Optical laminate and method for producing display device

By optimizing the relationship between the adhesive layer and the base film in the optical laminate to meet specific peeling force and thickness ratio, the problem of difficulty in peeling off the surface protective film during peeling is solved, and stable peeling and lamination of the optical laminate is achieved. , simplifying the process and ensuring the quality of the optical laminate.

CN115023635BActive Publication Date: 2024-10-29SUMITOMO CHEM CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202080095081.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-10-29
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

In the prior art, it is difficult to suppress the peeling of the surface protective film when peeling off the adhesive layer used to bond the optical laminate, making it difficult to peel off cleanly or causing scratches in subsequent processes.

Method used

By setting a specific relationship between the adhesive layer and the base film in the optical laminate, a specific peel force and thickness ratio are met to ensure that peeling of the surface protective film is not caused when the first base film is peeled off, and optimized adhesion is adopted The material combination of the agent layer and the base film can be adjusted to achieve a stable peeling process by adjusting the thickness and materials of the adhesive layer and base film.

Benefits of technology

It effectively inhibits the peeling of the surface protective film, ensures stable peeling and bonding of the optical laminate, avoids the occurrence of scratches and defects, and simplifies subsequent processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115023635B_ABST
    Figure CN115023635B_ABST
Patent Text Reader

Abstract

The present invention provides an optical laminate, which can suppress the peeling of a surface protective film provided on the surface opposite to the release film when peeling off a release film attached to the surface of an adhesive layer for bonding the optical laminate. The optical laminate comprises a polarizing laminate, a first adhesive layer laminated on the first surface of the polarizing laminate, a first substrate film laminated on the surface of the first adhesive layer opposite to the polarizing laminate, a second adhesive layer laminated on the second surface of the polarizing laminate, and a second substrate film laminated on the surface of the second adhesive layer opposite to the polarizing laminate, and the relationship of the following formula (1a) is satisfied. (A / B)×C≥800(1a).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing an optical layered body and a display device. Background Art

[0002] Japanese Patent Application Publication No. 2010-188550 (Patent Document 1) discloses a roll of an optical film having a first substrate film provided on a first surface via a first adhesive layer and a second substrate film provided on a second surface via a second adhesive layer. After the optical film is cut into a predetermined shape, the first adhesive layer exposed by peeling off the first substrate film is bonded to a display substrate.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-188550 Summary of the invention

[0006] Patent Document 1 describes adjusting the magnitude relationship of the adhesive force at the interface in order to suppress the floating that occurs between the base film and the optical film in a state of being wound into a roll.

[0007] An object of the present invention is to provide an optical laminate that can suppress the peeling of a surface protective film provided on the surface opposite to the release film when peeling the release film attached to the surface of the pressure-sensitive adhesive layer to which the optical laminate is bonded, and a method for producing a display device using the optical laminate.

[0008] The present invention provides the following optical layered body and a method for producing a display device.

[0009] [1] An optical laminate comprising: a polarizing laminate, a first adhesive layer laminated on a first surface of the polarizing laminate, a first substrate film laminated on a surface of the first adhesive layer opposite to the polarizing laminate, a second adhesive layer laminated on a second surface of the polarizing laminate, and a second substrate film laminated on a surface of the second adhesive layer opposite to the polarizing laminate.

[0010] The relationship of the following formula (1a) is satisfied.

[0011] (A / B)×C≥800 (1a)

[0012] [In formula (1a),

[0013] A is a value calculated from A1 / A2 when the 180° peeling force between the polarizing laminate and the second adhesive layer is A1 [gf / 25 mm] and the total thickness of the second substrate film and the second adhesive layer is A2 [μm],

[0014] B is a value calculated from B1 / B2 when the 180° peeling force between the first adhesive layer and the first base film is set to B1 [gf / 25 mm] and the thickness of the first base film is set to B2 [μm].

[0015] C is defined as the rigidity (Gurley unit) of the evaluation laminated body in which the first adhesive layer, the polarizing laminated body, the second adhesive layer, and the second base film are laminated in this order. ]

[0016] [2] The optical layered body according to [1], further satisfying the relationship of the following formula (2a).

[0017] (A / B)×C≤10000 (2a)

[0018] [3] The optical layered body according to [1] or [2], wherein A satisfies the relationship of the following formula (3a).

[0019] 0.1≤A≤1 (3a)

[0020] [4] The optical layered body according to any one of [1] to [3], wherein B satisfies the relationship of the following formula (4a).

[0021] 0.08≤B≤0.8 (4a)

[0022] [5] The optical layered body according to any one of [1] to [4], wherein C satisfies the relationship of the following formula (5a).

[0023] 200≤C≤3000 (5a)

[0024] [6] A method for manufacturing a display device, comprising the following steps:

[0025] a first base film peeling step of peeling the first base film from the optical laminate according to any one of [1] to [5] to expose the surface of the first pressure-sensitive adhesive layer; and

[0026] The laminating step is to laminate the surface where the first adhesive layer is exposed to a display element.

[0027] According to the present invention, an optical laminate can be provided which can suppress the peeling of a surface protective film provided on the surface opposite to the release film when peeling the release film adhered to the surface of the pressure-sensitive adhesive layer of the optical laminate, and a method for producing a display device using the optical laminate. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1It is a schematic cross-sectional view showing an example of the optical layered body of the present invention. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention with reference to the accompanying drawings, but the present invention is not limited to the following embodiments. In all the following drawings, the scales are appropriately adjusted to facilitate understanding of the various components, and the scales of the various components shown in the drawings are not necessarily consistent with the scales of the actual components.

[0030] [Display device]

[0031] Figure 1 This is a schematic cross-sectional view showing a mode when the optical laminate 100 ′ in which the first base film 22 is peeled off from the optical laminate 100 is bonded to the display element 200 to produce the display device 300 .

[0032] <Optical laminate>

[0033] The optical laminate 100 has a polarizing laminate 10, and has a first adhesive layer 21 laminated on the first surface of the polarizing laminate 10, a first substrate film 22 laminated on the surface of the first adhesive layer 21 opposite to the polarizing laminate 10, a second adhesive layer 31 laminated on the second surface of the polarizing laminate 10, and a second substrate film 32 laminated on the surface of the second adhesive layer 31 opposite to the polarizing laminate 10.

[0034] In the optical laminate 100, the surface of the first adhesive layer 21 becomes the bonding surface with the display element 200. The first base film 22 is a release film (spacer) laminated on the surface of the first adhesive layer 21 on the side opposite to the polarizing laminate 10 side. When the optical laminate 100 is bonded to the display element 200, the release film is peeled off from the optical laminate 100. The laminate after the first base film 22 is peeled off from the optical laminate 100 is referred to as the optical laminate 100'.

[0035] The second base film 32 is laminated on the second surface of the polarizing laminate 10 via the second adhesive layer 31, and functions as a surface protection film 30 together with the second adhesive layer 31. The second adhesive layer 31 is usually provided in advance on the second base film 32 to form the surface protection film 30, and the surface of the second adhesive layer 31 in the surface protection film 30 is bonded to the polarizing laminate 10 to form the optical laminate 100. The surface protection film 30 is usually peeled off from the optical laminate 100' after the optical laminate 100 is bonded to the display element 200.

[0036] The polarizing laminate 10 includes at least a polarizing plate, and may further include a front panel, a touch sensor panel, etc. The polarizing plate includes at least a polarizing film, and may also include a protective film, a retardation film, a brightness enhancement film, a laminating layer, etc.

[0037] The thickness of the optical layered body 100 varies depending on the function required of the optical layered body and the application of the optical layered body, and is not particularly limited, but is, for example, 20 to 2000 μm, preferably 30 to 1000 μm, more preferably 50 to 500 μm, and may be 100 μm or more.

[0038] The top view shape of the optical stack 100 can be, for example, a square shape, preferably a square shape having long sides and short sides, and more preferably a rectangle. When the shape of the surface direction of the optical stack 100 is a rectangle, the length of the long side can be, for example, 10 mm to 1400 mm, preferably 50 mm to 600 mm. The length of the short side is, for example, 5 mm to 800 mm, preferably 30 mm to 500 mm, and more preferably 50 mm to 300 mm. For each layer constituting the optical stack 100, the corners can be R-processed, or the ends can be cut or opened.

[0039] The optical laminate 100 can be used in the display device 300 . The method for manufacturing the display device 300 includes the steps of peeling the first base film 22 from the optical laminate 100 to expose the surface of the first adhesive layer 21 , and bonding the exposed surface of the first adhesive layer 21 to the display element 200 .

[0040] The display device 300 is not particularly limited, and examples thereof include organic electroluminescent (organic EL) display devices, inorganic electroluminescent (inorganic EL) display devices, liquid crystal display devices, and electroluminescent display devices. The optical stack 100 is preferably used for a flexible display device. When the optical stack 100 is used for an organic EL display device, the polarizing stack 10 in the optical stack 100 is preferably a circular polarizer, which can suppress reflected light by peeling off the first substrate film 22 from the optical stack 100 and bonding it to the visible side surface of the organic EL display element. When the optical stack 100 is used for a liquid crystal display device, the polarizing stack 10 in the optical stack 100 is preferably a linear polarizer or a circular polarizer, which can form image light by peeling off the first substrate film 22 from the optical stack 100 and bonding it to both sides of the liquid crystal display element.

[0041] The optical layered body 100 satisfies the relationship of the following formula (1a), and preferably satisfies the relationship of the following formula (1b).

[0042] (A / B)×C≥800 (1a)

[0043] (A / B)×C≥820 (1b)

[0044] The values ​​in the formula (1a) and the formula (1b) are as follows.

[0045] A is a value calculated from A1 / A2, where the 180° peeling force between the polarizing laminate 10 and the second adhesive layer 31 is A1 [gf / 25 mm] and the total thickness of the second base film 32 and the second adhesive layer 31 is A2 [μm].

[0046] B is a value calculated from B1 / B2, where the 180° peeling force between the first pressure-sensitive adhesive layer 21 and the first base film 22 is B1 [gf / 25 mm] and the thickness of the first base film 22 is B2 [μm].

[0047] C is the stiffness (Gurley unit) of the evaluation laminated body in which the first adhesive layer 21, the polarizing laminated body 10, the second adhesive layer 31, and the second base film 32 are laminated in this order. -3 Gurley unit.

[0048] Each value was measured by the method described in the Examples section described later.

[0049] The method for manufacturing a display device using the optical laminate 100 includes a first substrate film peeling step of peeling the first substrate film 22 from the optical laminate 100 to expose the surface of the first adhesive layer 21. The first substrate film peeling step includes, for example, the following operations: the optical laminate 100 is sucked and held from the surface side on which the surface protection film 30 is laminated, a tape is attached to the surface of the first substrate film 22, and the first substrate film 22 is pulled up through the tape to peel only the first substrate film 22. The first substrate film peeling step is intended to peel off the first substrate film 22, but sometimes the surface protection film 30 is peeled off. If the surface protection film 30 is peeled off, it is difficult to continue the first substrate film peeling step.

[0050] In the first substrate film peeling process, in order to suppress the peeling of the surface protection film 30, a method of increasing the adhesion between the surface protection film 30 and the polarizing laminate 10 to enhance the peeling force is considered. However, if the adhesion of the surface protection film 30 is increased, it is sometimes difficult to cleanly peel off the surface protection film 30 in subsequent processes, or undesirable conditions such as scratches may occur on the surface of the polarizing laminate 10 after peeling.

[0051] As a result of intensive studies, the present inventors have found that the peeling of the surface protection film 30 in the first base film peeling step can be suppressed by making the optical layered body 100 satisfy the relationship of the above formula (1a).

[0052] The optical layered body 100 preferably satisfies the relationship of the following formula (2a), and more preferably satisfies the relationship of the following formula (2b).

[0053] (A / B)×C≤10000 (2a)

[0054] (A / B)×C≤2000 (2b)

[0055] By making the optical laminate 100 satisfy the relationship of the above formula (2a), the surface protective film 30 can be easily and cleanly peeled off in the surface protective film peeling step of peeling off the surface protective film 30 after the first substrate film peeling step and the bonding step of bonding the optical laminate 100' to the display element 200. In addition, the peeling of the first substrate film 22 before the first substrate film peeling step can be suppressed.

[0056] From the viewpoint of being able to simply and cleanly peel off the surface protection film 30 in the surface protection film peeling process, the above-mentioned A in the above-mentioned formula (1a) preferably satisfies the relationship of the following formula (3a), and more preferably satisfies the relationship of the following formula (3b). The value of A can be adjusted by adjusting at least one of the material of the second substrate film 32, the material of the second adhesive layer 31, and the surface treatment of the bonding surface of the second adhesive layer 31 and the polarizing laminate 10 to adjust the value of A1, or by adjusting the total thickness A2 of the second substrate film 32 and the second adhesive layer. Examples of the surface treatment of the bonding surface include corona treatment, plasma treatment, and saponification treatment.

[0057] 0.1≤A≤1 (3a)

[0058] 0.15≤A≤0.6 (3b)

[0059] From the viewpoint of being able to simply and cleanly peel off the first substrate film 22 in the first substrate film peeling step, the above B in the above formula (1a) preferably satisfies the relationship of the following formula (4a), and more preferably satisfies the relationship of the following formula (4b). The value of B can be adjusted by adjusting at least one of the material of the first substrate film 22, the material of the first adhesive layer 21, and the surface treatment of the bonding surface between the first adhesive layer 21 and the first substrate film 22 to adjust the value of B1, or by adjusting the thickness B2 of the first substrate film 22. Examples of the surface treatment of the bonding surface include corona treatment, plasma treatment, and saponification treatment.

[0060] 0.08≤B≤0.8 (4a)

[0061] 0.1≤B≤0.4 (4b)

[0062] From the viewpoint of being able to suppress the peeling of the first substrate film 22 before the first substrate film peeling step and being able to impart flexibility to the optical laminate 100' or the polarizing laminate 10, the above C in the above formula (1a) preferably satisfies the relationship of the following formula (5a), and further preferably satisfies the relationship of the following formula (5b). By making the optical laminate 100' or the polarizing laminate 10 flexible, a flexible display device can be formed. The value of C can be adjusted by adjusting the material of the second substrate film 32, the laminate structure of the polarizing laminate 10, and the material and thickness of each layer used in the laminate structure.

[0063] 200≤C≤3000 (5a)

[0064] 300≤C≤2000 (5b)

[0065] The 180° peeling force A1 between the polarizing laminate 10 and the second adhesive layer 31 is preferably 10 gf / 25 mm or more, more preferably 14 gf / 25 mm or more, and can be 20 gf / 25 mm or more. The 180° peeling force A1 is preferably 50 gf / 25 mm or less, and can be 40 gf / 25 mm or less, and can be 30 gf / 25 mm or less.

[0066] The 180° peeling force B1 between the first adhesive layer 21 and the first substrate film 22 is preferably 1 gf / 25 mm or more, more preferably 5 gf / 25 mm or more, and may be 6 gf / 25 mm or more. The 180° peeling force B1 is preferably 20 gf / 25 mm or less, and may be 15 gf / 25 mm or less, and may be 10 gf / 25 mm or less.

[0067] The 180° peeling force A1 between the polarizing laminate 10 and the second adhesive layer 31 is preferably greater than the 180° peeling force B1 between the first adhesive layer 21 and the first base film 22 .

[0068] <First Adhesive Layer 21 >

[0069] The first adhesive layer 21 is laminated on the first surface of the polarizing laminate 10 in the optical laminate 100, and functions as a bonding layer between the polarizing laminate 10 and the display element. The first adhesive layer 21 can be composed of one layer, or two or more layers, but preferably one layer. The first adhesive layer 21 can be composed of an adhesive composition mainly composed of (meth) acrylic resin, rubber resin, polyurethane resin, ester resin, silicone resin, and polyvinyl ether resin. Among them, an adhesive composition based on a (meth) acrylic resin with excellent transparency, weather resistance, heat resistance, etc. is preferred. The adhesive composition can be an active energy ray-curable type or a thermosetting type.

[0070] As the (meth) acrylic resin (base polymer) used in the adhesive composition, it is preferred to use a polymer or copolymer using one or more of (meth) acrylic acid esters such as butyl (meth) acrylate, ethyl (meth) acrylate, isooctyl (meth) acrylate, 2-ethylhexyl (meth) acrylate as monomers. It is preferred to copolymerize the base polymer with a polar monomer. As polar monomers, monomers having carboxyl groups, hydroxyl groups, amide groups, amino groups, epoxy groups, etc., such as (meth) acrylic acid compounds, 2-hydroxypropyl (meth) acrylate compounds, hydroxyethyl (meth) acrylate compounds, (meth) acrylamide compounds, N,N-dimethylaminoethyl (meth) acrylate compounds, and glycidyl (meth) acrylate compounds can be cited.

[0071] The adhesive composition may contain only the above-mentioned base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include metal ions having a valence of more than two and forming a carboxylic acid metal salt with a carboxyl group, polyamine compounds forming an amide bond with a carboxyl group, polyepoxide compounds or polyols forming an ester bond with a carboxyl group, and polyisocyanate compounds forming an amide bond with a carboxyl group. Among them, polyisocyanate compounds are preferred.

[0072] The active energy ray-curable adhesive composition has the property of being cured by irradiation with active energy rays such as ultraviolet rays and electron beams, and has the property of being adhesive and being able to be closely attached to a coating such as a film even before irradiation with active energy rays, and being able to be cured by irradiation with active energy rays to adjust the close adhesion. The active energy ray-curable adhesive composition is preferably an ultraviolet curable type. The active energy ray-curable adhesive composition may further contain an active energy ray polymerizable compound on the basis of containing a base polymer and a crosslinking agent. It may contain a photopolymerization initiator, a photosensitizer, etc. as needed.

[0073] The adhesive composition may contain additives such as microparticles, beads (resin beads, glass beads, etc.), glass fibers, resins other than base polymers, thickeners, fillers (metal powder, other inorganic powders, etc.), antioxidants, ultraviolet absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, photopolymerization initiators, etc. for imparting light scattering properties.

[0074] The first adhesive layer 21 can be formed by applying an organic solvent dilution of the above-mentioned adhesive composition on the first surface of the substrate film or the polarizing laminate 10 and drying it. The substrate film is generally a thermoplastic resin film, and a release film subjected to a release treatment can be cited as a typical example. The release film can be, for example, a film made of a resin such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, or polyarylate, on the surface where the adhesive layer is to be formed, subjected to a release treatment such as silicone treatment.

[0075] For example, a separator film may be used as the first substrate film 22 , and an adhesive composition may be directly applied to the release-treated surface thereof to form an adhesive layer to form the first adhesive layer 21 . The adhesive layer with the separator film may be laminated on the first surface of the polarizing laminate 10 .

[0076] Alternatively, the first adhesive layer 21 may be formed by directly applying the adhesive composition on the first surface of the polarizing laminate 10 to form an adhesive layer, and a separator may be laminated on the outer surface of the first adhesive layer 21 as the first base film 22 .

[0077] When an adhesive layer is provided on the first surface of the polarizing laminate 10, the bonding surface of the polarizing laminate 10 and / or the bonding surface of the adhesive layer is preferably subjected to surface activation treatment such as plasma treatment, corona treatment, etc., and corona treatment is more preferably performed.

[0078] Alternatively, an adhesive sheet may be prepared in which the first adhesive layer 21 is formed by coating the adhesive composition on the second separation film, a separation film (first base film 22) is laminated on the formed adhesive layer, and the adhesive layer with the separation film after the second separation film is peeled off from the adhesive sheet is laminated on the polarizing laminate 10. The second separation film may have a weaker adhesion to the first adhesive layer 21 than the separation film (first base film 22) and may be easily peeled off.

[0079] The thickness of the first adhesive layer 21 is not particularly limited, and is, for example, preferably 1 μm to 100 μm, more preferably 3 μm to 50 μm, and may be 20 μm or more.

[0080] <First base film 22>

[0081] The first base film 22 is a release film (spacer) laminated on the surface of the first adhesive layer 21 opposite to the polarizing laminate 10. The surface of the first base film 22 in contact with the first adhesive layer 21 is preferably subjected to a release treatment.

[0082] The first substrate film 22 is preferably a thermoplastic resin film. Examples of the thermoplastic resin film include cyclic polyolefin resin films; cellulose acetate resin films composed of resins such as cellulose triacetate and cellulose diacetate; polyester resin films composed of resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resin films; (meth) acrylic resin films; polypropylene resin films, etc. The first substrate film 22 is preferably a polyester resin film, and more preferably a polyethylene terephthalate film.

[0083] The thickness B2 of the first base film 22 is preferably 15 μm or more, more preferably 20 μm or more, and more preferably 25 μm or more. The thickness B2 of the first base film 22 is preferably 80 μm or less, and more preferably 60 μm or less.

[0084] <Surface protection film 30>

[0085] The surface protection film 30 is composed of a second substrate film 32 and a second adhesive layer 31 laminated thereon. The surface protection film 30 has the function of protecting the second surface of the polarizing laminate 10. For example, after the optical laminate 100' is attached to the display element 200, the surface protection film 30 is peeled off from the polarizing laminate 10.

[0086] The resin constituting the second base film 32 is applicable to the above-mentioned description regarding the first base film 22 .

[0087] The adhesive composition constituting the second adhesive layer 31 can be applied to the above description related to the adhesive composition constituting the first adhesive layer 21. The thickness of the second adhesive layer 31 is not particularly limited, and is preferably 1 μm to 100 μm, more preferably 3 μm to 50 μm, and can be 20 μm or more. The surface protection film 30 can also use a commercially available product.

[0088] The total thickness A2 of the second substrate film 32 and the second adhesive layer 31 is preferably 30 μm or more, more preferably 40 μm or more, and may be 50 μm or more. The total thickness A2 of the second substrate film 32 and the second adhesive layer 31 is preferably 200 μm or less, more preferably 150 μm or less.

[0089] <Polarizing laminate 10>

[0090] (Polarizing Plate)

[0091] The polarizing laminate 10 includes at least a polarizing plate. The polarizing plate includes at least a linear polarizer layer. The polarizing plate is, for example, a circular polarizing plate, which includes at least a phase difference layer. The circular polarizing plate can absorb reflected external light in a display device, and thus can provide an anti-reflection function to the optical laminate.

[0092] The thickness of the polarizer is usually 5 μm or more, and may be 20 μm or more, 25 μm or more, or 30 μm or more. In addition, the thickness of the polarizer is preferably 80 μm or less, and more preferably 60 μm or less.

[0093] (Linear polarizer layer)

[0094] The linear polarizer layer has the function of selectively transmitting linear polarized light in a certain direction in the light of non-polarized light such as natural light. The linear polarizer layer can be provided with a stretched film or stretched layer adsorbed with a dichroic pigment, a solidified material containing a polymerizable liquid crystal compound and a dichroic pigment, and a liquid crystal layer in which the dichroic pigment is dispersed and oriented in the solidified material of the polymerizable liquid crystal compound, etc. as the polarizer layer. If the pigment is dispersed and oriented in a certain anisotropic medium, it sometimes looks colored from a certain direction and looks almost colorless from a direction perpendicular to it. The pigment that displays such a phenomenon is called a dichroic pigment. Compared with a stretched film or stretched layer adsorbed with a dichroic pigment, the linear polarizer layer using a liquid crystal layer as a polarizer layer has no restrictions in the bending direction, so it is preferred.

[0095] (Polarizer layer as a stretched film or stretched layer having a dichroic dye adsorbed thereon)

[0096] The polarizer layer of a stretched film having adsorbed dichroic dye can generally be manufactured through the following steps: a step of uniaxially stretching a polyvinyl alcohol resin film, a step of dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine so that the film adsorbs the dichroic dye, a step of treating the polyvinyl alcohol resin film having adsorbed dichroic dye with an aqueous boric acid solution, and a step of washing the film with water after the treatment with the aqueous boric acid solution.

[0097] The thickness of the polarizer layer is usually 30 μm or less, preferably 18 μm or less, and more preferably 15 μm or less. A thin polarizer layer is advantageous for thinning the circular polarizing plate. The thickness of the polarizer layer is usually 1 μm or more, for example 5 μm or more.

[0098] The polyvinyl alcohol resin can be obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith can be used. As other monomers copolymerizable with vinyl acetate, for example, unsaturated carboxylic acid compounds, olefin compounds, vinyl ether compounds, unsaturated sulfone compounds, and (meth)acrylamide compounds having an ammonium group can be cited.

[0099] The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and polyvinyl formal and polyvinyl acetal modified with aldehydes may be used. The polymerization degree of the polyvinyl alcohol resin is usually 1000 to 10000, preferably 1500 to 5000.

[0100] The polarizer layer as a stretching layer adsorbed with a dichroic pigment can be manufactured through the following steps: a step of applying a coating solution containing the above-mentioned polyvinyl alcohol resin on a substrate film, a step of uniaxially stretching the obtained laminated film, a step of dyeing the polyvinyl alcohol resin layer of the uniaxially stretched laminated film with a dichroic pigment so that it adsorbs the dichroic pigment and making the polarizer layer, a step of treating the film adsorbed with the dichroic pigment with an aqueous boric acid solution, and a step of washing with water after the treatment with the aqueous boric acid solution. The substrate film used to form the polarizer layer can be used as a protective layer for the polarizer layer. As required, the substrate film can be peeled off and removed from the polarizer layer. The material and thickness of the substrate film can be the same as the material and thickness of the thermoplastic resin film described later.

[0101] The polarizer layer of the stretched film or stretched layer adsorbed with the dichroic dye can be used directly as a linear polarizer layer, or a protective layer can be formed on one or both sides thereof to be used as a linear polarizer layer. As the protective layer, a thermoplastic resin film described later can be used. The thickness of the obtained linear polarizer layer is preferably 2 μm to 40 μm.

[0102] Examples of thermoplastic resin films include cyclic polyolefin resin films; cellulose acetate resin films composed of resins such as cellulose triacetate and cellulose diacetate; polyester resin films composed of resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resin films; (meth) acrylic resin films; polypropylene resin films, and other films known in the art. The polarizer layer and the protective layer may be laminated via a laminating layer described later.

[0103] From the viewpoint of thinning, the thickness of the thermoplastic resin film is usually 100 μm or less, preferably 80 μm or less, more preferably 60 μm or less, further preferably 40 μm or less, further preferably 30 μm or less, and is usually 5 μm or more, preferably 10 μm or more.

[0104] A hard coating layer can be formed on a thermoplastic resin film. The hard coating layer can be formed on one side of the thermoplastic resin film or on both sides. By providing a hard coating layer, a thermoplastic resin film with improved hardness and scratch resistance can be prepared. The hard coating layer can be formed in the same manner as the hard coating layer formed on the above-mentioned resin film.

[0105] (Polarizer layer as liquid crystal layer)

[0106] The polymerizable liquid crystal compound used to form the liquid crystal layer is a compound having a polymerizable reaction group and showing liquid crystal properties. The polymerizable reaction group is a group participating in the polymerization reaction, preferably a photopolymerizable reaction group. The photopolymerizable reaction group refers to a group that can participate in the polymerization reaction using active free radicals, acids, etc. generated by a photopolymerization initiator. As photopolymerizable functional groups, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. Among them, acryloyloxy, methacryloyloxy, vinyloxy, oxirane and oxetane are preferred, and acryloyloxy is more preferred. The type of polymerizable liquid crystal compound is not particularly limited, and rod-shaped liquid crystal compounds, disc-shaped liquid crystal compounds and mixtures thereof can be used. The liquid crystal properties of the polymerizable liquid crystal compound can be thermotropic liquid crystals or lyotropic liquid crystals. As a phase sequence structure, it can be a nematic liquid crystal or a smectic liquid crystal.

[0107] The dichroic dye used in the polarizer layer of the liquid crystal layer preferably has an absorption maximum wavelength (λMAX) in the range of 300 to 700 nm. Examples of such dichroic dyes include acridine dyes, The present invention relates to azo pigments, oxazine pigments, cyanine pigments, naphthalene pigments, azo pigments and anthraquinone pigments, etc., wherein preferred azo pigments. As azo pigments, monoazo pigments, disazo pigments, triazo pigments, tetraazo pigments and stilbene azo pigments, etc. can be mentioned, preferably disazo pigments and triazo pigments. Dichroic pigments can be used alone, or two or more can be combined, preferably three or more are combined. In particular, more preferably three or more azo compounds are combined. A part of the dichroic pigment can have a reactive group, and can have liquid crystal properties in addition.

[0108] The polarizer layer as a liquid crystal layer can be formed by, for example, applying a composition for forming a polarizer layer containing a polymerizable liquid crystal compound and a dichroic pigment on an orientation film formed on a substrate film, polymerizing and curing the polymerizable liquid crystal compound. The polarizer layer can be formed by applying a composition for forming a polarizer layer on a substrate film to form a coating film, and the coating film is stretched together with the substrate film to form a polarizer layer. The substrate film for forming a polarizer layer can be used as a protective layer for the polarizer layer. The material and thickness of the substrate film can be the same as the material and thickness of the above-mentioned thermoplastic resin film.

[0109] As the composition for forming a polarizer layer containing a polymerizable liquid crystal compound and a dichroic pigment and the manufacture method of the polarizer layer using the composition, the method described in Japanese Patent Publication No. 2013-37353, Japanese Patent Publication No. 2013-33249, Japanese Patent Publication No. 2017-83843, etc. can be exemplified. The composition for forming a polarizer layer can further contain additives such as a solvent, a polymerization initiator, a cross-linking agent, a leveling agent, an antioxidant, a plasticizer, and a sensitizer on the basis of containing a polymerizable liquid crystal compound and a dichroic pigment. These components can each use only one, or two or more can be used in combination.

[0110] The polymerization initiator that the composition for forming the polarizer layer may contain is a compound that can initiate the polymerization reaction of the polymerizable liquid crystal compound. From the viewpoint of being able to initiate the polymerization reaction under the condition of lower temperature, a photopolymerization initiator is preferred. Specifically, a photopolymerization initiator that can generate active free radicals or acids by the action of light can be cited, wherein a photopolymerization initiator that generates free radicals by the action of light is preferred. Relative to the total amount of 100 parts by weight of the polymerizable liquid crystal compound, the content of the polymerization initiator is preferably 1 to 10 parts by weight, more preferably 3 to 8 parts by weight. If it is within this range, the reaction of the polymerizable group is fully carried out, and it is easy to stabilize the orientation state of the liquid crystal compound.

[0111] The thickness of the polarizer layer as the liquid crystal layer is usually 10 μm or less, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 5 μm.

[0112] As the polarizer layer of liquid crystal layer, can be used as linear polarizer layer without peeling off and removing base material film, can also be used as linear polarizer layer by peeling off and removing base material film from polarizer layer. As the polarizer layer of liquid crystal layer, can form protective layer on one or both sides and be used as linear polarizer layer. As protective layer, above-mentioned thermoplastic resin film can be used.

[0113] The polarizer layer as the liquid crystal layer may have a cover layer on one or both sides thereof. The cover layer may be provided for the purpose of protecting the polarizer layer, etc. The cover layer may be formed, for example, by coating a material (composition) for forming the cover layer on the polarizer layer. As materials constituting the cover layer, for example, photocurable resins, water-soluble polymers, etc. may be cited. As materials constituting the cover layer, (meth) acrylic resins, polyvinyl alcohol resins, etc. may be used.

[0114] (Phase difference layer)

[0115] In the circular polarizer, the phase difference layer can be one layer or more than two layers. The phase difference layer can have a cover layer for protecting its surface, a substrate film for supporting the phase difference layer, etc. The phase difference layer includes a λ / 4 layer, and can further include at least one of a λ / 2 layer and a positive C layer. When the phase difference layer includes a λ / 2 layer, the λ / 2 layer and the λ / 4 layer are stacked in sequence from the linear polarizer layer side. When the phase difference layer includes a positive C layer, the λ / 4 layer and the positive C layer can be stacked in sequence from the linear polarizer layer side, or the positive C layer and the λ / 4 layer can be stacked in sequence from the linear polarizer layer side. The thickness of the phase difference layer is, for example, 0.1 μm to 10 μm, preferably 0.5 μm to 8 μm, and more preferably 1 μm to 6 μm.

[0116] The phase difference layer may be formed of a resin film exemplified as a material for the protective layer, or may be formed of a layer formed by curing a polymerizable liquid crystal compound. The phase difference layer may further include an orientation film. The phase difference layer may have a laminating layer for laminating the λ / 4 layer to the λ / 2 layer and the positive C layer.

[0117] When the phase difference layer is formed by curing a polymerizable liquid crystal compound, it can be formed by coating a composition containing a polymerizable liquid crystal compound on a substrate film and curing it. An orientation layer can be formed between the substrate film and the coating layer. The material and thickness of the substrate film can be the same as the material and thickness of the thermoplastic resin film. When the phase difference layer is formed by curing a polymerizable liquid crystal compound, it can be provided in an optical laminate in the form of an orientation layer and a substrate film. The phase difference layer can be laminated to the linear polarizer layer via a laminating layer.

[0118] (Lamination layer)

[0119] The laminating layer is a layer composed of a pressure-sensitive adhesive composition or an adhesive composition. The pressure-sensitive adhesive composition that is a material of the laminating layer is applicable to the above description regarding the pressure-sensitive adhesive composition constituting the first pressure-sensitive adhesive layer 21.

[0120] The adhesive composition as the material of the laminating layer can be formed by combining one or more of water-based adhesives, active energy ray-curing adhesives, etc. As water-based adhesives, for example, polyvinyl alcohol resin aqueous solutions, water-based two-component urethane emulsion adhesives, etc. can be cited. Active energy ray-curing adhesives are adhesives that are cured by irradiating active energy rays such as ultraviolet rays, and for example, adhesives containing polymerizable compounds and photopolymerization initiators, adhesives containing photoreactive resins, adhesives containing binder resins and photoreactive crosslinking agents can be cited. As the above-mentioned polymerizable compounds, photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, and photocurable urethane monomers, as well as oligomers from these monomers, etc. can be cited. As the above-mentioned photopolymerization initiator, compounds containing active species such as neutral free radicals, anionic free radicals, and cationic free radicals generated by irradiating active energy rays such as ultraviolet rays can be cited.

[0121] The thickness of the bonding layer may be, for example, 1 μm or more, preferably 1 μm to 25 μm, more preferably 2 μm to 15 μm, and further preferably 2.5 μm to 5 μm.

[0122] (Front Panel)

[0123] The polarizing laminate 10 may include a front panel or may not include a front panel. As long as the front panel is a plate-like body that can transmit light, the material and thickness are not limited, and it may be composed of only one layer or more than two layers. As the front panel 10, a plate-like body made of resin (such as a resin plate, a resin sheet, a resin film, etc.) and a plate-like body made of glass (such as a glass plate, a glass film, etc.) can be cited. The front panel 10 can constitute the outermost surface of the display device.

[0124] The thickness of the front panel may be, for example, 10 μm to 500 μm, preferably 30 μm to 200 μm, more preferably 40 μm to 100 μm, and may be 50 μm or more.

[0125] When the front panel is a plate-like body made of resin, the plate-like body made of resin is not limited as long as it can transmit light. As the resin constituting the plate-like bodies made of resin such as resin film, for example, films formed by macromolecules such as cellulose triacetate, cellulose acetate butyrate, ethylene-vinyl acetate copolymer, cellulose propionate, cellulose butyrate, cellulose acetate propionate, polyester, polystyrene, polyamide, polyetherimide, poly(methyl)acrylic acid, polyimide, polyether sulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyether ether ketone, polyether sulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyamide-imide, etc. can be enumerated. These macromolecules can be used alone or mixed with more than two kinds of use. From the viewpoint of improving strength and transparency, the resin film is preferably formed by macromolecules such as polyimide, polyamide, polyamide-imide.

[0126] The front panel is preferably a resin film or a resin film having a hard coating on the resin film. The hard coating can be formed on one side of the resin film or on both sides. By providing a hard coating, a resin film with improved hardness and scratch resistance can be made. The hard coating is, for example, a cured layer of an ultraviolet curable resin. As ultraviolet curable resins, for example, acrylic resins, silicone resins, polyester resins, polyurethane resins, amide resins, epoxy resins, etc. can be cited. In order to increase the strength, the hard coating can contain additives. The additives are not limited, and inorganic particles, organic particles, or mixtures thereof can be cited. When there are hard coatings on both sides of the resin film, the composition and thickness of each hard coating can be the same as or different from each other.

[0127] When the front panel is a glass plate, the glass plate is preferably tempered glass for display. The thickness of the glass plate may be, for example, 10 μm to 1000 μm, and may be 50 μm or more. By using a glass plate, a front panel having excellent mechanical strength and surface hardness can be formed.

[0128] When the optical laminate 100 is used in a display device, the front panel can not only have the function of protecting the front (screen) of the display device (function as a window film), but also have the function of a touch sensor, a blue light cutoff function, a viewing angle adjustment function, etc.

[0129] (Touch sensor panel)

[0130] The polarizing laminate 10 may further include a touch sensor panel. As a polarizing laminate 10 having a touch sensor panel, for example, a polarizing laminate having a front panel, a circular polarizer, and a touch sensor in sequence may be cited. The touch sensor panel is not limited as long as it is a panel having a sensor (i.e., a touch sensor) that can detect the touched position. The detection method of the touch sensor is not limited, and examples thereof include touch sensor panels such as a resistive film method, an electrostatic capacitance coupling method, an optical sensor method, an ultrasonic method, an electromagnetic induction coupling method, and a surface elastic wave method. From the perspective of low cost, it is preferred to use a touch sensor panel of a resistive film method or an electrostatic capacitance coupling method.

[0131] As an example of a touch sensor of a resistive film type, there can be cited a component consisting of a pair of substrates arranged opposite to each other, an insulating spacer sandwiched between the pair of substrates, a transparent conductive film provided on the front surface of the inner side of each substrate as a resistive film, and a touch position detection circuit. In an image display device provided with a touch sensor of a resistive film type, if the surface of the front panel is touched, the opposing resistive films are short-circuited and current flows through the resistive films. The touch position detection circuit detects the change in voltage at this time, thereby detecting the touched position.

[0132] As an example of a touch sensor of electrostatic capacitance coupling, there is a component composed of a substrate, a transparent electrode for position detection provided on the entire surface of the substrate, and a touch position detection circuit. In an image display device provided with a touch sensor of electrostatic capacitance coupling, if the surface of the front panel is touched, the transparent electrode is grounded at the touched point via the electrostatic capacitance of the human body. The touch position detection circuit detects the grounding of the transparent electrode, thereby detecting the touched position.

[0133] The thickness of the touch sensor panel may be, for example, 5 μm to 2000 μm, preferably 5 μm to 100 μm, and more preferably 5 μm to 50 μm.

[0134] The touch sensor panel may be a member having a touch sensor pattern formed on a base film. Examples of the base film are the same as those in the above description of the thermoplastic resin film. The thickness of the touch sensor pattern may be, for example, 1 μm to 20 μm.

[0135] [Method for producing optical layered body]

[0136] The optical laminate 100 can be manufactured by a method including a process of laminating each layer. The optical laminate 100 can be manufactured by a process of first forming the polarizing laminate 10 and then providing an adhesive layer on the first surface and the second surface thereof, or by a process of pre-providing an adhesive layer on a precursor having a surface forming the first surface of the polarizing laminate, or by pre-providing an adhesive layer on a precursor having a surface forming the second surface of the polarizing laminate, and manufacturing the optical laminate 100 having the polarizing laminate 10 through a process of laminating precursors.

[0137] [Application of display device]

[0138] The display device of the present invention can be used in mobile devices such as smart phones and tablet computers, televisions, digital photo frames, electronic signs, measuring instruments, meters, office equipment, medical equipment, electronic computers, etc.

[0139] Example

[0140] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0141] [Preparation of Constituent Elements of Polarizing Laminate]

[0142] (Liquid crystal polarizing plate having a polarizer layer as a liquid crystal layer)

[0143] An alignment film composition was applied to one side of a TAC film having a thickness of 25 μm, dried, and exposed to polarized light to form an alignment film. A liquid crystal composition containing a liquid crystal polymerizable compound and a dye was applied to the alignment film and dried. The composition was cured by ultraviolet irradiation to form a polarizer layer as a liquid crystal layer, thereby obtaining a liquid crystal polarizer.

[0144] (Stretched polarizing plate having a polarizer layer as a stretched layer)

[0145] The PVA film was uniaxially stretched and then dyed by immersion in a solution containing iodine, then immersed in a solution containing boric acid for crosslinking and dried to obtain a polarizer layer. A 13 μm thick transparent film made of COP was attached to one side of the polarizer layer with an adhesive to obtain a stretched polarizer.

[0146] (1 / 4 wavelength plate)

[0147] An alignment film composition is applied to one side of a PET film, dried and exposed to polarized light to form an alignment film. A liquid crystal composition containing a polymerizable liquid crystal compound is applied to the alignment film and dried. The alignment film is cured by ultraviolet irradiation to form a phase difference layer (1 / 4 wavelength layer) to obtain a 1 / 4 wavelength plate with a PET film. The laminate consisting of the alignment film and the phase difference layer (1 / 4 wavelength layer) is used as a 1 / 4 wavelength plate.

[0148] (1 / 2 wavelength plate)

[0149] An alignment film composition is applied to one side of a PET film, dried and exposed to polarized light to form an alignment film. A liquid crystal composition containing a polymerizable liquid crystal compound is applied to the alignment film and dried. The alignment film is cured by ultraviolet irradiation to form a phase difference layer (1 / 2 wavelength layer) to obtain a 1 / 2 wavelength plate with a PET film. The laminate consisting of the alignment film and the phase difference layer (1 / 2 wavelength layer) is used as a 1 / 2 wavelength plate.

[0150] (Positive C layer)

[0151] A vertical alignment film composition is applied to one side of a PET film, dried and exposed to form an alignment film. A liquid crystal composition containing a polymerizable liquid crystal compound is applied to the alignment film and dried. The phase difference layer (positive C layer) is formed by curing by ultraviolet irradiation, and a positive C layer with a PET film is obtained. The laminate composed of the alignment film and the phase difference layer is also used as a positive C layer.

[0152] (Liquid crystal polarizing plate for anti-reflection)

[0153] After a quarter-wave plate with a PET film is attached to the surface of the non-TAC film side of the liquid crystal polarizer using an adhesive, the PET film is peeled off. Further, a positive C phase difference layer with a PET film is attached to the surface of the quarter-wave plate using an adhesive, and the PET film is peeled off. An adhesive composition is applied to the surface of the positive C layer to form an adhesive layer (first adhesive layer), and an anti-reflection liquid crystal polarizer (circular polarizer) with an adhesive layer is obtained.

[0154] (Stretched polarizing plate for anti-reflection)

[0155] After a 1 / 2 wavelength plate with a PET film is attached to the surface of the non-COP film side of the stretched polarizer using an adhesive layer, the PET film is peeled off. After a 1 / 4 wavelength plate with a PET film is attached to the surface of the 1 / 2 wavelength plate using an adhesive, the PET film is peeled off. An adhesive composition is applied to the surface of the 1 / 4 wavelength plate to form an adhesive layer (first adhesive layer), and an anti-reflection stretched polarizer (circular polarizer) with an adhesive layer is obtained.

[0156] [Example 1]

[0157] A surface protective film A (polyethylene terephthalate (PET) film with an acrylic adhesive layer (second adhesive layer), Fujimori Industries, Ltd., AY-4212) is laminated on the TAC surface of the anti-reflection liquid crystal polarizer with an adhesive layer, and a release film F (50 μm thick PET treated with release treatment) is laminated on the adhesive layer to produce the optical laminate of Example 1.

[0158] <Measurement of each parameter>

[0159] (Measurement of 180° Peel Force A1 and Thickness A2 of Surface Protection Film)

[0160] The sample for measurement is cut into 2.5 cm width from the overall structure of the optical laminate of Example 1. The release film is peeled off from the cut optical laminate, and the surface of the adhesive layer (first adhesive layer) is bonded to the glass. The glass is fixed to a tensile force measuring device ("AG-1S" manufactured by Shimadzu Corporation). A portion of the surface protective film A is peeled off and fixed to the fixture of the tensile force measuring device. Under a 25°C environment, the surface protective film A is peeled off at a speed of 3.0 m / min in a manner that the peeling angle becomes 180°, and the peeling force A1 [gf / 25mm] is measured. The peeled surface protective film A is measured for thickness A2 [μm] using a contact film thickness measuring device ("MS-5C" manufactured by Nikon Corporation). Table 1 shows the values ​​of the 180° peeling force A1, the thickness A2 of the surface protective film, and the parameter A calculated from A1 / A2.

[0161] (Measurement of 180° Peel Force B1 and Release Film Thickness B2)

[0162] A sample for measurement is cut into 2.5 cm width from the overall structure of the optical laminate of Example 1. The surface protective film A is removed from the cut optical laminate, and the surface having the surface protective film A is bonded to the glass. The glass is fixed to a tensile force measuring device ("AG-1S" manufactured by Shimadzu Corporation), and a portion of the release film F (first substrate film) is peeled off and fixed to the fixture of the tensile force measuring device. Under a 25°C environment, the release film F is peeled off at a speed of 3.0 m / min in a manner that the peeling angle becomes 180°, and the peeling force B1 [gf / 25mm] is measured. For the peeled release film F, the thickness B2 [μm] is also measured using a contact film thickness measuring device ("MS-5C" manufactured by Nikon Corporation). Table 1 shows the 180° peeling force B1, the thickness B2 of the release film, and the values ​​of the parameter B calculated from B1 / B2.

[0163] (Determination of stiffness C)

[0164] A sample with a width of 2.54 cm and a length of 8.89 cm was cut from the overall structure of the optical laminate of Example 1. The release film F was removed from the sample and used as an evaluation laminate. The evaluation laminate stiffness C [Gurley unit] was measured using a stiffness tester (Gurley Company, Bending Stiffness Tester). Table 1 shows the calculated values ​​of stiffness C and (A / B)×C.

[0165] [Example 2]

[0166] An optical laminate of Example 2 was prepared in the same manner as in Example 1 except that surface protection film B (PET film with an acrylic pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer), manufactured by Fujimori Industries, AY-638) was used instead of surface protection film A, and various parameters were measured.

[0167] [Example 3]

[0168] An optical laminate of Example 3 was prepared in the same manner as in Example 1 except that surface protection film C (PET film with an acrylic pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer), manufactured by Fujimori Industries, AY(75)-638) was used instead of surface protection film A, and various parameters were measured.

[0169] [Example 4]

[0170] The optical laminate of Example 4 was prepared in the same manner as in Example 1, except that surface protective film D (a film in which an acrylic adhesive layer (second adhesive layer) having a thickness of 15 μm is formed by coating an adhesive composition on PET (second substrate film) having a thickness of 125 μm) was used instead of surface protective film A, and various parameters were measured.

[0171] [Example 5]

[0172] An optical layered body of Example 5 was produced in the same manner as in Example 1 except that a release film G made of PET having a thickness of 38 μm and subjected to a release treatment was used instead of the release film F, and various parameters were measured.

[0173] [Example 6]

[0174] An optical layered body of Example 6 was prepared in the same manner as in Example 3 except that a stretched polarizing plate for antireflection with a pressure-sensitive adhesive layer was used instead of the liquid crystal polarizing plate for antireflection with a pressure-sensitive adhesive layer, and various parameters were measured.

[0175] [Comparative Example 1]

[0176] An optical laminate of Comparative Example 1 was prepared in the same manner as in Example 1 except that Surface Protection Film E (PET film with an acrylic pressure-sensitive adhesive layer (second pressure-sensitive adhesive layer), manufactured by Fujimori Industries, Ltd., AY(75)-4212) was used instead of Surface Protection Film A, and various parameters were measured.

[0177] [Comparative Example 2]

[0178] An optical layered body of Comparative Example 2 was prepared in the same manner as in Example 5 except that a stretched polarizing plate for antireflection with a pressure-sensitive adhesive layer was used instead of the liquid crystal polarizing plate for antireflection with a pressure-sensitive adhesive layer, and various parameters were measured.

[0179] [Peeling evaluation]

[0180] The optical laminate produced in each embodiment and comparative example is placed and fixed by suction in a manner that the surface protective film contacts the adsorption table. The peeling tape is attached to the corner portion of the release film (first substrate film), and pulled up from the surface of the optical laminate in a manner that the peeling angle becomes 90°. The separation of the release film from the adhesive layer (first adhesive layer) surface is judged as normal peeling, and the peeling of the surface protective film from the surface of the polarizing laminate is judged as unqualified peeling (reverse peeling). The results are shown in Table 1.

[0181] [Table 1]

[0182]

[0183] Explanation of symbols

[0184] 100 , 100 ′ optical laminate, 10 polarizing laminate, 21 first adhesive layer, 22 first base film, 30 surface protection film, 31 second adhesive layer, 32 second base film, 200 display element, 300 display device.

Claims

1. An optical laminate, comprising: a polarizing laminate, a first adhesive layer laminated on a first surface of the polarizing laminate, a first substrate film laminated on a surface of the first adhesive layer opposite to the polarizing laminate, a second adhesive layer laminated on a second surface of the polarizing laminate, and a second substrate film laminated on a surface of the second adhesive layer opposite to the polarizing laminate, Satisfying the following relationship (1a), (A / B)×C≥800(1a) In formula (1a), A is a value calculated by A1 / A2 when the 180° peeling force between the polarizing laminate and the second adhesive layer is A1 and the total thickness of the second substrate film and the second adhesive layer is A2, wherein the unit of A1 is gf / 25 mm, and the unit of A2 is μm. B is a value calculated by B1 / B2 when the 180° peeling force between the first adhesive layer and the first substrate film is B1 and the thickness of the first substrate film is B2. The unit of B1 is gf / 25 mm, and the unit of B2 is μm. C is defined as the stiffness of the evaluation laminate in which the first pressure-sensitive adhesive layer, the polarizing laminate, the second pressure-sensitive adhesive layer, and the second base film are laminated in this order, and the stiffness is represented by Gurley units.

2. The optical layered body according to claim 1, in, Further satisfying the following relationship (2a), (A / B)×C≤10000(2a).

3. The optical layered body according to claim 1 or 2, in, The A satisfies the following relationship (3a): 0.1≤A≤1(3a).

4. The optical layered body according to claim 1 or 2, in, The B satisfies the following relationship (4a): 0.08≤B≤0.8(4a).

5. The optical layered body according to claim 3, in, The B satisfies the following relationship (4a): 0.08≤B≤0.8(4a).

6. The optical layered body according to claim 1 or 2, in, The C satisfies the following relationship (5a): 200≤C≤3000(5a).

7. The optical layered body according to claim 3, in, The C satisfies the following relationship (5a): 200≤C≤3000(5a).

8. The optical layered body according to claim 4, in, The C satisfies the following relationship (5a): 200≤C≤3000(5a).

9. The optical layered body according to claim 5, in, The C satisfies the following relationship (5a): 200≤C≤3000(5a).

10. A method for manufacturing a display device, comprising the following steps: a first base film peeling step of peeling the first base film from the optical laminate according to any one of claims 1 to 9 to expose the surface of the first pressure-sensitive adhesive layer; and The laminating step is to laminate the exposed surface of the first adhesive layer to a display element.

Citation Information

Patent Citations

  • Roll raw fabric and method for producing roll raw fabric

    JP2010188550A

  • Polarization element, circularly polarizing plate and method of manufacturing those

    JP2013033249A

  • Polarizer and method for manufacturing the same

    JP2013037353A

  • Polarizing plate

    JP2017083843A

  • Substrate-less double-sided pressure-sensitive adhesive sheet

    CN103857761A