Negative electrode active material, negative electrode layer and fluoride ion secondary battery
By using the composite of AlF3, Li3AlF6 and Li2ZrF6 as the negative active material, the problem of insufficient charge and discharge capacity caused by the insulation of the negative active material of the fluoride ion secondary battery is solved, and the battery performance is improved.
Patent Information
- Application Number
- CN202210027655.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-01-11
AI Technical Summary
Aluminum fluoride, the negative active material of fluoride ion secondary batteries, has insulating properties and is difficult to undergo electrochemical reactions, resulting in insufficient charge and discharge capacity.
A composite of AlF3, Li3AlF6 and Li2ZrF6 is used as the negative electrode active material. By controlling the molar ratio and particle size, the ion conductivity and voltage stability of the negative electrode layer are improved, thereby enhancing the charge and discharge capacity.
The charge and discharge capacity of the fluoride ion secondary battery is significantly improved, the voltage stability is improved, and the overall performance of the battery is enhanced.
Smart Images

Figure HDA0003464846430000011 
Figure HDA0003464846430000021 
Figure HDA0003464846430000031
Abstract
Description
Technical Field
[0001] The invention relates to a negative electrode active material, a negative electrode layer and a fluoride ion secondary battery. Background Art
[0002] Conventionally, lithium ion secondary batteries are widely used as secondary batteries having high energy density. In lithium ion secondary batteries, a separator is arranged between a positive electrode and a negative electrode, and an electrolyte is filled therein.
[0003] The electrolyte of a lithium ion secondary battery generally contains a flammable organic solvent, and therefore safety against heat may become a problem.
[0004] Therefore, fluoride ion secondary batteries are being studied as all-solid batteries in which a solid electrolyte layer is disposed between a positive electrode layer and a negative electrode layer (for example, see Patent Documents 1 to 6).
[0005] [Prior Technical Literature]
[0006] (Patent Document)
[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-87403
[0008] Patent Document 2: Japanese Patent Application Publication No. 2017-50113
[0009] Patent Document 3: Japanese Patent Application Publication No. 2019-29206
[0010] Patent Document 4: Japanese Patent Application Publication No. 2018-206755
[0011] Patent Document 5: Japanese Patent Application Publication No. 2018-198130
[0012] Patent Document 6: Japanese Patent Application Publication No. 2018-92863 Summary of the invention
[0013] [Problems to be solved by the invention]
[0014] Aluminum fluoride is being studied as a negative electrode active material for fluoride ion secondary batteries, but aluminum fluoride has insulating properties and thus is difficult to undergo electrochemical reactions.
[0015] Therefore, the applicant of this case proposed to use Li3AlF6 as the negative electrode active material of the fluoride ion secondary battery, but people hope to further improve the charge and discharge capacity of the fluoride ion secondary battery.
[0016] An object of the present invention is to provide a negative electrode active material capable of improving the charge and discharge capacity of a fluoride ion secondary battery.
[0017] [Technical means to solve the problem]
[0018] One aspect of the present invention is a negative electrode active material comprising AlF3, Li3AlF6 and Li2ZrF6.
[0019] The negative electrode active material may include a composite of AlF3, Li3AlF6 and Li2ZrF6.
[0020] Another aspect of the present invention is a negative electrode layer comprising the negative electrode active material.
[0021] Another aspect of the present invention is a fluoride ion secondary battery having the above-mentioned negative electrode layer, an electrolyte, and a positive electrode layer.
[0022] (Effects of the Invention)
[0023] According to the present invention, it is possible to provide a negative electrode active material capable of improving the charge and discharge capacity of a fluoride ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the X-ray diffraction (XRD) spectrum of the AlF3-Li3AlF6-Li2ZrF6 composite of Example 1.
[0025] Figure 2 These are the scanning electron microscope (SEM) photographs and electron probe microanalyzer (EPMA) analysis results of the AlF3-Li3AlF6-Li2ZrF6 complex of Example 1.
[0026] Figure 3 The graph shows the initial charge and discharge curves of the all-solid fluoride ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0027] Hereinafter, embodiments of the present invention will be described.
[0028] <Negative electrode active material>
[0029] The negative electrode active material of the present embodiment includes AlF 3 , Li 3 AlF 6 and Li 2 ZrF 6 . Therefore, when the negative electrode active material of the present embodiment is applied to a fluoride ion secondary battery, the charge and discharge capacity is improved.
[0030] Here, during charging, Li2ZrF6 is defluorinated earlier than AlF3 and Li3AlF6, so that the voltage of the fluoride ion secondary battery is stabilized. As a result, AlF3 and Li3AlF6 become easier to defluorinate, thereby improving the charge and discharge capacity of the fluoride ion secondary battery.
[0031] The molar ratio of Li3AlF6 to AlF3 is preferably 0.1 or more, and more preferably 0.5 or more. When the molar ratio of Li3AlF6 to AlF3 is 0.1 or more, Li3AlF6 comes into contact with inert AlF3 more, so defluorination of AlF3 becomes more likely to occur.
[0032] The molar ratio of Li2ZrF6 to AlF3 is preferably 0.1 or more and 3 or less, and more preferably 0.3 or more and 1.5 or less. When the molar ratio of Li2ZrF6 to AlF3 is 0.1 or more, the contact between Li2ZrF6 and inert AlF3 increases, and the voltage stability of the fluoride ion secondary battery is improved, so defluorination of AlF3 becomes easy to occur. In addition, when the molar ratio of Li2ZrF6 to AlF3 is 3 or less, the capacity and voltage of the fluoride ion secondary battery are improved.
[0033] The negative electrode active material of the present embodiment may further contain negative electrode active materials other than AlF, Li3AlF6 and Li2ZrF6.
[0034] The negative electrode active material other than AlF, Li3AlF6 and Li2ZrF6 is not particularly limited as long as it is a negative electrode active material that can be used for a fluoride ion secondary battery.
[0035] [Compounds of AlF3, Li3AlF6 and Li2ZrF6]
[0036] The negative electrode active material of this embodiment may also include a composite of AlF 3 , Li 3 AlF 6 and Li 2 ZrF 6 . Thus, the charge and discharge capacity of the negative electrode active material of this embodiment when applied to a fluoride ion secondary battery is improved.
[0037] In the composite of AlF3, Li3AlF6 and Li2ZrF6, for example, at least a portion of the surface of AlF3 and Li3AlF6 is coated with Li2ZrF6.
[0038] The particle size of the composite of AlF3, Li3AlF6 and Li2ZrF6 is preferably 1 mm or less, more preferably 200 μm or less. When the particle size of the composite of AlF3, Li3AlF6 and Li2ZrF6 is 1 mm or less, it is easy to form a uniform powder when preparing the powder composition for the negative electrode layer.
[0039] [Method for producing a composite of AlF3, Li3AlF6 and Li2ZrF6]
[0040] The composite of AlF3, Li3AlF6 and Li2ZrF6 is obtained by crushing AlF3, LiF and ZrF4 and then calcining them. At this time, LiF and ZrF4 react with a molar ratio of 2:1 to generate Li2ZrF6, and the remaining LiF reacts with AlF3 with a molar ratio of 3:1 to generate Li3AlF6, and there is residual AlF3.
[0041] The molar ratio of LiF to AlF3 is preferably 1 to 5. When the molar ratio of LiF to AlF3 is 1 to 5, the ion conductivity of the composite of AlF3, Li3AlF6 and Li2ZrF6 increases, so defluorination of AlF3 becomes easy to occur.
[0042] The molar ratio of ZrF4 to AlF3 is preferably 0.1 or more and 3 or less, and more preferably 0.3 or more and 1.5 or less. When the molar ratio of ZrF4 to AlF3 is 0.1 or more, the ion conductivity of the composite of AlF3, Li3AlF6 and Li2ZrF6 becomes high, so defluorination of AlF3 becomes easy to occur. In addition, when the molar ratio of ZrF4 to AlF3 is 3 or less, the capacity and voltage of the fluoride ion secondary battery are improved.
[0043] Examples of a method for pulverizing AlF 3 , LiF and ZrF 4 include a method of pulverizing using a ball mill.
[0044] The calcination temperature is preferably 850° C. or higher and 900° C. or lower. When the calcination temperature is 850° C. or higher, the reaction proceeds sufficiently, and when the calcination temperature is 900° C. or lower, evaporation of the raw material is suppressed.
[0045] The calcination time is preferably 1 hour or more and 3 hours or less. When the calcination time is 1 hour or more, the reaction proceeds sufficiently, and when the calcination time is 3 hours or less, evaporation of the raw material is suppressed.
[0046] <Negative electrode layer>
[0047] The negative electrode layer of the present embodiment contains the negative electrode active material of the present embodiment, and may further contain a conductive auxiliary agent, a solid electrolyte, and the like.
[0048] The total content of AlF3, Li3AlF6 and Li2ZrF6 in the negative electrode layer of the present embodiment is preferably 50% by mass or less, and more preferably 30% by mass or less. When the total content of AlF3, Li3AlF6 and Li2ZrF6 in the negative electrode layer of the present embodiment is 50% by mass or less, the charge and discharge capacity of the negative electrode layer of the present embodiment when applied to a fluoride ion secondary battery is improved.
[0049] [Conductive additive]
[0050] Examples of the conductive additive include carbon materials and the like.
[0051] The carbon material may also be carbon black.
[0052] Examples of carbon black include furnace black, Ketjen black, and acetylene black, and two or more types of carbon black may be used in combination.
[0053] [Solid Electrolyte]
[0054] Examples of the solid electrolyte include lanthanide fluorides doped with alkaline earth metal fluorides, alkaline earth metal fluorides, etc. Among these, lanthanide fluorides doped with alkaline earth metal fluorides are preferred in terms of ion conductivity.
[0055] The lanthanoid fluoride is not particularly limited, and examples thereof include LaF 3 , CeF 3 , SmF 3 , and NdF 3 . Two or more kinds of lanthanoid fluorides may be used in combination.
[0056] The alkaline earth metal fluoride doped with the lanthanoid fluoride is not particularly limited as long as it has ion conductivity, and examples thereof include CaF 2 , SrF 2 , and BaF 2 , and two or more thereof may be used in combination.
[0057] Examples of the lanthanide fluoride doped with the alkaline earth metal fluoride include La 0.9 Ba 0.1 F 2.9 、Ce 0.95 Ba 0.05 F 2.95 、Ce 0.95 Sr 0.05 F 2.95 、Ce 0.95 Ca 0.05 F 2.95 etc., and two or more kinds may be used in combination.
[0058] In the case where the negative electrode layer of the present embodiment includes a carbon material as a conductive aid, the lanthanum fluoride doped with alkaline earth metal fluoride may also be composited with the carbon material. That is, the negative electrode layer of the present embodiment may also include a composite of lanthanum fluoride doped with alkaline earth metal fluoride and a carbon material (hereinafter also referred to as a composite of lanthanum fluoride and a carbon material).
[0059] [Composite of lanthanide fluoride and carbon material]
[0060] In the composite of lanthanoid fluoride and carbon material, for example, at least a part of the surface of lanthanoid fluoride particles is coated with the carbon material.
[0061] The particle size of the composite of lanthanoid fluoride and carbon material is preferably 10 μm or less, more preferably 5 μm or less. When the particle size of the composite of lanthanoid fluoride and carbon material is 10 μm or less, ion conductivity and electron conductivity are improved.
[0062] From the viewpoint of the balance between ion conductivity and electron conductivity, the mass ratio of the carbon material to the lanthanoid fluoride doped with the alkaline earth metal fluoride is preferably 3 mass % or more and 20 mass % or less.
[0063] The content of the complex of lanthanum fluoride and carbon material in the negative electrode layer of the present embodiment is preferably 60 mass % or more and 70 mass % or less. When the content of the complex of lanthanum fluoride and carbon material in the negative electrode layer of the present embodiment is 60 mass % or more and 70 mass % or less, the discharge capacity when the negative electrode layer of the present embodiment is applied to a fluoride ion secondary battery is improved.
[0064] [Method for producing a composite of lanthanide fluoride and carbon material]
[0065] The method for manufacturing a composite of lanthanide fluoride and carbon material (hereinafter also referred to as composite) includes: a first step of obtaining a lanthanide fluoride-alkaline earth metal fluoride mixed powder; a second step of mixing the lanthanide fluoride-alkaline earth metal fluoride mixed powder with a carbon material to obtain a composite precursor; and a third step of calcining the composite precursor to obtain a composite.
[0066] The first step is to mix the lanthanide fluoride and the alkaline earth metal fluoride to obtain a lanthanide fluoride-alkaline earth metal fluoride mixed powder. That is, by mixing the lanthanide fluoride and the alkaline earth metal fluoride, the solid phase diffusion distance of the elements derived from the lanthanide fluoride and the alkaline earth metal fluoride can be shortened during calcination. In addition, after calcination, a lanthanide fluoride-alkaline earth metal fluoride mixed powder can be obtained in which the crystal structure of the lanthanide fluoride and the alkaline earth metal fluoride remains.
[0067] The method for mixing the lanthanoid fluoride and the alkaline earth metal fluoride is not particularly limited, and either a dry method or a wet method may be used. For example, a method of mixing using a mortar may be mentioned.
[0068] Furthermore, the conditions such as temperature and time for mixing the lanthanoid fluoride and the alkaline earth metal fluoride can be appropriately set.
[0069] In addition, in the first step, the lanthanide fluoride-alkaline earth metal fluoride mixed powder may be pulverized.
[0070] Examples of a method for pulverizing the lanthanoid fluoride-alkaline earth metal fluoride mixed powder include a method of pulverizing using a ball mill.
[0071] The second step is a step of mixing the lanthanide fluoride-alkaline earth metal fluoride mixed powder obtained in the first step with a carbon material to obtain a composite precursor.
[0072] The method for producing the composite body is to perform the second step in the pre-stage of the third step, and pre-mix the carbon material in the lanthanide fluoride-alkaline earth metal fluoride mixed powder, thereby obtaining a composite body precursor in which the carbon material is arranged on the surface of the lanthanide fluoride-alkaline earth metal fluoride mixed powder.
[0073] Therefore, in the third step, by calcining the composite precursor, a composite in which at least a part of the surface of the lanthanide fluoride particles doped with the alkaline earth metal fluoride is coated with the carbon material is obtained.
[0074] In addition, in the second step, a carbon material is arranged on the surface of the lanthanide fluoride-alkaline earth metal fluoride mixed powder, thereby suppressing the grain growth of the lanthanide fluoride-alkaline earth metal fluoride mixed powder and the coarsening of the particle size caused by the fusion of the particle interfaces during the crystallization process in the third step, thereby obtaining a composite that roughly maintains the particle size of the lanthanide fluoride-alkaline earth metal fluoride mixed powder.
[0075] In the second step, the method for mixing the lanthanide fluoride-alkaline earth metal fluoride mixed powder and the carbon material is not particularly limited, and either a dry method or a wet method may be used, and for example, a method of mixing using a mortar may be used.
[0076] Furthermore, when mixing the lanthanide fluoride-alkaline earth metal fluoride mixed powder and the carbon material, a shear force is preferably applied.
[0077] Furthermore, the conditions such as the temperature for mixing the lanthanoid fluoride-alkaline earth metal fluoride mixed powder and the carbon material can be appropriately set.
[0078] Furthermore, in the second step, the composite precursor may be pulverized.
[0079] Examples of a method for pulverizing the composite precursor include a method of pulverizing using a ball mill and a method of pulverizing using a mortar.
[0080] The third step is a step of calcining the composite precursor obtained in the second step to obtain a composite.
[0081] In the second step, a composite precursor is obtained in which a carbon material is arranged on the surface of the lanthanide fluoride-alkaline earth metal fluoride mixed powder. As a result, during the crystallization process in the third step, the grain growth of the lanthanide fluoride-alkaline earth metal fluoride mixed powder and the coarsening of the particle size caused by the fusion of the particle interfaces are suppressed. As a result, a composite is obtained in which the particle size of the composite precursor is roughly maintained.
[0082] Furthermore, the conditions for calcining the composite precursor can be appropriately set.
[0083] In addition, in the third step, the composite may be pulverized.
[0084] Examples of a method for pulverizing the composite include a method of pulverizing the composite using a mortar.
[0085] <Fluoride ion secondary battery>
[0086] The fluoride ion secondary battery of the present embodiment includes the negative electrode layer of the present embodiment, an electrolyte, and a positive electrode layer.
[0087] [Electrolytes]
[0088] The electrolyte may be an electrolyte solution, a solid electrolyte, or a gel electrolyte. Furthermore, the solid electrolyte or the gel electrolyte may be organic or inorganic.
[0089] As the solid electrolyte, a known solid electrolyte can be used. For example, as the solid electrolyte, the solid electrolyte included in the negative electrode layer of the present embodiment can also be used.
[0090] When a solid electrolyte is used as the electrolyte, the fluoride ion secondary battery of the present embodiment becomes an all-solid fluoride ion secondary battery. The all-solid fluoride ion secondary battery includes, for example, a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, a negative electrode layer, and a negative electrode current collector in this order.
[0091] [Positive electrode layer]
[0092] The positive electrode layer includes, for example, a positive electrode active material, a solid electrolyte, and a conductive aid. In this case, it is preferable to use a positive electrode layer that can obtain a sufficiently high standard electrode potential relative to the standard electrode potential of the negative electrode layer of this embodiment.
[0093] Examples of the positive electrode active material include Pb, Cu, Sn, Bi, and Ag.
[0094] Examples of solid electrolytes include PbSnF4, Ce 1-x Ba x F 3-x wait.
[0095] Examples of the conductive additive include carbon materials and the like.
[0096] [Positive electrode current collector and negative electrode current collector]
[0097] Examples of the positive electrode current collector include lead plates, aluminum foils, and the like, and examples of the negative electrode current collector include gold foils and the like.
[0098] [Example]
[0099] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the examples.
[0100] [Example 1]
[0101] An all-solid fluoride ion secondary battery was produced by the following method. Unless otherwise specified, each step was carried out in a purge-type glove box DBO-1.5B (manufactured by Miwa Seisakusho) equipped with an argon gas circulation purification device.
[0102] [Preparation of AlF3-Li3AlF6-Li2ZrF6 composite]
[0103] 4.7 g of AlF3 powder, 4.4 g of LiF powder, 0.9 g of ZrF4 powder, and 20 10 mm diameter silicon nitride grinding balls (manufactured by Fritsch) were placed in a premium line PL-7 dedicated container (manufactured by Fritsch) which is an 80 cc silicon nitride ball mill pot, and then sealed. Here, the molar ratio of AlF3, LiF, and ZrF4 is 1:3:0.5.
[0104] After the sealed ball mill pot was carried out of the glove box, a pulverization treatment was performed using a ball mill. At this time, the pulverization treatment conditions were as described below.
[0105] Speed: 400rpm
[0106] Crushing time: 15 minutes
[0107] Crushing times: 40 times
[0108] Rest time during crushing process: 5 minutes
[0109] Rotation reversing (reverse): open (ON)
[0110] After the ball mill tank was moved into the glove box, the AlF3-Li3AlF6-Li2ZrF6 mixed powder was recovered from the inside of the ball mill tank.
[0111] After the AlF3-Li3AlF6-Li2ZrF6 mixed powder was transferred into an alumina crucible, it was calcined using a small electric furnace KSL-1100X (manufactured by MTI) to obtain an AlF3-Li3AlF6-Li2ZrF6 composite. At this time, the calcination conditions were as described below.
[0112] Argon flow rate: 300cc / min (minute)
[0113] Heating rate: 184℃ / h (hour)
[0114] Maximum temperature reached: 900℃
[0115] Holding time at maximum temperature: 1 hour
[0116] Cooling speed: no control
[0117] Cooling method: Natural cooling
[0118] After the AlF3-Li3AlF6-Li2ZrF6 complex was recovered from the inside of the alumina crucible, it was pulverized for 5 to 10 minutes using an agate mortar and pestle.
[0119] The AlF3-Li3AlF6-Li2ZrF6 composite was analyzed using XRD.
[0120] exist Figure 1 The XRD spectrum of AlF3-Li3AlF6-Li2ZrF6 complex is shown in Figure 1 The XRD spectra of AlF3, LiF, ZrF4, Li3AlF6 and Li2ZrF6 are also shown.
[0121] Depend on Figure 1 It can be seen that in the XRD spectrum of the AlF3-Li3AlF6-Li2ZrF6 complex, the peaks originating from the raw materials LiF and ZrF4 disappear, and the peaks originating from the products Li3AlF6 and Li2ZrF6 appear.
[0122] The AlF3-Li3AlF6-Li2ZrF6 complex was observed using a scanning electron microscope-electron probe micro analyzer (SEM-EPMA). At this time, the elements mapped were Al and Zr.
[0123] exist Figure 2 The SEM photograph and EPMA analysis results of the AlF3-Li3AlF6-Li2ZrF6 complex are shown in FIG.
[0124] Depend on Figure 2 It can be seen that in the AlF3-Li3AlF6-Li2ZrF6 complex, the surfaces of AlF3 and Li3AlF6 are coated with Li2ZrF6.
[0125] [Ce 0.95 Ba 0.05 F 2.95 -Production of AB complex]
[0126] (First step)
[0127] After weighing 8.598 g of CeF3 powder (manufactured by Sigma-Aldrich; purity 99.99%) and 0.402 g of BaF2 powder (manufactured by High Purity Chemical Research Institute; purity 99.9%), use an agate mortar and pestle to mix for 5 to 10 minutes to obtain a CeF3-BaF2 mixed powder.
[0128] The CeF3-BaF2 mixed powder and 20 silicon nitride grinding balls (manufactured by Feichi) with a diameter of 10 mm were placed in an Advanced Line PL-7 dedicated container (manufactured by Feichi) which was an 80 cc silicon nitride ball mill pot and then sealed.
[0129] After the sealed ball mill pot was carried out of the glove box, a pulverization treatment was performed using a ball mill. At this time, the pulverization treatment conditions were as described below.
[0130] Speed: 800rpm
[0131] Crushing time: 60 minutes
[0132] Crushing times: 40 times
[0133] Rest time during crushing process: 5 minutes
[0134] Rotation reversing (reverse): open (ON)
[0135] After the ball mill tank was moved into the glove box, the CeF3-BaF2 mixed powder was recovered from the inside of the ball mill tank.
[0136] (Second step)
[0137] Using an agate mortar and pestle, 700 mg of CeF3-BaF2 mixed powder and 50 mg of acetylene black (AB) (DENKA BLACK) (manufactured by Denka Company Limited) were mixed to obtain CeF3-BaF2 mixed powder. 0.95 Ba 0.05 F 2.95 -AB complex precursor.
[0138] Ce 0.95 Ba 0.05 F 2.95 -AB complex precursor, 20 10mm diameter zirconium oxide grinding balls (manufactured by Fei Chi), and 20 10mm diameter silicon nitride grinding balls (manufactured by Fei Chi) are placed in an advanced production line PL-7 dedicated container (manufactured by Fei Chi) which is an 80cc silicon nitride ball mill pot and then sealed.
[0139] After the sealed ball mill pot was carried out of the glove box, a pulverization treatment was performed using a ball mill. At this time, the pulverization treatment conditions were as described below.
[0140] Speed: 800rpm
[0141] Crushing time: 60 minutes
[0142] Crushing times: 40 times
[0143] Rest time during crushing process: 5 minutes
[0144] Rotation reversing (reverse): open (ON)
[0145] After the ball mill is moved into the glove box, Ce is recovered from the inside of the ball mill. 0.95 Ba 0.05 F 2.95 -AB complex precursor. Using an agate mortar and pestle, the recovered Ce 0.95 Ba 0.05 F 2.95 -AB complex precursor is crushed for 5 to 10 minutes.
[0146] (Third step)
[0147] Ce 0.95 Ba 0.05 F 2.95The AB composite precursor was transferred into an alumina crucible and calcined using a small electric furnace KSL-1100X (manufactured by MTI) to obtain Ce 0.95 Ba 0.05 F 2.95 -AB complex. At this time, the calcination conditions are as described below.
[0148] Argon flow rate: 300cc / min (minute)
[0149] Heating rate: 184℃ / h (hour)
[0150] Maximum temperature reached: 1100℃
[0151] Holding time at maximum temperature: 1 hour
[0152] Cooling speed: no control
[0153] Cooling method: Natural cooling
[0154] Recovery of Ce from the inside of an alumina crucible 0.95 Ba 0.05 F 2.95 -AB complex, and then pulverize it for 5 to 10 minutes using an agate mortar and pestle.
[0155] [Preparation of powder composition for negative electrode layer]
[0156] 250 mg of AlF3-Li3AlF6-Li2ZrF6 complex and Ce 0.95 Ba 0.05 F 2.95 750 mg of the AB complex and 40 g of silicon nitride grinding balls (manufactured by Feichi) having a diameter of 2 mm were placed in a 45 cc silicon nitride ball mill pot of Advanced Line PL-7 dedicated container (manufactured by Feichi), and then sealed.
[0157] After the sealed ball mill pot was carried out of the glove box, a pulverization treatment was performed using a ball mill. At this time, the pulverization treatment conditions were as described below.
[0158] Speed: 300rpm
[0159] Crushing time: 15 minutes
[0160] Crushing times: 40 times
[0161] Rest time during crushing process: 5 minutes
[0162] Rotation reversing (reverse): open (ON)
[0163] After the ball mill pot was moved into the glove box, the negative electrode layer powder composition was recovered from the inside of the ball mill pot.
[0164] [Preparation of powder for positive electrode layer (PbSnF4-AB complex)]
[0165] 63.7 mass % of lead fluoride powder (manufactured by High Purity Chemical), 29.6 mass % of tin fluoride powder (manufactured by High Purity Chemical), and 6.7 mass % of DENKA BLACK (manufactured by Denka Company Limited) as AB were mixed in a ball mill and calcined at 400°C for 1 hour in an argon atmosphere to prepare a PbSnF4-AB composite.
[0166] [Powder for solid electrolyte layer (Ce 0.95 Ba 0.05 F 2.95 )
[0167] (First step)
[0168] After weighing 8.598 g of CeF3 powder (manufactured by Sigma-Aldrich; purity 99.99%) and 0.402 g of BaF2 powder (manufactured by High Purity Chemical Research Institute; purity 99.9%), use an agate mortar and pestle to mix for 5 to 10 minutes to obtain a CeF3-BaF2 mixed powder.
[0169] The CeF3-BaF2 mixed powder and 20 silicon nitride grinding balls (manufactured by Feichi) with a diameter of 10 mm were placed in an Advanced Line PL-7 dedicated container (manufactured by Feichi) which was an 80 cc silicon nitride ball mill pot and then sealed.
[0170] After the sealed ball mill pot was carried out of the glove box, a pulverization treatment was performed using a ball mill. At this time, the pulverization treatment conditions were as described below.
[0171] Speed: 800rpm
[0172] Crushing time: 60 minutes
[0173] Crushing times: 40 times
[0174] Rest time during crushing process: 5 minutes
[0175] Rotation reversing (reverse): open (ON)
[0176] After the ball mill tank was moved into the glove box, the CeF3-BaF2 mixed powder was recovered from the inside of the ball mill tank.
[0177] (Second step)
[0178] The CeF3-BaF2 mixed powder was transferred into an alumina crucible and calcined using a small electric furnace KSL-1100X (manufactured by MTI) to obtain Ce 0.95 Ba 0.05 F 2.95 At this time, the calcination conditions are as follows.
[0179] Argon flow rate: 300cc / min (minute)
[0180] Heating rate: 184℃ / h (hour)
[0181] Maximum temperature reached: 1100℃
[0182] Holding time at maximum temperature: 1 hour
[0183] Cooling speed: no control
[0184] Cooling method: Natural cooling
[0185] Recovery of Ce from the inside of an alumina crucible 0.95 Ba 0.05 F 2.95 Then, use an agate mortar and pestle to grind for 5 to 10 minutes.
[0186] [Fabrication of all-solid fluoride ion secondary battery]
[0187] A tablet forming machine was used to press at a pressure of 40 MPa to produce a cylindrical pellet-type cell formed by powder pressing. Specifically, a gold foil (manufactured by Nilaco; purity 99.99%) with a thickness of 20 μm as a negative electrode collector, 10 mg of a powder composition for a negative electrode layer, 150 mg of a solid electrolyte layer powder, 20 mg of a positive electrode layer powder, a lead plate (manufactured by Nilaco; purity 99.99%) with a thickness of 200 μm as a positive electrode active material and a positive electrode collector, and an aluminum foil (manufactured by Nilaco; purity 99+%) with a thickness of 20 μm as a positive electrode collector were put into a tablet forming machine in this order to produce a pellet-type cell.
[0188] [Example 2]
[0189] When preparing the powder composition for the negative electrode layer, a mixture of 28 mg of AlF3 powder, 110 mg of Li3AlF6 powder and 112 mg of Li2ZrF6 powder (molar ratio 0.5:1:0.8) was used instead of 250 mg of AlF3-Li3AlF6-Li2ZrF6 complex, and the pulverizing conditions were changed as follows. Otherwise, an all-solid fluoride ion secondary battery was prepared in the same manner as in Example 1.
[0190] Speed: 300rpm
[0191] Crushing time: 15 minutes
[0192] Crushing times: 40 times
[0193] Rest time during crushing process: 5 minutes
[0194] Rotation reversing (reverse): open (ON)
[0195] [Comparative Example 1]
[0196] An all-solid fluoride ion secondary battery was produced in the same manner as in Example 2, except that Li3AlF6 powder was used instead of the mixture of AlF3 powder, Li3AlF6 powder and Li2ZrF6 powder when producing the powder composition for the negative electrode layer.
[0197] [Comparative Example 2]
[0198] An all-solid fluoride ion secondary battery was produced in the same manner as in Example 2, except that Li2ZrF6 powder was used instead of AlF3 powder or a mixture of Li3AlF6 powder and Li2ZrF6 powder when producing the powder composition for the negative electrode layer.
[0199] [AlF3-Li3AlF6-Li2ZrF6 complex and Ce 0.95 Ba 0.05 F 2.95 -AB complex particle size]
[0200] The powder was photographed using a scanning electron microscope SU-6600 (manufactured by Hitachi High-technologies), and the length of the powder in the SEM image of multiple fields of view was measured to obtain the particle size.
[0201] As a result, AlF3-Li3AlF6-Li2ZrF6 complex and Ce 0.95 Ba 0.05 F 2.95 The particle sizes of the -AB complex are 200 μm and 50 μm, respectively.
[0202] [Charge and discharge test]
[0203] A constant current charge and discharge test of an all-solid fluoride ion secondary battery was performed. Specifically, a potential constant current instrument (Potentio galvanostat) SI1287 / 1255B (manufactured by Solartron) was used, and the current during charging was set to 0.04 mA, the current during discharging was set to 0.02 mA, and the lower limit voltage was set to -2.44 V and the upper limit voltage was set to -0.1 V. The constant current charge and discharge test was performed starting from charging in a vacuum environment at 140°C.
[0204] exist Figure 3 Graphs showing the initial charge and discharge curves of the all-solid fluoride ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2.
[0205] Depend on Figure 3 It can be seen that the all-solid fluoride ion secondary batteries of Examples 1 and 2 have higher charge and discharge capacities than the all-solid fluoride ion secondary batteries of Comparative Examples 1 and 2.
Claims
1. A negative electrode active material comprising AlF3, Li3AlF6 and Li2ZrF6.
2. The negative electrode active material according to claim 1, wherein A complex comprising AlF3, Li3AlF6 and Li2ZrF6. 3 . A negative electrode layer comprising the negative electrode active material according to claim 1 . 4 . A fluoride ion secondary battery comprising the negative electrode layer according to claim 3 , an electrolyte and a positive electrode layer.
Citation Information
Patent Citations
Fluoride ion battery
JP2017050113A
Fluoride ion all solid state battery
JP2018092863A
Fluoride ion battery
JP2018198130A
Positive electrode active material and fluoride ion battery
JP2018206755A
Fluoride ion battery
JP2019029206A