Pneumatic tires
By using a release agent coating with a thickness of 0.1 μm to 100 μm or a silicon content of 0.1% to 10.0% by weight on the inner surface of the tread of a pneumatic tire, the problem that the amount of release agent coating affects air retention and sealing properties is solved. , avoiding the deterioration of rim offset and achieving good air retention and sealing.
Patent Information
- Application Number
- CN202210704202.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-02-08
- Filing Date
- 2017-11-14
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2037-11-14
AI Technical Summary
When existing pneumatic tires are vulcanized using air bags, too little release agent coating affects air retention, too much coating causes sealing deterioration, and the powdery release agent is sprayed onto the bead, causing the rim to shift when driving. Sexual deterioration.
Use an air bag coated with a release agent for vulcanization, ensuring that the thickness of the release agent on the inner surface of the tread is between 0.1 μm and 100 μm or the amount of silicon is between 0.1 and 10.0% by weight, and detected by electron microscopy and X-ray fluorescence analysis. , to avoid excessive adhesion of the release agent on the bead.
It achieves good air retention and sealing when repairing flat tires, while avoiding deterioration of rim deflection and improving the overall performance of the tire.
Smart Images

Figure CN115008946B_ABST
Abstract
Description
[0001] This application is a divisional application of the Chinese patent application with the application date of November 14, 2017, application number 201780085644.7, and invention name: "Pneumatic tire and its manufacturing method". Technical Field
[0002] The present invention relates to a pneumatic tire and a method for manufacturing the same, and more specifically, to a pneumatic tire and a method for manufacturing the same, which uses a bladder having a coating formed of a release agent for vulcanization and has a small amount of the release agent attached to the inner surface of the tire, thereby achieving both air retention and sealing performance during repair of a flat tire without deteriorating rim deviation during driving. Background Art
[0003] When a green tire is vulcanized using a bladder, the bladder is easily attached to the inner surface of the green tire. Therefore, a release agent is applied to the inner surface of the green tire to prevent the green tire and the bladder from sticking to each other (for example, Patent Document 1).
[0004] However, when the mold release agent is applied to the inner surface of the tire, if the amount of the release agent applied is too small, the air retention provided by the release agent cannot be fully obtained. On the other hand, if the amount of the release agent applied is too large, the release agent repels the flat tire repair fluid when the flat tire is repaired, and there is a problem of deterioration in the sealing performance. In addition, when a powdered release agent is used, when the release agent is applied to the inner surface of the tire, the release agent sometimes scatters to the bead portion, and the pneumatic tire vulcanized and formed in a state where a large amount of the release agent is attached near the bead portion has a problem of deterioration in the rim deflection during driving.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 5-96546 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] The object of the present invention is to provide a pneumatic tire and a method for manufacturing the same, which is vulcanized using a bladder having a coating formed of a release agent and has a small amount of the release agent attached to the inner surface of the tire, thereby achieving both air retention and sealing performance during flat tire repair without deteriorating rim deviation during driving.
[0010] Technical Solution
[0011] The pneumatic tire of the present invention for achieving the above object is a pneumatic tire vulcanized using a bladder having a coating layer formed of a release agent, wherein the thickness of the release agent measured by an electron microscope on the inner surface of the tread portion is 0.1 μm to 100 μm.
[0012] The pneumatic tire of the present invention is a pneumatic tire vulcanized using a bladder having a coating layer formed of a release agent, wherein the amount of silicon in the release agent detected by X-ray fluorescence analysis on the inner surface of the tread portion is 0.1% by weight to 10.0% by weight.
[0013] The method for manufacturing a pneumatic tire of the present invention is a method for manufacturing a pneumatic tire using a bladder having a coating layer formed of a release agent to vulcanize a green tire, characterized in that the thickness of the release agent detected by an electron microscope on the inner surface of the tread portion of the pneumatic tire after vulcanization is 0.1 μm to 100 μm.
[0014] In addition, the manufacturing method of the pneumatic tire of the present invention is a manufacturing method of the pneumatic tire using an air bladder having a coating formed by a release agent to vulcanize a raw tire, characterized in that the amount of silicon in the release agent detected by X-ray fluorescence analysis on the inner surface of the tread portion of the pneumatic tire after vulcanization is 0.1 weight % to 10.0 weight %.
[0015] Beneficial Effects
[0016] In the present invention, by using an air bag with a coating formed by a release agent for vulcanization, the thickness of the release agent on the inner surface of the tire can be 0.1 μm to 100 μm, or the amount of silicon in the release agent can be 0.1 wt% to 10.0 wt%. In this way, when a small amount of release agent is attached to the inner surface of the tire, the release agent prevents air from passing through the inner surface of the tire, and the air retention is good. On the other hand, the sealing performance during the repair of a flat tire can be improved. In addition, according to the present invention, unlike the case where a powdered release agent is sprayed onto the inner surface of the tire as in the past, the release agent will not excessively adhere to the bead portion, so the rim deviation will not be deteriorated. As a result, both air retention and sealing performance during the repair of a flat tire can be achieved without deteriorating the rim deviation during driving. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] [ Figure 1 ] is a meridian cross-sectional view showing a pneumatic tire constructed according to an embodiment of the present invention.
[0018] [ Figure 2 ] is an enlarged cross-sectional view showing a portion of a pneumatic tire constructed according to an embodiment of the present invention. DETAILED DESCRIPTION
[0019] Hereinafter, the structure of the present invention will be described in detail with reference to the accompanying drawings. Figure 1 , CL is the tire center line.
[0020] like Figure 1 As shown, the pneumatic tire formed by the embodiment of the present invention comprises: a tread portion 1 extending in the tire circumferential direction and forming a ring shape; a pair of sidewall portions 2, 2, arranged on both sides of the tread portion 1; and a pair of bead portions 3, 3, arranged on the radial inner side of these sidewall portions 2 in the tire.
[0021] A carcass layer 4 is mounted between a pair of bead portions 3, 3. The carcass layer 4 includes a plurality of reinforcing cords extending in the tire radial direction and folded back from the inside to the outside of the tire around a bead core 5 disposed at each bead portion 3. A bead core 6 formed of a rubber composition and having a triangular cross section is disposed on the outer periphery of the bead core 5.
[0022] On the other hand, a plurality of belt layers 7 are buried on the outer peripheral side of the carcass layer 4 at the tread portion 1. These belt layers 7 include a plurality of reinforcing cords inclined relative to the tire circumferential direction, and are configured so that the reinforcing cords cross each other between layers. In the belt layer 7, the inclination angle of the reinforcing cords relative to the tire circumferential direction is set in the range of 10° to 40°, for example. As the reinforcing cords of the belt layer 7, steel cords are preferably used. On the outer peripheral side of the belt layer 7, for the purpose of improving high-speed durability, at least one belt covering layer 8 is arranged, and the belt covering layer 8 is formed by arranging reinforcing cords at an angle of, for example, less than 5° relative to the tire circumferential direction. As the reinforcing cords of the belt covering layer 8, organic fiber cords such as nylon and aramid are preferably used.
[0023] Furthermore, a plurality of main grooves 9 extending in the tire circumferential direction are formed in the tread portion 1 , and a plurality of rows of land portions 10 are defined in the tread portion 1 by these main grooves 9 .
[0024] It should be noted that the above-described tire internal structure is a representative example of a pneumatic tire, but is not limited thereto.
[0025] like Figure 2 As shown, in the above-mentioned pneumatic tire, the transfer layer 12 of the release agent exists on the inner side of the tire radial direction of the tire inner surface 11. By using the bladder having a coating layer formed of the release agent to vulcanize the green tire, in the pneumatic tire after the vulcanization, the transfer layer 12 of the release agent is transferred to the tire inner surface 11. In this way, the transferred release agent is not transferred to the entire surface of the tire inner surface 11, but is spread on the tire inner surface.
[0026] The thickness g of the transfer layer 12 of the release agent is 0.1 μm to 100 μm. The thickness g of the transfer layer 12 of the release agent can be detected using an electron microscope. When measuring the thickness g of the transfer layer 12 of the release agent using an electron microscope, a sample cut out of the pneumatic tire along the tire width direction is used to measure the thickness at multiple locations in the sample (for example, four locations in the tire circumferential direction and three locations in the tire width direction). Then, the thickness g (average thickness) of the transfer layer 12 of the release agent is calculated by averaging the measured values measured at the above multiple locations.
[0027] On the other hand, the amount of silicon in the release agent on the inner surface of the tread portion 1 is 0.1 wt% to 10.0 wt%. In the present invention, when specifying the amount of the release agent on the inner surface of the tread portion 1, the amount of silicon, which is the main component of a general release agent, is used as an index. The amount of silicon can be detected by X-ray fluorescence analysis. Generally, there are FP method (fundamental parameter method) and calibration curve method for X-ray fluorescence analysis. In the present invention, the FP method is used. When measuring the amount of the release agent (silicon), a sheet sample (size: width 70 mm, length 100 mm) obtained by peeling off the carcass layer and the inner liner at multiple locations (for example, four locations in the tire circumferential direction and three locations in the tire width direction, a total of seven locations) of the above-mentioned pneumatic tire is used, and measurement samples (size: width 13 mm to 15 mm, length 35 mm to 40 mm) at four corners and one location in the center are further extracted from each sheet sample, and the amount of the release agent is measured for each measurement sample using an X-ray fluorescence analysis device. Then, by averaging the measured values of the five measured samples of each of the above-mentioned sheet samples, the amount of release agent in each sheet sample is calculated, and the calculated values are respectively included in the range of 0.1 wt% to 10.0 wt%. In addition, the fluorescent X-ray particles have an inherent energy proportional to the atomic number, and the element can be determined by measuring the inherent energy. Specifically, the inherent energy of silicon is 1.74±0.05keV. It should be noted that the number of fluorescent X-ray particles (X-ray intensity) of the release agent (silicon) is in the range of 0.1cps / μA to 1.5cps / μA.
[0028] The transfer layer 12 of the release agent is preferably partially disposed on a portion of the tire inner surface 11 in the tire width direction including at least a region from the upper end position of one bead core 6 to the upper end position of the other bead core 6. Figure 1 As shown in FIG. 1 , this area corresponds to the area X including the maximum width position of the tire. By forming the transfer layer 12 of the release agent on at least the area corresponding to the area X on the tire inner surface 11, it is possible to improve both the air retention and the sealing performance when repairing a flat tire. Furthermore, it is more preferred that the transfer layer 12 of the release agent is partially arranged in a part of the area in the tire width direction including at least the lower part of the belt layer 7 (in the Figure 1 Area Y shown).
[0029] As the components that can be incorporated into the transfer layer 12 formed by the release agent, for example, there can be cited components containing silicone components as effective ingredients. As silicone components, polyorganosiloxanes can be cited, for example, dialkyl polysiloxanes, alkylphenyl polysiloxanes, alkyl aralkyl polysiloxanes, 3,3,3-trifluoropropyl methyl polysiloxane, etc. can be cited. Dialkyl polysiloxanes are, for example, dimethyl polysiloxane, diethyl polysiloxane, methyl isopropyl polysiloxane, methyl dodecyl polysiloxane. Alkyl phenyl polysiloxanes are, for example, methyl phenyl polysiloxane, dimethyl siloxane / methyl phenyl siloxane copolymers, and dimethyl siloxane / diphenyl siloxane copolymers. Alkyl aralkyl polysiloxanes are, for example, methyl (phenylethyl) polysiloxane, methyl (phenylpropyl) polysiloxane. These polyorganosiloxanes can be used alone or in combination of two or more.
[0030] As described above, by using a bladder having a coating formed of a release agent for vulcanization, the thickness g of the release agent on the inner surface 11 of the tire can be set to 0.1 μm to 100 μm, or the amount of silicon in the release agent can be set to 0.1 wt% to 10.0 wt%. In this way, when a small amount of release agent is attached to the inner surface 11 of the tire, the release agent prevents air from passing through the inner surface 11 of the tire, and the air retention is good. On the other hand, the sealing performance during the repair of a flat tire can be improved. Here, if the thickness of the release agent on the inner surface 11 of the tire is thinner than 0.1 μm, or the amount of silicon in the release agent is less than 0.1 wt%, the adhesion between the green tire and the bladder during vulcanization cannot be fully prevented. If the thickness of the release agent is thicker than 100 μm, or the amount of silicon in the release agent is more than 10.0 wt%, the release agent repels the flat tire repair liquid during the repair of the flat tire, and there is a tendency for the sealing performance to deteriorate. In particular, the deterioration of the sealing performance is significant near the belt end.
[0031] Furthermore, according to the present invention, unlike the conventional method of spraying a powdered release agent onto the tire inner surface 11, the release agent does not excessively adhere to the vicinity of the bead portion 3, thereby not deteriorating the rim runout. As a result, both air retention and sealing performance during flat tire repair can be achieved without deteriorating the rim runout during driving.
[0032] Next, the manufacturing method of the pneumatic tire of the present invention is described. When the green tire is vulcanized, the air bladder is covered with a release agent in advance (preferably by baking and coating), and a coating formed of the release agent is formed on the outer surface of the air bladder. The process of forming the coating on the outer surface of the air bladder is carried out, for example, while storing at 150°C for one hour, at 90°C for four hours, or at room temperature for eight hours after applying the release agent. In addition, the process of forming the coating on the outer surface of the air bladder is carried out within the range of one or more and three or less times. The green tire is vulcanized using the air bladder with the coating formed as described above.
[0033] As described above, by vulcanizing using a bladder having a coating formed of a release agent, the thickness g of the release agent on the inner surface 11 of the tire can be set to 0.1 μm to 100 μm, or the amount of silicon in the release agent can be set to 0.1 wt % to 10.0 wt %. In this way, when a small amount of release agent is attached to the inner surface 11 of the tire, the release agent prevents air from passing through the inner surface 11 of the tire, and the air retention is good. On the other hand, the sealing performance during the repair of a flat tire can be improved. In addition, according to the present invention, unlike the case where a powdered release agent is sprayed onto the inner surface 11 of the tire as in the past, the release agent does not excessively adhere to the vicinity of the bead portion 3, and thus does not deteriorate the rim deflection performance. As a result, both the air retention performance and the sealing performance during the repair of a flat tire can be achieved without deteriorating the rim deflection performance during driving.
[0034] In particular, it is preferred that, in the process of forming a coating on the outer surface of the airbag, the coating covering time t (hour) and temperature T (°C) satisfy the conditions of t ≥ -0.0571T + 9.14 and 10°C ≤ T ≤ 180°C. In addition, it is more preferred to set the temperature T to 90°C and the covering time t to 4 hours, and it is further preferred to set the temperature T to 150°C and the covering time t to 1 hour. By satisfying such conditions, in an airbag with a coating, the time for applying a release agent can be shortened, and the shortening of the service life of the airbag can be prevented. Here, the higher the temperature T (°C), the shorter the time it takes to form the coating, but the airbag is prone to deterioration, shortening the service life of the airbag.
[0035] Examples
[0036] Pneumatic tires with a tire size of 275 / 35ZR20 vulcanized using a bladder having a coating formed of a release agent were prepared. Examples 1 to 3 tires were prepared with the presence or absence of a release agent on the tire inner surface and the thickness (μm) of the release agent on the tire inner surface as shown in Table 1.
[0037] In addition, tires of Comparative Examples 1 to 3 were prepared. Comparative Example 1 had the same structure as Example 1, except that a rigid core was used instead of a bladder for vulcanization and there was no mold release agent on the inner surface of the tire. Comparative Example 2 had the same structure as Example 1, except that the thickness of the mold release agent on the inner surface of the tire was set to 110 μm. Comparative Example 3 had the same structure as Example 1, except that a powdered mold release agent was sprayed onto the inner surface of the tire for vulcanization and the thickness of the mold release agent on the inner surface of the tire was set to 110 μm.
[0038] It should be noted that in Table 1, the thickness (μm) of the release agent on the inner surface of the tire is the value obtained by measuring the thickness of the release agent at four locations in the tire circumferential direction and three locations in the tire width direction of each sample tire after the production process using a scanning electron microscope (SEM-EDX), and averaging these measured values.
[0039] The air retention performance, the sealing performance during flat tire repair, and the rim runout performance of these test tires were evaluated according to the following test methods, and the results are collectively shown in Table 1.
[0040] Air retention:
[0041] Each test tire was assembled on a wheel with a rim size of 20×9.5J, and placed under the conditions of air pressure of 270 kPa and temperature of 21°C for 24 hours. The air pressure was measured after 42 days with the initial air pressure of 250 kPa, and the slope of the gas leakage from the 15th day to the 42nd day was calculated. The evaluation results were expressed as an index using the reciprocal of the measured value, with Comparative Example 1 as 100. The larger the index value, the better the air retention.
[0042] Leakage during flat tire repair:
[0043] A leaking hole (4 mm in diameter) was opened on the shoulder of each test tire. Next, the tire with the leaking hole was attached to a drum tester, 450 mL of tire leaking sealant was injected from the tire valve, and air was filled to make the tire internal pressure 200 kPa. Afterwards, the intermittent operation of the above-mentioned tire was repeated under the conditions of a load of 4.17 kN and a speed of 30 km per hour, and the running distance (flat tire repair distance) until the leaking hole was sealed without air leakage was measured. Whether there is air leakage is confirmed by spraying soapy water on the part of the above-mentioned leaking hole to confirm whether the soapy water has turned into foam. The evaluation results are evaluated based on the number of cycles of intermittent operation, and the situation of being sealed within 10 cycles is set to 0, the situation of being sealed for more than 11 cycles is set to Δ, and the situation of being unsealed is set to ×.
[0044] Rim offset:
[0045] Each test tire was assembled on a wheel with a rim size of 20×9.5J, and emergency braking was performed 10 times under the conditions of a driving speed of 50km / h and an air pressure of 230kPa to measure the deviation between the rim and the tire. The evaluation results were expressed as an index using the reciprocal of the measured value, with Comparative Example 1 as 100. The larger the index value, the better the rim deviation.
[0046] [Table 1]
[0047]
[0048]
[0049] As can be seen from Table 1, the pneumatic tires of Examples 1 to 3 do not deteriorate the rim runout during running, and improve the air retention and sealing properties during flat tire repair, as compared with Comparative Example 1.
[0050] On the other hand, in Comparative Example 2, the thickness of the release agent on the inner surface of the tire is relatively thick, so the sealing performance during the repair of the flat tire is reduced. In Comparative Example 3, the release agent is sprayed on the inner surface of the tire and adheres to the bead portion (the contact portion with the rim), so the rim runout performance is reduced.
[0051] Next, tires of Examples 4 to 6 were prepared in the same manner as Examples 1 to 3: in a pneumatic tire vulcanized using an air bladder having a coating formed of a release agent, the presence or absence of a release agent on the inner surface of the tire and the amount (weight %) of the release agent (silicon) on the inner surface of the tire were set as shown in Table 2.
[0052] In addition, tires of Comparative Examples 4 to 6 were prepared. For Comparative Example 4, a rigid core was used instead of a bladder for vulcanization, and no mold release agent was used. For Comparative Example 5, the same structure as Example 4 was used except that the amount of mold release agent (silicon) on the inner surface of the tire was set to 11%. For Comparative Example 6, the same structure as Example 4 was used except that a powdered mold release agent was sprayed onto the inner surface of the tire for vulcanization, and the amount of mold release agent (silicon) on the inner surface of the tire was set to 45%.
[0053] It should be noted that the amount of the release agent (silicon) on the inner surface of the tire in Table 2 is the average of the calculated values based on the amount of the release agent (silicon) measured at four locations in the tire circumferential direction and three locations in the tire width direction of each test tire after the production process using an energy dispersive X-ray fluorescence analyzer (EDX-720 manufactured by Shimadzu Corporation). The measurement conditions were vacuum, voltage 50 kV, current 100 μA, integration time 50 seconds, collimator 100 μA, and a 100 μm diameter.
[0054] The air retention performance, the sealing performance during flat tire repair, and the rim runout performance of these test tires were evaluated, and the results are shown in Table 2.
[0055] [Table 2]
[0056]
[0057]
[0058] As can be seen from Table 2, the pneumatic tires of Examples 4 to 6 do not deteriorate the rim runout during running, and improve the air retention and sealing properties during flat tire repair, as compared to Comparative Example 4.
[0059] On the other hand, in Comparative Example 5, the amount of mold release agent on the inner surface of the tire is relatively large, so the sealing performance during the repair of the flat tire is reduced. In Comparative Example 6, since the mold release agent is sprayed on the inner surface of the tire and adheres to the bead portion (the contact portion with the rim), the rim runout performance is reduced.
[0060] Explanation of symbols
[0061] 1 Tread
[0062] 2 Side wall
[0063] 3 Bead section
[0064] 11 Tire inner surface
[0065] 12 Transfer layer
Claims
1. A pneumatic tire comprising: a pair of sidewalls disposed on both sides of a tread portion; and a pair of bead portions disposed radially inward of the sidewalls, wherein a bead core is embedded in each bead portion, and a bead core is disposed on the outer periphery of each bead core, and vulcanized using a bladder having a coating formed of a release agent, wherein the pneumatic tire is characterized in that: The transfer layer formed by transferring the release agent is arranged only on a partial area of the tire inner surface in the tire width direction, the partial area including the area from the upper end position of one bead core to the upper end position of the other bead core, The thickness of the transfer layer of the release agent detected by an electron microscope on the inner surface of the tread portion of the pneumatic tire after vulcanization is 0.1 μm to 100 μm.
2. A pneumatic tire comprising: a pair of sidewalls disposed on both sides of a tread portion; and a pair of bead portions disposed radially inward of the sidewalls, wherein a bead core is embedded in each bead portion, and a bead core is disposed on the outer periphery of each bead core, and vulcanized using a bladder having a coating formed of a release agent, wherein the pneumatic tire is characterized in that: The transfer layer formed by transferring the release agent is arranged only on a partial area of the tire inner surface in the tire width direction, the partial area including the area from the upper end position of one bead core to the upper end position of the other bead core, The amount of silicon in the transfer layer of the release agent detected by X-ray fluorescence analysis on the inner surface of the tread portion of the pneumatic tire after vulcanization is 0.1% by weight to 10.0% by weight.
3. A pneumatic tire comprising: a pair of sidewalls disposed on both sides of a tread portion; and a pair of bead portions disposed radially inward of the sidewalls, a carcass layer being mounted between the pair of bead portions, a belt layer being disposed on the outer peripheral side of the carcass layer of the tread portion, and vulcanized using a bladder having a coating formed of a release agent, wherein: The transfer layer formed by transferring the release agent is arranged only on a partial area of the tire inner surface in the tire width direction, the partial area including the lower part of the belt layer, The thickness of the transfer layer of the release agent detected by an electron microscope on the inner surface of the tread portion of the pneumatic tire after vulcanization is 0.1 μm to 100 μm.
4. A pneumatic tire comprising: a pair of sidewalls disposed on both sides of a tread portion; and a pair of bead portions disposed radially inward of the sidewalls, a carcass layer being mounted between the pair of bead portions, a belt layer being disposed on the outer peripheral side of the carcass layer of the tread portion, and vulcanized using a bladder having a coating formed of a release agent, wherein: The transfer layer formed by transferring the release agent is disposed only on a partial area in the tire width direction of the tire inner surface, the partial area including the lower part of the belt layer, The amount of silicon in the transfer layer of the release agent detected by X-ray fluorescence analysis on the inner surface of the tread portion of the pneumatic tire after vulcanization is 0.1% by weight to 10.0% by weight.
Citation Information
Patent Citations
Flat pneumatic radial tire for heavy duty and method of manufacturing the same
CN101203391A
Method for producing polymer sheet for inner liner and method for producing pneumatic tire
CN102019733A
Inflatable tire
CN103242578A
Method for producing pneumatic tire
CN105745064A
Tire vulcanizing bladder
JP2014091272A