Resin sheet with trichomes and molded product thereof
The resin sheet with trichomes and a polymer alloy layer addresses the issue of appearance abnormalities by enhancing durability and resistance to sunscreen, ensuring a smooth and resistant surface.
Patent Information
- Application Number
- CN202180009433.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-15
- Filing Date
- 2021-01-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-12
AI Technical Summary
Resin sheets with thermoplastic polyurethane outermost layers suffer from appearance abnormalities such as cracks or wrinkles when exposed to sunscreen, lacking in both light resistance and chemical resistance.
A resin sheet design featuring a surface layer with regularly arranged trichomes and a second layer composed of a polymer alloy of polycarbonate and polyester resins, with thermoplastic polyurethane as the surface layer material, to enhance durability and resistance.
The design provides a resin sheet with improved touch, light resistance, and chemical resistance, preventing cracks and wrinkles even when exposed to sunscreen.
Smart Images

Figure CN114981082B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin sheet having hair-like bodies and a molded product thereof. Background Art
[0002] Conventionally, paper and polymer sheet materials have been used as automobile interior materials or accessory housings, electronic equipment or home appliance housings, wallpaper and other building materials, toy or game machine housings, and components of daily necessities. In addition, as a method for imparting good tactile properties to the surface of a sheet material, for example, Patent Document 1 proposes a resin sheet having hairs regularly arranged on the surface.
[0003] On the other hand, when the composite material is used as an interior product such as an instrument panel or a sheet of an automobile, yellowing due to ultraviolet rays may become a problem.
[0004] Patent Document 1: International Publication No. 2018 / 016562 Summary of the invention
[0005] Problem that the invention aims to solve
[0006] Therefore, as a material having light resistance, a resin sheet using a thermoplastic polyurethane resin as the outermost layer is proposed. However, such a resin sheet is known to have a problem of appearance abnormality such as cracks or wrinkles on the outermost layer when cosmetics such as sunscreen applied to the skin adhere to it.
[0007] The problem to be solved by the present invention is to provide a resin sheet having good touch, light resistance and chemical resistance and a molded product thereof.
[0008] Solutions for solving problems
[0009] That is, the present inventors have studied various means and have found that: a resin sheet having a surface layer having regularly arranged trichomes on one side and a second layer directly laminated on the surface layer, wherein the material of the surface layer, i.e., thermoplastic polyurethane resin, is not changed, and a polymer alloy resin of a polycarbonate resin and a polyester resin is used as the material of the second layer, thereby suppressing the occurrence of cracks or wrinkles even when a sunscreen is applied, thereby completing the present invention.
[0010] The present invention for solving the above-mentioned problems is constituted as follows.
[0011] (1) A resin sheet comprising a surface layer having regularly arranged trichomes on one surface thereof and a second layer directly laminated on a surface of the surface layer opposite to the trichomes, wherein the surface layer comprises a thermoplastic polyurethane resin and the second layer comprises a polymer alloy resin of a polycarbonate resin and a polyester resin.
[0012] (2) The resin sheet according to (1), wherein the thermoplastic polyurethane resin is a resin containing hexamethylene diisocyanate (HDI) and a carbonate polyol as raw materials.
[0013] (3) The resin sheet according to (1) or (2), further comprising a base material layer on the surface of the second layer opposite to the surface on which the surface layer is laminated.
[0014] (4) The resin sheet according to any one of (1) to (3), wherein the average height of the trichomes is 30 μm to 500 μm, the average diameter of the trichomes is 1 μm to 50 μm, and the average interval between the trichomes is 20 μm to 200 μm.
[0015] (5) A molded article, which is a molded article of the resin sheet according to any one of (1) to (4).
[0016] (6) The molded article according to (5), which is molded on the surface of an automobile interior material, an electronic device, an electronic device exterior material, a cosmetic container, or a container member.
[0017] (7) A method for producing a molded article according to (5) or (6), comprising subjecting the resin sheet according to any one of (1) to (4) to vacuum press molding, insert molding, or in-mold molding.
[0018] Effects of the Invention
[0019] According to the present invention, a resin sheet having good touch, light resistance and chemical resistance and a molded product thereof can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic longitudinal sectional view showing the resin sheet according to the first embodiment of the present invention.
[0021] Figure 2 yes Figure 1 Schematic top view of a resin sheet.
[0022] Figure 3 It is a schematic longitudinal sectional view showing a laminated structure of a resin sheet according to a second embodiment of the present invention. DETAILED DESCRIPTION
[0023] Hereinafter, various embodiments of the resin sheet will be described, and then a method for producing the resin sheet will be described. However, when a specific description described in one embodiment is also applicable to other embodiments, the description will be omitted in other embodiments.
[0024] [First embodiment]
[0025] The resin sheet of the first embodiment of the present invention is a resin sheet having a surface layer having regularly arranged trichomes on one surface and a second layer directly laminated on the surface of the surface layer on the opposite side to the trichomes, wherein the surface layer comprises a thermoplastic polyurethane resin, and the second layer comprises a polymer alloy resin of a polycarbonate resin and a polyester resin.
[0026] like Figure 1 As shown in , the trichomes and the surface layer are directly laminated with the second layer. That is, the layer structure of the resin sheet according to the first embodiment has a structure of trichomes and the surface layer / the second layer from top to bottom.
[0027] <Surface layer>
[0028] The surface layer (1a) is a layer that becomes the base of the trichomes, and in the reference numeral 1, it refers to the portion other than the trichomes 1b on the surface. The thickness of the surface layer refers to the thickness from the base of the trichomes to the surface on the opposite side of the surface layer. The average thickness of the surface layer is preferably 15 μm to 1000 μm, and more preferably 150 μm to 800 μm. By setting it to 15 μm or more, the height of the trichomes can be fully developed. In addition, by setting it to 1000 μm or less, the trichomes can be formed efficiently. There is no structural boundary between the surface layer and the trichomes, and a continuous phase can be formed. The so-called no structural boundary means that the surface layer and the trichomes are formed into an integral shape, and there is no structurally clear boundary between them. In addition, the so-called formation of a continuous phase means that there is no joint between the surface layer and the trichomes and it is not discontinuous (becoming a continuous phase). In this respect, it is different from a structure in which trichomes are implanted in the surface layer. The surface layer and the trichomes may have the same composition, and the bonding between the surface layer and the trichomes may include a covalent bond. A covalent bond is a chemical bond formed by sharing an electron pair between two atoms. In thermoplastic resins, which are chain molecules formed by connecting monomers, each polymer is bonded by a covalent bond, which is stronger than a van der Waals bond or a hydrogen bond between polymer molecules.
[0029] In addition, the surface layer and the trichomes may also be derived from a different thermoplastic resin sheet of the same solid. The term "derived from the same solid thermoplastic resin sheet" means, for example, that the trichomes and the surface layer are directly or indirectly obtained based on the same resin sheet.
[0030] In addition, the surface layer and the hair-like bodies can also be formed by the same solid thermoplastic resin sheet. The so-called being formed by the same solid thermoplastic resin sheet means that the hair-like bodies and the surface layer are directly formed by processing one resin sheet.
[0031] Since there is no structural boundary between the surface layer and the trichomes, a continuous phase is formed, thereby suppressing the trichomes from separating from the surface layer due to external stimulation, and a sheet with good touch is obtained. In addition, it can be manufactured with fewer steps than the case of implanting trichomes.
[0032] The surface layer and the trichomes are composed of the same resin composition with thermoplastic resin as the main component. The so-called thermoplastic resin as the main component means that the thermoplastic resin contains 50% by mass or more, preferably 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. As the thermoplastic resin in one embodiment of the present invention, a thermoplastic polyurethane resin can be used. In other embodiments, at least one thermoplastic resin selected from styrene resin, olefin resin, polyvinyl chloride resin, thermoplastic elastomer, and fluorine resin can be further included.
[0033] Thermoplastic polyurethane resin is a resin with isocyanate and polyol as reaction raw materials. As a combination thereof, the isocyanate can be selected from diphenylmethane diisocyanate (MDI) series, H 12 MDI series, hexamethylene diisocyanate (HDI) series, polyol is any combination of polyether series, polyester series, polycarbonate series, and multiple combinations may also be used. In one embodiment of the present invention, a combination of HDI series isocyanate and carbonate series polyol can be used appropriately.
[0034] As the styrene resin, homopolymers or copolymers of styrene monomers such as styrene, α-methylstyrene, p-methylstyrene, dimethylstyrene, p-tert-butylstyrene, chlorostyrene, etc., copolymers of these styrene monomers with other monomers, such as styrene-acrylonitrile copolymers (AS resins), or polymers of the above styrene monomers with other monomers, such as graft polymers graft-polymerized in the presence of diene rubber polymers such as polybutadiene, styrene-butadiene copolymers, polyisoprene, and polychloroprene, such as high-impact polystyrene (HIPS resins), styrene-acrylonitrile graft polymers (ABS resins), etc. can be used. In addition, styrene thermoplastic elastomers can also be used.
[0035] Polyolefin resins refer to resins made of polymers containing α-olefins as monomers, including polyethylene resins and polypropylene resins. As polyethylene resins, high-density polyethylene, low-density polyethylene, linear low-density polyethylene, linear medium-density polyethylene, etc. can be used. In addition, not only monomers, but also copolymers or grafts or blends having these structures can be used. As the latter resin, for example, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylate copolymers, ethylene-methacrylate copolymers, ethylene-vinyl acetate-vinyl chloride copolymers can be cited, and resins having polar groups in polyethylene chains are copolymerized and blended, such as those blended with terpolymers of acid anhydrides.
[0036] In addition, as the polypropylene resin, homopolypropylene, random polypropylene, block polypropylene, etc. can be used. When homopolypropylene is used, the structure of the homopolypropylene can be any one of isotactic, atactic, and syndiotactic. When using random polypropylene, as the α-olefin copolymerized with propylene, it is preferably a carbon number of 2 to 20, and more preferably a carbon number of 4 to 12, for example, ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, and 1-decene can be used. When using block polypropylene, block copolymers (block polypropylene), block copolymers containing rubber components, or graft copolymers can be used. In addition to using these olefin resins alone, other olefin resins can also be used in combination.
[0037] As the polyvinyl chloride resin, a vinyl chloride homopolymer or a copolymer of vinyl chloride and other comonomers can be used. When the polyvinyl chloride is a copolymer, it can be a random copolymer or a graft copolymer. As an example of a graft copolymer, for example, an ethylene-vinyl acetate copolymer or a thermoplastic urethane polymer is used as a main polymer and vinyl chloride is grafted thereon. The polyvinyl chloride of this embodiment means a soft polyvinyl chloride that can be extruded and is a composition containing additives such as a polymer plasticizer. As the polymer plasticizer, a well-known polymer plasticizer can be used, for example, ethylene copolymer polymer plasticizers such as ethylene-vinyl acetate-carbon monoxide copolymer, ethylene-(meth)acrylate-carbon monoxide copolymer, and ethylene-vinyl acetate copolymer with a high vinyl acetate content can be cited as preferred examples.
[0038] Thermoplastic elastomers include those having a structure of combining a soft polymer substance and a hard polymer substance. Specifically, styrene-based elastomers, olefin-based elastomers, vinyl chloride-based elastomers, polyester-based elastomers, and polyamide-based elastomers can be cited. These elastomers can be selected and used from those generally available on the market.
[0039] As fluorine-based resins, homopolymers of vinylidene fluoride and vinylidene fluoride copolymers with vinylidene fluoride as the main component can be used. Polyvinylidene fluoride (PVDF) resin is a crystalline resin showing various crystalline structures such as α-type, β-type, γ-type, and αp-type. As vinylidene fluoride copolymers, for example, vinylidene fluoride-hexafluoropropylene copolymers, vinylidene fluoride-tetrafluoroethylene copolymers, vinylidene fluoride-chlorotrifluoroethylene copolymers, vinylidene fluoride-trifluoroethylene copolymers, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene terpolymers, vinylidene fluoride-chlorotrifluoroethylene-hexafluoropropylene terpolymers, and mixtures of two or more thereof can be cited.
[0040] The melt mass flow rate of the thermoplastic resin at 190° C. to 300° C. is preferably 4 g / 10 minutes or more. By setting it to 4 g / 10 minutes or more, the transferability of the shape of the trichomes can be improved. It should be noted that the melt mass flow rate is a value measured under a load (2.16 kg to 10.0 kg) in a test temperature range of 190° C. to 300° C. in accordance with JIS K 7210.
[0041] Thermoplastic resin can form alloy with each thermoplastic resin in any ratio within the scope that does not hinder the effect of the present invention. Furthermore, other additives may also be contained. As other additives, within the scope that does not hinder the effect of the present invention, colorants such as water-repellent and oil-repellent, pigment, dye may be added; mold release agents such as silicone oil or alkyl ester system; fiber-shaped reinforcing agents such as glass fiber; granular particles such as talcum, clay, silica or flaky particles such as mica as fillers; low-molecular antistatic agents such as salt compounds of sulfonic acid and alkali metals or high-molecular antistatic agents such as polyetheresteramide, flame retardants, antibacterial agents, antiviral agents, thermal stabilizers, etc. may be added. In addition, waste resins produced in the resin sheet manufacturing process may also be mixed and used.
[0042] As water-repellent and oil-repellent, silicon-based water-repellent, carnauba wax, and fluorine-based water-repellent and oil-repellent can be cited. As silicon, organic polysiloxane, dimethyl polysiloxane, methylphenyl polysiloxane, methyl hydrogen polysiloxane, etc. can be cited, among which dimethyl polysiloxane is preferably used. As a commercial product, for example, "Clinbell CB50-PP", "Clinbell CB-30PE", "Clinbell CB-1", "Clinbell CB-50AB" (Fuji Chemical Co., Ltd.) and the like in which silicon is alloyed in a resin can be cited. Carnauba wax can be cited as a commercial product "Carnauba No. 1" (NIKKORICA Co., Ltd.), and the fluorine-based water-repellent and oil-repellent can be cited as a surfactant with a perfluoroalkyl group, and as a commercial product, "Surflon KT-PA" (AGC SEIMI Chemical Co., Ltd.) and the like can be cited. The addition amount of the water-repellent and oil-repellent is preferably 0.5% by mass to 25% by mass. When the content is less than 0.5% by mass, a sufficient water-repellent and oil-repellent effect may not be obtained, and when the content exceeds 25% by mass, moldability may be deteriorated.
[0043] As antistatic agent, polyether ester amide polymer antistatic agent, ion polymer polymer antistatic agent etc. can be cited. Polyether ester amide polymer antistatic agent can be cited as commercially available "Pelestat 230", "Pelestat6500", "Pelectron AS", "Pelectron HS" (made by Sanyo Chemical Co., Ltd.) etc. Ion polymer polymer antistatic agent can be cited as commercially available "Entira SD100", "Entira MK400" (made by Mitsui-DuPont Polychemical Co., Ltd.) etc. The addition amount of antistatic agent is preferably 5% to 30% by mass. When it is less than 5% by mass, it is possible that sufficient antistatic property cannot be obtained, and when it exceeds 30% by mass, the production cost rises.
[0044] As an antibacterial agent, any one of an inorganic system and an organic system can be added. If dispersibility is considered, an inorganic system is preferably used. Specifically, inorganic antibacterial agents of metal ions (Ag, Zn, Cu), shell-burned calcium antibacterial agents, etc. can be cited. As a commercially available product of an inorganic antibacterial agent of metal ions, "Bactekiller BM102VT" (made by Fuji Chemical Co., Ltd.), "Novaron VZF200", "Novaron (AG300)" (made by Toagosei Co., Ltd.), "KM-10D-G", "IM-10D-L" (made by Sinanen Zeomic Co., Ltd.), etc. can be cited. As a shell-burned calcium antibacterial agent, "Scallow" (made by FID Co., Ltd.), etc. can be cited. The addition amount of the antibacterial agent is preferably 0.5% by mass to 5% by mass. When it is less than 0.5% by mass, it is possible that sufficient antibacterial property cannot be obtained, and when it exceeds 5% by mass, the production cost rises.
[0045] As lubricant release agent, alkyl release agents such as aliphatic hydrocarbon compounds, higher fatty acid compounds, higher aliphatic alcohol compounds, fatty acid amide compounds, silicone release agents, fluorine release agents, etc. can be used. When using a release agent, its addition amount is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and further preferably 0.1 to 2 parts by mass in a total of 100 parts by mass with the resin composition. By making the addition amount 0.01 parts by mass or more, the demoulding effect is likely to be reduced, and by making it 5 parts by mass or less, the possibility of seeping out to the surface of the sheet is reduced.
[0046] In addition, a masterbatch prepared by alloying a lubricant and a mold release agent in advance into a thermoplastic resin may also be used. For example, a commercially available masterbatch based on a urethane-based thermoplastic elastomer may include "Wax Master V" (manufactured by BASF Corporation). In consideration of production efficiency, a masterbatch is preferably used. The amount of the masterbatch added is preferably 1 to 8 parts by mass, more preferably 2 to 7 parts by mass, and further preferably 3 to 6 parts by mass in a total of 100 parts by mass of the resin composition.
[0047] <Trichomes>
[0048] The so-called trichomes (1b), such as Figure 1 As shown in , it refers to the part extending from the surface of the surface layer (1a) in a hair-like manner. The trichomes are regularly arranged on the surface of the surface layer. Here, the so-called regular arrangement means that the trichomes are not randomly arranged, that is, they are arranged regularly (for example, at a certain interval) in one direction or two directions. Whether the arrangement of the trichomes is regular is determined by the arrangement state of the roots of the trichomes. In a certain embodiment, the trichomes are located on the surface layer at a specific interval, and the positions of the bottom surfaces of the trichomes are regularly arranged in the longitudinal direction and the transverse direction of the surface layer. In addition, the arrangement form of the trichomes is not particularly limited, and a checkerboard arrangement or a staggered arrangement can be selected in a vertical and horizontal arrangement. By arranging the trichomes regularly on the surface of the surface layer, it is easy to show good touch evenly and without inconsistency. The trichomes are reversed by applying a load such as sliding a finger, and a finger mark that looks different in gloss and color from the surrounding parts can be formed. In addition, the trichomes can be used to achieve a suede-like texture.
[0049] The average height (h) of the trichomes is preferably 30 to 500 μm, more preferably 30 to 250 μm, and even more preferably 30 to 200 μm. When the average height is 30 μm or more, a good touch can be sufficiently ensured, and when the average height is 500 μm or less, a good touch such as a moist feel, a soft feel, and a fluffy feel can be obtained.
[0050] When the trichomes are almost upright with respect to the surface layer, the length from the base to the tip of the trichomes represents the height of the trichomes. On the other hand, when the trichomes are inclined with respect to the surface layer or when the trichomes have a winding portion, the distance from the portion of the trichomes farthest from the surface of the surface layer to the surface of the surface layer is regarded as the height h of the trichomes. In addition, for the distance from the tip of the trichomes to the center of the base, the total value of the intervals subdivided by measuring at multiple points is regarded as the length L of the trichomes.
[0051] The average height and average length of trichomes can be determined by measuring the height and length of trichomes at arbitrary locations on the resin sheet using an electron microscope and image processing software, and using the arithmetic mean of the measured values.
[0052] The average diameter (d) of the trichomes is preferably 1 μm to 50 μm, more preferably 5 μm to 30 μm. By setting the average diameter of the trichomes to 1 μm or more, good touch can be ensured, and by setting the average diameter of the trichomes to 50 μm or less, good touch such as moist feeling, soft feeling, and fluffy feeling can be obtained. The average diameter of the trichomes is determined by measuring the diameter of the middle height (h / 2) of the trichomes at several locations on the resin sheet using an electron microscope and image processing software, and the value is set as the arithmetic mean of the measured values.
[0053] The aspect ratio of the trichomes can be expressed as (average height of the trichomes / average diameter of the trichomes). The aspect ratio of the trichomes is preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 5. By setting the aspect ratio to 2 or more, good touch can be ensured, and by setting the aspect ratio to 20 or less, good touch such as moist, soft, and fluffy feeling can be obtained, and the possibility that the ratio of the height to the length of the trichomes becomes less than a certain level can be reduced.
[0054] On the other hand, the aspect ratio may be based on the average bottom diameter of the trichomes. The average bottom diameter of the trichomes is preferably 10 μm to 150 μm. The average bottom diameter of the trichomes is a value obtained by measuring the intervals between adjacent trichomes at several locations on the resin sheet and using the arithmetic mean of the measured values. The aspect ratio based on the bottom diameter of the trichomes is preferably 1.0 to 10, more preferably 1.0 to 5, and even more preferably 1.0 to 2.5. By setting the aspect ratio to 1.0 or more, good tactile properties can be ensured, and by setting the aspect ratio to 10 or less, not only good tactile properties such as moist, soft, and fluffy feeling can be obtained, but also the possibility of the ratio of the height to the length of the trichomes being below a certain level can be reduced.
[0055] The average interval (t) of the trichomes is preferably 20 μm to 200 μm, more preferably 40 μm to 150 μm. The interval of the trichomes is, for example, Figure 2 As shown in , it means the distance between the center of the base of the trichome and the center of the base of the adjacent trichome. By setting the average interval to 20 μm or more, good touch can be ensured, and by setting it to 200 μm or less, good touch such as moist feeling, soft feeling, and fluffy feeling can be obtained. The average interval between trichomes is a value obtained by measuring the interval between adjacent trichomes at several locations on the resin sheet and using the arithmetic mean of the measured values.
[0056] The shape of the trichome is not particularly limited, but may be a shape that extends in a direction away from the surface layer and gradually tapers as it approaches the tip, or may be a shape that has a bulge formed at the tip. That is, it may be a shape that gradually decreases in cross-sectional area as it leaves the surface layer, and then becomes larger once and then ends. In addition, the shape of the tip of the trichome may be a bud or mushroom shape. In addition, the trichome may have a base end portion extending in a direction away from the surface layer, and a portion extending from the base end portion and bending with a constant curvature or gradually changing the curvature, and may further have a portion rolled into a spiral or swirl shape. In this case, the tip of the trichome may be folded inside. By adopting such a shape, a good touch is exhibited. In addition, by making the bud or mushroom-shaped portion hollow, a better touch is exhibited. When the bud or mushroom shape is formed at the tip of the hair, the ratio of the average diameter of the width of the bud or mushroom shape to the average diameter of the trichome is preferably 1.1 times or more. The height of the bud or mushroom shape is preferably 7 μm or more. The average diameter of the trichomes, the average diameter of the width of the bud-shaped or mushroom-shaped shapes, and the height are measured from electron scanning microscope photographs and are set as values using arithmetic mean values. The trichomes are made of a thermoplastic resin. As the thermoplastic resin, the same resin as that used in the above-mentioned surface layer can be used.
[0057] The thermoplastic resin contained in the surface layer and the trichomes may at least partially form a three-dimensional crosslinked structure (e.g., a three-dimensional network structure). For example, in one embodiment, at least a portion of the trichomes is crosslinked, in another embodiment, the entire surface of the trichomes is crosslinked, and in yet another embodiment, the entire trichomes (from the boundary with the surface layer to the front end) are crosslinked. Examples of methods for forming a crosslinked body include a method of irradiating an electron beam to a surface having trichomes after forming a resin sheet, and a method of adding an organic peroxide and forming the crosslinked body by heating and humidifying during or after molding the resin sheet. Examples of commercially available products of the resin to which an organic peroxide has been added include "Linklon" manufactured by Mitsubishi Chemical Corporation. In this embodiment, it is preferred that the crosslinked body (electron beam crosslinked body) is formed by irradiation with an electron beam.
[0058] <Second floor>
[0059] As the second layer in the resin sheet according to the first embodiment, a thermoplastic resin having excellent adhesion to the surface layer is preferably used, and a resin having a polymer alloy resin of a polycarbonate resin and a polyester resin as a main component can be used. The mass ratio of the polycarbonate resin to the polyester resin is preferably 50:50 to 90:10, more preferably 60:40 to 80:20, and further preferably 65:35 to 75:25.
[0060] Here, the polymer alloy resin refers to a polymer multi-component system, and may be a polymer blend having a certain compatibility through mixing or the like, a block copolymer or a graft copolymer obtained through copolymerization, or a mixture of incompatible resins.
[0061] As polycarbonate resins, those derived from aliphatic dihydroxy compounds or those derived from aromatic dihydroxy compounds can be cited. For example, those derived from aromatic dihydroxy compounds can be preferably used, and those derived from aromatic dihydroxy compounds (bisphenols) in which two aromatic dihydroxy compounds are bonded via a certain bonding group are particularly preferred. These can be produced by a well-known production method of polycondensation of dihydroxy compounds with phosgene or carbonate, and the production method is not limited, and commercially available resins can also be used.
[0062] As the polyester resin, polyethylene terephthalate, polybutylene terephthalate, polyethylene 2,6-naphthalate, polymethylene terephthalate can be used, and as the copolymer component, for example, a polyester resin copolymerized with a diol component such as diethylene glycol, neopentyl glycol, polyalkylene glycol, or a dicarboxylic acid component such as adipic acid, sebacic acid, phthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid can be used.
[0063] In the second layer, other additives may be contained as needed. As other additives, in the scope that does not hinder the effect of the present invention, lubricating materials such as water repellent, oil repellent, pigment, dye, silicone oil or alkyl ester system, fiber-shaped reinforcing agents such as glass fiber, granular particles such as talcum, clay, silica or mica, salt compounds such as sulfonic acid and alkali metals as fillers, low-molecular antistatic agents or polymer antistatic agents such as polyether ester amide, flame retardants, antibacterial agents, antiviral agents, thermal stabilizers, etc. may be added. In addition, the waste resin produced in the resin sheet manufacturing process may also be mixed. In addition, in the present embodiment, in the scope that does not hinder the effect of the present invention, the substrate layer may also partially have a cross-linked structure.
[0064] In the present embodiment, the second layer may partially have a cross-linked structure within a range that does not hinder the effects of the present invention.
[0065] The average thickness of the second layer is preferably 50 to 1500 μm, more preferably 100 to 1000 μm, and even more preferably 150 to 500 μm. When the thickness is 50 μm or more, the film forming process becomes easier, and when the thickness is 1500 μm or less, the production cost can be reduced.
[0066] <Resin Sheet>
[0067] In this embodiment, "tactile properties" refers to the feel of the surface of the resin sheet and the skin feel. Whether the surface of the resin sheet feels comfortable when touched is judged, and if it feels comfortable, the skin feel such as moist, soft, and fluffy is considered good.
[0068] The resin sheet according to one embodiment of the present invention was subjected to a xenon lamp accelerated light fastness tester at a black panel temperature of 63°C and an irradiance of 60 W / m 2 The color difference ΔE* of the resin sheet before and after the test when irradiated for 500 hours is preferably 10 or less, more preferably 5 or less, and further preferably 3 or less. If the color difference ΔE* of the resin sheet is 10 or less, there is little discoloration even when used in a place irradiated with ultraviolet light, and thus it is suitable for use as a car interior material, etc.
[0069] In addition, the resin sheet in one embodiment of the present invention has chemical resistance. The so-called chemical resistance means resistance to specific chemicals. In this embodiment, it means resistance to sunscreen, for example, it means that even if the sunscreen is applied and heated in an oven at 80°C for 4 hours, the occurrence of appearance abnormalities such as cracks or interlayer peeling is suppressed. As long as it is resistant to sunscreen, it is suitable for molding and use on the surface of daily necessities or car interior materials to which the sunscreen may adhere.
[0070] In one embodiment of the present invention, the thickness of the resin sheet refers to the thickness of the sheet obtained by adding the average height of the trichomes, the average thickness of the surface layer, and the average thickness of the second layer. The sheet thickness is preferably 65 μm to 1600 μm, more preferably 115 μm to 1050 μm, and even more preferably 165 μm to 550 μm. By setting the thickness to 65 μm or more, a good touch can be sufficiently ensured, and by setting the thickness to 1600 μm or less, the manufacturing cost can be reduced.
[0071] [Second Embodiment]
[0072] As an example of the resin sheet involved in the second embodiment of the present invention, Figure 3 As shown in the figure, the resin sheet has a base layer (3) formed on the surface of the second layer (2) opposite to the surface on which the surface layer (1) is laminated. That is, the layer structure of the resin sheet involved in the second embodiment is, from top to bottom, the hair-like body and the surface layer (1), the second layer (2), and the base layer (3).
[0073] Here, since the trichomes are the same as those described in the first embodiment, the description thereof will be omitted. However, the thickness of the trichomes and the surface layer represented by the sum of the average height of the trichomes and the average thickness of the surface layer is preferably 150 μm to 1500 μm, more preferably 150 μm to 1050 μm, and further preferably 150 μm to 500 μm. By setting the thickness to 150 μm or more, good tactile properties can be ensured, and by setting the thickness to 1500 μm or less, production costs can be reduced.
[0074] The material of the second layer is the same as that described in the first embodiment, and thus its description is omitted. The thickness of the second layer is preferably 5 μm to 50 μm, more preferably 7 μm to 30 μm, and further preferably 8 μm to 20 μm.
[0075] <Base material layer>
[0076] As the base layer in the resin sheet according to the second embodiment, a thermoplastic resin having excellent adhesion to the second layer is preferably used, and a resin containing acrylonitrile-ethylene-propylene-diene-styrene (AES) resin as a main component can be used.
[0077] In addition, thermoplastic resins such as styrene resins, olefin resins, polyester resins, nylon resins, acrylic resins, and thermoplastic elastomers can be used in any proportions, and those alloyed with polycarbonate resins can be particularly preferably used. The mass ratio is preferably 99:1 to 20:80, more preferably 80:20 to 30:70, and further preferably 60:40 to 40:60. In addition, when laminating, there is lamination by coextrusion molding, or lamination by extrusion lamination molding using an unstretched film or a biaxially stretched film, or dry lamination molding.
[0078] As nylon-based resins, lactam polymers such as caprolactam and laurolactam; polymers of aminocarboxylic acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid; aliphatic diamines such as hexamethylenediamine, decamethylenediamine, dodecamethylenediamine, 2,2,4- or 2,4,4-trimethylhexamethylenediamine; alicyclic diamines such as 1,3- or 1,4-bis(aminomethyl)cyclohexane and bis(p-aminocyclohexylmethane); diamine units such as aromatic diamines such as m- or p-phenylenediamine; condensation products of dicarboxylic acid units such as aliphatic dicarboxylic acids such as adipic acid, suberic acid, and sebacic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid, and copolymers thereof, etc. can be used. For example, there are nylon 6, nylon 9, nylon 11, nylon 12, nylon 66, nylon 610, nylon 611, nylon 612, nylon 6T, nylon 6I, nylon MXD6, nylon 6 / 66, nylon 6 / 610, nylon 6 / 6T, nylon 6I / 6T, etc. Among them, nylon 6 and nylon MXD6 are preferred.
[0079] As long as it is a vinyl polymer based on a methacrylate monomer, it can be used as an acrylic resin, and its structure is not particularly limited. As methacrylate monomers, for example, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate and hexyl methacrylate can be cited. In addition, the alkyl groups such as propyl, butyl, pentyl and hexyl in the methacrylate monomer can be straight chains or branched. The methacrylate resin can be a homopolymer of a methacrylate monomer or a copolymer of multiple methacrylate monomers, and can also have monomer units of ethylene, propylene, butadiene, styrene, α-methylstyrene, acrylonitrile and acrylic acid, etc., which are well-known vinyl compounds other than methacrylate.
[0080] In the substrate layer, other additives may be contained as needed. As other additives, in the scope that does not hinder the effect of the present invention, lubricating materials such as water repellent, oil repellent, pigment, dye, silicone oil or alkyl ester system, fiber-shaped reinforcing agents such as glass fiber, granular particles such as talcum, clay, silica or mica, salt compounds of sulfonic acid and alkali metals etc. as fillers, low molecular antistatic agents or high molecular antistatic agents such as polyether ester amide, ultraviolet light absorbers, flame retardants, antibacterial agents, antiviral agents, thermal stabilizers etc. may be added as colorants such as water repellent, oil repellent, pigment, dye, silicone oil or alkyl ester system, etc. additives such as flaky particles, sulfonic acid and alkali metal etc. etc. may be added. In addition, the waste resin produced in the resin sheet manufacturing process may also be mixed. In addition, in the present embodiment, in the scope that does not hinder the effect of the present invention, the substrate layer may partially have a cross-linked structure.
[0081] In addition, in the present embodiment, the base material layer may partially have a crosslinked structure within a range not hindering the effects of the present invention.
[0082] In this embodiment, the average thickness of the substrate layer is preferably 50 to 1500 μm, more preferably 100 to 1000 μm, and further preferably 150 to 500 μm. When the thickness is 50 μm or more, the film forming process becomes easy, and when the thickness is 1500 μm or less, the production cost can be reduced.
[0083] [Manufacture of resin sheet]
[0084] The method for producing the resin sheet according to the present invention is not limited and may be produced by any method, but typically includes the steps of melt-extruding a raw material resin and providing regularly arranged hair-like bodies on at least one surface of the obtained extruded resin sheet.
[0085] When making a multilayer resin sheet, any resin sheet molding method can be used. For example, a feed block or a multi-manifold die can be used. In addition, the layer structure of each embodiment of the resin sheet of the present invention is basically as described above. In addition, for example, as long as no deterioration of physical properties is observed, waste raw materials generated in the manufacturing process of the resin sheet or molded container of the present invention can be added to the base material layer or laminated as another layer.
[0086] The method of imparting trichomes is not particularly limited, and any method known to those skilled in the art can be used. For example, a method of manufacturing using an extrusion molding method, a method of manufacturing using a roll-to-roll method, a method of manufacturing using a photolithography method, a method of manufacturing using a hot press method, a method of manufacturing using a pattern roll and a UV curable resin, a method of manufacturing using a 3D printer, a method of embedding trichomes in a resin layer and then covalently bonding them through a polymerization reaction, etc.
[0087] For example, when using the extrusion molding method, the resin sheet of the present invention can be manufactured by extruding the resin sheet by a T-die method, and casting it with a transfer roll and a touch roll having a concave-convex processing so as to give the trichome shape to the surface of the resin sheet.
[0088] As a transfer roller that has been processed with concave and convex parts, a roller surface that is regularly provided with fine concave and convex parts of several μm to several hundred μm in size by laser engraving, electroforming, etching, steel core engraving, etc. can be used. Here, the so-called regular means that the concave and convex parts are arranged in a non-random manner, that is, they are arranged neatly in one direction or two directions. As the configuration of the concave and convex parts in a certain embodiment, a checkerboard configuration or a staggered configuration in a vertical and horizontal configuration can be selected. As the shape of the concave and convex part, for example, if it is the shape of the concave part, a cone (cone, quadrangular pyramid, triangular pyramid, hexagonal pyramid, etc.), a semicircle, a rectangle (quadrangular prism), etc. can be cited. As a size, the opening diameter of the concave part, the depth of the concave part, and the interval of the concave part shape are several μm to hundreds of μm. As the material of the transfer roller, for example, metal, ceramic, etc. can be used. The interval between the trichomes can be adjusted by adjusting the interval between the concave parts of the transfer roller, and the height of the trichomes can be adjusted by adjusting the depth of the concave parts of the transfer roller, and the touch can also be adjusted thereby.
[0089] In addition, it is preferred to perform high aspect ratio concave-convex processing on the transfer roller surface. For example, the aspect ratio (concave depth / concave opening diameter) when processing the concave shape on the transfer roller surface is preferably 1.0 to 9.0. In order to perform high aspect ratio concave-convex processing on the transfer roller surface, laser engraving or electroforming is particularly preferred because it is suitable for precision processing in the depth direction compared to etching, sandblasting, steel core engraving, etc.
[0090] As the material of the transfer roller, for example, metal, ceramic, etc. can be used. On the other hand, as the contact roller, various materials can be used, for example, a roller made of silicone rubber, NBR rubber, EPT rubber, butyl rubber, chloroprene rubber, or fluororubber can be used. In one embodiment, a contact roller with a rubber hardness (JIS K 6253) of 40 to 100 can be used. In addition, a Teflon (registered trademark) layer can also be formed on the surface of the contact roller.
[0091] As the contact roller, various materials can be used, for example, a roller made of silicone rubber, NBR rubber, EPT rubber, butyl rubber, chloroprene rubber, or fluororubber can be used. In one embodiment, a contact roller having a rubber hardness (JIS K 6253) of 40 to 100 can be used. In addition, a Teflon (registered trademark) layer can also be formed on the surface of the contact roller.
[0092] The resin sheet of this embodiment can be produced by using the roller group of the transfer roller and the touch roller.
[0093] In one embodiment, the temperature of the transfer roller is adjusted to a temperature near the crystal melting temperature, glass transition temperature or melting point of the thermoplastic resin (for example, 100 to 150° C. when random polypropylene is used), and the pinch pressure between the transfer roller and the contact roller is set to 30 to 120 kg / cm 2 The resin sheet of the present embodiment can be produced by casting. The cast resin sheet is pulled at a line speed of 0.5 to 30 m / min using a pinch roll or the like.
[0094] In addition, although the above-mentioned embodiment has been specifically described, it is not limited to these.
[0095] [Molding products]
[0096] The molded product of the present invention is a molded product using the resin sheet of the present invention. The resin sheet of the present invention can correspond to general molding. As a molding method, in addition to insert molding and in-mold molding, there are also general vacuum molding and pressure molding. As applications of these, there can be cited a method of heating and softening the resin sheet in a vacuum state, opening it under atmospheric pressure and covering (molding) it on the surface of an existing molded product, etc., but it is not limited to these. In addition, as a method for heating and softening the sheet before molding, well-known sheet heating methods such as radiation heating by non-contact heating infrared heaters can be used. In a vacuum pressure molding of a certain embodiment, for example, the resin sheet is heated at a surface temperature of 60°C to 220°C for 20 seconds to 480 seconds, and then molded to the surface of an existing molded product. Depending on the shape of the surface, it can be stretched to 1.05 to 2.50 times.
[0097] [thing]
[0098] The resin sheet having hair-like bodies on the surface according to the present invention can be used for applications requiring the good touch properties described above. For example, the resin sheet of the present invention can be used as an automobile interior material, an electronic device, an electronic device exterior material, a cosmetic container or a container member, a stationery member, a lighting fixture member, and a daily necessities member.
[0099] As the automobile interior material, as the part that the hand touches in the automobile, a steering wheel, an instrument panel, a joystick, a switch, etc. can be cited. For example, the interior material that the above-mentioned resin sheet is molded and laminated on the surface of the well-known instrument panel, a pillar (such as Japanese Patent Gazette No. 2009-184421) can be cited. By laminating the resin sheet, it can become an interior material that is given good tactility. As the material of the laminated resin sheet, considering light resistance and chemical resistance, olefin resin, vinyl chloride resin, and urethane elastomer are preferred. The method of laminating the resin sheet and the interior material is not particularly limited.
[0100] As the outer covering material of electronic equipment, there can be cited the signaling machine housing of the keyless entry system, the housing of a smart phone, the protective shell of a smart phone (smartphone case), the housing of a music player, the housing of a game console, the housing of a digital camera, the housing of an electronic notebook, the housing of an electronic calculator, the housing of a tablet computer, the housing of a portable personal computer, a keyboard, a mouse, etc. For example, there can be cited a portable signaling machine in which the resin sheet of the present invention is molded and bonded to the surface of the housing of the portable signaling machine of the well-known keyless entry system (e.g., Japanese Patent Gazette No. 2005-228911). By bonding the resin sheet, a portable signaling machine having good tactile properties can be obtained. As the material of the bonded resin sheet, olefin resins and urethane elastomers are preferred. There is no particular limitation on the method of bonding the resin sheet to the housing.
[0101] As cosmetic container components, containers for face cream, dressing cream, foundation, and eye shadow can be cited, for example, a cosmetic container in which the resin sheet of the present invention is molded and bonded to the surface of the cover member of the well-known foundation container (Japanese Patent Publication No. 2017-29608) can be cited. By bonding the resin sheet, a cosmetic container with good tactility can be obtained. As the material of the bonded resin sheet, olefin resins and urethane elastomers are preferred. There is no particular limitation on the method of bonding with the resin sheet.
[0102] As stationery components, book covers, notebook covers, pencil case covers, etc. can be cited. For example, the sheet of the present invention can be used to make well-known book covers (such as Japanese Patent Publication No. 2007-246122) to give good tactile properties and waterproof book covers. In addition, the form of the book cover is not particularly limited. As the material of the sheet, olefin resins and urethane elastomers are preferred. The method of using the resin sheet to make is not particularly limited.
[0103] As lighting equipment components, there can be cited lighting equipment for indoor use or in-vehicle use, for example, a lighting device in which the resin sheet of the present invention is molded and bonded to the surface of a cover member of a well-known LED lighting device. By bonding the resin sheet, an LED lighting device having good tactile properties and light diffusion properties can be obtained. As the material of the bonded resin sheet, olefin resins and fluorine resins are preferred. There is no particular limitation on the method of bonding the resin sheet.
[0104] As components of daily necessities, toilet articles, indoor mats, table sheets, etc. can be cited. For example, a toilet device can be cited in which the resin sheet of the present invention is molded and bonded to the surface of the toilet seat component of the toilet device. By bonding the resin sheet, a toilet device with a toilet seat having good tactile properties can be obtained. As the material of the bonded resin sheet, olefin resin, vinyl chloride resin, fluorine resin is preferred. There is no particular limitation on the method of bonding the resin sheet.
[0105] Furthermore, a trichome sheet having characters or patterns printed on the surface of the trichome by a general printing method (offset printing, gravure printing, flexographic printing, screen printing, hot stamping, etc.) can be prepared and applied to the above-mentioned uses. The material of the printed resin sheet is not particularly limited, but it is preferably considered to have printability comparable to the ink used for printing.
[0106] In addition, the resin sheet of the present invention can be laminated (dry lamination, extrusion lamination) with printed materials (paper, metal film, etc.) printed with text, patterns, etc., non-woven fabrics, etc. to form a laminated body, for example, laminated on the printed surface of a business card to produce a business card with tactile properties. The material of the laminated resin sheet is not particularly limited.
[0107] Example
[0108] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the contents of Examples and the like.
[0109] Various raw materials used in Examples and the like are shown below.
[0110] (1) Trichomes and surface layer
[0111] (A-1) TPU (urethane elastomer) "XN2001: HDI / polycarbonate" (manufactured by Tosoh Corporation)
[0112] (A-2) TPU (urethane elastomer) "A3085A10: HDI / polycarbonate" (manufactured by BASF)
[0113] (A-3) TPU (urethane elastomer) "ET880: MDI / polyether" (manufactured by BASF)
[0114] (B) Release agent masterbatch "Wax Master V" (manufactured by BASF)
[0115] (2) Second layer
[0116] (C-1) PC / polyester "SP3002" (manufactured by Sumika Polycarbonate Co., Ltd.)
[0117] (C-2) AES "Unibrite UB-311" (made by A&L Co., Ltd., Japan)
[0118] (C-3) PC / AES "Techniace W-101" (made by A&L Co., Ltd., Japan)
[0119] ·(C-4)ABS "DENKA ABS GT-R-61A" (manufactured by DENKA Co., Ltd.)
[0120] (3) Base material layer
[0121] (D-1) AES "Unibrite UB-311" (made by A&L Co., Ltd., Japan)
[0122] The methods for evaluating various properties of the resin sheets produced in Examples and Comparative Examples and the molded products obtained by vacuum pressure molding of the resin sheets are as follows.
[0123] (1) Average height of trichomes, average length of trichomes, average diameter of trichomes, average spacing between trichomes, average thickness of surface layer
[0124] The height (h) of the trichomes, the diameter (d) of the trichomes, the interval (t) between the trichomes, and the thickness of the surface layer of the resin sheet were measured using a laser microscope (VK-X100, manufactured by KEYENCE). The sample to be measured was cut into cross-sections from any three locations of the resin sheet using a microtome. The average height of the trichomes was measured for each sample, and the arithmetic mean of the 30 measured values was used. The average diameter of the trichomes was measured for each sample at the middle height (h / 2) of 10 trichomes, and the arithmetic mean of the 30 measured values was used. The average interval between the trichomes was measured for each sample at 10 locations between the center of the root of the trichomes and the center of the root of the adjacent trichomes, and the arithmetic mean of the 30 measured values was used. The average thickness of the surface layer was measured for each sample at 10 locations from the root of the trichomes to the other layer interface, and the arithmetic mean of the 30 measured values was used.
[0125] (2) Good tactile sensory evaluation
[0126] Good tactile properties A total of 10 people, 5 men and 5 women, were asked to touch the resin sheet for sensory evaluation. The specific tactile feeling (smoothness, moist feeling, etc.) when touching the surface of the resin sheet was evaluated, and the tactile feeling felt by the largest number of people was regarded as the tactile feeling of the resin sheet surface.
[0127] (3) Light resistance test
[0128] The thermoplastic resin raw material of the trichomes and the surface layer was made into a sheet with a thickness of about 0.3 mm by a hot press, and irradiated for 500 hours at a black panel temperature of 63±3°C and an irradiation intensity of 60 W / m2 using a xenon lamp accelerated light fastness tester (xenon lamp weathering tester, SUGA Test Co., Ltd.), and the color difference (transmittance method) ΔE* of the sheet before and after the test was measured using a colorimeter Color meter ZE6000 (manufactured by Nippon Denshoku Industries).
[0129] (4) Chemical resistance test
[0130] Evenly apply 0.5 g of commercially available sunscreen on a 50 mm x 50 mm section of the resin sheet. Place it in an oven at 80°C for 4 hours. Take out the resin sheet, rinse the surface with water, visually observe the state of the section coated with the sunscreen, and evaluate the resistance to the sunscreen using the following standards. Neutrogena's "UltraSheer Dry-touch Sunscreen SPF 45" (containing 3% avobenzone, 10% homosalate, 5% octisalate, 2.8% octocrylene, and 6% phenol) was used as the sunscreen.
[0131] ○: Although slight cracks, wrinkles, swelling, peeling, etc. were observed in a part of the tested portion, the appearance had no practical problem.
[0132] △: Slight cracks, wrinkles, swelling, peeling, etc. were observed in the entire tested portion, and the appearance was poor, which was problematic in practical use.
[0133] ×: Cracks, wrinkles, swelling, peeling, etc. were observed in part of the tested portion, and the appearance was problematic in practical use.
[0134] (5) Evaluation of excipient properties
[0135] The resin sheet was heated in a vacuum atmosphere using a double-sided vacuum forming machine (NGF-0709-S, manufactured by Fuse Vacuum Co., Ltd.), and then the surface of a smartphone cover prepared in an atmospheric pressure atmosphere was vacuum-pressed to form a molded product. The sheet was heated for 40 to 300 seconds at a surface temperature of 80 to 220°C, and stretched to 1.5 times at the most stretched part.
[0136] Evaluation of the shaping property The sheet followability on the side of the smartphone case was evaluated by appearance. As the evaluation criteria, the case where the sheet could follow was marked as ○, and the case where the sheet could not follow (the case where there was a gap between the smartphone case and the sheet) was marked as ×.
[0137] The heights of 10 trichomes before and after molding were measured, and the arithmetic mean of the 30 measured values was used to calculate (average height of trichomes after molding) / (average height of trichomes before molding) as the average trichome height maintenance rate.
[0138] [Examples 1 to 5, Comparative Examples 1 to 3]
[0139] The (A) TPU and (B) release agent masterbatch which form the hair-like body and the surface layer flow out from a 40 mm single screw extruder, and the (C) thermoplastic resin which forms the second layer flows out from a 65 mm single screw extruder. The resin sheet extruded by the T-die method is cast using a transfer roll which is embossed by chromium oxide spraying and laser engraving and adjusted to 60°C to 150°C and a silicone rubber touch roll with a rubber hardness of 70 adjusted to 10°C to 90°C, and is pulled at a linear speed of 1m / min to 15m / min using a pinch roll. Thus, a resin sheet having the composition, thickness and surface shape shown in Table 1 is obtained.
[0140] [Example 6]
[0141] A three-layer resin sheet was obtained by lamination molding, and the surface of the resin sheet was casted by a transfer roll and a touch roll with concave and convex processing by electroforming, and pulled at a line speed of 1 m / min to 15 m / min using a pinch roll. Thus, a three-layer resin sheet having the composition, thickness and surface shape shown in Table 1 was obtained.
[0142] Using the resin sheets obtained in the respective Examples and Comparative Examples, evaluation tests were carried out on various properties. Table 1 shows the results.
[0143] [Table 1]
[0144]
[0145] From the results shown in Table 1, the following can be known.
[0146] All the resin sheets of Examples 1 to 6 satisfied the evaluation criteria for good touch, light resistance, chemical resistance, and shaping. On the other hand, in the chemical resistance test, the thermoplastic polyurethane resin of the surface layer of the resin sheets of Comparative Examples 1 to 3 swelled and easily peeled off from the second layer.
[0147] The shapes of the resin sheets obtained in Examples 1 to 4 were observed using a field emission scanning electron microscope (FE-SEM, JSM-7001F, manufactured by JEOL Ltd.).
[0148] From the scanning electron microscope image, it was observed that the trichomes were not tangled with each other and stretched in a certain direction. In addition, the shape of the trichomes was a shape in which the cross-sectional area gradually decreased as the distance from the surface layer was removed, or a shape in which the cross-sectional area gradually decreased and then expanded and ended. In addition, it was observed that the front end of the trichomes in which the cross-sectional area gradually decreased as the distance from the surface layer was removed and then expanded and ended was a bud-shaped or mushroom-shaped part, and the bud-shaped or mushroom-shaped part was partially hollow. It is speculated that such a shape provides a better touch.
[0149] The present invention has been described above using various embodiments. Of course, the technical scope of the present invention is not limited by the scope described in the above embodiments. It is clear to those skilled in the art that various changes or improvements can be made to the above embodiments. In addition, it is clear from the description of the patent claims that such changes or improvements can also be included in the technical scope of the present invention.
[0150] Description of Reference Numerals
[0151] 1: Trichome and surface layer
[0152] 1a: Surface layer
[0153] 1b: Trichome,
[0154] d: trichome diameter
[0155] h: height of trichomes
[0156] t: spacing of trichomes
[0157] 2: Second layer
[0158] 3: Base material layer
Claims
1. A resin sheet comprising a surface layer having regularly arranged trichomes on one surface, and a second layer directly laminated on the surface of the surface layer opposite to the trichomes, wherein the surface layer comprises a thermoplastic polyurethane resin, and the second layer comprises a polymer alloy resin of a polycarbonate resin and a polyester resin, and the mass ratio of the polycarbonate resin to the polyester resin is 50:50 to 90:
10. 2 . The resin sheet according to claim 1 , wherein the thermoplastic polyurethane resin is a resin containing hexamethylene diisocyanate (HDI) and a carbonate-based polyol as raw materials. 3 . The resin sheet according to claim 1 , further comprising a base material layer on the surface of the second layer opposite to the surface on which the surface layer is laminated. The resin sheet according to any one of claims 1 to 3, wherein the average height of the trichomes is 30 μm to 500 μm, the average diameter of the trichomes is 1 μm to 50 μm, and the average interval between the trichomes is 20 μm to 200 μm. 5 . A molded article, which is a molded article of the resin sheet according to claim 1 . 6 . The molded article according to claim 5 , which is molded on the surface of an automobile interior material, an electronic device, an electronic device exterior material, a cosmetic container, or a container member.
7. A method for producing a molded article according to claim 5 or 6, comprising subjecting the resin sheet according to any one of claims 1 to 4 to vacuum pressure molding, insert molding or in-mold molding.
Citation Information
Patent Citations
Mobile electronic apparatus
JP2005228911A
lid
JP2007246122A
Cover panel
JP2009184421A
Cosmetic container
JP2017029608A
Thermoplastic resin sheet having hairlike body and molded product thereof
WO2018016562A1