A low halo electrically controlled dimming film and its preparation method and automobile window
By setting the refractive index gradient changes in the PDLC film and filling particles to form optical traps, the halo problem of PDLC film on the automotive sunroof is solved, and the transparency and permeability of the film is improved.
Patent Information
- Application Number
- CN202210720585.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-06-23
AI Technical Summary
There is obvious halo phenomenon in automotive sunroof applications, mainly due to differences in base film thickness, conductive film layer thickness, PDLC layer thickness and liquid crystal droplet size, coating composition deviation and refractive index mismatch.
The refractive index gradient between the PDLC layer, the microdiffusion layer, the first microdiffusion layer, the PDLC layer, the second microdiffusion layer, and the second conductive film layer are arranged using the structures of the sequentially overlapped first conductive film layer, the microdiffusion layer and the conductive film layer. Change and fill the microdiffusion layer with spherical or ellipsoidal particles to form optical traps to increase absorption and reduce reflectivity.
It effectively reduces the halo phenomenon of the dimming film when powered on, improves the atomization effect and permeability when powered off, and achieves ideal light transmission and diffusion effects.
Smart Images

Figure CN115061307B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a dimming film and a preparation method and application thereof, in particular to a low-halo electrically controlled dimming film and a preparation method thereof and an automobile window. Background Art
[0002] PDLC film is a new type of functional optoelectronic film, also known as electrically controlled liquid crystal dimming film. Through the control of an external electric field, the dimming film can be quickly switched between the two states of colorless transparency and milky white opaque. Liquid crystal dimming film is widely used and can be used wherever there is glass. It is usually used in high-end hotel rooms, museums, banks, conference rooms, store windows, etc. It has privacy protection, space transparency, security and defense, and light adjustment.
[0003] With the advancement of dimming film technology, the performance of dimming film has been continuously improved and has begun to be used in automobiles. When PDLC film is used in automobile sunroofs, it is found that there is a very obvious halo phenomenon in the transparent state. The main reasons for the halo when the PDLC film is powered on are the thickness of the base film, the thickness of the conductive film layer, the thickness of the PDLC layer, the size difference of the liquid crystal droplets, the deviation of the coating composition, the mismatch of the refractive index, etc. Users are not satisfied with the halo phenomenon and it is urgently needed to be improved. Summary of the invention
[0004] In order to overcome the deficiencies of the prior art, the present invention provides a low-halo electrically-controlled dimming film without obvious halo phenomenon, and a preparation method and application thereof.
[0005] The technical solution adopted by the present invention to solve its technical problem is:
[0006] A low-halo electrically controlled dimming film comprises a first conductive film layer, a first micro-diffusion layer, a PDLC layer, a second micro-diffusion layer and a second conductive film layer stacked in sequence, wherein the refractive indices of the PDLC layer, the first micro-diffusion layer and the first conductive film layer vary in a gradient; and the refractive indices of the PDLC layer, the second micro-diffusion layer and the second conductive film layer vary in a gradient.
[0007] The refractive index of the PDLC layer is respectively smaller than the refractive index of the first micro diffusion layer and the refractive index of the second micro diffusion layer, and the refractive index of the first micro diffusion layer and the second micro diffusion layer are respectively smaller than the refractive index of the first conductive film layer and the refractive index of the second conductive film layer.
[0008] The refractive index of the PDLC layer is 1.5-1.6, the refractive index of the first micro-diffusion layer and the refractive index of the second micro-diffusion layer are 1.6-1.7 respectively, and the refractive index of the first conductive film layer and the second conductive film layer are 1.7-1.8 respectively.
[0009] The refractive index of the first micro-diffusion layer is the same as that of the second micro-diffusion layer, and the refractive index of the first conductive film layer is the same as that of the second conductive film layer, so that the gradient changes of the PDLC layer 3 and the micro-diffusion layers and conductive film layers on both sides are the same, and the overall product effect is better.
[0010] The first micro-diffusion layer and the second micro-diffusion layer are both resin adhesive layers, the resin adhesive layers are filled with spherical particles or ellipsoidal particles, and some of the spherical particles or ellipsoidal particles are exposed on the outer surface of the resin adhesive layer.
[0011] The diameter of the spherical particles or ellipsoidal particles includes at least a first diameter and a second diameter, the spherical particles or ellipsoidal particles of the first diameter account for 1-10% of the volume of the first micro-diffusion layer or the second micro-diffusion layer, and the spherical particles or ellipsoidal particles of the second diameter account for 1-10% of the volume of the first micro-diffusion layer or the second micro-diffusion layer.
[0012] The thickness of the first micro-diffusion layer and the second micro-diffusion layer are 2-4 micrometers respectively, the first diameter of the spherical particles or ellipsoidal particles is 0.5-2 micrometers, and the second diameter of the spherical particles or ellipsoidal particles is 3-5 micrometers.
[0013] Spherical particles or ellipsoidal particles of two sizes are used, and some of the spherical particles or ellipsoidal particles are exposed on the rubber surface, making the surface of the micro-diffusion layer uneven, forming an optical trap, increasing the absorption rate, and reducing the reflectivity, so that the dimming film has a better atomization effect when the power is off and better permeability when the power is on, achieving ideal light transmission and diffusion effects.
[0014] The method for preparing the above-mentioned low halo electrically controlled dimming film comprises the following steps:
[0015] Step 1: Select 2 base films, sputter ITO films on the base films respectively to obtain a first conductive film layer and a second conductive film layer, wherein the first conductive film layer and the second conductive film layer have no halo, and the sputtering is a magnetron sputtering coating method, and the obtained ITO conductive film has good thickness uniformity.
[0016] Step 2: coating a first micro-diffusion layer on the ITO surface of the first conductive film layer, and coating a second micro-diffusion layer on the ITO surface of the second conductive film layer, the coating method is slit coating, the raw material of the micro-diffusion layer is extruded and sprayed along the gap of the coating mold under a certain pressure and a certain flow rate and transferred to the ITO surface of the ITO conductive film, the first micro-diffusion layer and the second micro-diffusion layer both contain spherical particles or ellipsoidal particles exposed on the surface of the layer structure.
[0017] The slit coating method has the advantages of fast coating speed, high precision, uniform thickness, and the refractive index of the micro-diffusion layer is consistent at all locations. The coating system is closed, which can prevent pollutants from entering during the coating process, has high slurry utilization rate, and can maintain stable slurry properties.
[0018] Step 3: Dropping PDLC material between the first micro-diffusion layer and the second micro-diffusion layer to form a PDLC layer, the spacer can ensure the thickness uniformity of the PDLC layer, and rolling the whole layer, and obtaining a liquid crystal film after UV curing.
[0019] The PDLC material is composed of liquid crystal, UV glue and spacers, and is a PDLC component prepared according to a patent for a wide temperature dimming film and a preparation method thereof with publication number "CN108594509A".
[0020] In the step 2, the spherical particles are SiO 2 Particles or TiO 2 Particles or Si 3 N 4 particle.
[0021] In the step 1, the thickness of the base film is 178-198 microns, the sheet resistance of the first conductive film layer and the second conductive film layer is 50-150Ω, the visible light transmittance is 20-90%, and the haze is 0.2-2.
[0022] In the step 3, the size of the liquid crystal droplets of the PDLC layer is 1 to 2 microns. In the PDLC layer 3, the liquid crystal exists in the polymer matrix in the form of micron-sized droplets. The refractive index between the ITO conductive film, the micro-diffusion layer and the PDLC layer is set to change in a gradient, which can compensate for the size difference of 1 to 2 microns of the liquid crystal droplets in the PDLC layer and reduce the halo phenomenon.
[0023] In the step 3, the rolled liquid crystal film is cured by ultraviolet light, the UV light intensity is 4-30mw / cm², the curing temperature is 18-26°C, and the curing time is 2-4min.
[0024] In addition, the present invention can also adopt a roll-to-roll continuous production method to produce a low-halo electrically controlled dimming film, first coating a micro-diffusion layer on an ITO conductive film and performing UV light curing, then coating a PDLC layer on the micro-diffusion layer of one of the ITO conductive films by a slit coating method, and then laminating the micro-diffusion layer of another ITO conductive film on the PDLC layer, and finally performing UV curing.
[0025] A low-halo electrically-controlled dimming film is used on a car sunroof or other windows. The low-halo electrically-controlled dimming film is the low-halo electrically-controlled dimming film mentioned above, or is the low-halo electrically-controlled dimming film prepared by the above preparation method.
[0026] The beneficial effects of the present invention are:
[0027] 1. The present invention provides a low-halo electrically controlled dimming film and a preparation method and application thereof. The prepared dimming film includes a first conductive film layer, a first micro-diffusion layer, a PDLC layer, a second micro-diffusion layer and a second conductive film layer stacked in sequence. The refractive indexes of the PDLC layer, the micro-diffusion layer and the conductive film layer are arranged to change in a gradient, thereby compensating for the size difference of 1 to 2 microns of liquid crystal droplets in the PDLC layer, reducing the halo problem of the dimming film when power is turned on. When the dimming film is applied to a car sunroof, the dimming film in a transparent state has no obvious halo phenomenon under sunlight or strong light.
[0028] 2. In addition, the first micro-diffusion layer and the second micro-diffusion layer of the present invention contain spherical particles or ellipsoidal particles of two particle sizes, and some of the spherical particles or ellipsoidal particles are exposed from the adhesive surface, so that the surface of the micro-diffusion layer is uneven, forming an optical trap, increasing the absorption rate, and reducing the reflectivity, so that the dimming film has a better atomization effect when the power is off, and better permeability when the power is on, achieving an ideal light transmission and diffusion effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0030] Figure 1 is a schematic structural diagram of embodiment 1 of the present invention;
[0031] Figure 2 It is a schematic structural diagram of embodiment 4 of the present invention. DETAILED DESCRIPTION
[0032] In the following embodiments, all parts not emphasized are at normal temperature and pressure.
[0033] Embodiment 1:
[0034] Reference Figure 1 A low halo electrically controlled dimming film comprises a first conductive film layer 1, a first micro-diffusion layer 2, a PDLC layer 3, a second micro-diffusion layer 4 and a second conductive film layer 5 which are stacked in sequence, wherein the refractive indexes of the PDLC layer 3, the first micro-diffusion layer 2 and the first conductive film layer 1 vary in a gradient; and the refractive indexes of the PDLC layer 3, the second micro-diffusion layer 4 and the second conductive film layer 5 vary in a gradient.
[0035] The refractive index of the PDLC layer 3 is respectively smaller than the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are respectively smaller than the refractive index of the first conductive film layer 1 and the refractive index of the second conductive film layer 5 .
[0036] The refractive index of the PDLC layer 3 is 1.55, the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 are 1.62 respectively, and the refractive index of the first conductive film layer 1 and the second conductive film layer 5 are 1.78 respectively.
[0037] The refractive index of the first micro-diffusion layer 2 is the same as the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first conductive film layer 1 is the same as the refractive index of the second conductive film layer 5 .
[0038] The first micro-diffusion layer 2 and the second micro-diffusion layer 4 are both resin adhesive layers, and the resin adhesive layers are filled with spherical particles 6, and some of the spherical particles 6 are exposed on the outer surface of the resin adhesive layer.
[0039] The diameter of the spherical particles 6 includes at least a first diameter and a second diameter. The spherical particles 6 of the first diameter account for 5% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 , and the spherical particles 6 of the second diameter account for 5% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 .
[0040] The thickness of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are 3 micrometers respectively, the first diameter of the spherical particles 6 is 1 micrometer, and the second diameter of the spherical particles 6 is 4 micrometers.
[0041] The method for preparing the above-mentioned low halo electrically controlled dimming film comprises the following steps:
[0042] Step 1: Select 2 base films with a thickness of 188 μm, and sputter ITO films on the base films respectively to obtain a first conductive film layer 1 and a second conductive film layer 5; the sheet resistance of the first conductive film layer 1 and the second conductive film layer 5 is 120Ω, the visible light transmittance is 84%, and the haze is 0.5.
[0043] Step 2: Coat the first micro-diffusion layer 2 on the ITO surface of the first conductive film layer 1, and coat the second micro-diffusion layer 4 on the ITO surface of the second conductive film layer 5. The first micro-diffusion layer 2 and the second micro-diffusion layer 4 both contain spherical particles 6 exposed on the surface of the layer structure. The spherical particles 6 are SiO 2 particle.
[0044] Step 3: Drop the PDLC material between the first micro-diffusion layer 2 and the second micro-diffusion layer 4 to form a PDLC layer 3, wherein the size of the liquid crystal droplets of the PDLC layer 3 is 1-2 microns, and the whole is rolled and cured by ultraviolet light to obtain a liquid crystal film, wherein the UV light intensity of the ultraviolet light curing is 6mw / cm², the curing temperature is 24°C, and the curing time is 3min.
[0045] A low-halo electrically-controlled dimming film is used on a car sunroof or other windows. The low-halo electrically-controlled dimming film is the low-halo electrically-controlled dimming film mentioned above, or is the low-halo electrically-controlled dimming film prepared by the above preparation method.
[0046] The present embodiment provides a low-halo electrically controlled dimming film and a preparation method and application thereof. The prepared dimming film includes a first conductive film layer 1, a first micro-diffusion layer 2, a PDLC layer 3, a second micro-diffusion layer 4 and a second conductive film layer 5 which are stacked in sequence. The refractive indexes of the PDLC layer, the micro-diffusion layer and the conductive film layer are arranged to vary in a gradient, thereby compensating for the size difference of 1 to 2 microns of the liquid crystal droplets in the PDLC layer 3, reducing the halo problem of the dimming film when power is turned on. When the dimming film is applied to a car sunroof, the dimming film in a transparent state has no obvious halo phenomenon under sunlight or strong light.
[0047] In addition, the first micro-diffusion layer 2 and the second micro-diffusion layer 4 of the present embodiment contain spherical particles 6 or ellipsoidal particles 7 of two particle sizes, and some of the spherical particles 6 or ellipsoidal particles 7 are exposed from the glue surface, so that the surface of the micro-diffusion layer is uneven, forming an optical trap, increasing the absorption rate and reducing the reflectivity, so that the dimming film has a better atomization effect when the power is off and a better permeability when the power is on, achieving an ideal light transmission and diffusion effect.
[0048] Embodiment 2:
[0049] A low-halo electrically controlled dimming film comprises a first conductive film layer 1, a first micro-diffusion layer 2, a PDLC layer 3, a second micro-diffusion layer 4 and a second conductive film layer 5 which are stacked in sequence. The refractive indices of the PDLC layer 3, the first micro-diffusion layer 2 and the first conductive film layer 1 vary in gradient; the refractive indices of the PDLC layer 3, the second micro-diffusion layer 4 and the second conductive film layer 5 vary in gradient.
[0050] The refractive index of the PDLC layer 3 is respectively smaller than the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are respectively smaller than the refractive index of the first conductive film layer 1 and the refractive index of the second conductive film layer 5 .
[0051] The refractive index of the PDLC layer 3 is 1.5, the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 are 1.6 respectively, and the refractive index of the first conductive film layer 1 and the second conductive film layer 5 are 1.7 respectively.
[0052] The refractive index of the first micro-diffusion layer 2 is the same as the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first conductive film layer 1 is the same as the refractive index of the second conductive film layer 5 .
[0053] The first micro-diffusion layer 2 and the second micro-diffusion layer 4 are both resin adhesive layers, and the resin adhesive layers are filled with spherical particles 6, and some of the spherical particles 6 are exposed on the outer surface of the resin adhesive layer.
[0054] The diameter of the spherical particles 6 includes at least a first diameter and a second diameter. The spherical particles 6 of the first diameter account for 3% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 , and the spherical particles 6 of the second diameter account for 3% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 .
[0055] The thickness of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are respectively 2 micrometers, the first diameter of the spherical particles 6 is 0.5 micrometers, and the second diameter of the spherical particles 6 is 3 micrometers.
[0056] The method for preparing the above-mentioned low halo electrically controlled dimming film comprises the following steps:
[0057] Step 1: Select 2 base films with a thickness of 188 μm, and sputter ITO films on the base films respectively to obtain a first conductive film layer 1 and a second conductive film layer 5; the sheet resistance of the first conductive film layer 1 and the second conductive film layer 5 is 120Ω, the visible light transmittance is 84%, and the haze is 0.5.
[0058] Step 2: Coat the first micro-diffusion layer 2 on the ITO surface of the first conductive film layer 1, and coat the second micro-diffusion layer 4 on the ITO surface of the second conductive film layer 5. The first micro-diffusion layer 2 and the second micro-diffusion layer 4 both contain spherical particles 6 exposed on the surface of the layer structure. The spherical particles 6 are SiO 2 particle.
[0059] Step 3: Drop the PDLC material between the first micro-diffusion layer 2 and the second micro-diffusion layer 4 to form a PDLC layer 3, wherein the size of the liquid crystal droplets of the PDLC layer 3 is 1-2 microns, and the whole is rolled and cured by ultraviolet light to obtain a liquid crystal film, wherein the UV light intensity of the ultraviolet light curing is 6mw / cm², the curing temperature is 24°C, and the curing time is 3min.
[0060] A low-halo electrically-controlled dimming film is used on a car sunroof or other windows. The low-halo electrically-controlled dimming film is the low-halo electrically-controlled dimming film mentioned above, or is the low-halo electrically-controlled dimming film prepared by the above preparation method.
[0061] Embodiment 3:
[0062] A low-halo electrically controlled dimming film comprises a first conductive film layer 1, a first micro-diffusion layer 2, a PDLC layer 3, a second micro-diffusion layer 4 and a second conductive film layer 5 which are stacked in sequence. The refractive indices of the PDLC layer 3, the first micro-diffusion layer 2 and the first conductive film layer 1 vary in gradient; the refractive indices of the PDLC layer 3, the second micro-diffusion layer 4 and the second conductive film layer 5 vary in gradient.
[0063] The refractive index of the PDLC layer 3 is respectively smaller than the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are respectively smaller than the refractive index of the first conductive film layer 1 and the refractive index of the second conductive film layer 5 .
[0064] The refractive index of the PDLC layer 3 is 1.6, the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 are 1.7 respectively, and the refractive index of the first conductive film layer 1 and the second conductive film layer 5 are 1.8 respectively.
[0065] The refractive index of the first micro-diffusion layer 2 is the same as the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first conductive film layer 1 is the same as the refractive index of the second conductive film layer 5 .
[0066] The first micro-diffusion layer 2 and the second micro-diffusion layer 4 are both resin adhesive layers, and the resin adhesive layers are filled with spherical particles 6, and some of the spherical particles 6 are exposed on the outer surface of the resin adhesive layer.
[0067] The diameter of the spherical particles 6 includes at least a first diameter and a second diameter. The spherical particles 6 of the first diameter account for 8% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 , and the spherical particles 6 of the second diameter account for 8% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 .
[0068] The thickness of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are 4 micrometers respectively, the first diameter of the spherical particles 6 is 2 micrometers, and the second diameter of the spherical particles 6 is 5 micrometers.
[0069] The method for preparing the above-mentioned low halo electrically controlled dimming film comprises the following steps:
[0070] Step 1: Select 2 base films with a thickness of 188 μm, and sputter ITO films on the base films respectively to obtain a first conductive film layer 1 and a second conductive film layer 5; the sheet resistance of the first conductive film layer 1 and the second conductive film layer 5 is 120Ω, the visible light transmittance is 84%, and the haze is 0.5.
[0071] Step 2: Coat the first micro-diffusion layer 2 on the ITO surface of the first conductive film layer 1, and coat the second micro-diffusion layer 4 on the ITO surface of the second conductive film layer 5. The first micro-diffusion layer 2 and the second micro-diffusion layer 4 both contain spherical particles 6 exposed on the surface of the layer structure. The spherical particles 6 are SiO 2 particle.
[0072] Step 3: Drop the PDLC material between the first micro-diffusion layer 2 and the second micro-diffusion layer 4 to form a PDLC layer 3, wherein the size of the liquid crystal droplets of the PDLC layer 3 is 1-2 microns, and the whole is rolled and cured by ultraviolet light to obtain a liquid crystal film, wherein the UV light intensity of the ultraviolet light curing is 6mw / cm², the curing temperature is 24°C, and the curing time is 3min.
[0073] A low-halo electrically-controlled dimming film is used on a car sunroof or other windows. The low-halo electrically-controlled dimming film is the low-halo electrically-controlled dimming film mentioned above, or is the low-halo electrically-controlled dimming film prepared by the above preparation method.
[0074] Embodiment 4:
[0075] Reference Figure 2 A low halo electrically controlled dimming film comprises a first conductive film layer 1, a first micro-diffusion layer 2, a PDLC layer 3, a second micro-diffusion layer 4 and a second conductive film layer 5 which are stacked in sequence, wherein the refractive indexes of the PDLC layer 3, the first micro-diffusion layer 2 and the first conductive film layer 1 vary in a gradient; and the refractive indexes of the PDLC layer 3, the second micro-diffusion layer 4 and the second conductive film layer 5 vary in a gradient.
[0076] The refractive index of the PDLC layer 3 is respectively smaller than the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are respectively smaller than the refractive index of the first conductive film layer 1 and the refractive index of the second conductive film layer 5 .
[0077] The refractive index of the PDLC layer 3 is 1.55, the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 are 1.62 respectively, and the refractive index of the first conductive film layer 1 and the second conductive film layer 5 are 1.78 respectively.
[0078] The refractive index of the first micro-diffusion layer 2 is the same as the refractive index of the second micro-diffusion layer 4 , and the refractive index of the first conductive film layer 1 is the same as the refractive index of the second conductive film layer 5 .
[0079] The first micro-diffusion layer 2 and the second micro-diffusion layer 4 are both resin adhesive layers, and the resin adhesive layers are filled with ellipsoidal particles 7, and some of the ellipsoidal particles 7 are exposed on the outer surface of the resin adhesive layer.
[0080] The diameter of the ellipsoidal particles 7 includes at least a first diameter and a second diameter. The ellipsoidal particles 7 of the first diameter account for 5% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 , and the ellipsoidal particles 7 of the second diameter account for 5% of the volume of the first micro-diffusion layer 2 or the second micro-diffusion layer 4 .
[0081] The thickness of the first micro-diffusion layer 2 and the second micro-diffusion layer 4 are respectively 3 micrometers, the first diameter of the ellipsoidal particles 7 is 1 micrometer, and the second diameter of the ellipsoidal particles 7 is 4 micrometers.
[0082] The method for preparing the above-mentioned low halo electrically controlled dimming film comprises the following steps:
[0083] Step 1: Select 2 base films with a thickness of 188 μm, and sputter ITO films on the base films respectively to obtain a first conductive film layer 1 and a second conductive film layer 5; the sheet resistance of the first conductive film layer 1 and the second conductive film layer 5 is 120Ω, the visible light transmittance is 84%, and the haze is 0.5.
[0084] Step 2: Coat the first micro-diffusion layer 2 on the ITO surface of the first conductive film layer 1, and coat the second micro-diffusion layer 4 on the ITO surface of the second conductive film layer 5. Both the first micro-diffusion layer 2 and the second micro-diffusion layer 4 contain ellipsoidal particles 7 exposed on the surface of the layer structure.
[0085] Step 3: Drop the PDLC material between the first micro-diffusion layer 2 and the second micro-diffusion layer 4 to form a PDLC layer 3, wherein the size of the liquid crystal droplets of the PDLC layer 3 is 1-2 microns, and the whole is rolled and cured by ultraviolet light to obtain a liquid crystal film, wherein the UV light intensity of the ultraviolet light curing is 6mw / cm², the curing temperature is 24°C, and the curing time is 3min.
[0086] A low-halo electrically-controlled dimming film is used on a car sunroof or other windows. The low-halo electrically-controlled dimming film is the low-halo electrically-controlled dimming film mentioned above, or is the low-halo electrically-controlled dimming film prepared by the above preparation method.
[0087] Comparative Example 1:
[0088] The refractive index of the first conductive film layer 1 and the refractive index of the second conductive film layer 5 are both 1.6, the refractive index of the first micro-diffusion layer 2 and the refractive index of the second micro-diffusion layer 4 are both 1.6, the refractive index of the PDLC layer is 1.6, and the other parts are the same as those in Embodiment 1.
[0089] Comparative Example 2:
[0090] The first micro-diffusion layer 2 and the second micro-diffusion layer 4 are light-cured acrylic adhesives, and no spherical particles or ellipsoidal particles are filled inside. Other parts are the same as those in the first embodiment.
[0091] Comparative test: The products of Examples 1 to 4 and the products of Comparative Examples 1 and 2 were cut into samples of 1000*2000mm in size, and the halo in the energized transparent state was tested under 5000lx white light, and whether there was obvious halo phenomenon was observed with the naked eye.
[0092] The experimental results show that the products of Examples 1 to 4 do not have obvious halo phenomenon under naked eye observation. The product of Comparative Example 1 has obvious halo phenomenon under naked eye observation. This is because the refractive index between the multilayer structures is the same, which cannot make up for the 1-2 micron size difference of the liquid crystal droplets in the PDLC layer, so the product will have halo phenomenon when powered on. The product of Comparative Example 2 has a slight atomization effect when powered on under naked eye observation, and the transmittance is slightly insufficient compared with the products of Examples 1 to 4 and Comparative Example 1. This is because the micro-diffusion layer in a smooth and flat state cannot form optical traps, has a low absorption rate, and a high reflectivity.
[0093] The above implementation modes cannot limit the protection scope of the present invention. The equivalent modifications and changes made by those skilled in the art without departing from the overall concept of the present invention are still within the scope of the present invention.
Claims
1. A low halo electrically controlled dimming film, characterized in that The invention comprises a first conductive film layer (1), a first micro-diffusion layer (2), a PDLC layer (3), a second micro-diffusion layer (4) and a second conductive film layer (5) which are stacked in sequence, wherein the refractive indices of the PDLC layer (3), the first micro-diffusion layer (2) and the first conductive film layer (1) vary in a gradient; the refractive indices of the PDLC layer (3), the second micro-diffusion layer (4) and the second conductive film layer (5) vary in a gradient; the refractive index of the PDLC layer (3) is 1.5-1.6, the refractive index of the first micro-diffusion layer (2) and the refractive index of the second micro-diffusion layer (4) are respectively 1.6-1.7, and the refractive index of the first conductive film layer (1) and the second conductive film layer (5) are respectively 1.7-1.8; the refractive index of the first micro-diffusion layer (2) is the same as the refractive index of the second micro-diffusion layer (4), and the refractive index of the first conductive film layer (1) is the same as the refractive index of the second conductive film layer (5).
2. The low halo electrically controlled dimming film according to claim 1, characterized in that The refractive index of the PDLC layer (3) is respectively smaller than the refractive index of the first micro-diffusion layer (2) and the refractive index of the second micro-diffusion layer (4); and the refractive index of the first micro-diffusion layer (2) and the second micro-diffusion layer (4) are respectively smaller than the refractive index of the first conductive film layer (1) and the refractive index of the second conductive film layer (5).
3. The low halo electrically controlled dimming film according to claim 1, characterized in that The first micro-diffusion layer (2) and the second micro-diffusion layer (4) are both resin adhesive layers, the resin adhesive layers are filled with spherical particles (6) or ellipsoidal particles (7), and some of the spherical particles (6) or ellipsoidal particles (7) are exposed on the outer surface of the resin adhesive layer.
4. The low halo electrically controlled dimming film according to claim 3, characterized in that The diameter of the spherical particles (6) or ellipsoidal particles (7) includes at least a first diameter and a second diameter, the spherical particles (6) or ellipsoidal particles (7) of the first diameter occupy 1 to 10% of the volume of the first micro-diffusion layer (2) or the second micro-diffusion layer (4), and the spherical particles (6) or ellipsoidal particles (7) of the second diameter occupy 1 to 10% of the volume of the first micro-diffusion layer (2) or the second micro-diffusion layer (4).
5. The low halo electrically controlled dimming film according to claim 4, characterized in that The thickness of the first micro-diffusion layer (2) and the second micro-diffusion layer (4) are respectively 2 to 4 micrometers, the first diameter of the spherical particles (6) or ellipsoidal particles (7) is 0.5 to 2 micrometers, and the second diameter of the spherical particles (6) or ellipsoidal particles (7) is 3 to 5 micrometers.
6. A method for preparing a low-halo electrically controlled dimming film according to any one of claims 3 to 5, characterized in that The following steps are involved: Step 1: Select two base films and sputter ITO thin films on the base films respectively to obtain a first conductive film layer (1) and a second conductive film layer (5); Step 2: coating a first micro-diffusion layer (2) on the ITO surface of the first conductive film layer (1), and coating a second micro-diffusion layer (4) on the ITO surface of the second conductive film layer (5), wherein both the first micro-diffusion layer (2) and the second micro-diffusion layer (4) contain spherical particles (6) or ellipsoidal particles (7) exposed on the surface of the layer structure; Step three: dripping the PDLC material between the first micro-diffusion layer (2) and the second micro-diffusion layer (4) to form a PDLC layer (3), rolling the whole, and curing with ultraviolet light to obtain a liquid crystal film.
7. The method for preparing the low-halo electrically controlled dimming film according to claim 6, characterized in that In the step 2, the spherical particles (6) are SiO2 particles, TiO2 particles or Si3N4 particles.
8. The method for preparing the low-halo electrically controlled dimming film according to claim 6, characterized in that In the step 1, the thickness of the base film is 178-198 micrometers, the sheet resistance of the first conductive film layer (1) and the second conductive film layer (5) is 50-150Ω, the visible light transmittance is 20-90%, and the haze is 0.2-2.
9. The method for preparing the low-halo electrically controlled dimming film according to claim 6, characterized in that In the step 3, the size of the liquid crystal droplets of the PDLC layer (3) is 1-2 micrometers.
10. An automobile window using a low halo electrically controlled dimming film, characterized in that The low-halo electrically-controlled dimming film is the low-halo electrically-controlled dimming film according to any one of claims 1 to 5, or the low-halo electrically-controlled dimming film prepared by the preparation method according to any one of claims 6 to 9.