Method for manufacturing an anode for a lithium battery cell
By forming a multi-layer SEI layer on the anode of the lithium ion battery, the lithium salt in the non-aqueous liquid electrolyte solution is used to apply SEI on the anode of the lithium ion battery to generate electrolyte, which solves the growth of lithium dendrites and 'moss-like' structures in the lithium ion battery. The problem of improving the cycle efficiency and application life of the battery and providing stability during the manufacturing process.
Patent Information
- Application Number
- CN202111532652.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-19
- Filing Date
- 2021-12-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-15
AI Technical Summary
The Li metal electrodes of lithium-ion batteries have large volume changes and high reactivity, resulting in the growth of "moss-like" lithium structure and lithium dendrites, which reduces the circulation efficiency and application life of lithium-ion batteries.
Before assembly of the lithium-ion battery anode, by forming a solid electrolyte interface (SEI) layer, multi-layer SEI is applied on the raw anode using lithium salts in the non-aqueous liquid electrolyte solution to generate electrolytes, forming a SEI layer with flexible and mechanical protection, inhibiting Growth of lithium dendrites and 'mossy' structures.
It effectively inhibits the growth of lithium dendrites and ‘moss-like’ structures, improves the circulation efficiency and application life of lithium-ion batteries, and provides stability in a non-inert environment during the manufacturing process.
Smart Images

Figure CN114975889B_ABST
Abstract
Description
Background Art
[0001] Lithium-ion batteries are a type of rechargeable battery in which lithium ions move between a negative electrode and a positive electrode. Liquid, solid, and polymer electrolytes can facilitate the movement of lithium ions between the anode and cathode. Due to their high energy density and ability to withstand continuous charge and discharge cycles, lithium-ion batteries have applications in handheld personal communication devices and automotive systems. The large volume change and high reactivity of the Li metal electrode can lead to "moss-like" lithium structures and / or lithium dendrite growth, which can reduce the cycle efficiency and application of such lithium-ion batteries. Summary of the invention
[0002] Provided herein are methods for forming an anode for a lithium-ion battery cell having a solid electrolyte interface (SEI) layer that is formed prior to assembling the anode into a battery cell. The SEI layer described herein inhibits or prevents the growth of Li dendrites and / or "moss-like" structures during battery pack cycling and also exhibits flexible properties that provide mechanical protection for the lithium anode and the accompanying battery cell structure. In addition, the formation of the SEI layer can produce a hydrophobic electrode intermediate that allows it to be transported and / or stored in a non-inert environment between manufacturing steps.
[0003] The concepts described herein provide a method for manufacturing an anode for a lithium-ion battery cell. The method includes forming a solid electrolyte interface (SEI) layer on a green anode prior to assembly into a battery cell by applying a first SEI-generating electrolyte to the green anode to form a first intermediate anode, applying a second SEI-generating electrolyte to the first intermediate anode to form a second intermediate anode, and applying a third SEI-generating electrolyte to the second intermediate anode to form a battery anode, wherein the battery anode includes a green anode having a SEI layer. The green anode includes a metal strip having an electroactive material deposited on at least one side.
[0004] One aspect of the present disclosure includes manufacturing a battery anode by sequentially applying one or different SEI-generating electrolytes to a green anode to form a battery anode having a solid electrolyte interface (SEI) layer, and manufacturing a lithium-ion battery cell by assembling the battery anode into a battery pack, wherein the battery pack includes a cathode and a separator, and adding a battery electrolyte to the battery pack prior to sealing.
[0005] Another aspect of the present disclosure includes applying a first SEI-generating electrolyte to a green anode by applying a first non-aqueous liquid electrolyte solution to the green anode, the first non-aqueous liquid electrolyte solution comprising a first lithium salt dissolved in an organic solvent.
[0006] Another aspect of the present disclosure includes applying a first SEI-generating electrolyte to a green anode by applying a first non-aqueous liquid electrolyte solution to the green anode, the first non-aqueous liquid electrolyte solution comprising a first mixture of lithium salts dissolved in an organic solvent.
[0007] Another aspect of the present disclosure includes applying the second SEI-forming electrolyte to the first intermediate anode by applying a second non-aqueous liquid electrolyte solution to the first intermediate anode, the second non-aqueous liquid electrolyte solution comprising a second lithium salt dissolved in an organic solvent.
[0008] Another aspect of the present disclosure includes applying the SEI-generating electrolyte to the first intermediate anode by applying a second non-aqueous liquid electrolyte solution to the first intermediate anode, the second non-aqueous liquid electrolyte solution comprising a second mixture of lithium salts dissolved in an organic solvent.
[0009] Another aspect of the present disclosure includes applying a third SEI-forming electrolyte to the second intermediate anode by applying a third non-aqueous liquid electrolyte solution to the second intermediate anode, the third non-aqueous liquid electrolyte solution comprising a third lithium salt dissolved in an organic solvent.
[0010] Another aspect of the present disclosure includes applying a third SEI-forming electrolyte to the second intermediate anode by applying a third non-aqueous liquid electrolyte solution to the second intermediate anode, the third non-aqueous liquid electrolyte solution comprising a third mixture of lithium salts dissolved in an organic solvent.
[0011] Another aspect of the present disclosure includes first, second and third SEI-forming electrolytes as a non-aqueous liquid electrolyte solution, the non-aqueous liquid electrolyte solution including a lithium salt dissolved in an organic solvent, wherein the lithium salt includes one or a mixture of the following: lithium hexafluorophosphate (LiPF6); lithium perchlorate (LiClO4); lithium tetrachloroaluminate (LiAlCl4); lithium bis(oxalate)borate (LiB(C2O4)2) (LiBOB); lithium nitrate (LiNO3), lithium bis(trifluoromethanesulfonyl imide) (LITFSI) (LiN(CF3SO2)2); lithium fluorosulfonyl imide (LiN(FSO2)2) (LIFSI).
[0012] Another aspect of the present disclosure includes performing a first drying step after applying the first SEI-forming electrolyte to the green anode.
[0013] Another aspect of the present disclosure includes performing a second drying step after applying the second SEI-forming electrolyte to the first intermediate anode.
[0014] Another aspect of the present disclosure includes performing a third drying step after applying the third SEI-forming electrolyte to the second intermediate anode.
[0015] Another aspect of the present disclosure includes assembling a battery anode into a battery pack, wherein the battery pack includes a cathode and a separator; and adding a battery electrolyte to the battery pack prior to sealing, wherein the battery electrolyte has a different chemical composition than the first, second, and third SEI-forming electrolytes.
[0016] Another aspect of the present disclosure includes evaluating the SEI layer on the battery anode before assembling the battery anode into a battery pack; and assembling the battery anode into the battery pack only when the SEI layer on the battery anode meets a minimum standard.
[0017] Expected benefits of utilizing this process include avoiding partial wetting of the electrode or homogeneous reaction kinetics that can occur during SEI formation inside the battery, with its associated lithium plating, electrolyte decomposition and gassing, and other issues that affect battery cell quality.
[0018] The present invention also includes the following technical solutions.
[0019] Scheme 1. A method for manufacturing a battery anode for a lithium-ion battery cell, the method comprising:
[0020] A solid electrolyte interface (SEI) layer is formed on the green anode, comprising:
[0021] applying a first SEI-forming electrolyte to the green anode to form a first intermediate anode;
[0022] applying a second SEI-forming electrolyte to the first intermediate anode to form a second intermediate anode; and
[0023] applying a third SEI-forming electrolyte to the second intermediate anode to form a battery anode;
[0024] wherein the battery anode comprises the green anode having the SEI layer; and
[0025] The green anode includes a metal strip having an electroactive material deposited on at least one side.
[0026] Option 2. The method according to Option 1, wherein applying the first SEI-generating electrolyte to the green anode comprises: applying a first non-aqueous liquid electrolyte comprising a first lithium salt dissolved in an organic solvent to the green anode.
[0027] Option 3. A method according to Option 2, wherein the first SEI-generating electrolyte includes a non-aqueous liquid electrolyte solution, the non-aqueous liquid electrolyte solution contains a lithium salt dissolved in an organic solvent, wherein the lithium salt includes one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide.
[0028] Option 4. The method according to Option 1, wherein applying the first SEI-generating electrolyte to the green anode comprises: applying a first non-aqueous liquid electrolyte solution comprising a first mixture of lithium salts dissolved in an organic solvent to the green anode.
[0029] Option 5. The method according to Option 1, wherein applying the second SEI-forming electrolyte to the first intermediate anode comprises: applying a second non-aqueous liquid electrolyte solution comprising a second lithium salt dissolved in an organic solvent to the first intermediate anode.
[0030] Option 6. A method according to Option 5, wherein the second SEI-generating electrolyte includes a non-aqueous liquid electrolyte solution, the non-aqueous liquid electrolyte solution contains a lithium salt dissolved in an organic solvent, wherein the lithium salt includes one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide.
[0031] Option 7. The method according to Option 1, wherein applying the SEI-generating electrolyte to the first intermediate anode comprises: applying a second non-aqueous liquid electrolyte solution comprising a second mixture of lithium salts dissolved in an organic solvent to the first intermediate anode.
[0032] Option 8. The method according to Option 1, wherein applying the third SEI-forming electrolyte to the second intermediate anode comprises: applying a third non-aqueous liquid electrolyte solution comprising a third lithium salt dissolved in an organic solvent to the second intermediate anode.
[0033] Option 9. A method according to Option 8, wherein the third SEI-generating electrolyte includes a non-aqueous liquid electrolyte solution, the non-aqueous liquid electrolyte solution contains a lithium salt dissolved in an organic solvent, wherein the lithium salt includes one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide.
[0034] Option 10. The method according to Option 1, wherein applying the third SEI-forming electrolyte to the second intermediate anode comprises: applying a third non-aqueous liquid electrolyte solution comprising a third mixture of lithium salts dissolved in an organic solvent to the second intermediate anode.
[0035] Scheme 11. The method according to Scheme 1 further includes:
[0036] After applying the first SEI-forming electrolyte to the green anode, performing a first drying step;
[0037] performing a second drying step after applying the second SEI-forming electrolyte to the first intermediate anode; and
[0038] After applying the third SEI-forming electrolyte to the second intermediate anode, a third drying step is performed.
[0039] Scheme 12. The method according to Scheme 1 further comprises:
[0040] Assembling the battery anode into a battery pack, wherein the battery pack includes a cathode and a separator; and
[0041] A battery electrolyte is added to the battery pack prior to sealing, wherein the battery electrolyte has a different chemical composition than the first SEI generating electrolyte, the second SEI generating electrolyte, and the third SEI generating electrolyte.
[0042] A method for manufacturing a lithium-ion battery cell, comprising:
[0043] Manufacturing of battery anodes, including:
[0044] sequentially applying a SEI-forming electrolyte to a green anode to form a battery anode having a solid electrolyte interface (SEI) layer;
[0045] Assembling the battery anode into a battery pack, wherein the battery pack includes a cathode and a separator; and
[0046] A battery electrolyte is added to the battery pack prior to sealing, wherein the battery electrolyte has a different chemical composition than the SEI-generating electrolyte.
[0047] Option 14. The method according to Option 13 further includes evaluating the SEI layer on the battery anode before assembling the battery anode into a battery pack; and
[0048] Only when the SEI layer on the battery anode meets the minimum standard, the battery anode is assembled into the battery pack.
[0049] Embodiment 15. The method according to Embodiment 13, wherein sequentially applying the SEI-generating electrolyte to the green anode comprises: applying a non-aqueous liquid electrolyte solution comprising a lithium salt dissolved in an organic solvent to the green anode.
[0050] Embodiment 16. The method according to Embodiment 13, wherein sequentially applying the SEI-generating electrolyte to the green anode comprises applying a non-aqueous liquid electrolyte solution, the non-aqueous liquid electrolyte solution comprising a mixture of lithium salts dissolved in an organic solvent.
[0051] Embodiment 17. The method according to Embodiment 13, wherein sequentially applying the SEI-generating electrolyte to the green anode comprises: applying a non-aqueous liquid electrolyte solution comprising a lithium salt dissolved in a mixture of an organic solvent to the green anode.
[0052] Embodiment 18. The method according to Embodiment 13, wherein sequentially applying the SEI-generating electrolyte to the green anode comprises: applying a non-aqueous liquid electrolyte solution comprising a plurality of lithium salts dissolved in a mixture of organic solvents to the green anode.
[0053] Option 19. A method according to Option 13, wherein sequentially applying the SEI-generating electrolyte to the raw anode includes applying a non-aqueous liquid electrolyte solution, wherein the non-aqueous liquid electrolyte solution includes one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide dissolved in an organic solvent.
[0054] Embodiment 20. The method according to embodiment 13 further includes performing a drying step after each sequential application of the SEI-forming electrolyte.
[0055] The above summary is not intended to represent every possible embodiment or every aspect of the present disclosure. On the contrary, the above summary is intended to illustrate some of the novel aspects and features disclosed herein. The above features and advantages and other features and advantages of the present disclosure will be apparent from the following detailed description of representative embodiments and modes for implementing the present disclosure when combined with the accompanying drawings and the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] One or more embodiments will now be described by way of example with reference to the accompanying drawings, in which:
[0057] Figure 1 and Figure 2 schematically illustrates a battery cell according to the present disclosure; and
[0058] Figure 3 and Figure 4 Schematically illustrates a method for manufacturing a reference Figure 1 and Figure 2 Elements of the SEI formation process of the battery anode of the battery cell.
[0059] The drawings are not necessarily drawn to scale and may present somewhat simplified representations of various preferred features of the present disclosure as disclosed herein, including, for example, specific dimensions, orientations, locations, and shapes. The details associated with such features will be determined in part by the specific intended application and use environment. DETAILED DESCRIPTION
[0060] As described and illustrated herein, the components of the disclosed embodiments may be arranged and designed according to a variety of different configurations. Therefore, the following detailed description is not intended to limit the scope of the present disclosure as claimed, but merely represents possible embodiments thereof. In addition, although many specific details are set forth in the following description in order to provide a thorough understanding of the embodiments disclosed herein, certain embodiments may be practiced without some of these details. In addition, for clarity, certain technical materials understood in the relevant technical field are not described in detail to avoid unnecessarily obscuring the present disclosure.
[0061] An electrochemical cell, or battery cell, includes an anode and a cathode, an electrolyte, and a separator assembled in a container. Electrochemical cells can be electrically connected into stacks to increase overall output, such as into lithium-ion battery packs.
[0062] Lithium-ion electrochemical cells operate by reversibly transferring lithium ions between an anode and a cathode with a separator and an electrolyte disposed therebetween. The electrolyte is used to conduct the lithium ions and may be in the form of a liquid, gel or solid. The lithium ions move from the cathode to the anode during charging of the battery and move in the opposite direction when discharging the battery.
[0063] The anode and cathode are each electrically connected to a current collector, which can be a metal, such as copper for the anode and aluminum for the cathode. During use of the battery, the current collectors associated with the anode and cathode are connected by an external circuit that allows an electrical current generated by electrons to pass between the negative electrode and the positive electrode to compensate for the transport of lithium ions.
[0064] The electrodes can be incorporated into various commercial battery designs, such as prismatic cells, wound cylindrical cells, coin cells, pouch cells or other suitable battery shapes. These batteries can include a single electrode structure for each polarity or a stacked structure having multiple positive and negative electrodes assembled in parallel and / or series electrical connections. In particular, the battery can include a stack of alternating anodes and cathodes with a separator disposed therebetween.
[0065] Referring now to the drawings, which are provided for the purpose of illustrating certain exemplary embodiments and not for the purpose of limiting these exemplary embodiments, Figure 1 and Figure 2 A lithium-ion battery cell 10 is schematically illustrated and includes a battery anode 12, a cathode 20, a battery electrolyte 26 disposed between the battery anode 12 and the cathode 20, and a separator 28. The battery anode 12, cathode 20, and battery electrolyte 26 are enclosed in a container 30, which may be, for example, a hard (e.g., metal) casing or a soft (e.g., polymer) bag. The battery anode 12 and cathode 20 are located on opposite sides of a separator 28, which is a microporous device made of a polymer or other material that is capable of conducting lithium ions and, in one embodiment, is capable of conducting the battery electrolyte 26. The battery electrolyte 26 is a liquid electrolyte that includes one or more lithium salts dissolved in a non-aqueous solvent that has been specifically formulated and prepared for use in the lithium-ion battery cell 10. The battery anode 12 includes an anode current collector 14 to which an electroactive material 16 is applied. In one embodiment, the electroactive material 16 is a lithium intercalation matrix material. Details of forming the battery anode 12 are described in detail in detail in the accompanying drawings. Figure 3 . Cathode 20 includes a cathode current collector 22 having an active material 24 applied thereto. For example, the active material may be a lithium metal oxide active material. For example, active material 24 is capable of storing lithium ions at a higher potential than electroactive material 16. Anode current collector 14 and cathode current collector 22 are connected by an interruptible external circuit 40 that allows current to pass between the battery anode 12 and cathode 20 to electrically balance the migration of lithium ions.
[0066] If specific reference Figure 2 As shown, the anode current collector 14 includes an electroactive material 16 which is a carbon layer deposited on one face with a solid electrolyte interface (SEI) layer 18 formed thereon. The anode current collector 14 and the electroactive material 16 form a raw anode 15 .
[0067] The green anode 15 includes an anode current collector 14 made of copper having a thickness of 4um-25um. The electroactive material 16 can be a single-sided layer (as shown) or a double-sided layer, wherein the layer is 50um-200um thick. The electroactive material 16 is composed of an active material, a binder, a conductive additive, and other additives. The green anode 15 can be manufactured by slurry casting, drying process, or another electrode manufacturing process, but is not limited.
[0068] The SEI layer 18 is formed on the green anode 15 by sequentially applying a plurality of SEI-generating electrolytes to the electroactive material 16 of the green anode 15 to form the battery anode 12. After non-destructive quality testing, the battery anode 12 is assembled into the battery cell 10. The process of sequentially applying a plurality of SEI-generating electrolytes to the electroactive material 16 of the green anode 15 to form the battery anode 12 may include, in one embodiment, applying one SEI-generating electrolyte to the electroactive material 16 of the green anode 15 multiple times, and removing the green anode 15 during interim periods, and in some embodiments removing residues and allowing the green anode to rest and / or dry.
[0069] Alternatively, the process of sequentially applying multiple SEI-forming electrolytes to the electroactive material 16 of the raw anode 15 to form the battery anode 12 may include: in one embodiment, sequentially applying different SEI-forming electrolytes to the electroactive material 16 of the raw anode 15, removing the raw anode 15 during intermediate periods, and in some embodiments, removing residues and allowing the raw anode to rest and / or dry to avoid side reactions between SEI-forming electrolytes, avoid cross-contamination of subsequently used SEI-forming electrolytes, and avoid dilution of subsequently used SEI-forming electrolytes.
[0070] In this way, the SEI layer 18 can be multi-layered, having different components that gradually grow onto the green anode 15 in different amounts. In addition, the formation of the SEI layer 18 can be accelerated by using a specific SEI generating electrolyte, such as a low viscosity electrolyte. In addition, a high viscosity electrolyte can be used to improve the formation of the SEI layer 18, but avoid the concerns associated with wetting the separator 28. In addition, incompatible solvents and salts can be used in different steps of the SEI formation process 300 to obtain the best SEI quality. In addition, the battery electrolyte 26 selected for use in the battery cell can be designed and customized specifically for the battery cell operation, and have a different chemical composition than the SEI generating electrolyte.
[0071] The SEI formation electrolyte may be one or more of a non-aqueous liquid electrolyte solution comprising a lithium salt and an organic solvent. This includes one or more lithium salts dissolved in one or a mixture of organic solvents. In certain variations, an aqueous solvent (ie, a water-based solvent) or a mixed solvent (eg, a non-aqueous solvent system comprising at least 1% by weight of water) may also be used in the SEI formation electrolyte.
[0072] Alternatively, other SEI-generating electrolytes may be employed, either in liquid or gel form, which are capable of conducting lithium ions between the anode and the lithium source prior to the SEI.
[0073] Examples of lithium salts that may be used include one or more of the following: lithium hexafluorophosphate (LiPF6); lithium perchlorate (LiClO4); lithium tetrachloroaluminate (LiAlCl4); lithium bis(oxalato)borate (LiB(C2O4)2) (LiBOB); lithium nitrate (LiNO3), lithium bis(trifluoromethanesulfonyl imide) (LITFSI) (LiN(CF3SO2)2); lithium fluorosulfonyl imide (LiN(FSO2)2) (LIFSI) or others, without limitation.
[0074] Examples of organic solvents may include: dimethyl ether, dimethyl carbonate (DMC), dimethoxyethane (DME, such as 1,2-dimethoxyethane), 1-2-diethoxyethane, 1,3-dimethoxypropane (DMP), 2-methyltetrahydrofuran, ethylene carbonate (EC), propylene carbonate, butyl carbonate, diethyl carbonate, ethyl methyl carbonate (EMC), combinations thereof, or others, without limitation. In certain variations, the SEI-generating electrolyte may include a solvent mixture, such as EC:DMC = 1:1.
[0075] Reference now Figure 3 and Figure 4 , continue to refer to Figure 1 and Figure 2 , showing one embodiment of an SEI formation process 300, which illustrates a process for manufacturing a battery anode 12 by forming an SEI layer 18 onto a green anode 15 prior to assembling the battery anode 12 into a battery cell 10. The SEI layer 18 is formed on the electroactive material 16 of the green anode 15. The SEI layer 18 is formed on the green anode 15 by sequentially applying a plurality of SEI-forming electrolytes to the electroactive material 16 of the green anode 15 (steps 302 to 312). The resulting battery anode 12 produced by forming the SEI layer 18 on the green anode 15 is subjected to testing (step 314) and subsequently assembled into a battery cell (step 316), wherein the battery cell includes a cathode and a separator. Prior to sealing (step 320), the battery electrolyte 26 (also shown as Figure 4 Elements 404 in ) are introduced into the battery cell (step 318).
[0076] Fabricating a battery anode 12 for a lithium-ion battery cell 10 includes forming a solid electrolyte interface (SEI) layer 18 on the electroactive material 16 of the raw anode 15. This includes forming a first SEI-forming electrolyte 401 ( Figure 4 ) is applied to the electroactive material 16 of the green anode 15 (step 302), thereby forming a first intermediate anode. Figure 44 is shown as element 411. The first SEI formation electrolyte 401 is a first non-aqueous liquid electrolyte solution, which includes a lithium salt or a mixture of lithium salts dissolved in an organic solvent. The first SEI formation electrolyte can be applied to the electroactive material 16 of the raw anode 15 in the following manner, namely: spraying the first SEI formation electrolyte onto the raw anode 15, immersing the raw anode 15 in a bath containing the first SEI formation electrolyte 401 (as shown in reference Figure 4 As shown), brushing the first SEI-generating electrolyte onto the green anode 15, or by another method.
[0077] The first intermediate anode 411 may be subjected to a post-treatment step (step 304) to remove residues of the first SEI-generating electrolyte and / or allow the first SEI-generating electrolyte to rest and / or dry. This is done under specific conditions to avoid side reactions between the first and second SEI-generating electrolytes, cross-contamination of the subsequently used second SEI-generating electrolyte, and dilution of the subsequently used second SEI-generating electrolyte.
[0078] A second SEI-forming electrolyte 402 is applied to the electroactive material 16 of the first intermediate anode (step 306), thereby forming a second intermediate anode. Figure 4 4. The second SEI formation electrolyte 402 is a second non-aqueous liquid electrolyte solution, which includes a lithium salt or a mixture of lithium salts in an organic solvent. The second SEI formation electrolyte is applied to the electroactive material 16 of the first intermediate anode 411 by spraying the second SEI formation electrolyte onto the first intermediate anode, immersing the first intermediate anode in a bath containing the second SEI formation electrolyte (as shown in reference Figure 4 As shown), brushing the second SEI-generating electrolyte onto the first intermediate anode, or by another method.
[0079] The second intermediate anode 412 may be subjected to a post-treatment step (step 308) to remove residues of the second SEI-generating electrolyte and / or to allow the second intermediate anode 412 to rest and / or dry. This is done under specific conditions to avoid side reactions between the second and third SEI-generating electrolytes, to avoid cross-contamination of the third SEI-generating electrolyte used subsequently, and to avoid dilution of the third SEI-generating electrolyte used subsequently.
[0080] A third SEI-forming electrolyte 403 is applied to the electroactive material 16 of the second intermediate anode (step 310), thereby forming a third intermediate anode. Figure 4The third SEI formation electrolyte is a third non-aqueous liquid electrolyte solution, which includes a lithium salt or a mixture of lithium salts in an organic solvent. The third SEI formation electrolyte is applied to the electroactive material 16 of the second intermediate anode by spraying the third SEI formation electrolyte onto the second intermediate anode, immersing the second intermediate anode in a bath containing the third SEI formation electrolyte (as shown in reference Figure 4 As shown), brushing the third SEI-generating electrolyte onto the second intermediate anode, or by another method.
[0081] The third intermediate anode 413 may be subjected to a post-treatment step (step 312) to remove residues of the third SEI-forming electrolyte and / or allow the third intermediate anode to rest and / or dry. This is done under specific conditions to avoid side reactions between the third electrolyte and subsequent electrolytes such as the battery electrolyte 26, to avoid cross-contamination of subsequently used electrolytes, and to avoid dilution of subsequently used electrolytes.
[0082] Other conditions associated with applying the first, second, and third SEI-forming electrolytes include, in one embodiment, applying the corresponding first, second, or third SEI-forming electrolyte in an inert environment at atmospheric pressure and a temperature in the range of 0° C. to 200° C. for a period of time between 30 seconds and up to 72 hours, wherein the applied potential is 0 V to 10 V, the applied current has a current of 0 to 100 mA / cm at the electrode, and the applied potential is 0 V to 10 V. 2 The applied surface pressure on the anode is 0.05 MPa to 30 MPa, depending on the application-related details of the corresponding first, second or third SEI-forming electrolyte.
[0083] The third intermediate anode 413 is subjected to non-destructive testing (step 314), which may be: X-ray fluorescence (XRF) spectroscopy analysis; optical analysis, in which a laser beam is scanned over the surface of the third intermediate anode 312 while monitoring reflection and / or refraction; or another non-destructive test, which may be used to evaluate quality parameters on the third intermediate anode 413 based thereon, such as the structural integrity of the SEI layer, the consistency of the SEI layer on the surface, the occurrence of defects in the SEI layer, the thickness of the SEI layer, the morphology of the SEI layer, etc.
[0084] Online quality analysis of the anode SEI can be used to identify defects in the SEI layer across the surface of the third intermediate anode 413 before battery assembly, and thus improve the yield rate before battery assembly. The quality of the SEI layer can be monitored in real time, thereby facilitating monitoring and adjustment of the SEI formation process 300.
[0085] When the test indicates that the third intermediate anode 413 does not meet the corresponding requirements for structural integrity, consistency, occurrence of defects, thickness, morphology, etc. (314)(0), the results are analyzed (step 315) to determine whether the problem with the third intermediate anode can be solved by reapplying the third SEI forming electrolyte by repeating steps 310 and 312 (step 315(1)), or whether the third intermediate anode should be removed from the process and recycled (step 322).
[0086] When the test shows that the third intermediate anode meets the requirements (314) (1), the third intermediate anode becomes the battery anode. Figure 4 The battery anode 414 is assembled into a cell pack (step 316), wherein the cell pack includes a cathode 416 and a separator 415. Another electrolyte 404, i.e., a reference Figure 1 The battery electrolyte 26 described above is introduced into the battery pack (step 318) and the battery pack is sealed (step 320). Figure 4 The battery pack in also shows a second anode 418, a second cathode 420 and a second separator 417, which are completely separated by separator 430, which is illustrated to show that two or more layers of batteries having anodes, cathodes and separators can be combined into a finished battery cell pack.
[0087] SEI formation is a complex but critical process in battery manufacturing. SEI forms on the anode and is highly determinative of battery performance. Electrolyte components play a major role in SEI formation. By preparing the battery anode and forming the SEI layer in the manner described herein, partially wetted electrodes and uncontrolled reaction kinetics within the battery cell during high-rate SEI formation, which can lead to lithium plating, electrolyte decomposition and gassing, and other battery cell quality issues caused by SEI formation within the battery, are reduced or avoided.
[0088] Various electrolytes can be formulated and selected based on the application. This includes selecting an SEI-forming electrolyte specifically for forming an SEI layer 18 on the green anode before the anode is assembled in the battery cell, and selecting a battery electrolyte 26 specifically for electrochemical service in use after the anode is assembled in the battery cell.
[0089] The SEI layer can be formed onto the anode prior to cell assembly (either 1-sided or double-sided coating) without reaction constraints that might otherwise be imposed by the cathode or cell stack structure.
[0090] In this way, the formation of the SEI layer on the anode can be individually designed and performed in order to optimize regulation and cell performance.
[0091] In this way, the reactions related to the formation of the SEI layer are mainly completed outside the assembled battery cell, where the formation of the SEI layer is achieved with more precise reaction control and less restriction on reaction kinetics due to the layered structure in the battery. Although the formation of the SEI layer is completed in a layered battery structure, there may be many inhomogeneities along the electrode surface and between electrodes located in different layers in the battery, which is undesirable.
[0092] In this way, in-line quality monitoring can identify defects in the SEI layer before the anode is assembled into a battery cell and thus improve yield both before and after battery assembly.
[0093] Using non-destructive and non-contact diagnostic methods, the quality of the SEI layer can be directly monitored during battery manufacturing. The formation of the SEI layer on the anode can be monitored at different locations on the same anode or between different anodes in the same battery to provide consistent SEI formation quality. Multiple SEI generation electrolyte systems can be used during the formation of the SEI layer to obtain a gradual growth of the SEI layer. Different SEI generation electrolyte systems can be individually designed and used to form the SEI layer on the anode and operate in the battery for a long time.
[0094] In addition, during the formation of the SEI layer, an SEI-generating electrolyte that is incompatible with the cathode chemistry can be used. The formation of the SEI layer on the anode is not affected by the conditions of the cathode, such as slow or improper wetting, limited lithium content, and diffusion restrictions on electrons, heat, and gases. In this way, battery degassing and aging can occur primarily before the battery cell assembly step, thereby avoiding possible gas release within the battery and providing appropriate electrolyte exposure during the reaction.
[0095] The detailed description and drawings or figures are support and description of the present teaching, but the scope of the present teaching is limited only by the claims. Although some best modes and other embodiments for carrying out the present teaching have been described in detail, there are various alternative designs and embodiments for practicing the present teaching defined in the claims.
Claims
1. A method for manufacturing a battery anode for a lithium-ion battery cell, the method include: A solid electrolyte interface (SEI) layer is formed on the green anode, comprising: applying a first electrolyte that forms a solid electrolyte interface to the green anode to form a first intermediate anode; post-treating the first intermediate anode to remove residues of the first electrolyte forming the solid electrolyte interface and / or allowing the first electrolyte forming the solid electrolyte interface to rest and / or dry, thereby avoiding side reactions between the first electrolyte forming the solid electrolyte interface and the second electrolyte forming the solid electrolyte interface, cross contamination of the second electrolyte forming the solid electrolyte interface, and dilution of the second electrolyte forming the solid electrolyte interface; applying a second electrolyte that forms a solid electrolyte interface to the first intermediate anode to form a second intermediate anode; post-treating the second intermediate anode to remove residues of the second electrolyte forming the solid electrolyte interface and / or allowing the second intermediate anode to rest and / or dry, thereby avoiding side reactions between the second electrolyte forming the solid electrolyte interface and the third electrolyte forming the solid electrolyte interface, cross contamination of the third electrolyte forming the solid electrolyte interface, and dilution of the third electrolyte forming the solid electrolyte interface; applying a third electrolyte that generates a solid electrolyte interface to the second intermediate anode to form a third intermediate anode; post-treating the third intermediate anode to remove residues of the third electrolyte that forms the solid electrolyte interface and / or allowing the third intermediate anode to rest and / or dry; Wherein, applying the corresponding first electrolyte for forming a solid electrolyte interface, the second electrolyte for forming a solid electrolyte interface, and the third electrolyte for forming a solid electrolyte interface occurs under the following conditions: in an inert environment at atmospheric pressure at a temperature of 0°C-200°C for a period of 30 seconds to 72 hours, wherein the applied potential is 0V-10V, the applied current has a value of 0-100mA / cm 2 The current surface density is 0.05 MPa to 30 MPa, and the applied surface pressure on the corresponding green anode, the first intermediate anode and the second intermediate anode is 0.05 MPa to 30 MPa; The third intermediate anode is subjected to a non-destructive test, and a quality parameter on the third intermediate anode is evaluated based on the test; When the test indicates that the third intermediate anode does not meet the corresponding requirements for structural integrity, consistency, occurrence of defects, thickness, and morphology, reapplying the third electrolyte that forms a solid electrolyte interface, which includes applying the third electrolyte that forms a solid electrolyte interface to the second intermediate anode to form a third intermediate anode, and performing the post-treatment on the third intermediate anode; and When the test shows that the third intermediate anode has met the requirements, the third intermediate anode becomes the battery anode, wherein the battery anode comprises the green anode having the solid electrolyte interface layer; and The green anode includes a metal strip having an electroactive material deposited on at least one side.
2. The method according to claim 1, in, Applying the first electrolyte that creates a solid electrolyte interface to the green anode includes applying a first non-aqueous liquid electrolyte that includes a first lithium salt dissolved in an organic solvent to the green anode.
3. The method according to claim 2, in, The first electrolyte for generating a solid electrolyte interface comprises a non-aqueous liquid electrolyte solution, wherein the non-aqueous liquid electrolyte solution contains a lithium salt dissolved in an organic solvent, wherein the lithium salt comprises one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide.
4. The method according to claim 1, in, Applying the first electrolyte that creates a solid electrolyte interface to the green anode includes applying a first non-aqueous liquid electrolyte solution including a first mixture of lithium salts dissolved in an organic solvent to the green anode.
5. The method according to claim 1, in, Applying the second electrolyte that creates a solid electrolyte interface to the first intermediate anode includes applying a second non-aqueous liquid electrolyte solution including a second lithium salt dissolved in an organic solvent to the first intermediate anode.
6. The method according to claim 5, in, The second electrolyte for generating a solid electrolyte interface comprises a non-aqueous liquid electrolyte solution, wherein the non-aqueous liquid electrolyte solution contains a lithium salt dissolved in an organic solvent, wherein the lithium salt comprises one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide.
7. The method according to claim 1, in, Applying the solid electrolyte interface-forming electrolyte to the first intermediate anode includes applying a second non-aqueous liquid electrolyte solution including a second mixture of lithium salts dissolved in an organic solvent to the first intermediate anode.
8. The method according to claim 1, in, Applying the solid electrolyte interface-forming third electrolyte to the second intermediate anode includes applying a third nonaqueous liquid electrolyte solution including a third lithium salt dissolved in an organic solvent to the second intermediate anode.
9. The method according to claim 8, in, The third electrolyte for generating a solid electrolyte interface comprises a non-aqueous liquid electrolyte solution, wherein the non-aqueous liquid electrolyte solution contains a lithium salt dissolved in an organic solvent, wherein the lithium salt comprises one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide.
10. The method according to claim 1, in, Applying the third solid electrolyte interface-forming electrolyte to the second intermediate anode includes applying a third non-aqueous liquid electrolyte solution including a third mixture of lithium salts dissolved in an organic solvent to the second intermediate anode.
11. The method according to claim 1, further comprising: include: After applying the first electrolyte that forms the solid electrolyte interface to the green anode, performing a first drying step; After applying the second electrolyte that forms the solid electrolyte interface to the first intermediate anode, performing a second drying step; as well as After applying the third electrolyte forming a solid electrolyte interface to the second intermediate anode, a third drying step is performed.
12. The method according to claim 1, further comprising: include: Assembling the battery anode into a battery pack, wherein the battery pack includes a cathode and a separator; and A battery electrolyte is added to the battery pack prior to sealing, wherein the battery electrolyte has a different chemical composition than the first electrolyte that creates a solid electrolyte interface, the second electrolyte that creates a solid electrolyte interface, and the third electrolyte that creates a solid electrolyte interface.
13. A method for manufacturing a lithium-ion battery cell, method include: The method of claim 1 for producing a battery anode, comprising: sequentially applying a solid electrolyte interface-forming electrolyte to a green anode to form a battery anode having a solid electrolyte interface (SEI) layer; Assembling the battery anode into a battery pack, wherein the battery pack includes a cathode and a separator; and A battery electrolyte is added to the battery pack prior to sealing, wherein the battery electrolyte has a different chemical composition than the solid electrolyte interface-forming electrolyte.
14. The method according to claim 13, in, Only when the solid electrolyte interface layer on the battery anode meets the minimum standard, the battery anode is assembled into the battery pack.
15. The method according to claim 13, in, Sequentially applying the solid electrolyte interface-forming electrolyte to the green anode includes applying a non-aqueous liquid electrolyte solution including a lithium salt dissolved in an organic solvent to the green anode.
16. The method according to claim 13, in, Sequentially applying the solid electrolyte interface-forming electrolyte to the green anode includes applying a non-aqueous liquid electrolyte solution including a mixture of lithium salts dissolved in an organic solvent.
17. The method according to claim 13, in, Sequentially applying the solid electrolyte interface-forming electrolyte to the green anode includes applying a non-aqueous liquid electrolyte solution including a lithium salt dissolved in a mixture of an organic solvent to the green anode.
18. The method according to claim 13, in, Sequentially applying the solid electrolyte interface-forming electrolyte to the green anode includes applying a non-aqueous liquid electrolyte solution including a plurality of lithium salts dissolved in a mixture of organic solvents to the green anode.
19. The method according to claim 13, in, Sequentially applying the electrolyte that forms the solid electrolyte interface to the raw anode includes applying a non-aqueous liquid electrolyte solution, wherein the non-aqueous liquid electrolyte solution includes one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrachloroaluminate, lithium bis(oxalate)borate, lithium nitrate, lithium bis(trifluoromethanesulfonyl imide) or lithium fluorosulfonyl imide dissolved in an organic solvent.
20. The method of claim 13, further comprising performing a drying step after each sequential application of the solid electrolyte interface forming electrolyte.