A kind of golden jianzhan
Through the mixing of red clay and kaolin in a specific proportion and multi-step roasting process, the difficulty of firing and glaze quality of Jianzhan is solved, and the effect of no patches, no pores and golden oil drops on the glaze is achieved, which enhances the art of Jianzhan and collection value.
Patent Information
- Application Number
- CN202210634888.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Jianzhan is difficult to fire, and it is prone to bubbles, deformation, and difficult to form glaze surface, resulting in many pinholes on the glaze surface, affecting the beauty, artistic and collection value.
Use a specific ratio of red clay and kaolin to mix, crush and grind and perform multi-step roasting in an electric kiln to control temperature and diesel delivery to ensure glaze thickness and texture.
The glaze surface is prepared without patches and pores, and the oil droplets are golden. It has rich and beautiful glaze color and profound artistic heritage, which enhances the artistic and collection value of Jianzan.
Smart Images

Figure CN115043642B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porcelain, and in particular to a Jin Yao Jian ware. Background Art
[0002] Jianzhan is a shining pearl in the history of Chinese ceramics and is deeply loved by people. Jianzhan has a simple shape, unpredictable glaze color, colorful and so on. Jianzhan is a shining pearl in the history of ceramics and is famous for its outstanding artistic level. Compared with other porcelains, it has a unique beauty.
[0003] However, Jianzhan is very difficult to fire, and it is often difficult to master the formula, firing atmosphere and temperature selection. Improper selection of firing technology can easily have a great adverse effect on the final product of Jianzhan, resulting in defects such as bubbling, deformation, difficulty in forming glaze and patterns, and a large number of pinholes in the glaze, which seriously affects the appearance of Jianzhan and reduces its artistic, collection and economic value.
[0004] As the appreciation and artistic level continue to improve, the demand for Jianzhan with beautiful appearance is also getting higher and higher. How to fire a Jianzhan with beautiful appearance to improve the artistic and collection value of Jianzhan has become a hot topic of research in the porcelain industry today.
[0005] Therefore, this field needs to develop a Jian ware with beautiful appearance, artistic and collection value. Summary of the invention
[0006] The purpose of the present invention is to provide a Jinyao Jianzhan with excellent appearance, thereby improving the artistic and collection value of the Jianzhan.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention provides a preparation process of Jinyao Jianzhan, the process comprising the following steps:
[0009] (1) 2.5-3.5 parts by weight of laterite and 6-8 parts by weight of kaolin are mixed, crushed, washed with water, passed through an 80-120 mesh sieve, filtered, refined, and aged to obtain green clay; the green clay is formed by wheel throwing, trimmed, biscuit fired at 830-840° C. for 7.5-8.5 hours, and taken out to obtain a green body;
[0010] (2) grinding 5.5-6.5 parts by weight of glaze stone, 1.5-2.5 parts by weight of potassium feldspar, 0.8-1.2 parts by weight of limestone, 0.1-0.4 parts by weight of talc, 0.1-0.5 parts by weight of iron oxide and 7-9 parts by weight of water, passing through a 80-120 mesh sieve, and aging for 1.5-2.5 days to obtain a glaze slurry;
[0011] (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body having a glaze thickness of 1.0-1.4 mm;
[0012] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0013] (4.1) The furnace temperature is raised from room temperature to 480-520°C at a rate of 280-320°C / h, then raised from 480-520°C to 880-920°C at a rate of 220-260°C / h, then raised from 880-920°C to 1030-1070°C at a rate of 90-130°C / h, and kept at 1030-1070°C for 1.5-2.5 min, then raised from 1030-1070°C to 1180-1220°C at a rate of 90-130°C / h, and kept at 1180-1220°C for 1.5-2.5 min, and then raised from 1180-1220°C to 1280-1320°C at a rate of 55-75°C / h;
[0014] (4.2) Keep the temperature at 1280-1320℃ for 2.3-2.7h, add oil firewood into the electric kiln at 1280-1320℃, add once every 2.5-3.5min, for a total of 7 times, the amount of oil firewood added is 55-65g, 55-65g, 75-85g, 75-85g, 90-110g, 90-110g, 90-110g per 0.16-0.20 cubic meter of the electric kiln space, and the electric kiln is powered off after the last addition of oil firewood;
[0015] (4.3) When the furnace temperature drops to 1200-1240℃, add 55-65g of fuel oil into the electric kiln at a rate of 0.16-0.20 cubic meters of furnace space. After adding fuel oil, open the furnace door 2.5-3.5 minutes later. When the furnace temperature drops to 1115-1125℃, close the furnace door.
[0016] (4.4) When the furnace temperature drops to 1097-1103℃, 1087-1093℃ and 1077-1083℃, 35-45g of wood is added into the electric kiln for every 0.16-0.20 cubic meters of the furnace space. After the last addition of wood, the furnace door is opened and closed after 5-7 minutes. After 15-25 minutes, the furnace temperature is increased to 940-980℃ at a rate of 70-90℃ / h. After being kept at 940-980℃ for 0.8-1.2h, the electric kiln is powered off and the furnace door is opened to cool down to room temperature, thereby obtaining Jin Yao Jian Zhan.
[0017] In a preferred embodiment of the present invention, the process comprises the following steps:
[0018] (1) 2.7-3.3 parts by weight of laterite and 6.8-7.2 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green mud; the green mud is formed by wheel throwing, trimmed, biscuit fired at 840-860° C. for 7.5-8.5 hours, and taken out to obtain a green body;
[0019] (2) grinding 5.8-6.2 parts by weight of glaze stone, 1.8-2.2 parts by weight of potassium feldspar, 0.9-1.1 parts by weight of limestone, 0.1-0.3 parts by weight of talc, 0.2-0.4 parts by weight of iron oxide and 7.8-8.2 parts by weight of water, passing through a 100-mesh sieve, and aging for 2 days to obtain a glaze slurry;
[0020] (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body having a glaze thickness of 1.1-1.3 mm;
[0021] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0022] (4.1) The furnace temperature is raised from room temperature to 490-510°C at a rate of 290-310°C / h, then raised from 490-510°C to 890-910°C at a rate of 230-250°C / h, then raised from 890-910°C to 1040-1060°C at a rate of 100-120°C / h, and kept at 1040-1060°C for 1.8-2.2 min, then raised from 1040-1060°C to 1190-1210°C at a rate of 100-120°C / h, and kept at 1190-1210°C for 1.8-2.2 min, and then raised from 1190-1210°C to 1290-1310°C at a rate of 60-70°C / h;
[0023] (4.2) Keep the temperature at 1290-1310°C for 2.3-2.7 hours, add oil firewood into the electric kiln at 1290-1310°C, once every 2.8-3.2 minutes, for a total of 7 times, the amount of oil firewood added is 58-62g, 58-62g, 78-82g, 78-82g, 95-105g, 95-105g, 95-105g per 0.17-0.19 cubic meters of the electric kiln space, and the electric kiln is powered off after the last addition of oil firewood;
[0024] (4.3) When the furnace temperature drops to 1210-1230℃, add 58-62g of fuel oil into the electric kiln at a rate of 100-200g per 0.17-0.19 cubic meters of the electric kiln space. After 2.8-3.2 minutes of adding fuel oil, open the furnace door. When the furnace temperature drops to 1118-1122℃, close the furnace door.
[0025] (4.4) When the furnace temperature drops to 1098-1102℃, 1088-1092℃ and 1078-1082℃, 38-42g of wood is added into the electric kiln for every 0.17-0.19 cubic meters of the furnace space. After the last addition of wood, the furnace door is opened. After 5.8-6.2 minutes, the furnace door is closed. After 18-22 minutes, the furnace temperature is increased to 950-970℃ at a rate of 78-82℃ / h. After being kept at 950-970℃ for 0.9-1.1 hours, the electric kiln is powered off, and the furnace door is opened to cool down to room temperature, thereby obtaining Jin Yao Jian Zhan.
[0026] In a preferred embodiment of the present invention, the process comprises the following steps:
[0027] (1) 3 parts by weight of red clay and 7 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green clay; the green clay is formed by wheel throwing, trimmed, bisque fired at 850° C. for 8 hours, and taken out to obtain a green body;
[0028] (2) grinding 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 1 part by weight of limestone, 0.2 parts by weight of talc, 0.3 parts by weight of iron oxide and 8 parts by weight of water, passing through a 100-mesh sieve, and aging for 2 days to obtain a glaze slurry;
[0029] (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body with a glaze thickness of 1.2 mm;
[0030] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0031] (4.1) The furnace temperature is raised from room temperature to 500°C at a rate of 300°C / h, then raised from 500°C to 900°C at a rate of 240°C / h, then raised from 900°C to 1050°C at a rate of 110°C / h, and then kept at 1050°C for 2 min, then raised from 1050°C to 1200°C at a rate of 110°C / h, and then kept at 1200°C for 2 min, and then raised from 1200°C to 1300°C at a rate of 65°C / h;
[0032] (4.2) Keep the temperature at 1300℃ for 2.5h. Add oil-fired fuel into the electric kiln at 1300℃ for 7 times every 3min. The amount of oil-fired fuel added is 60g, 60g, 80g, 80g, 100g, 100g, and 100g per 0.18m3 of the electric kiln space. After the last addition of oil-fired fuel, the electric kiln is powered off.
[0033] (4.3) When the furnace temperature drops to 1220℃, add 60g of fuel oil into the electric kiln at a rate of 0.18 cubic meters of furnace space. After adding fuel oil and fuel, open the furnace door 3 minutes later. When the furnace temperature drops to 1120℃, close the furnace door.
[0034] (4.4) When the furnace temperature drops to 1100℃, 1090℃ and 1080℃, 40g of firewood is added into the electric kiln for every 0.18 cubic meters of furnace space. After the last addition of firewood, the furnace door is opened and closed after 6 minutes. After 20 minutes, the furnace temperature is increased to 960℃ at a rate of 80℃ / h. After being kept at 960℃ for 1 hour, the electric kiln is powered off and the furnace door is opened to cool it to room temperature, thus obtaining Jin Yao Jianzhan.
[0035] In a preferred embodiment of the present invention, in the step (2), the grinding is performed in a ball mill.
[0036] In a preferred embodiment of the present invention, in the step (2), glaze stone, potassium feldspar, limestone, talc, iron oxide and water are put into a ball mill for grinding.
[0037] In a preferred embodiment of the present invention, the normal temperature is 18-22°C, preferably 20°C.
[0038] In a preferred embodiment of the present invention, the red soil comes from Shuiji Town, Jianyang District, Nanping City, Fujian Province.
[0039] In a preferred embodiment of the present invention, the kaolin comes from Shuiji Town, Jianyang District, Nanping City, Fujian Province.
[0040] In a preferred example of the present invention, the glaze stone comes from Nanlin Village, Jianyang District, Nanping City, Fujian Province.
[0041] In a preferred embodiment of the present invention, the Jinyao Jianzhan is as shown in the attached specification. Figure 1 , Figure 2 and Figure 3 shown.
[0042] The second aspect of the present invention provides a Jin Yao Jian Zhan, which is prepared by the process described in the first aspect of the present invention.
[0043] In a preferred embodiment of the present invention, the Jinyao Jianzhan is as shown in the attached specification. Figure 1 , Figure 2 and Figure 3 shown.
[0044] Within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below can be combined with each other to form a new or preferred technical solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is the Jin Yao Jianzhan prepared in Example 1 of the present invention.
[0046] Figure 2 This is the Jin Yao Jianzhan prepared in Example 1 of the present invention.
[0047] Figure 3 This is the Jin Yao Jianzhan prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0048] The present invention develops a preparation process of Jin Yao Jian Zhan. The glaze surface of Jin Yao Jian Zhan prepared by the process of the present invention has Yao change, and the oil droplets are golden, which is called Jin Yao. The magnificent characteristics are unique and beautiful, just like a matrix that nourishes all things. The oil droplets are feathered with textures, moisturizing, and mimicking vividness. The hairs of Jin Yao Jian Zhan are fine and clear, dense and well-arranged, with a strong sense of layering. The glaze surface has no spots, no pores, and good texture. It has rich and beautiful glaze colors and profound artistic heritage and charm, and thus has beautiful artistic and collection value.
[0049] the term
[0050] As used herein, the terms "include", "comprises", and "comprising" are used interchangeably, and include not only open definitions, but also semi-closed and closed definitions. In other words, the terms include "consisting of", "consisting essentially of".
[0051] In the present invention, the oilwood is a pine root rich in pine resin and can burn violently.
[0052] As used herein, the term "parts by weight" may be any fixed weight expressed in milligrams, grams or kilograms (such as 1 mg, 1 g or 1 kg, etc.). For example, a combination consisting of 1 part by weight of component a and 9 parts by weight of component b may be a combination of 1 gram of component a + 9 grams of component b, or a combination of 10 grams of component a + 90 grams of component b, etc. In the combination, the percentage content of a component = (the weight part of the component / the sum of the weight parts of all components) × 100%. Therefore, in a composition consisting of 1 part by weight of component a and 9 parts by weight of component b, the content of component a is 10%, and the content of component b is 90%.
[0053] Jinyao Jianzhan
[0054] The present invention provides a Jinyao Jianzhan, and the Jinyao Jianzhan prepared by the process has a beautiful appearance and collection value. Preferably, the Jinyao Jianzhan of the present invention is as follows Figure 1 , Figure 2 and Figure 3 shown.
[0055] In a preferred embodiment of the present invention, a preparation process of Jinyao Jianzhan is provided, and the process comprises the following steps:
[0056] (1) 2.5-3.5 parts by weight of laterite and 6-8 parts by weight of kaolin are mixed, crushed, washed with water, passed through an 80-120 mesh sieve, filtered, refined, and aged to obtain green clay; the green clay is formed by wheel throwing, trimmed, biscuit fired at 830-840° C. for 7.5-8.5 hours, and taken out to obtain a green body;
[0057] (2) grinding 5.5-6.5 parts by weight of glaze stone, 1.5-2.5 parts by weight of potassium feldspar, 0.8-1.2 parts by weight of limestone, 0.1-0.4 parts by weight of talc, 0.1-0.5 parts by weight of iron oxide and 7-9 parts by weight of water, passing through a 80-120 mesh sieve, and aging for 1.5-2.5 days to obtain a glaze slurry;
[0058] (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body having a glaze thickness of 1.0-1.4 mm;
[0059] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0060] (4.1) The furnace temperature is raised from room temperature to 480-520°C at a rate of 280-320°C / h, then raised from 480-520°C to 880-920°C at a rate of 220-260°C / h, then raised from 880-920°C to 1030-1070°C at a rate of 90-130°C / h, and kept at 1030-1070°C for 1.5-2.5 min, then raised from 1030-1070°C to 1180-1220°C at a rate of 90-130°C / h, and kept at 1180-1220°C for 1.5-2.5 min, and then raised from 1180-1220°C to 1280-1320°C at a rate of 55-75°C / h;
[0061] (4.2) Keep the temperature at 1280-1320℃ for 2.3-2.7h, add oil firewood into the electric kiln at 1280-1320℃, add once every 2.5-3.5min, for a total of 7 times, the amount of oil firewood added is 55-65g, 55-65g, 75-85g, 75-85g, 90-110g, 90-110g, 90-110g per 0.16-0.20 cubic meter of the electric kiln space, and the electric kiln is powered off after the last addition of oil firewood;
[0062] (4.3) When the furnace temperature drops to 1200-1240℃, add 55-65g of fuel oil into the electric kiln at a rate of 0.16-0.20 cubic meters of furnace space. After adding fuel oil, open the furnace door 2.5-3.5 minutes later. When the furnace temperature drops to 1115-1125℃, close the furnace door.
[0063] (4.4) When the furnace temperature drops to 1097-1103℃, 1087-1093℃ and 1077-1083℃, 35-45g of wood is added into the electric kiln for every 0.16-0.20 cubic meters of the furnace space. After the last addition of wood, the furnace door is opened and closed after 5-7 minutes. After 15-25 minutes, the furnace temperature is increased to 940-980℃ at a rate of 70-90℃ / h. After being kept at 940-980℃ for 0.8-1.2h, the electric kiln is powered off and the furnace door is opened to cool down to room temperature, thereby obtaining Jin Yao Jian Zhan.
[0064] In a preferred embodiment of the present invention, a preparation process of Jinyao Jianzhan is provided, and the process comprises the following steps:
[0065] (1) 2.7-3.3 parts by weight of laterite and 6.8-7.2 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green mud; the green mud is formed by wheel throwing, trimmed, biscuit fired at 840-860° C. for 7.5-8.5 hours, and taken out to obtain a green body;
[0066] (2) grinding 5.8-6.2 parts by weight of glaze stone, 1.8-2.2 parts by weight of potassium feldspar, 0.9-1.1 parts by weight of limestone, 0.1-0.3 parts by weight of talc, 0.2-0.4 parts by weight of iron oxide and 7.8-8.2 parts by weight of water, passing through a 100-mesh sieve, and aging for 2 days to obtain a glaze slurry;
[0067] (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body having a glaze thickness of 1.1-1.3 mm;
[0068] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0069] (4.1) The furnace temperature is raised from room temperature to 490-510°C at a rate of 290-310°C / h, then raised from 490-510°C to 890-910°C at a rate of 230-250°C / h, then raised from 890-910°C to 1040-1060°C at a rate of 100-120°C / h, and kept at 1040-1060°C for 1.8-2.2 min, then raised from 1040-1060°C to 1190-1210°C at a rate of 100-120°C / h, and kept at 1190-1210°C for 1.8-2.2 min, and then raised from 1190-1210°C to 1290-1310°C at a rate of 60-70°C / h;
[0070] (4.2) Keep the temperature at 1290-1310°C for 2.3-2.7 hours, add oil firewood into the electric kiln at 1290-1310°C, once every 2.8-3.2 minutes, for a total of 7 times, the amount of oil firewood added is 58-62g, 58-62g, 78-82g, 78-82g, 95-105g, 95-105g, 95-105g per 0.17-0.19 cubic meters of the electric kiln space, and the electric kiln is powered off after the last addition of oil firewood;
[0071] (4.3) When the furnace temperature drops to 1210-1230℃, add 58-62g of fuel oil into the electric kiln at a rate of 100-200g per 0.17-0.19 cubic meters of the electric kiln space. After 2.8-3.2 minutes of adding fuel oil, open the furnace door. When the furnace temperature drops to 1118-1122℃, close the furnace door.
[0072] (4.4) When the furnace temperature drops to 1098-1102℃, 1088-1092℃ and 1078-1082℃, 38-42g of wood is added into the electric kiln for every 0.17-0.19 cubic meters of the furnace space. After the last addition of wood, the furnace door is opened. After 5.8-6.2 minutes, the furnace door is closed. After 18-22 minutes, the furnace temperature is increased to 950-970℃ at a rate of 78-82℃ / h. After being kept at 950-970℃ for 0.9-1.1 hours, the electric kiln is powered off, and the furnace door is opened to cool down to room temperature, thereby obtaining Jin Yao Jian Zhan.
[0073] In a preferred embodiment of the present invention, the preparation process of the Jinyao Jianzhan of the present invention comprises the following steps:
[0074] (1) 3 parts by weight of red clay and 7 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green clay; the green clay is formed by wheel throwing, trimmed, bisque fired at 850° C. for 8 hours, and taken out to obtain a green body;
[0075] (2) grinding 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 1 part by weight of limestone, 0.2 parts by weight of talc, 0.3 parts by weight of iron oxide and 8 parts by weight of water, passing through a 100-mesh sieve, and aging for 2 days to obtain a glaze slurry;
[0076] (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body with a glaze thickness of 1.2 mm;
[0077] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0078] (4.1) The furnace temperature is raised from room temperature to 500°C at a rate of 300°C / h, then raised from 500°C to 900°C at a rate of 240°C / h, then raised from 900°C to 1050°C at a rate of 110°C / h, and then kept at 1050°C for 2 min, then raised from 1050°C to 1200°C at a rate of 110°C / h, and then kept at 1200°C for 2 min, and then raised from 1200°C to 1300°C at a rate of 65°C / h;
[0079] (4.2) Keep the temperature at 1300℃ for 2.5h. Add oil-fired fuel into the electric kiln at 1300℃ for 7 times every 3min. The amount of oil-fired fuel added is 60g, 60g, 80g, 80g, 100g, 100g, and 100g per 0.18m3 of the electric kiln space. After the last addition of oil-fired fuel, the electric kiln is powered off.
[0080] (4.3) When the furnace temperature drops to 1220℃, add 60g of fuel oil into the electric kiln at a rate of 0.18 cubic meters of furnace space. After adding fuel oil and fuel, open the furnace door 3 minutes later. When the furnace temperature drops to 1120℃, close the furnace door.
[0081] (4.4) When the furnace temperature drops to 1100℃, 1090℃ and 1080℃, 40g of firewood is added into the electric kiln for every 0.18 cubic meters of furnace space. After the last addition of firewood, the furnace door is opened and closed after 6 minutes. After 20 minutes, the furnace temperature is increased to 960℃ at a rate of 80℃ / h. After being kept at 960℃ for 1 hour, the electric kiln is powered off and the furnace door is opened to cool it to room temperature, thus obtaining Jin Yao Jianzhan.
[0082] In a preferred example of the present invention, the preparation process of the Jin Yao Jian Zhan is prepared as described in the method described in specific embodiment 1 of the present invention.
[0083] In a preferred embodiment of the present invention, the Jinyao Jianzhan of the present invention is as shown in the attached specification. Figure 1 , Figure 2 and Figure 3 shown.
[0084] The main excellent effects of the present invention include:
[0085] The present invention develops a Jin Yao Jian teak with excellent appearance and artistic value. The glaze surface of the Jin Yao Jian teak prepared by the process of the present invention has a Yao change, and the oil droplets are golden, which is called Jin Yao. The magnificent characteristics are unique and beautiful, just like a matrix that contains the nourishment of all things. The oil droplets are feathered with textures, moisturizing, and mimicking vividness. The hairs of the Jin Yao Jian teak are fine and clear, dense and well-proportioned, with a strong sense of layering. The glaze surface has no spots, no pores, and good texture. It has rich and beautiful glaze colors and profound artistic heritage and charm, and thus has beautiful artistic and collection value.
[0086] The present invention is further described below in conjunction with specific examples. It should be understood that the following specific examples are based on the technical solution and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to these examples.
[0087] Examples and Comparative Examples
[0088] The red clay comes from Shuiji Town, Jianyang District, Nanping City, Fujian Province; the kaolin comes from Shuiji Town, Jianyang District, Nanping City, Fujian Province; and the glaze stone comes from Nanlin Village, Jianyang District, Nanping City, Fujian Province.
[0089] Example 1: Jinyao Jianzhan
[0090] The preparation process of Jinyao Jianzhan includes the following steps:
[0091] (1) 3 parts by weight of laterite and 7 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green clay; the green clay is formed by wheel throwing, trimmed, bisque fired at 850° C. for 8 h, and taken out to obtain a green body.
[0092] (2) 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 1 part by weight of limestone, 0.2 parts by weight of talc, 0.3 parts by weight of iron oxide and 8 parts by weight of water are put into a ball mill and ground, passed through a 100-mesh sieve, and aged for 2 days to obtain a glaze slurry.
[0093] (3) Apply the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body with a glaze thickness of 1.2 mm.
[0094] (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps:
[0095] (4.1) The furnace temperature is raised from room temperature of 20°C to 500°C at a rate of 300°C / h, then raised from 500°C to 900°C at a rate of 240°C / h, then raised from 900°C to 1050°C at a rate of 110°C / h, and then kept at 1050°C for 2 min, then raised from 1050°C to 1200°C at a rate of 110°C / h, and then kept at 1200°C for 2 min, then raised from 1200°C to 1300°C at a rate of 65°C / h;
[0096] (4.2) Keep the temperature at 1300℃ for 2.5h. Add oil-fired fuel into the electric kiln at 1300℃ for 7 times every 3min. The amount of oil-fired fuel added is 60g, 60g, 80g, 80g, 100g, 100g, and 100g per 0.18m3 of the electric kiln space. After the last addition of oil-fired fuel, the electric kiln is powered off.
[0097] (4.3) When the furnace temperature drops to 1220℃, add 60g of fuel oil into the electric kiln at a rate of 0.18 cubic meters of furnace space. After adding fuel oil and fuel, open the furnace door 3 minutes later. When the furnace temperature drops to 1120℃, close the furnace door.
[0098] (4.4) When the furnace temperature drops to 1100℃, 1090℃ and 1080℃, 40g of firewood is added into the electric kiln for every 0.18 cubic meters of furnace space. After the last addition of firewood, the furnace door is opened and closed after 6 minutes. After 20 minutes, the furnace temperature is increased to 960℃ at a rate of 80℃ / h. After being kept at 960℃ for 1 hour, the electric kiln is powered off and the furnace door is opened to cool it to a normal temperature of 20℃, thus obtaining Jin Yao Jianzhan.
[0099] Effect evaluation:
[0100] The Jianzhan prepared in this embodiment 1 is a Jinyao Jianzhan. Figure 1 , Figure 2 and Figure 3 As shown, it can be seen that the glaze surface of the Jin Yao Jian Zhan prepared in Example 1 has a Yao change, and the oil droplets are golden, which is called Jin Yao. It has magnificent characteristics and is unique among the flowers, like a matrix that contains the nourishment of all things. The oil droplets are feathered with textures, moisturizing, and mimicking vividness. The hairs of the Jin Yao Jian Zhan are fine and clear, densely arranged, and layered. The glaze surface has no spots, no pores, and good texture. It has rich and beautiful glaze colors and profound artistic heritage and charm, and thus has beautiful artistic and collection value.
[0101] Comparative Example 1
[0102] The preparation process of Jianzhan in this comparative example 1 is the same as that in Example 1, except that: Step (2):
[0103] (2) 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 0.2 parts by weight of talc, 0.3 parts by weight of iron oxide and 8 parts by weight of water are put into a ball mill and ground, passed through a 100-mesh sieve, and aged for 2 days to obtain a glaze slurry.
[0104] The glaze surface of the Jianzhan prepared in this comparative example 1 has no oil drops.
[0105] Comparative Example 2
[0106] The preparation process of Jianzhan in this comparative example 2 is the same as that in Example 1, except that: Step (2):
[0107] (2) 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 1 part by weight of limestone, 0.2 parts by weight of talc and 8 parts by weight of water are put into a ball mill and ground, passed through a 100-mesh sieve, and aged for 2 days to obtain a glaze slurry.
[0108] The oil droplets on the glaze of the Jian ware prepared in Comparative Example 2 are small and densely packed.
[0109] Comparative Example 3
[0110] The preparation process of Jianzhan in this comparative example 3 is the same as that in Example 1, except that: Step (2):
[0111] (2) 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 1 part by weight of limestone, 0.3 parts by weight of iron oxide and 8 parts by weight of water are put into a ball mill and ground, passed through a 100-mesh sieve, and aged for 2 days to obtain a glaze slurry.
[0112] The shape of the oil droplets on the glaze surface of the Jianzhan prepared in Comparative Example 3 is abnormal and irregular.
[0113] Comparative Example 4
[0114] The preparation process of the Jianzhan in Comparative Example 4 is the same as that in Example 1, except that: (4) the glazed body obtained in step (3) is fired in an electric kiln, and the firing comprises the following steps:
[0115] (4.1) The furnace temperature is raised from room temperature of 20°C to 500°C at a rate of 300°C / h, then raised from 500°C to 900°C at a rate of 240°C / h, then raised from 900°C to 1050°C at a rate of 110°C / h, and then kept at 1050°C for 2 min, then raised from 1050°C to 1200°C at a rate of 110°C / h, and then kept at 1200°C for 2 min, then raised from 1200°C to 1300°C at a rate of 65°C / h;
[0116] (4.2) Keep the temperature at 1300℃ for 2.5h. Add oil-fired fuel into the electric kiln at 1300℃ for 7 times every 3min. The amount of oil-fired fuel added is 60g, 60g, 80g, 80g, 100g, 100g, and 100g per 0.18m3 of the electric kiln space. After the last addition of oil-fired fuel, the electric kiln is powered off.
[0117] (4.3) Open the furnace door and cool down to room temperature of 20℃ to obtain Jianzhan.
[0118] The Jian ware prepared in Comparative Example 4 has no golden oil droplets on the glaze, a dull glaze, blurred texture, a rough glaze, and a poor texture.
[0119] Comparative Example 5
[0120] The preparation process of the Jianzhan in this comparative example 5 is the same as that in Example 1, except that: (4) the glazed body obtained in step (3) is fired in an electric kiln, and the firing comprises the steps of:
[0121] (4.1) The furnace temperature is raised from room temperature of 20°C to 500°C at a rate of 300°C / h, then raised from 500°C to 900°C at a rate of 240°C / h, then raised from 900°C to 1050°C at a rate of 110°C / h, and then kept at 1050°C for 2 min, then raised from 1050°C to 1200°C at a rate of 110°C / h, and then kept at 1200°C for 2 min, then raised from 1200°C to 1300°C at a rate of 65°C / h;
[0122] (4.2) Keep the temperature at 1300℃ for 2.5h, then add fuel oil into the electric kiln at 1300℃, once every 3min, for a total of 7 times, with 80g of fuel oil added each time for every 0.18m3 of the electric kiln space. After the last addition of fuel oil, the electric kiln is powered off;
[0123] (4.3) When the furnace temperature drops to 1100℃, 1090℃ and 1080℃, 40g of firewood is added into the electric kiln for every 0.18 cubic meters of furnace space. After the last addition of firewood, the furnace door is opened and closed after 6 minutes. After 20 minutes, the furnace temperature is increased to 960℃ at a rate of 80℃ / h. After being kept at 960℃ for 1 hour, the electric kiln is powered off and the furnace door is opened to cool it to a normal temperature of 20℃, thus obtaining Jin Yao Jianzhan.
[0124] The Jian ware prepared in comparative example 5 has a glaze surface without feathering and has feathered oil droplets with patterns, and the glaze surface is dull and has a poor texture.
[0125] The above is an implementation scheme of the present invention designed for a case. It should be pointed out that for ordinary technicians in this technical field, several improvements can be made without departing from the principle of the present invention, and these improvements should also be regarded as the scope of protection of the present invention.
Claims
1. A preparation process of Jinyao Jianzhan, It is characterized in that The process comprises the following steps: (1) 2.5-3.5 parts by weight of laterite and 6-8 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 80-120 mesh sieve, filtered, refined, and aged to obtain green mud; the green mud is formed by wheel throwing, trimmed, biscuit fired at 830-840° C. for 7.5-8.5 hours, and taken out to obtain a green body; (2) grinding 5.5-6.5 parts by weight of glaze stone, 1.5-2.5 parts by weight of potassium feldspar, 0.8-1.2 parts by weight of limestone, 0.1-0.4 parts by weight of talc, 0.1-0.5 parts by weight of iron oxide and 7-9 parts by weight of water, passing through a 80-120 mesh sieve, and aging for 1.5-2.5 days to obtain a glaze slurry; (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body having a glaze thickness of 1.0-1.4 mm; (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps: (4.1) The furnace temperature is raised from room temperature to 480-520℃ at a rate of 280-320℃ / h, then raised from 480-520℃ to 880-920℃ at a rate of 220-260℃ / h, then raised from 880-920℃ to 1030-1070℃ at a rate of 90-130℃ / h, and kept at 1030-1070℃ for 1.5-2.5min, then raised from 1030-1070℃ to 1180-1220℃ at a rate of 90-130℃ / h, and kept at 1180-1220℃ for 1.5-2.5min, then raised from 1180-1220℃ to 1280-1320℃ at a rate of 55-75℃ / h; (4.2) Keep the temperature at 1280-1320℃ for 2.3-2.7h. Add oil-fired fuel into the electric kiln at 1280-1320℃, once every 2.5-3.5min, for a total of 7 times. The amount of oil-fired fuel added is 55-65g, 55-65g, 75-85g, 75-85g, 90-110g, 90-110g, 90-110g per 0.16-0.20 cubic meter of the electric kiln space. After the last addition of oil-fired fuel, the electric kiln is powered off. (4.3) When the furnace temperature drops to 1200-1240℃, add 55-65g of fuel oil into the electric kiln at a rate of 100-200g per 0.16-0.20 cubic meters of the electric kiln space. After 2.5-3.5 minutes of adding fuel oil, open the furnace door. When the furnace temperature drops to 1115-1125℃, close the furnace door. (4.4) When the furnace temperature drops to 1097-1103℃, 1087-1093℃ and 1077-1083℃, 35-45g of firewood is added into the electric kiln for every 0.16-0.20 cubic meters of furnace space. After the last addition of firewood, the furnace door is opened and closed after 5-7 minutes. After 15-25 minutes, the furnace temperature is increased to 940-980℃ at a rate of 70-90℃ / h. After maintaining at 940-980℃ for 0.8-1.2h, the electric kiln is powered off and the furnace door is opened to cool down to room temperature, thereby obtaining Jin Yao Jian Zhan.
2. The process according to claim 1, It is characterized in that The process comprises the following steps: (1) 2.7-3.3 parts by weight of laterite and 6.8-7.2 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green mud; the green mud is formed by wheel throwing, trimmed, biscuit fired at 840-860° C. for 7.5-8.5 hours, and taken out to obtain a green body; (2) grinding 5.8-6.2 parts by weight of glaze stone, 1.8-2.2 parts by weight of potassium feldspar, 0.9-1.1 parts by weight of limestone, 0.1-0.3 parts by weight of talc, 0.2-0.4 parts by weight of iron oxide and 7.8-8.2 parts by weight of water, passing through a 100-mesh sieve, and aging for 2 days to obtain a glaze slurry; (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body having a glaze thickness of 1.1-1.3 mm; (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps: (4.1) The furnace temperature is raised from room temperature to 490-510°C at a rate of 290-310°C / h, then raised from 490-510°C to 890-910°C at a rate of 230-250°C / h, then raised from 890-910°C to 1040-1060°C at a rate of 100-120°C / h, and kept at 1040-1060°C for 1.8-2.2 min, then raised from 1040-1060°C to 1190-1210°C at a rate of 100-120°C / h, and kept at 1190-1210°C for 1.8-2.2 min, then raised from 1190-1210°C to 1290-1310°C at a rate of 60-70°C / h; (4.2) Keep the temperature at 1290-1310℃ for 2.3-2.7h. Add oil-fired fuel into the electric kiln at 1290-1310℃, once every 2.8-3.2min, for a total of 7 times. The amount of oil-fired fuel added is 58-62g, 58-62g, 78-82g, 78-82g, 95-105g, 95-105g, and 95-105g per 0.17-0.19 cubic meter of the electric kiln space. After the last addition of oil-fired fuel, the electric kiln is powered off. (4.3) When the furnace temperature drops to 1210-1230℃, add 58-62g of fuel oil into the electric kiln at a rate of 100-200g per 0.17-0.19 cubic meters of the electric kiln space. After 2.8-3.2 minutes of adding fuel oil, open the furnace door and close the furnace door when the furnace temperature drops to 1118-1122℃. (4.4) When the furnace temperature drops to 1098-1102℃, 1088-1092℃ and 1078-1082℃, 38-42g of firewood is added into the electric kiln for every 0.17-0.19 cubic meters of furnace space respectively. After the last addition of firewood, the furnace door is opened. After 5.8-6.2 minutes, the furnace door is closed. After 18-22 minutes, the furnace temperature is increased to 950-970℃ at a rate of 78-82℃ / h. After keeping at 950-970℃ for 0.9-1.1 hours, the electric kiln is powered off, the furnace door is opened and the temperature is lowered to room temperature, thus obtaining Jin Yao Jian Zhan.
3. The process according to claim 1, It is characterized in that The process comprises the following steps: (1) 3 parts by weight of laterite and 7 parts by weight of kaolin are mixed, crushed, washed with water, passed through a 100-mesh sieve, filtered, refined, and aged to obtain green clay; the green clay is formed by wheel throwing, trimmed, bisque fired at 850° C. for 8 hours, and taken out to obtain a green body; (2) grinding 6 parts by weight of glaze stone, 2 parts by weight of potassium feldspar, 1 part by weight of limestone, 0.2 parts by weight of talc, 0.3 parts by weight of iron oxide and 8 parts by weight of water, passing through a 100-mesh sieve, and aging for 2 days to obtain a glaze slurry; (3) applying the glaze slurry prepared in step (2) to the green body prepared in step (1) to obtain a glazed green body with a glaze thickness of 1.2 mm; (4) calcining the glazed body obtained in step (3) in an electric kiln, wherein the calcining comprises the following steps: (4.1) The furnace temperature is raised from room temperature to 500°C at a rate of 300°C / h, then raised from 500°C to 900°C at a rate of 240°C / h, then raised from 900°C to 1050°C at a rate of 110°C / h, and then kept at 1050°C for 2 min, then raised from 1050°C to 1200°C at a rate of 110°C / h, and then kept at 1200°C for 2 min, and then raised from 1200°C to 1300°C at a rate of 65°C / h; (4.2) Keep the furnace at 1300℃ for 2.5h. Add oil-fired fuel into the furnace at 1300℃, once every 3min, for a total of 7 times. The amount of oil-fired fuel added is 60g, 60g, 80g, 80g, 100g, 100g, and 100g per 0.18 cubic meter of the furnace space. After the last addition of oil-fired fuel, the furnace is powered off. (4.3) When the furnace temperature drops to 1220℃, add 60g of fuel oil into the electric kiln at a rate of 0.18 cubic meters of furnace space. After adding fuel oil and fuel, open the furnace door 3 minutes after the addition of fuel oil and fuel. When the furnace temperature drops to 1120℃, close the furnace door. (4.4) When the furnace temperature drops to 1100℃, 1090℃ and 1080℃, 40g of firewood is added into the electric kiln for every 0.18 cubic meters of furnace space. After the last addition of firewood, the furnace door is opened and closed after 6 minutes. After 20 minutes, the furnace temperature is increased to 960℃ at a rate of 80℃ / h. After being kept at 960℃ for 1 hour, the electric kiln is powered off and the furnace door is opened to cool it to room temperature, thus obtaining the Jin Yao Jianzhan.
4. A kind of Jinyao Jianzhan, It is characterized in that The Jin Yao Jian Zhan is prepared by the process as described in claim 1.