mass content of concentrated phosphoric acid, nitric acid, and hydrochloric acid in the modifier solution is 25-50%.
[0035] In one embodiment, the modifier solution of the present invention may be heated during the preparation process, and the heating temperature is, for example, 50-100°C.
[0036] The present invention does not particularly limit γ-Al 2 O 3 The carrier is impregnated with the modifier solution by equal volume impregnation, spray impregnation, etc., and then dried to obtain the hydrogenation catalyst carrier. In one embodiment, the drying temperature is 100° C. to 120° C., and the drying time is 2 h to 14 h.
[0037] In the hydrogenation catalyst carrier thus prepared, the mass content of fluorine in the organic modifier accounts for 0.62-12.5% of the hydrogenation catalyst carrier and / or the mass content of boron in the organic modifier accounts for 0.25-10% of the hydrogenation catalyst carrier.
[0038] The present invention also provides a method for preparing a hydrogenation catalyst, comprising impregnating the above-mentioned hydrogenation catalyst carrier with an impregnation liquid including an active component precursor, and drying and calcining to obtain a hydrogenation catalyst; the active component precursor is one or more of a Ni precursor, a Co precursor, a W precursor and a Mo precursor.
[0039] In one embodiment, the active component precursor is a mixture of one of a Ni precursor and a Co precursor and one of a W precursor and a Mo precursor. The present invention does not particularly limit the mass content of the active component precursor in the impregnation solution. In one embodiment, the mass content of the active component precursor in the impregnation solution is 15-35%.
[0040] Thus, a hydrogenation catalyst is prepared, in which the mass content of fluorine in the organic modifier is 0.5-10% and / or the mass content of boron in the organic modifier is 0.2-8%; the mass content of the active component in the hydrogenation catalyst of the present invention in terms of metal is 15-35%.
[0041] Therefore, the present invention adopts γ-Al 2 O 3 The carrier is pre-impregnated with an organic modifier to improve the dispersion effect of active metals in the supported hydrogenation catalyst. The catalyst prepared by this method has greatly improved the synergistic effect between active metals and has a high catalyst hydrogenation activity.
[0042] The introduction of the organic modifier of the present invention can affect the existence form, dispersion state, sulfidation behavior and active phase type of the active metal, thereby affecting the activity of the catalyst. The organic modifier can effectively inhibit the CoMoO 4 and Co 3 O 4 The formation of crystals such as Co and Mo makes the Co and Mo atoms in the Co and Mo catalysts more evenly distributed on the catalyst surface, thereby promoting the synergistic effect between Co and Mo; at the same time, the organic modifier can moderately weaken the interaction between the active metal and the support, making the Mo species easier to sulfide and form MoS with a large number of stacking layers. 2 The lamellae are beneficial to the formation of Co-Mo-SⅡ type active phase, thus significantly promoting the HDS activity of CoMo catalyst.
[0043] Organic modifiers can also be used with Ni 2+ The NiMoO 4 , which improves the dispersion of active metals and promotes the hydrodesulfurization activity of the catalyst.
[0044] The present invention uses γ-Al 2 O 3 The carrier is impregnated with the same organic modifier and with different active metals to obtain hydrogenation catalysts, and the hydrogenation catalysts are measured by X-ray diffraction to obtain Figure 1 XRD spectrum of the catalyst. Curve A is the XRD spectrum of the MoNi active metal system catalyst. 3 The content is 17.3%, and the NiO content is 4.7%. Curve B is the XRD spectrum of the WNi active metal system catalyst. 3 The content is 20.9%, and the NiO content is 4.6%. Curve C is the XRD spectrum of the MoCo active metal system catalyst. 3 The content is 17.7%, and the CoO content is 4.3%. Curve D is the XRD spectrum of the MoNiCo active metal system catalyst. 3 The content is 14.7%, the NiO content is 2.3%, and the CoO content is 1.7%. Curve E is the XRD spectrum of the WMoNi active metal system catalyst. 3The content is 22.7%, the content of MoO is 2.9%, and the content of NiO is 2.1%. Figure 1 It can be seen from the spectra that the XRD peaks of all catalysts are basically the same, and no similar 4 、Co 3 O 4 and NiMoO 4 The characteristic peaks of the crystal indicate that the active metals in the catalyst prepared by the present invention are dispersed more evenly on the surface of the carrier.
[0045] The present invention conducts H treatment on a catalyst prepared by impregnating an organic modifier and a catalyst prepared by not impregnating an organic modifier (the other processes of the two are completely the same). 2 -TPR measurement, obtained Figure 2 Shown H 2 -TPR comparison spectrum. Curve A represents the H 2 -TPR spectrum, curve B represents the H 2 -TPR spectrum. The preparation method of the catalyst corresponding to curve B is described in Example 1, and the preparation method of the catalyst corresponding to curve A is described in Comparative Example 1. Compared with curve A, the high-temperature reduction peak and the low-temperature reduction peak of curve B both move toward the low-temperature direction, indicating that the modification of the organic modifier can weaken the interaction between the active component and the carrier. If the interaction between the active component and the carrier is too strong, inert spinel structure species, such as the common nickel aluminum spinel, are easily generated. By weakening the interaction force between the active component and the carrier, it is beneficial for the oxidized active component to form a highly active center after sulfurization, thereby improving the hydrogenation activity of the catalyst.
[0046] The present invention also conducts DRUVS measurement on the catalyst prepared by impregnating the organic modifier and the catalyst prepared by not impregnating the organic modifier (the other processes of the two are exactly the same), and obtains Figure 3 DRUVS comparison spectrum shown. Figure 3 As shown, curve A represents the DRUVS spectrum of the catalyst prepared without impregnation of the organic modifier, and curve B represents the DRUVS spectrum of the catalyst prepared with impregnation of the organic modifier. The preparation method of the catalyst corresponding to curve A is described in Comparative Example 1, and the preparation method of the catalyst corresponding to curve B is described in Example 1. Curve A has obvious peaks at 590nm and 630nm, which is NiAl 2 O 4 The characteristic bands of spinel. The characteristic bands of catalyst B at 590nm and 630nm are not obvious, and an obvious characteristic band of octahedral nickel species appears at 420nm. NiAl 2 O 4The elimination of spinel and the formation of octahedral Ni species are both beneficial to the nickel promoter effect, thereby improving the hydrogenation activity of the catalyst.
[0047] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art.
[0048] Example 1
[0049] (1) γ-Al 2 O 3 Preparation of vector
[0050] Weigh 1000g of pseudo-boehmite powder, 50g of Tianqing powder, 30g of citric acid, and 700ml of 3-5m% (the following examples are also mass content) of dilute nitric acid, mix them evenly, extrude them with an extruder, dry them at 110°C for 10h, and calcine them at 550°C in air atmosphere to obtain γ-Al 2 O 3 carrier.
[0051] (2) Preparation of organic modifier solution
[0052] Weigh 500g of deionized water, add 20g of concentrated phosphoric acid (mass concentration is 85%, the same as in the following examples), the role of concentrated phosphoric acid is to prepare a uniform and stable solution, heat to 50°C while stirring, add 200g of 3,5-difluorobenzoyl hydrazide and 130g of 4-vinylbenzene boronic acid, continue to heat to 70°C, and keep the temperature constant for 3 hours. After the constant temperature is completed, naturally cool to room temperature and set aside.
[0053] (3)γ-Al 2 O 3 Carrier impregnation with organic modifier
[0054] Using the unsaturated spray impregnation method, weigh 500g of the γ-Al prepared in step (1) 2 O 3 The carrier is sprayed with 150 ml of the organic modifier solution prepared in step (2), and then dried at 110° C. for 5 hours.
[0055] (4) Mo-Ni / γ-Al 2 O 3 Catalyst preparation
[0056] Weigh 500g of the carrier prepared in step (3), and measure 332ml of an impregnation solution containing molybdenum and nickel, wherein the precursor of molybdenum is ammonium tetramolybdate and the precursor of nickel is nickel nitrate. Molybdenum accounts for 10-25m% of the catalyst mass as molybdenum trioxide, and nickel accounts for 2-7m% of the catalyst mass as nickel oxide. The catalyst is impregnated for 30 minutes with equal volumes, dried at 110°C for 2 hours, and calcined at 460°C to obtain a finished catalyst.
[0057] Example 2
[0058] (1) Ti-modified γ-Al 2 O 3 Preparation of vector
[0059] Weigh 950g pseudo-boehmite powder, 50g metatitanic acid, 50g Tianqing powder, 30g citric acid, and 700ml of 3-5m% dilute nitric acid, mix them evenly, extrude them into a strip by an extruder, dry them at 110℃ for 10h, and calcine them at 550℃ in air atmosphere to obtain Ti-modified γ-Al 2 O 3 carrier.
[0060] (2) Preparation of organic modifier solution
[0061] Weigh 500g of deionized water, add 30g of concentrated phosphoric acid to it, the purpose of concentrated phosphoric acid is to prepare a uniform and stable solution, heat it to 55°C while stirring, add 220g of 4-amino-2-fluoropyridine and 120g of 2-aminoethyl diphenylborate, continue to heat it to 60°C, and keep the temperature constant for 3 hours. After the constant temperature is completed, cool it naturally to room temperature and set aside.
[0062] (3) Ti-modified γ-Al 2 O 3 Carrier impregnation with organic modifier
[0063] Using the unsaturated spray impregnation method, weigh 500g of the Ti-modified γ-Al prepared in step (1) 2 O 3 The carrier is sprayed with 155 ml of the organic modifier solution prepared in step (2), and then dried at 110° C. for 5 hours.
[0064] (4) Mo-Co / γ-Al 2 O 3 Catalyst preparation
[0065] Weigh 500g of the carrier prepared in step (3), and measure 322ml of an impregnation solution containing molybdenum and cobalt, wherein the precursor of molybdenum is ammonium tetramolybdate and the precursor of cobalt is cobalt nitrate. Molybdenum accounts for 10-25m% of the catalyst mass as molybdenum trioxide, and cobalt accounts for 2-7m% of the catalyst mass as cobalt oxide. The catalyst is impregnated with equal volumes for 30 minutes, dried at 110°C for 2 hours, and calcined at 450°C to obtain a finished catalyst.
[0066] Comparative Example 1
[0067] (1) γ-Al 2 O 3 Preparation of vector
[0068] Weigh 1000g pseudo-boehmite powder, 50g Tianqing powder, 30g citric acid, and 700ml of 3-5% dilute nitric acid, mix them evenly, extrude them into strips using an extruder, dry them at 110℃ for 10h, and calcine them at 550℃ in air atmosphere to obtain γ-Al 2 O 3 carrier.
[0069] (2) Mo-Ni / γ-Al 2 O 3 Catalyst preparation
[0070] Weigh 500g of the carrier prepared in step (1), and measure 347ml of an impregnation solution containing molybdenum and nickel, wherein the precursor of molybdenum is ammonium tetramolybdate and the precursor of nickel is nickel nitrate. Molybdenum accounts for 10-25m% of the catalyst mass as molybdenum trioxide, and nickel accounts for 2-7m% of the catalyst mass as nickel oxide. The catalyst is impregnated for 30 minutes with equal volumes, dried at 110°C for 2 hours, and calcined at 460°C to obtain a finished catalyst.
[0071] Comparative Example 2
[0072] (1) Ti-modified γ-Al 2 O 3 Preparation of vector
[0073] Weigh 950g pseudo-boehmite powder, 50g metatitanic acid, 50g Tianqing powder, 30g citric acid, and 700ml of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip by an extruder, dry them at 110℃ for 10h, and calcine them at 550℃ in air atmosphere to obtain Ti-modified γ-Al 2 O 3 carrier.
[0074] (2) Mo-Co / γ-Al 2 O 3 Catalyst preparation
[0075] Weigh 500g of the carrier prepared in step (1), and measure 327ml of an impregnation solution containing molybdenum and cobalt, wherein the precursor of molybdenum is ammonium tetramolybdate, and the precursor of nickel is nickel nitrate. Molybdenum accounts for 10-25m% of the catalyst mass as molybdenum trioxide, and nickel accounts for 2-7m% of the catalyst mass as nickel oxide. The catalyst is impregnated with equal volumes for 30 minutes, dried at 110°C for 2 hours, and calcined at 450°C to obtain a finished catalyst.
[0076] The catalyst prepared in the above Examples 1-2 and Comparative Examples 1-2 was used to evaluate the hydrogenation activity of 100 ml of the catalyst, and the raw material oil was evaluated as inferior kerosene. Wherein, (1) sulfurization conditions: the catalyst was first pre-sulfurized for 25 hours with kerosene containing 2 wt% carbon disulfide under a hydrogen atmosphere at 290°C and a pressure of 7.0 MPa, and then the raw material was added; (2) reaction conditions: reaction temperature 300°C, pressure 5.0 MPa, space velocity (volume) 2.0 h -1 , hydrogen to oil (volume) ratio is 300. The evaluation results are shown in Table 1.
[0077] Table 1 Catalyst activity evaluation results
[0078] project Crude oil Example 1 Example 2 Comparative Example 1 Comparative Example 2 Sulfur, μg / g 2324 8.2 8.4 36.5 37.4 Nitrogen, μg / g 125 12.1 12.0 20.5 20.4 Aromatic content, Φ% 22.5 14.0 13.8 16.7 16.4
[0079] As shown in Table 1, compared with the catalysts prepared in Comparative Examples 1 and 2, the sulfur content, nitrogen content and aromatic content in the oil product obtained after the catalyst prepared by the method of the present invention is subjected to hydrogenation catalysis on the crude oil are lower, which indicates that the catalyst prepared by the method of the present invention has higher hydrodesulfurization, denitrogenation activity and aromatic saturation activity.
[0080] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a hydrogenation catalyst, It is characterized in that The preparation method is: γ-Al 2 O 3 The carrier is impregnated with a modifier solution and dried to obtain a hydrogenation catalyst carrier; The hydrogenation catalyst carrier is impregnated with an impregnation solution including an active component precursor, and dried and calcined to obtain a hydrogenation catalyst; The modifier solution includes an organic modifier, and the organic modifier includes one or more of 3,5-difluorobenzohydrazide, 4-amino-2-fluoropyridine, heptafluorobutyric anhydride, 4-vinylphenylboric acid, 2-aminoethyl diphenylborate and 4-carboxyphenylboric acid.
2. The method for preparing the hydrogenation catalyst according to claim 1, It is characterized in that The γ-Al 2 O 3 The preparation of the carrier includes: kneading an aluminum-containing precursor, a binder, a peptizing agent and water, and then extruding, drying and calcining to obtain γ-Al 2 O 3 carrier.
3. The method for preparing the hydrogenation catalyst according to claim 2, It is characterized in that The γ-Al 2 O 3 A modification aid is added during the preparation of the carrier, and the modification aid includes one or more of a B-containing compound, a Zr-containing compound, a Si-containing compound, a P-containing compound, and a Ti-containing compound.
4. The method for preparing the hydrogenation catalyst according to claim 1, It is characterized in that The mass content of the organic modifier in terms of fluorine in the hydrogenation catalyst carrier is 0.62%-12.5%, and / or the mass content of the organic modifier in terms of boron in the hydrogenation catalyst carrier is 0.25%-10%.
5. The method for preparing the hydrogenation catalyst according to claim 2, It is characterized in that The γ-Al 2 O 3 The drying temperature after the carrier is impregnated with the modifier solution is 100°C to 120°C, and the drying time is 2h to 14h; the γ-Al 2 O 3 The drying temperature in the preparation process of the carrier is 100° C. to 120° C., and the drying time is 2 h to 14 h.
6. The method for preparing the hydrogenation catalyst according to claim 1, It is characterized in that The active component precursor is one or more of a Ni precursor, a Co precursor, a W precursor and a Mo precursor.
7. A hydrogenation catalyst, It is characterized in that The hydrogenation catalyst is obtained by the preparation method of the hydrogenation catalyst according to any one of claims 1 to 6.
8. The hydrogenation catalyst according to claim 7, It is characterized in that The mass content of fluorine in the organic modifier is 0.5%-10% of the hydrogenation catalyst and / or the mass content of boron in the organic modifier is 0.2%-8% of the hydrogenation catalyst; and / or the mass content of active components in terms of metal is 15%-35% of the hydrogenation catalyst.
Citation Information
Patent Citations
Fraction oil hydrodesulfurizing catalyst and its prepn process
CN101089132A
Molybdenum-nickel hydrogenation catalyst and preparation method thereof
CN101590416A
Preparation method of hydrotreating catalyst
CN101940929A
Hydrofined catalyst and preparing process thereof
CN1052501A
Hydrorefining catalyst for fraction oil and its preparing process
CN1289828A