Positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
By controlling the proportion of W existing on the surface and inside the secondary particles of the lithium metal composite oxide, the problem of insufficient safety and cycle characteristics of the Ni-Co cathode active material in the battery is solved, and higher cycle characteristics are achieved. and security.
Patent Information
- Application Number
- CN202180009649.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-31
- Filing Date
- 2021-01-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-01-22
Smart Images

Figure CN115004407B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery. Background Art
[0002] In recent years, Ni-Co-based positive electrode active materials with high Ni content have been widely used in high-capacity batteries. Patent Document 1 discloses a technology for suppressing the increase of positive electrode resistance accompanying charge and discharge cycles by attaching a compound containing Li and W to the surface of primary particles of the Ni-Co-based positive electrode active material.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2017 / 018099 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] However, if W is added, the surface reactivity of the positive electrode active material increases, thereby increasing the reactivity with the electrolyte, and batteries using Ni-Co-based positive electrode active materials with a high Ni content may have reduced safety. Patent Document 1 does not consider battery safety, and there is still room for improvement.
[0008] Therefore, an object of the present application is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery that contributes to improvement of cycle characteristics and safety.
[0009] Solutions for solving problems
[0010] The positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present application is characterized in that it comprises a lithium metal composite oxide, wherein the lithium metal composite oxide has secondary particles formed by aggregation of primary particles, and W exists on the surface of the secondary particles of the lithium metal composite oxide and inside the secondary particles. The positive electrode active material for a non-aqueous electrolyte secondary battery is composed of the general formula Li α Ni a Co b Al c M d W e O β(wherein, 0.9≤α≤1.2, 0.8≤a≤0.96, 0<b≤0.10, 0<c≤0.10, 0≤d≤0.1, 0.0003≤e / (a+b+c+d+e)≤0.002, 1.9≤β≤2.1, a+b+c+d=1, M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo and Zn) indicates that, relative to the total amount of W present on the surface of the secondary particles of the lithium metal composite oxide and inside the secondary particles, the proportion of W present on the surface of the secondary particles of the lithium metal composite oxide is 25% to 45%.
[0011] A nonaqueous electrolyte secondary battery as one embodiment of the present application is characterized by comprising a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode contains the positive electrode active material for a nonaqueous electrolyte secondary battery.
[0012] Effects of the Invention
[0013] According to one embodiment of the present application, a nonaqueous electrolyte secondary battery having improved cycle characteristics and safety can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is an axial cross-sectional view of a cylindrical secondary battery as an example of an embodiment. DETAILED DESCRIPTION
[0015] Hereinafter, an example of an embodiment of the non-aqueous electrolyte secondary battery involved in the present application is described in detail. The following example shows a cylindrical battery in which a wound electrode body is housed in a cylindrical battery case, but the electrode body is not limited to the wound type, and may also be a laminated type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated one sheet each through a separator. In addition, the battery case is not limited to a cylindrical shape, and may be, for example, a square, a coin shape, etc., or may be a battery case composed of a laminate sheet including a metal layer and a resin layer.
[0016] Figure 1 It is an axial cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1 In the secondary battery 10 shown, an electrode body 14 and a nonaqueous electrolyte (not shown) are housed in an outer casing 15. The electrode body 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. It should be noted that, in the following, for the sake of convenience, the sealing body 16 side is set as "upper" and the bottom side of the outer casing 15 is set as "lower".
[0017] The open end of the outer body 15 is blocked by the sealing body 16, thereby the interior of the secondary battery 10 is sealed. Insulating plates 17 and 18 are respectively provided above and below the electrode body 14. The positive lead 19 passes through the through hole of the insulating plate 17 and extends upward, and is welded to the lower surface of the filter 22 which is the bottom plate of the sealing body 16. In the secondary battery 10, the cover 26 which is the top plate of the sealing body 16 electrically connected to the filter 22 becomes the positive terminal. On the other hand, the negative lead 20 passes through the through hole of the insulating plate 18 and extends to the bottom side of the outer body 15, and is welded to the bottom inner surface of the outer body 15. In the secondary battery 10, the outer body 15 becomes the negative terminal. It should be noted that when the negative lead 20 is provided at the terminal portion, the negative lead 20 passes through the outside of the insulating plate 18 and extends to the bottom side of the outer body 15, and is welded to the bottom inner surface of the outer body 15.
[0018] The outer body 15 is, for example, a metal outer can in a cylindrical shape with a bottom. A gasket 27 is provided between the outer body 15 and the sealing body 16 to ensure the airtightness of the interior of the secondary battery 10. The outer body 15 has a groove portion 21 for supporting the sealing body 16, which is formed by pressing the side portion from the outside. The groove portion 21 is preferably formed in an annular shape along the circumferential direction of the outer body 15, and supports the sealing body 16 on its upper surface through the gasket 27.
[0019] The sealing body 16 has a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cover 26 stacked in order from the electrode body 14 side. The components constituting the sealing body 16 have, for example, a disc shape or a ring shape, and the components except the insulating member 24 are electrically connected to each other. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective central portions, and an insulating member 24 is sandwiched between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat, for example, the lower valve body 23 breaks, whereby the upper valve body 25 expands toward the cover 26 side and moves away from the lower valve body 23, thereby cutting off the electrical connection between the two. If the internal pressure rises further, the upper valve body 25 breaks, and the gas is discharged from the opening 26a of the cover 26.
[0020] Hereinafter, the positive electrode 11 , the negative electrode 12 , the separator 13 , and the nonaqueous electrolyte constituting the secondary battery 10 , particularly the positive electrode active material contained in the negative electrode mixture layer constituting the positive electrode 11 , will be described in detail.
[0021] [positive electrode]
[0022] The positive electrode, for example, has a positive electrode current collector such as a metal foil, and a positive electrode mixture layer formed on the positive electrode current collector. The positive electrode current collector can use a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, a film having the metal on the surface, etc. The positive electrode mixture layer, for example, includes a positive electrode active material, a binding material, a conductive material, etc. The positive electrode can be made, for example, by applying a positive electrode mixture slurry including a positive electrode active material, a binding material, a conductive material, etc. on a positive electrode core, drying it to form a positive electrode mixture layer, and then rolling the positive electrode mixture layer.
[0023] Examples of the conductive material contained in the positive electrode mixture layer include carbon black (CB), acetylene black (AB), Ketjen black, graphite and other carbonaceous particles, etc. These may be used alone or in combination of two or more.
[0024] As the binder contained in the positive electrode mixture layer, for example, fluorine resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, etc. can be cited. They can be used alone or in combination of two or more.
[0025] The positive electrode active material contained in the positive electrode mixture layer is composed of the general formula Li α Ni a Co b Al c M d W e O β (wherein, 0.9≤α≤1.2, 0.8≤a≤0.96, 0<b≤0.10, 0<c≤0.10, 0≤d≤0.1, 0.0003≤e / (a+b+c+d+e)≤0.002, 1.9≤β≤2.1, a+b+c+d=1, M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo and Zn). The molar fraction of W is 0.03 mol% to 0.2 mol%, preferably 0.04 mol% to 0.1 mol%, relative to the total molar number of metal elements other than Li in the positive electrode active material. Here, the molar fraction of the metal element contained in the positive electrode active material is measured by inductively coupled plasma atomic emission spectrometry (ICP-AES).
[0026] The positive electrode active material includes a lithium metal composite oxide having secondary particles formed by aggregation of primary particles, and W exists on the surface of the secondary particles of the lithium metal composite oxide and inside the secondary particles. Here, W exists inside the secondary particles, which means that W exists between the primary particles constituting the secondary particles.
[0027] The secondary particles of the lithium metal composite oxide are particles having a volume-based median particle size (D50) of preferably 3 μm to 30 μm, more preferably 5 μm to 25 μm, and particularly preferably 7 μm to 15 μm. D50 refers to the particle size at which the cumulative frequency of the volume-based particle size distribution from the side with the smaller particle size becomes 50%, also known as the median diameter. The particle size distribution of the secondary particles of the lithium metal composite oxide can be measured using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by MicrotracBEL Corporation) and water as a dispersion medium.
[0028] The particle size of the primary particles constituting the secondary particles is, for example, 0.05 μm to 1 μm. The particle size of the primary particles is measured as the diameter of a circumscribed circle in a particle image observed by a scanning electron microscope (SEM).
[0029] The lithium metal composite oxide can be prepared by the general formula Li α Ni a Co b Al c M d O β (wherein, 0.9≤α≤1.2, 0.8≤a≤0.96, 0<b≤0.10, 0<c≤0.10, 0≤d≤0.1, 1.9≤β≤2.1, a+b+c+d=1, M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo and Zn). By using a lithium metal composite oxide of the Ni-Co-Al system, the battery can be made high-capacity, and the cation mixing of Ni entering the site of Li can be suppressed. It should be noted that the positive electrode active material may contain lithium metal composite oxides or other compounds other than those represented by the above general formula within the scope that does not impair the purpose of the present application. The molar fraction of the metal element contained in the lithium metal composite oxide is determined by ICP-AES in the same way as the positive electrode active material.
[0030] α, which represents the ratio of Li in the lithium metal composite oxide, preferably satisfies 0.9≤α≤1.2, and more preferably satisfies 0.95≤α≤1.05. When α is less than 0.9, the battery capacity may be reduced compared with the case where α satisfies the above range. When α exceeds 1.2, the charge-discharge cycle characteristics may be reduced compared with the case where α satisfies the above range.
[0031] a, which represents the ratio of Ni to the total molar number of metal elements other than Li in the lithium metal composite oxide, preferably satisfies 0.8≤a≤0.96, and more preferably satisfies 0.88≤a≤0.92. By making a greater than or equal to 0.8, a high-capacity battery is obtained. In addition, by making a less than or equal to 0.96, other elements such as Co and Al can be included, thereby suppressing cation mixing.
[0032] b, which represents the ratio of Co to the total number of moles of metal elements other than Li in the lithium metal composite oxide, preferably satisfies 0<b≤0.10, and more preferably satisfies 0.04≤b≤0.06.
[0033] c, which represents the ratio of Al to the total molar number of metal elements other than Li in the lithium metal composite oxide, preferably satisfies 0<c≤0.10, and more preferably satisfies 0.04≤c≤0.06. It is believed that Al does not undergo an oxidation number change during charge and discharge, so by being included in the transition metal layer, the structure of the transition metal layer is stabilized. When c exceeds 0.10, Al impurities are sometimes generated, and the battery capacity is reduced.
[0034] M (M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo and Zn) is an arbitrary component. d, which represents the ratio of M to the total number of moles of metal elements other than Li in the lithium metal composite oxide, preferably satisfies 0≤d≤0.1.
[0035] The ratio of W present on the surface of the secondary particles of the lithium metal composite oxide relative to the total amount of W present on the surface of the secondary particles of the lithium metal composite oxide and inside the secondary particles (hereinafter referred to as the W surface presence ratio) is 25% to 45%. By setting the W surface presence ratio to this range, the reaction with the electrolyte can be suppressed, and the resistance increase of the battery caused by repeated charge and discharge can be suppressed, thereby suppressing the reduction of the battery capacity.
[0036] The W surface existence rate is calculated as the percentage of the amount of W existing on the secondary particle surface relative to the total amount of W existing on the surface and inside the secondary particle. The total amount of W and the amount of W existing on the surface of the secondary particle are measured as follows.
[0037] (1) Determination of the total amount of W present on the surface of secondary particles and inside the secondary particles
[0038] After 10 mL of aqua regia was added to 0.2 g of the powder of the positive electrode active material, 2.5 mL of hydrofluoric acid was added, and the powder was completely dissolved by heating to prepare an aqueous solution. The aqueous solution was fixed to 100 mL with ion exchange water, and the result of measuring the W concentration by ICP-AES was used as the total amount of W present on the surface of the secondary particles and inside the secondary particles.
[0039] (2) Measurement of the amount of W present on the surface of secondary particles
[0040] 4g of the powder of the positive electrode active material was stirred in 400mL of a sodium hydroxide solution with a concentration of 0.01 mol / L at 40°C for 5 minutes, and then filtered with a syringe filter with a pore size of 0.45μm to obtain a filtrate. After 2.5mL of aqua regia was added to 4mL of the filtrate, 0.6mL of hydrofluoric acid was added, and the powder remaining in the filtrate was completely dissolved by heating to prepare an aqueous solution. The aqueous solution was fixed to 100mL with ion exchange water, and the result obtained by measuring the W concentration by ICP-AES was used as the total amount of W present on the surface of the secondary particles.
[0041] On the surface of the secondary particles and inside the secondary particles, W may exist in the form of a W compound containing W. The W compound may contain Li. Examples of the W compound include tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, Li6W2O9), and ammonium tungstate.
[0042] Next, an example of a method for producing a positive electrode active material will be described.
[0043] The method for manufacturing a positive electrode active material includes at least: a process of mixing a composite oxide containing Ni, Co, and Al with a Li compound and calcining to obtain a lithium metal composite oxide; a process of washing the lithium metal composite oxide with water and dehydrating it to obtain a filter cake-like composition with a specified moisture content; and a process of mixing the filter cake-like composition with a W raw material and performing a heat treatment.
[0044] <Lithium Metal Composite Oxide Synthesis Step>
[0045] First, a composite oxide containing Ni, Co, and Al, and a Li compound such as lithium hydroxide and lithium carbonate are prepared. The composite oxide can be obtained by heat treating a composite hydroxide such as a nickel-cobalt-aluminum composite hydroxide obtained by coprecipitation. Next, the composite oxide and the Li compound are mixed, and the mixture is calcined and then crushed to obtain particles of a lithium metal composite oxide.
[0046] <Cake-like composition preparation step>
[0047] Next, the lithium metal composite oxide is washed with water and dehydrated to obtain a cake-like composition. The lithium metal composite oxide can use the particulate matter obtained through the above synthesis process. Through washing with water, the unreacted portion of the Li compound added in the synthesis process of the lithium metal composite oxide and impurities other than the Li compound can be removed. During washing with water, for example, 300 g to 5000 g of the lithium metal composite oxide can be added per 1 L of water. Washing with water can also be repeated multiple times. Dehydration after washing with water can be carried out using a filter press, for example. The moisture content of the washed cake-like composition can be adjusted through the dehydration conditions. According to the research of the present inventors, it has been clarified that by reducing the moisture content of the cake-like composition, the existence ratio of W inside the secondary particles of the lithium metal composite oxide can be increased. By adjusting the moisture content of the washed cake-like composition to a specified range, the W surface existence ratio can be made 25% to 45%. Regarding the moisture content of the cake-like composition, 10 g of the cake-like composition is left standing in a vacuum at 120 °C for 2 hours to be dried, and the mass change of the cake-like composition before and after drying is divided by the mass of the cake-like composition before drying to calculate it.
[0048] <W addition process>
[0049] A W raw material is added to the cake-like composition to obtain a tungsten additive. After washing, a part of the Li compound also remains in the cake-like composition. On the surface of the lithium metal composite oxide contained in the cake-like composition, the remaining Li compound dissolves in the water contained in the cake-like composition to generate an alkaline aqueous solution. If a W raw material is added to the cake-like composition, the W raw material dissolves in the alkaline aqueous solution and diffuses on the surface and inside of the secondary particles of the lithium metal composite oxide. Examples of the W raw material include tungsten oxide (WO3), lithium tungstate (Li2WO4, Li4WO5, Li6W2O9), etc.
[0050] Furthermore, the tungsten additive is heat-treated to produce a positive electrode active material. The heat treatment conditions are not particularly limited. For example, the heat treatment temperature can be set to 150 °C to 400 °C, and the heat treatment time can be set to 0.5 hours to 15 hours. The W surface existence ratio can also be adjusted using the heat treatment conditions. For example, by making the heat treatment temperature a higher temperature, the W surface existence ratio can be reduced. In this case, it is speculated that the moisture on the surface of the secondary particles of the lithium metal composite oxide decreases, so the reaction on the surface of the secondary particles is less likely to occur, and the reaction inside the secondary particles is promoted.
[0051] [Negative electrode]
[0052] The negative electrode has a negative electrode collector such as a metal foil, and a negative electrode mixture layer formed on the negative electrode collector. The negative electrode collector can use a foil of a metal such as copper that is stable within the potential range of the negative electrode, a film having the metal configured on the surface, etc. The negative electrode mixture layer contains a negative electrode active material, and it is appropriate to contain a thickening material, a binding material, etc. The negative electrode can be made, for example, as follows: the negative electrode active material, the thickening material, and the binding material are in a specified weight ratio, and the negative electrode mixture slurry dispersed in water is applied to the negative electrode collector, and after the coating is dried, it is rolled to form a negative electrode mixture layer on both sides of the negative electrode collector.
[0053] As the negative electrode active material, a carbon material that can store and release lithium ions can be used. In addition to graphite, non-graphitizable carbon, graphitizable carbon, fibrous carbon, coke, carbon black, etc. can be used. Furthermore, as non-carbon materials, silicon, tin, and alloys and oxides thereof can be used.
[0054] As the binder, similarly to the case of the positive electrode, PTFE or the like can be used, and styrene-butadiene copolymer (SBR) or a modified form thereof can be used. As the thickener, carboxymethyl cellulose (CMC) or the like can be used.
[0055] [Spacer]
[0056] The spacer 13 may be made of, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous membranes, woven fabrics, nonwoven fabrics, and the like. Suitable materials for the spacer include olefin resins such as polyethylene and polypropylene, and cellulose. The spacer 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, a multilayer spacer including a polyethylene layer and a polypropylene layer may be used, and a spacer 13 having a surface coated with materials such as aramid resins and ceramics may be used.
[0057] [Non-aqueous electrolyte]
[0058] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous electrolyte is not limited to a liquid electrolyte (electrolyte) and can be a solid electrolyte using a gel-like polymer or the like. The non-aqueous solvent can use, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen substituted body formed by replacing at least a portion of hydrogen of these solvents with a halogen atom such as fluorine.
[0059] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone and γ-valerolactone; and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate.
[0060] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ether, 1,2-dimethoxyethane, ethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl ether, Alkenyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and other chain ethers, etc.
[0061] As the halogen-substituted product, fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylates such as methyl fluoropropionate (FMP), and the like are preferably used.
[0062] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1<x<6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lower aliphatic carboxylic acid lithium, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C l F 2l+1 SO2)(C m F 2m+1SO2) {1, m is an integer greater than 1} and other imide salts. The lithium salt may be used alone or in combination. Among these, LiPF6 is preferably used from the viewpoint of ion conductivity, electrochemical stability, etc. The concentration of the lithium salt is preferably set to 0.8 to 1.8 mol per 1 L of solvent.
[0063] Example
[0064] Hereinafter, the present application will be further described by way of examples, but the present application is not limited to these examples.
[0065] [Preparation of positive electrode active material]
[0066] <Example 1>
[0067] With the general formula Ni 0.91 Co 0.04 Al 0.05 Lithium hydroxide monohydrate (LiOH·H2O) is mixed in such a manner that the total amount of Ni, Co, and Al of the composite oxide represented by O2 and the molar ratio of Li become 1:1.02, and the mixture is calcined to obtain a lithium metal composite oxide. Next, the lithium metal composite oxide is washed with water and dehydrated using a filter press to obtain a filter cake-like composition having a specified moisture content. Furthermore, WO3 is added to the filter cake-like composition to obtain a W-added filter cake-like composition. The amount of WO3 added is such that W is 0.08 mol% relative to the total molar number of metal elements other than Li in the W-added filter cake-like composition. Furthermore, the W-added filter cake-like composition is subjected to an oxygen flow with an oxygen concentration of 95% (a flow rate of 5 L / min. per 1 kg of the mixture), and is subjected to a temperature increase rate of 2°C / min., and is heat treated from room temperature to 650°C, and then is heat treated from 650°C to 800°C at a temperature increase rate of 1°C / min., to obtain the positive electrode active material of Example 1. The composition of the positive electrode active material of Example 1 was analyzed by ICP-AES, and the result was LiNi 0.91 Co 0.04 Al 0.05 W 0.0008 O2.
[0068] [Production of positive electrode]
[0069] 100 parts by mass of the above-mentioned positive electrode active material, 1 part by mass of acetylene black (AB) as a conductive material, and 0.9 parts by mass of polyvinylidene fluoride (PVdF) as a binding material are mixed, and then an appropriate amount of N-methyl-2-pyrrolidone (NMP) is added to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry is applied to both sides of the positive electrode collector formed by aluminum foil, and after the coating is dried, the coating is rolled using a calendering roller, cut to a specified electrode size, and a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode core is obtained. It should be noted that an exposed portion exposed on the surface of the positive electrode core is provided on a part of the positive electrode.
[0070] [Production of negative electrode]
[0071] Graphite is mixed in a manner of 94 parts by mass and SiO is mixed in a manner of 6 parts by mass, and this is used as a negative electrode active material. 95 parts by mass of the negative electrode active material, 3 parts by mass of carboxymethyl cellulose (CMC) as a thickening material, and 2 parts by mass of styrene-butadiene rubber (SBR) as a binding material are mixed, and then an appropriate amount of water is added to prepare a negative electrode mixture slurry. The negative electrode mixture slurry is applied to both sides of a negative electrode core formed by copper foil, and after the coating film is dried, the coating film is rolled using a calendering roller, and cut into a specified electrode size to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode core. It should be noted that an exposed portion exposed on the surface of the negative electrode core is provided on a part of the negative electrode.
[0072] [Preparation of non-aqueous electrolyte]
[0073] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a volume ratio of 30:70. Lithium hexafluorophosphate (LiPF6) was added to the mixed solvent so as to have a concentration of 1 mol / L to prepare a non-aqueous electrolyte.
[0074] [Production of test battery cells]
[0075] An aluminum lead was installed on the exposed portion of the positive electrode, a nickel lead was installed on the exposed portion of the negative electrode, the positive electrode and the negative electrode were wound into a spiral shape with a separator made of a polyethylene microporous film interposed therebetween, and then press-formed in the radial direction to produce a flat wound electrode body. The electrode body was housed in an outer casing, the non-aqueous electrolyte was injected, and the opening of the outer casing was sealed to obtain a test battery cell.
[0076] [Cycle test]
[0077] The test cell was subjected to a cycle test, and the discharge capacity at the first cycle and the discharge capacity at the 400th cycle of the cycle test were obtained, and the capacity retention rate was calculated by the following formula.
[0078] Capacity retention rate (%) = (400th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100
[0079] The cycle test was performed as follows. For the test battery cell, constant current charging was performed at a constant current of 0.5 It until the battery voltage reached 4.2 V, and constant voltage charging was performed at 4.2 V until the current value reached 1 / 50 It. Thereafter, constant current discharge was performed at a constant current of 0.5 It until the battery voltage reached 2.5 V. This charge and discharge cycle was repeated for 400 cycles.
[0080] [ARC Trial]
[0081] The above test battery cell was charged at a constant current of 0.3 It until the battery voltage reached 4.2 V under an environment of 25°C, and then charged at a constant voltage of 4.2 V until the current value reached 0.05 It, thus becoming a charged state. Thereafter, the above-mentioned charged test battery cell was placed in an adiabatic runaway reaction calorimeter (ARC), and the temperature of the battery cell was observed using a thermocouple installed in the test battery cell, thereby measuring the self-heating rate (°C / min.) of the test battery cell under an adiabatic environment. Specifically, the temperature was increased at 5°C / min. and the temperature of the test battery cell was repeatedly measured. According to the Arrhenius curve, adiabatic control was switched to when the self-heating rate reached 1°C / min., and control was continued until heat was generated. The battery temperature (°C) when the self-heating rate of the test battery cell reached 2°C / min. was defined as the thermal runaway temperature.
[0082] <Example 2>
[0083] A test cell was prepared and evaluated in the same manner as in Example 1 except that the water content of the cake-like composition was increased.
[0084] <Example 3>
[0085] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of WO 3 added was 0.1 mol % based on the total molar number of metal elements other than Li in the W-added cake-like composition.
[0086] <Example 4>
[0087] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of WO 3 added was 0.07 mol % based on the total molar number of metal elements other than Li in the W-added cake-like composition.
[0088] <Example 5>
[0089] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of WO 3 added was 0.05 mol % based on the total molar number of metal elements other than Li in the W-added cake-like composition.
[0090] <Example 6>
[0091] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of WO 3 added was 0.04 mol % based on the total molar number of metal elements other than Li in the W-added cake-like composition.
[0092] <Comparative Example 1>
[0093] A test cell was prepared and evaluated in the same manner as in Example 2 except that the moisture content of the filter cake composition was increased and the amount of WO3 added was adjusted to 0.15 mol % of W relative to the total molar number of metal elements other than Li in the W-added filter cake composition.
[0094] <Comparative Example 2>
[0095] A test cell was prepared and evaluated in the same manner as in Comparative Example 1 except that the amount of WO3 added was 0.08 mol % of W relative to the total molar number of metal elements other than Li in the composition on the W-added filter cake.
[0096] <Comparative Example 3>
[0097] A test cell was prepared and evaluated in the same manner as in Example 1 except that the amount of WO 3 added was 0.03 mol % based on the total molar number of metal elements other than Li in the W-added cake-like composition.
[0098] The evaluation results of each test cell of the examples and comparative examples are shown in Table 1. In Table 1, the results of the examples and comparative examples show relative values when the capacity retention rate (%) and thermal runaway temperature (° C.) of the test cell of Comparative Example 1 are set to 100. In addition, Table 1 also shows the mole fraction of W relative to the total number of moles of metal elements other than Li in the W-added filter cake-like composition (W addition amount) and the W surface existence rate.
[0099] [Table 1]
[0100]
[0101] For Examples 1 to 6 in which the W surface presence rate is reduced compared to Comparative Examples 1 and 2, the capacity retention rate increases and the thermal runaway temperature rises. It is speculated that by reducing the W surface presence rate, the reaction at the surface of the secondary particles of the lithium metal composite oxide can be suppressed, thereby improving the cycle characteristics and safety. On the other hand, the capacity retention rate and thermal runaway temperature of Comparative Example 3 in which the W surface presence rate is less than 25% are basically the same as those of Comparative Example 1. Therefore, from the perspective of cycle characteristics and safety, a W surface presence rate of 25% to 45% is appropriate.
[0102] Description of Reference Numerals
[0103] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 outer body, 16 sealing body, 17, 18 insulating plate, 19 positive electrode lead, 20 negative electrode lead, 21 groove part, 22 filter, 23 lower valve body, 24 insulating member, 25 upper valve body, 26 cover, 26a opening, 27 gasket
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium metal composite oxide, wherein the lithium metal composite oxide has secondary particles formed by aggregation of primary particles, and W exists on the surface of the secondary particles and inside the secondary particles of the lithium metal composite oxide, The positive electrode active material for the non-aqueous electrolyte secondary battery is composed of the general formula Li α Ni a Co b Al c M d W e O β Represents, wherein, 0.9≤α≤1.2, 0.8≤a≤0.96, 0<b≤0.10, 0<c≤0.10, 0≤d≤0.1, 0.0003≤e / (a+b+c+d+e)≤0.002, 1.9≤β≤2.1, a+b+c+d=1, M is at least one element selected from Mn, Fe, Ti, Si, Nb, Zr, Mo and Zn, The ratio of W present on the surface of the secondary particle of the lithium metal composite oxide is 25% to 45% relative to the total amount of W present on the surface of the secondary particle of the lithium metal composite oxide and inside the secondary particle. On the surface of the secondary particles and inside the secondary particles, W exists in the state of tungsten oxide. 2 . A non-aqueous electrolyte secondary battery comprising: a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode comprises the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 .
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery positive electrode active material and nonaqueous electrolyte secondary battery
WO2017018099A1
Positive electrode active material for nonaqueous electrolyte secondary cell, method for manufacturing same, and nonaqueous electrolyte secondary cell in which said positive electrode active material is used
CN107210441A
Nonaqueous electrolyte secondary battery positive electrode active material and nonaqueous electrolyte secondary battery
CN107851793A
Cathode active material for lithium secondary battery, production method therefor, and lithium secondary battery comprising same
CN110268561A
Positive electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing the same, and nonaqueous electrolyte secondary battery including the positive electrode active material
JP2013125732A