Method for preparing moisture-resistant immune detection glass fiber probe, moisture-resistant protective liquid and preparation method thereof

By using an anti-humidity protective solution to coat the glass fiber probe, the problem of hydrolysis of the silane coupling agent in a humid environment is solved, the active life of the antigen or antibody is extended, and the reliability of the detection and the flexibility of production are improved. .

CN115015539BActive Publication Date: 2024-10-08星童医疗技术(苏州)有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210650863.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-09
Publication Date
2024-10-08
Estimated Expiration
2042-06-09

AI Technical Summary

Technical Problem

Silane coupling agents are easily hydrolyzed after surface modification of inorganic substrates, affecting the immobilization and activity of enzymes or proteins, especially in humid environments, resulting in reduced immobilization effects.

Method used

Use an anti-humidity protective solution, including surfactants, stabilizers, preservatives and buffers, and coat it by immersing the glass fiber probe modified with a silane coupling agent to increase the anti-humidity performance and prolong the resistance of the antigen or antibody to humidity. Resist time.

Benefits of technology

It significantly extends the active life of the antigen or antibody fixed on the surface of the glass fiber probe by the silane coupling agent, improves the reliability of detection, and reduces the control requirements for the humidity of the storage environment, making it suitable for mass production and large-scale use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115015539B_ABST
    Figure CN115015539B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a moisture-resistant immunoassay glass fiber probe, a moisture-resistant protective solution, and its preparation method. The glass fiber probe preparation method includes the following steps: S10, depositing a silane coupling agent on the surface of the glass fiber probe; S20, preparing a phosphate buffer solution, an antibody or antigen solution, a blocking solution, a washing solution, and a moisture-resistant protective solution; the moisture-resistant protective solution includes a surfactant, a stabilizer, a preservative, a pH adjuster, and purified water; S30, immersing the area of ​​the glass fiber probe with the deposited silane coupling agent sequentially in the phosphate buffer solution, the antibody or antigen solution, the blocking solution, the first washing solution, the second washing solution, and the moisture-resistant protective solution for a certain period of time to complete the antigen or antibody coating; S40, drying the coated glass fiber probe to obtain the moisture-resistant immunoassay glass fiber probe. The test probe of this invention, after treatment with the moisture-resistant protective solution, significantly prolongs the time that the antigen or antibody immobilized on the surface of the glass fiber probe resists humidity, thus significantly extending the active lifespan of the antigen or antibody.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of medical devices, in particular to a method for preparing a moisture-resistant immune detection glass fiber probe, a moisture-resistant protective liquid and a preparation method thereof. Background Art

[0002] Silane coupling agent is one of the four commonly used silicone products (silicone oil, silicone rubber, silicone resin and silane coupling agent), which is mainly used for the treatment and modification of the surface of glass fiber and other substrates, the immobilization of enzymes or proteins on the glass surface, inorganic fillers, sealants and tackifiers, etc. There are hundreds of types of silane coupling agents, and their general structural formula is: YR-SiX3, where Y is an active organic functional group, such as amino, epoxy, thiol, etc., R is a saturated or unsaturated aliphatic carbon chain skeleton, and X is a characteristic group bound to silicon atoms, such as methoxy, chloro, ethoxy, acetoxy, etc., which can connect to the surface of glass fiber and other substrates.

[0003] When silane coupling agent is used as a modifier on the surface of inorganic substrates such as glass fiber, hydrophobic groups are added to the surface of inorganic particles to change their surface properties, reduce surface energy, significantly improve hydrophobicity, and achieve a water contact angle of >100o. Since silane coupling agent itself contains organic groups, enzymes or proteins can be physically adsorbed on the surface of inorganic substrates such as glass fiber through its surface hydrophobicity, and can also be covalently coupled to its surface through organic groups to achieve the immobilization of enzymes or proteins.

[0004] However, in actual use, it is found that when silane coupling agents are used as modifiers on the surfaces of inorganic matrices such as glass fibers, they can indeed greatly enhance the hydrophobicity of their surfaces. However, their long-term storage requires a closed and dry environment. Even in a normal humidity environment, the silane coupling agents will gradually hydrolyze and further affect the immobilization and activity of immobilized proteins or enzymes on the surfaces of matrices such as glass fibers. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems existing in the prior art and to provide a method for preparing a moisture-resistant immunoassay glass fiber probe, a moisture-resistant protective liquid and a preparation method thereof.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] A method for preparing a moisture-resistant immunoassay glass fiber probe comprises the following steps:

[0008] S10, depositing a silane coupling agent on the surface of the glass fiber probe;

[0009] S20, preparing a phosphate buffer solution, an antibody or antigen solution, a blocking solution, a cleaning solution and an anti-wetting protection solution required for coating the glass fiber probe; the anti-wetting protection solution includes a surfactant, a stabilizer, a preservative, a pH regulator and purified water;

[0010] S30, immersing the area on the glass fiber probe where the silane coupling agent is deposited in the phosphate buffer solution, the antibody or antigen solution, the blocking solution, the first cleaning solution, the second cleaning solution and the anti-wet protection solution in sequence for a certain period of time to complete the antigen or antibody coating;

[0011] S40, drying the coated glass fiber probe to obtain a moisture-resistant immunoassay glass fiber probe.

[0012] Preferably, in the processing method, the anti-moisture protection solution includes 0.01% to 0.1% (V / V) surfactant, 0.01% to 0.1% (V / V) preservative, 1% to 20% (m / v) stabilizer and 0.01 to 0.1M buffer.

[0013] Preferably, in the processing method, the surfactant is at least one of Triton X-100, Triton X-405 and Tween-20;

[0014] Preferably, in the processing method, the stabilizer is at least one of trehalose, mannitol and sucrose.

[0015] Preferably, in the processing method, the buffer is acetic acid-sodium acetate buffer or MES buffer.

[0016] Preferably, in the processing method, in S30, when the glass fiber probe is immersed in any liquid, the container containing the liquid and the bracket fixing the glass fiber probe are shaken by a shaking table.

[0017] Preferably, in the processing method, the glass fiber probe stays in the anti-wetting buffer for a time between 20 and 40 seconds.

[0018] The anti-humidity protection liquid comprises 0.01% to 0.1% (V / V) of a surfactant, 0.01% to 0.1% (V / V) of a preservative, 1% to 20% (m / v) of a stabilizer and 0.01 to 0.1M of a buffer solution.

[0019] Preferably, in the anti-moisture protection liquid, the surfactant is at least one of Triton X-100, Triton X-405 and Tween-20.

[0020] Preferably, in the anti-moisture protection solution, the stabilizer is at least one of trehalose, mannitol and sucrose.

[0021] Preferably, in the anti-moisture protection solution, the buffer is acetic acid-sodium acetate buffer or MES buffer.

[0022] Preferably, in the anti-moisture protection liquid, the pH value of the anti-moisture protection liquid is between 4.0 and 6.5.

[0023] The method for preparing the anti-humidity protection liquid is characterized by comprising the following steps:

[0024] S1, prepare corresponding amounts of sucrose, glacial acetic acid, Tween-20, preservatives, purified water and sodium hydroxide solution according to the recipe;

[0025] S2, placing sucrose in a container, adding glacial acetic acid, Tween-20, and a preservative, and then adding purified water to a specified volume to obtain a mixture;

[0026] S3, stirring the mixture obtained in S2 by a magnetic stirrer;

[0027] S4, adding sodium hydroxide solution to the stirred mixed solution to adjust the pH value of the mixed solution to a target range, and then fixing the volume to a target volume to obtain an anti-moisture protection solution.

[0028] The advantages of the technical solution of the present invention are mainly reflected in:

[0029] After the glass fiber probe of the present invention is modified by a silane coupling agent, during coating, the glass fiber probe fixed with an antigen or antibody is immersed in an anti-humidity protection liquid and then dried, so that the moisture resistance of the coated glass fiber probe can be greatly improved, and the humidity resistance time of the antigen or antibody fixed on the surface of the glass fiber probe by the silane coupling agent is significantly prolonged, so that the active life of the antigen or antibody is significantly prolonged, and the reliability of the detection is effectively guaranteed.

[0030] The test probe prepared by the present invention effectively reduces the humidity control requirements for the production environment and the storage environment, which is beneficial to the production, storage, transportation and use of the product.

[0031] The test probe of the present invention is easy to produce in batches and can be mass-produced and used.

[0032] The anti-moisture protection liquid of the present invention can have the best effect by studying and designing the components and dosage, and the anti-moisture protection liquid of the present solution is easy to prepare and is convenient for popularization and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the principle of using the test probe to perform an immune test reaction in the present invention;

[0034] Figure 2It is a comparison diagram of the fluorescence signals detected by the two test probes treated with the anti-wetting protection solution of Example 1 and the common buffer solution in the immunoassay of the present invention;

[0035] Figure 3 It is a comparison diagram of the fluorescence signals detected by the two test probes treated with the anti-wetting protection solution of Example 2 and the common buffer solution in the immunoassay of the present invention;

[0036] Figure 4 It is a comparison diagram of the fluorescence signals detected by the two test probes treated with the anti-wetting protection solution of Example 3 and the common buffer solution in the immunoassay of the present invention. DETAILED DESCRIPTION

[0037] The purpose, advantages and features of the present invention will be illustrated and explained by the non-limiting description of the following preferred embodiments. These embodiments are only typical examples of the application of the technical solution of the present invention, and any technical solution formed by equivalent replacement or equivalent transformation falls within the scope of protection claimed by the present invention.

[0038] In the description of the scheme, it should be noted that the terms "center", "upper", "lower", "left", "right", "front", "back", "vertical", "purification level", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of description and simplified description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance. Moreover, in the description of the scheme, with the operator as a reference, the direction close to the operator is the proximal end, and the direction away from the operator is the distal end.

[0039] The method for preparing the moisture-resistant immunoassay glass fiber probe disclosed in the present invention is described in detail below, which comprises the following steps:

[0040] S10, depositing a silane coupling agent on the surface of the glass fiber probe;

[0041] S20, preparing the phosphate buffer solution, antibody or antigen solution, blocking solution, cleaning solution and anti-moisture protection solution required for coating the glass fiber probe;

[0042] S30, immersing the area on the glass fiber probe where the silane coupling agent is deposited in the phosphate buffer solution, the antibody or antigen solution, the blocking solution, the first cleaning solution, the second cleaning solution and the anti-wet protection solution in sequence for a certain period of time to complete the antigen or antibody coating;

[0043] S40, drying the coated glass fiber probe to obtain a moisture-resistant immunoassay glass fiber probe.

[0044] After the test probe of the present invention is surface-modified by a silane coupling agent, a process of immersing in an anti-humidity protection liquid is added during the coating process, so that after the test probe is dried, the humidity resistance time of the antigen or antibody fixed to the surface of the glass fiber matrix by the silane coupling agent is significantly prolonged, thereby significantly prolonging the active life of the antigen or antibody.

[0045] The glass fiber probe is, for example, a pure quartz probe of 20mm*Ф1mm. A silane coupling agent is uniformly deposited on the surface of the pure quartz probe by a known vapor deposition method. The silane coupling agent is, for example, 3-aminopropyltrimethoxysilane, which improves the hydrophobicity of the probe surface, thereby more efficiently adsorbing protein-like substances, and the amino group (NH2) on the surface can be used as a covalently coupled organic group to be covalently coupled with the protein.

[0046] The antigen or antibody stock solution takes procalcitonin (PCT) antibody solution as an example, and its concentration is 20ug / ml.

[0047] The blocking solution can be a known feasible material, such as BSA blocking solution, which is not limited here. The first cleaning solution and the second cleaning solution can be a known feasible material, such as PBST solution, which is not limited here.

[0048] The anti-humidity protection liquid can be made of known materials. In the present invention, the anti-humidity protection liquid includes a buffer, a surfactant, a stabilizer and a preservative. More specifically, the anti-humidity protection liquid includes 0.01% to 0.1% (V / V) of a surfactant, 0.01% to 0.1% (V / V) of a preservative, 1% to 20% (m / v) of a stabilizer and 0.01 to 0.1M of a buffer.

[0049] The buffer is mainly used to ensure the pH value of the system, so that it has a certain acidity, so that the anti-wetting protection liquid is positively charged, thereby protecting the organic groups (such as amino, thiol, etc.) in the silane coupling agent from being neutralized or hydrolyzed. The buffer can be an acetic acid-sodium acetate buffer or an MES buffer, preferably an acetic acid-sodium acetate buffer.

[0050] The acetic acid-sodium acetate buffer keeps the pH value of the anti-humidity protection liquid at about 4.0 to 6.5. This is because the inventors found that when the pH value exceeds 6.5, the silane adhesive will be hydrolyzed or neutralized, causing its surface to lose hydrophobicity and unable to fix substances such as proteins; and when the pH value is lower than 4.0, it will cause excessive acidity, and the fixed protein substances will be denatured and inactivated. At the same time, when the pH value is lower, for example, when the pH value is greater than 4.0 and less than 5.5, the acetic acid-sodium acetate buffer has a stronger buffering capacity and can better resist interference from most samples, air or moisture.

[0051] The surfactant is mainly used to reduce the surface tension of the glass fiber probe, form micelles on the surface of the glass fiber probe, and protect the hydrophobic groups inside the micelles to prevent the immobilized enzymes or protein substances from denaturing. Preferably, the surfactant is at least one of Triton X-100, Triton X-405 and Tween-20, preferably Tween-20, which can increase hydrophilicity and prevent non-specific binding. The inventors have found through research that when the Tween-20 is too little, it cannot resist non-specific binding, and when it is too much, it will affect the binding between proteins.

[0052] The stabilizer is mainly used to keep the immobilized enzymes or proteins relatively stable and prevent them from being denatured or inactivated due to surface treatment measures. The stabilizer is at least one of trehalose, mannitol, and sucrose, preferably sucrose, because sucrose has better water solubility and stability, and forms a coating on the surface of the matrix to isolate the air, thereby protecting the proteins bound to the silane adhesive and preventing them from being oxidized and denatured by air.

[0053] The anti-humidity protection liquid is prepared according to the optimal formula, and the preparation process is as follows:

[0054] S1, prepare corresponding amounts of sucrose, glacial acetic acid, Tween-20, preservatives, purified water and sodium hydroxide solution according to the recipe;

[0055] S2, placing sucrose in a container, adding glacial acetic acid, Tween-20, and a preservative, and then adding purified water to a specified volume to obtain a mixture;

[0056] S3, stirring the mixture obtained in S2 by a magnetic stirrer;

[0057] S4, adding sodium hydroxide solution to the stirred mixed solution to adjust the pH value of the mixed solution to a target range, and then fixing the volume to a target volume to obtain an anti-moisture protection solution.

[0058] After all the required materials are prepared, the glass fiber probe is coated. Correspondingly, S30 includes the following steps:

[0059] The glass fiber probes deposited with the silane coupling agent are installed in the probe bracket. The distribution pattern of the glass fiber probes on the probe bracket is consistent with the hole distribution pattern and hole spacing of the 96-well plate.

[0060] The phosphate buffer solution for coating, PCT antibody solution, blocking solution, first cleaning solution, second cleaning solution and anti-wetting protection solution were dispensed into a 96-well plate at 250 ul each.

[0061] Fix a 96-well plate filled with phosphate buffer solution on a shaking table, fix a probe holder on the shaking table, and immerse the glass fiber probe on the probe holder in the phosphate buffer solution of the 96-well plate. The shaking table shakes at a set speed for a first target time, which can be designed as needed, such as 10 seconds.

[0062] After the shaking table shakes for the first target time, remove the probe holder and the 96-well plate containing phosphate buffer solution from the shaking table; fix the 96-well plate containing PCT antibody solution on the shaking table, fix the probe holder on the shaking table, and immerse the glass fiber probe on the probe holder in the phosphate buffer solution of the 96-well plate, and shake the shaking table at a set speed for the second target time. The second target time can be designed as needed, preferably between 170-200 seconds, and preferably around 180 seconds.

[0063] After the shaking table shakes for the second target time, remove the probe holder and the 96-well plate containing the PCT antibody solution from the shaking table; fix the 96-well plate containing the blocking solution on the shaking table, fix the probe holder on the shaking table, and immerse the glass fiber probe on the probe holder in the blocking solution of the 96-well plate. The shaking table shakes at a set speed for the third target time. The third target time can be designed as needed, and is preferably around 60 seconds.

[0064] After the shaking table has been shaking for the third target time, remove the probe holder and the 96-well plate filled with blocking solution from the shaking table; fix the 96-well plate filled with the first cleaning solution (PBST solution) on the shaking table, fix the probe holder on the shaking table, and immerse the glass fiber probe on the probe holder in the first cleaning solution of the 96-well plate, and shake the shaking table at a set speed for the fourth target time. The fourth target time can be designed as needed, and is preferably about 10 seconds here.

[0065] After the shaking table shakes for the fourth target time, remove the probe holder and the 96-well plate containing the first cleaning solution from the shaking table; fix the 96-well plate containing the second cleaning solution (PBST solution) on the shaking table, fix the probe holder on the shaking table, and immerse the glass fiber probe on the probe holder in the second cleaning solution of the 96-well plate, and shake the shaking table at a set speed for the fourth target time. The fourth target time can be designed as needed, and is preferably about 10 seconds here.

[0066] After the shaking table has shaken for the fifth target time, remove the probe holder and the 96-well plate containing the second cleaning solution from the shaking table; fix the 96-well plate containing the anti-moisture protection solution on the shaking table, fix the probe holder on the shaking table, and immerse the glass fiber probe on the probe holder in the anti-moisture protection solution of the 96-well plate. The shaking table shakes at a set speed for the sixth target time. The sixth target time can be designed as needed, preferably between 20-40 seconds, and more preferably 30 seconds. After the processing is completed, remove the probe holder from the shaking table.

[0067] When drying, take the test probe out of the probe holder and dry it at 40°C for about 4 hours. The drying can be done in a drying oven.

[0068] The formula of the anti-humidity protection liquid of the present invention is analyzed below in conjunction with specific embodiments:

[0069] The reagents involved in the following examples are:

[0070] Sucrose, purity>98%, Sigma brand corresponding products can be used;

[0071] Tween-20, you can use the corresponding product of Sigma brand;

[0072] Glacial acetic acid, purity>99.9995%, using the corresponding product produced by Sinopharm Group;

[0073] Sodium hydroxide solution, purity>96%, can be AR, the corresponding product produced by Sinopharm Group;

[0074] Proclin300 (preservative), corresponding products of Sigma brand can be used.

[0075] Example 1

[0076] Taking the preparation of 1L of anti-humidity protection liquid as an example, its specific components and contents are as follows:

[0077] Component name content sucrose 150g glacial acetic acid 6mL Tween-20 0.5mL Proclin300 0.5mL Sodium hydroxide solution Adjust pH to the specified range Purified water Make up to 1L

[0078] The specific configuration process is as follows:

[0079] Weigh 150g of sucrose using an electronic balance and put it into a beaker;

[0080] Add 6 mL of glacial acetic acid, 0.5 mL of Tween-20, 0.5 mL of proclin 300 to a beaker, and then add purified water to 900 mL to obtain a mixture.

[0081] After the mixture was stirred and mixed by a magnetic stirrer, the pH value was adjusted to a corresponding range with a 10N NaOH solution, and the volume was fixed to 1 L with a volumetric flask to obtain the anti-moisture protection solution.

[0082] Example 2

[0083] Taking the preparation of 1L of anti-humidity protection liquid as an example, its specific components and contents are as follows:

[0084] Component name content sucrose 200g glacial acetic acid 3mL Tween-20 1mL Proclin300 1mL Sodium hydroxide solution Adjust pH to the specified range Purified water Make up to 1L

[0085] The preparation process of the anti-humidity protection liquid in Example 2 is the same as that in Example 1, and will not be described in detail here.

[0086] Example 3

[0087] Taking the preparation of 1L of anti-humidity protection liquid as an example, its specific components and contents are as follows:

[0088] Component name content sucrose 50g glacial acetic acid 1.5mL Tween-20 0.1mL Proclin300 0.1mL Sodium hydroxide solution Adjust pH to the specified range Purified water Make up to 1L

[0089] The preparation process of the anti-humidity protection liquid in Example 3 is the same as that in Example 1, which will not be described in detail here.

[0090] According to the formula and configuration formula of the above-mentioned embodiment 1 to embodiment 3, three kinds of anti-moisture protection liquids are prepared and set aside for use.

[0091] In order to test the effect of the anti-moisture protection liquid, a test probe was prepared according to the above-mentioned test probe preparation method. For the convenience of comparison, the test probes coated with ordinary buffer solution and the test probes coated with the anti-moisture protection liquid of the above three embodiments were exposed to an environment of about 87% humidity prepared by saturated potassium chloride for about 4 hours, 8 hours, 24 hours, and 48 hours respectively.

[0092] Then, the above-mentioned test probes are used to perform immunodetection and compare the detected fluorescent signals. For example, the immunodetection can be performed according to the double antibody sandwich method. During the detection, the corresponding cleaning solution, PCT antigen, biotinylated PCT detection antibody, avidin-labeled cyanine dye 5 (SA-cy5), etc. need to be prepared. The specific process of immunodetection is a known technology and is not the innovation of this scheme, so it will not be described here. After the immune reaction, according to the attached Figure 1 Shown are the structure and principle of reading and detecting the fluorescent signal.

[0093] After the immunoassay, the differences in the fluorescence signals were analyzed and detected, as shown in Tables (1), (2) and (3).

[0094] Table (1): Data table of fluorescence signal detected by immunoassay using two test probes treated with the anti-humidity protection solution of Example 1 and the common buffer solution:

[0095]

[0096]

[0097] Table (2): Data table of fluorescence signal detected by immunoassay of two test probes treated with the anti-humidity protection solution of Example 2 and the common buffer solution:

[0098]

[0099]

[0100] Table (3): Data table of fluorescence signal detected by immunoassay using two test probes treated with the anti-humidity protection solution of Example 3 and the common buffer solution:

[0101]

[0102] It can be seen from the data in the above tables (1), (2) and (3) that, compared with the test probes that have not been treated with anti-moisture protection liquid, the test probes that have been treated with anti-moisture protection liquid and stored in a relatively humid environment, when used in immunoassays, have significantly more detection fluorescence signals, and the detection results are more effective and more accurate; and the deviation of different test results is very small and the consistency is high.

[0103] There are many implementation methods of the present invention, and all technical solutions formed by equivalent transformation or equivalent transformation fall within the protection scope of the present invention.

Claims

1. A method for preparing a moisture-resistant immune detection glass fiber probe, characterized in that: The steps include: S10, depositing a silane coupling agent on the surface of the glass fiber probe; S20, preparing the phosphate buffer solution, antibody or antigen solution, blocking solution, cleaning solution and anti-wetting protection solution required for coating the glass fiber probe; the anti-wetting protection solution includes 5%-20% (m / v) sucrose, 0.015-0.03 (v / v) glacial acetic acid, 0.01%-0.1% (v / v) Tween-20, preservative, purified water and sodium hydroxide solution, and the pH value of the anti-wetting protection solution is between 4.0 and 6.5; S30, immersing the area on the glass fiber probe where the silane coupling agent is deposited in the phosphate buffer solution, the antibody or antigen solution, the blocking solution, the first cleaning solution, the second cleaning solution and the anti-wet protection solution in sequence for a certain period of time to complete the antigen or antibody coating; S40, drying the coated glass fiber probe to obtain a moisture-resistant immunoassay glass fiber probe.

2. The preparation method according to claim 1, characterized in that: In the above S30, when the glass fiber probe is immersed in any liquid, the container containing the liquid and the bracket fixing the glass fiber probe are shaken by the shaking table.

3. The preparation method according to any one of claims 1-2, characterized in that: The glass fiber probe stays in the anti-wetting buffer for 20-40 seconds.

4. An anti-humidity protection liquid for a glass fiber probe with a silane coupling agent deposited on the surface, characterized in that: include 5%-20% (m / v) sucrose; 0.015-0.03 (v / v) glacial acetic acid; 0.01% to 0.1% (v / v) Tween-20; preservative; Purified water; Sodium hydroxide solution, The pH value of the anti-humidity protection liquid is between 4.0 and 6.

5.

5. The method for preparing the anti-humidity protection liquid according to claim 4, characterized in that: The steps include: S1, prepare corresponding amounts of sucrose, glacial acetic acid, Tween-20, preservatives, purified water and sodium hydroxide solution according to the recipe; S2, placing sucrose in a container, adding glacial acetic acid, Tween-20, and a preservative, and then adding purified water to a specified volume to obtain a mixture; S3, stirring the mixture obtained in S2 by a magnetic stirrer; S4, adding sodium hydroxide solution to the stirred mixed solution to adjust the pH of the mixed solution to a target range, and then fixing the volume to a target volume to obtain an anti-moisture protection solution.

Citation Information

Patent Citations

  • Novel biological chip substrate as well as preparation method and application thereof

    CN108503565A

  • Analysis method of silane-coupling agent aqueous solution, and manufacturing method of humidity sensor element using the same

    JP2005077233A

  • Probe carrier, method for producing the same and method for preserving the same

    JP2006149337A

  • Probe carrier and probe medium and method for manufacturing the same

    JP2006170832A

  • Multi-analyte microarrays using tag-specific antibodies and tag-anchored antibodies

    US20130310277A1