Method for producing an optically variable security element
By using hydrophilic and hydrophobic imprinting paint layers and flexible or hard printing tools in anti-counterfeiting elements, combined with UV and thermoplastic hardening technology, the problem of registration fluctuation in the existing technology is solved, and the registration accuracy and optical effect of anti-counterfeiting elements are improved. .
Patent Information
- Application Number
- CN202210236386.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-25
- Filing Date
- 2022-03-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-03-11
AI Technical Summary
Existing optically variable anti-counterfeiting elements suffer from registration fluctuations in the printing ink or embossed paint layer during the manufacturing process, resulting in insufficient registration accuracy, especially in the range of less than 50 μm. It is difficult to achieve accurate registration.
By applying hydrophilic and hydrophobic embossing paint layers with different characteristic areas on the carrier, and using flexible or hard printing tools, top pressure rollers and compensation layers, combined with UV and thermoplastic hardening technology, high precision of both embossing paint layers is achieved Registration and optical effects.
It improves the registration accuracy of different embossed paint layers in anti-counterfeiting elements, ensures the stability of optical variable effects and the clarity of visual impressions, solves the problem of registration fluctuations, and achieves high-resolution embossed structures.
Smart Images

Figure CN115122801B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing an optically variable security element for providing security for valuables, the security element comprising a carrier and a feature layer having a first and a second feature area, in which different first or second embossing lacquer layers are present. Background Art
[0002] Data carriers such as value documents or ID documents and other valuable items such as brand-name goods are often provided with security elements for security purposes, which can verify the authenticity of the data carrier and at the same time serve as protection against unauthorized copying. The security element can be designed, for example, in the form of a security thread embedded in a banknote, a cover film for a banknote with a hole, an applied security strip, a self-supporting transfer element or also in the form of a characteristic area applied directly on the value document.
[0003] Some time ago, optically variable security elements were proposed, which have two relief structures arranged at different height levels and each provided with a color coating, which are embossed in a matching embossing lacquer layer, see WO 2020 / 011390 A1, WO 2020 / 011391 A1 and WO 2020 / 011392 A1. However, in order to observe the lower relief structure, the observer usually has to look through the embossing lacquer layer of the higher relief structure, so that depending on the desired visual impression, there can be considerable restrictions on the coloring of the embossing lacquer, in particular of the higher embossing lacquer layer.
[0004] If multiple printing inks or embossing lacquer layers are applied to a substrate during the production of such security elements, the inevitable register fluctuations in the printing press prevent the layers from being accurately registered in a plane to less than about 50 μm. These register fluctuations may occur both longitudinally and transversely to the printed surface. Summary of the invention
[0005] Starting from this, the object of the present invention is to provide a method by which an optically variable security element of the type according to the invention can be produced which has a high register accuracy of the first and second different embossing lacquer layers.
[0006] This object is achieved according to the invention by a method for producing a security element for securing valuable objects.
[0007] In order to solve the technical problem, the present invention provides a method for manufacturing a security element, which can be used in particular to provide security for valuables. The security element to be manufactured comprises a feature layer having a first and a second feature area, in which different first or second embossing lacquer layers are present.
[0008] In a first aspect of the invention, in the method a first hydrophilic layer of embossing lacquer is applied to the carrier in the first feature region, the applied layer is embossed with an embossed structure producing the first optical effect and hardened.
[0009] Furthermore, different layers of a second embossing lacquer are provided on a printing tool and, in a printing step, the printing tool is brought into contact with the carrier and the second embossing lacquer is thereby transferred.
[0010] The carrier can remain permanently in the security element or it can be a production carrier which is removed from the security element after the security element has been transferred to the target substrate.
[0011] In the printing step, the second embossing lacquer is advantageously transferred only into the second feature regions which are not coated with the hydrophilic embossing lacquer.
[0012] The different, second embossing lacquer layer is advantageously provided on the printing tool over the entire surface or over the entire area.
[0013] Preferably, the carrier is moistened with the first embossing lacquer layer before the printing step and in the process the moistening agent is transferred exclusively to the hydrophilic first embossing lacquer layer of the first feature regions.
[0014] The second characteristic region is preferably a region having a hydrophobic surface.
[0015] In an advantageous method development, in the printing step, a layer of a second embossing lacquer is provided on a flexible printing tool, in particular a printing cylinder having compressible elements, which is deformed locally by the pressure tip produced by the already hardened first lacquer layer.
[0016] In a further, equally advantageous method development, in the printing step a second layer of embossing lacquer is provided on a printing tool, in particular a hard printing cylinder, and a soft press roller is used to generate the counterpressure, which is locally deformed by the pressure tip generated by the already hardened first lacquer layer.
[0017] In a further, likewise advantageous method direction, a flexible compensation layer is arranged on the carrier, which compensation layer is deformed locally during the printing step by the pressure tips generated by the already hardened first lacquer layer.
[0018] In an advantageous embodiment, the first embossing lacquer is applied in a structured manner, for example, printed in a structured manner in the first feature region. However, it is also possible that the first embossing lacquer is first applied over the entire surface and then removed again regionally, for example, by a corrosion (or etching) step, in order to thereby achieve the desired structuring. A particularly high resolution can be achieved in the following case, that is, the first embossing lacquer is first applied over the entire surface on the carrier (or applied to the entire surface of the carrier) according to an advantageous embodiment and then structured into a wetted first feature region and a dewetted second feature region by a residue-free embossing method by approaching a structured embossing mold, wherein at the same time, an embossed structure that produces a first optical effect is embossed into the wetted first feature region by the structured embossing mold.
[0019] The first embossing lacquer can be cured advantageously by the action of radiation, in particular by UV (ultraviolet) radiation, but also by IR (infrared) radiation or exposure to electron beams. The use of UV-curing embossing lacquer is advantageous in particular when the embossing lacquer is structured with high resolution by the described residue-free embossing method.
[0020] According to a second aspect of the invention, in the method a first embossing lacquer layer with a lower surface energy is applied to the carrier in the first feature region, the applied layer is embossed with an embossed structure producing a first optical effect and is cured.
[0021] Subsequently, a second, different embossing lacquer layer with a lower viscosity and a higher surface tension is applied over the entire surface, and the second embossing lacquer is dewetted from the first feature regions coated with the first embossing lacquer into the second feature regions.
[0022] If necessary, the application and dewetting process is repeated in order to collect a sufficient amount of second embossing lacquer for embossing in the second feature region.
[0023] In the second aspect of the invention, the carrier can also remain permanently in the security element or it can be a production carrier which is removed from the security element after the security element has been transferred to the target substrate.
[0024] In both aspects of the invention, a second embossed structure is advantageously embossed into the embossing lacquer layer of the second embossing lacquer, said second embossed structure producing the second optical effect. Advantageously, the second embossed structure is transferred exclusively into the second embossing lacquer layer by using, preferably in the layer structure of the security element, a flexible embossing tool, a soft embossing top roller or a flexible compensating layer in order to transfer the second embossed structure exclusively into the second embossing lacquer layer.
[0025] The embossed structures of the first and second embossing lacquer layers are advantageously situated at essentially the same height, which means in particular that the middle heights of the two embossed structures do not differ by more than the height difference within each embossed structure.
[0026] It is preferred in both aspects if the two embossing lacquers have different curing properties, and the embossing lacquers particularly preferably also have different optical properties.
[0027] As embossing lacquer, a lacquer which hardens by physical drying, in particular a thermoplastic embossing lacquer, can be applied in each case. If the first and second embossing lacquer are each formed by a thermoplastic embossing lacquer, the first and second embossing lacquer advantageously have different softening temperatures which preferably differ by more than 10° C., particularly preferably by more than 25° C., in particular by more than 50° C.
[0028] In a configuration which is also advantageous in both respects, it is provided that as one embossing lacquer a radiation-hardening, in particular UV-hardening, embossing lacquer is applied and as the other embossing lacquer a thermoplastic embossing lacquer is applied.
[0029] The embossing lacquer can be applied in particular in different colors, different transparencies and / or different brightness. The embossing lacquer is preferably gloss-dyed and is therefore both colored and partially translucent.
[0030] The embossing lacquer layers of the first and second feature regions are advantageously arranged next to each other without gaps and without overlap.
[0031] In an advantageous further development of the invention, the first and second embossing lacquer layers are provided with a common reflection-enhancing coating, in particular a highly refractive or metallic coating, which is preferably applied after the first and second embossing lacquers have been embossed with corresponding embossed structures that produce different first and second optical effects.
[0032] The embossed structures of the first and second embossing lacquer layers advantageously each comprise structural elements whose structural dimensions in the plane are between 30 μm and 200 μm, in particular between 50 μm and 150 μm. One or both embossed structures advantageously comprise a micromirror arrangement as a structural element, which has directionally reflecting micromirrors, in particular non-diffractive mirrors, and preferably plane mirrors, concave mirrors and / or Fresnel mirrors.
[0033] It goes without saying that the optically variable security element may contain other layers, such as protective layers, covering layers or additional functional layers, machine-readable elements, primer layers or heat-sealing lacquer layers, which are however not essential elements of the invention and are therefore not described further. The security element to be produced is advantageously a security thread, in particular a window security thread or a pendulum security thread, a tear-off security thread, a security tape, a security strip, a patch or a label for application to security papers, value documents, etc.
[0034] The UV embossing lacquers and thermoplastic lacquers (also called thermoplastics) used generally have the properties described below, although lacquers with different properties can also be used for special applications.
[0035] Conventional UV embossing paint is first significantly easier to emboss than thermoplastic embossing paint. For example, for UV embossing, liquid embossing paint can be applied to the film first. The embossing paint reaches the embossing mold without contacting the roller. The film with embossing paint is contacted with the embossing mold by means of a top pressure roller, wherein the paint surface adopts or forms the structure of the embossing mold. In theory, no pressure is required in any slow process, and the paint will simply flow into the structure and squeeze out the air. However, in practice, the embossing process on the machine is not arbitrarily slow, so when embossing with too small a top pressure roller pressure, the paint can no longer completely squeeze out the air within a preset time. Therefore, when there are certain requirements for speed and bubble-free performance, it is actually worked with a certain embossing pressure. If UV curing is not performed, after the film is removed from the embossing mold, the paint will flow again immediately after contacting the embossing mold. However, in practice, the film wraps around the embossing mold to a certain extent. If the film with paint contacts the embossing mold through a top pressure roller, the film usually no longer spontaneously detaches from the embossing mold. After the embossing roller, in a virtually pressure-free area, a UV emitter is arranged, which crosslinks the UV lacquer while it is still in contact with the embossing mold. Only after this reaction is the film removed from the embossing mold. The entire process usually runs continuously. The lacquer that hardens in this way is usually a thermosetting plastic.
[0036] Thermoplastic embossing is generally different from the UV embossing described. Thermoplastics are solid at room temperature and therefore non-flowable, and when the temperature rises, they become able to be embossed at a certain temperature. If the temperature rises further, the paint becomes viscous, which limits the meaningful embossing using standard embossing molds. However, molds with non-stick coatings can be used if necessary. In the case of thermoplastic embossing, the embossing punch can be heated, embossing is carried out at an elevated temperature, and if necessary, the embossing punch is slightly cooled again before demoulding. In the roll-to-roll process, there is usually no cooling before demoulding. There, in the case of thermoplastic embossing, the film can be heated, for example, in contact with the embossing mold, embossed at the highest temperature and demoulded immediately without entering the sticky area of the thermoplastic. Advantageously, this higher heating that makes the thermoplastic actually liquid is avoided.
[0037] In order to avoid the adhesion of thermoplastics with lower melting points, the embossing mold is advantageously provided with a non-stick coating. Alternatively, a metallization of the embossing lacquer that is not embossed can be provided to avoid adhesion, or it can be ensured that the thermoplastic with higher melting point becomes higher melting point only at a later time. This can be ensured, for example, by means of a crosslinking agent (e.g. isocyanate) mentioned elsewhere or also by radiation crosslinking. For example, two thermoplastic embossable UV raw materials can be placed side by side, wherein one of the two formulations contains a photoinitiator. After the first embossing, exposure can be carried out, in which case demoulding can be carried out afterwards, because even without contact with the embossing mold, the solid lacquer will also obtain an embossed structure. The formulation containing the photoinitiator thus increases the melting point and can no longer be deformed under the previous embossing conditions. Then a second embossing can be carried out. The second "thermoplastic" either remains uncrosslinked or is post-crosslinked by electron beam hardening, because the latter process can be carried out without a photoinitiator. Alternatively, the second thermoplastic may also contain a photoinitiator which is not active at the wavelength of the first emitter.
[0038] In addition to the above-mentioned and advantageous configurations of the embossing lacquers, it is also possible in principle to use embossing lacquers which harden or crosslink thermally rather than photochemically. For example, some embossing lacquers have a softening temperature T1 and a hardening temperature T2>T1. Such embossing lacquers can be formed, for example, based on acrylates with isocyanates.
[0039] A further working step consists in selectively heating one of the embossing lacquers. In this case, a region with a substance that can be selectively excited (in the UV / visible / infrared or electrically / capacitively / magnetically with an alternating field) selectively causes only the region containing this substance to heat up. In this way, for example, two regions with UV embossing lacquers can also be provided and treated, in particular embossed, one after the other.
[0040] In the context of the present description, a layout of characteristic regions with exact registration (passergenau, or exact fit) means in particular a layout in which the characteristic regions adjoin one another or are arranged at predetermined, defined small distances from one another. Small distances are in particular distances of a few micrometers or tens of micrometers up to 100 micrometers, and in some applications up to 200 micrometers. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Other embodiments and advantages of the present invention are described below with reference to the accompanying drawings, which are not shown to scale or proportion in order to improve clarity.
[0042] In the attached picture:
[0043] Figure 1 A schematic diagram showing a banknote with an optically variable security element;
[0044] Figure 2 In the schematic diagram, a security element having a carrier substrate with an embossed feature layer is shown;
[0045] Figure 3 (a) to (d) show four intermediate steps in the production of a security element having a feature layer with two thermoplastic embossing lacquers having different softening temperatures;
[0046] Figure 4 (a) to (d) show four intermediate steps in the production of a security element having a feature layer made of thermoplastic embossing lacquer and UV embossing lacquer;
[0047] Figure 5 In (a) to (c) intermediate steps are shown when producing a security element by using a flexible embossing mould;
[0048] Figure 6 (a) to (c) show intermediate steps in the production of security elements by using a hard embossing mold in combination with a soft embossing top roller;
[0049] Figure 7 (a) to (c) show intermediate steps in the production of a security element in whose layer structure a flexible compensation layer is provided;
[0050] Figure 8(a) to (d) show intermediate steps in the application of two different embossing lacquers next to each other in the feature layer without register fluctuations;
[0051] Fig. 9 In (a) to (c) intermediate steps are shown in further variants for applying two different embossing lacquers next to each other in a feature layer without register fluctuations;
[0052] Fig.10 In (a) to (c) intermediate steps are shown in a further variant for applying two different embossing lacquers next to each other in a feature layer without register fluctuations;
[0053] Fig.11 (a) and (b) show intermediate steps in the application of a UV embossing lacquer layer and in the high-resolution structuring;
[0054] Fig.12 In (a) and (b) intermediate steps are shown in a further possibility for applying two different embossing lacquers next to each other in a feature layer without register fluctuations;
[0055] Fig.13 (a) to (c) show intermediate steps in a method for applying two different embossing lacquers in register by means of mechanical layer removal; and
[0056] Fig.14 (a) to (d) show intermediate steps in a method for applying two different embossing lacquers in register by means of a selective lift-off medium. DETAILED DESCRIPTION
[0057] The present invention will now be explained using a security element for banknotes as an example. Figure 1 For this purpose, a schematic diagram of a banknote 10 is shown, which has an optically variable security element 12 in the form of a glued-on transfer element. However, it goes without saying that the invention is not limited to transfer elements and banknotes, but can be used in all types of security elements, for example in labels on goods and packaging or in the security of documents, identity cards, passports, credit cards, health cards, etc. For banknotes and similar documents, in addition to transfer elements (such as stickers with or without their own carrier layer), for example, security threads or security strips are also conceivable.
[0058] Despite the flat design of the security element 12, the security element 12 gives the observer a three-dimensional impression and, for example, simultaneously displays a binary color and effect change when the banknote 10 is tilted, wherein a first three-dimensional pattern (Motiv, or thematic object) appears in a first color when viewed from a first viewing direction and a second three-dimensional pattern appears in a second color when viewed from a second viewing direction.
[0059] These visual effects and a large number of other visual effects can be advantageously produced by a security element in which two or more embossed lacquer layers are arranged side by side in register in the plane of the security element, the embossed lacquer layers being purposefully provided with different, mutually independent embossed structures. In addition to the different embossed structures, the embossed lacquer layers also advantageously have other different properties, i.e. in particular different visual properties, such as different colors, transparencies and / or brightness. In this way, the optically variable effect produced by embossing on the one hand and the visual effect produced by the additional properties of the embossed lacquer layers on the other hand can be coordinated with each other in perfect register.
[0060] To illustrate, Figure 2 The schematic diagram shows a security element 20 having a carrier film 22 in the form of a transparent PET film, which is provided with an embossed feature layer 24. The feature layer 24 consists of an alternating sequence of feature areas 30, 40 of the desired shape and size (only one of the feature areas is respectively provided with a reference number), which differ from one another by the different varnish colors of the applied embossing lacquer layers 32, 42 and the different designs of the corresponding embossed structures 34, 44.
[0061] The embossed structures 34, 44 of the two feature areas 30, 40 are substantially at the same height level in a common plane and are provided with a common reflection-enhancing metal coating 26, such as a vapor-deposited aluminum layer. In the present embodiment, the metallized embossed structure is smoothed by a lacquer layer 28, and the security element can be bonded to a desired target substrate, such as a banknote 10, by an adhesive layer 29. After bonding, the carrier substrate 22 can be removed or remain in the security element as a protective film.
[0062] The security element 20 is designed for viewing through the varnished embossed lacquer layers 32, 42. In this case, the observer 14 views the metallized embossed structure 34 through the embossed lacquer layer region 32 in the feature region 30, and he views the metallized embossed structure 44 through the embossed lacquer layer region 42 in the feature region 40. The embossed lacquer 32 can be varnished red, for example, and the embossed structure 34 can produce a curved view of the number "10" as a pattern, while the embossed lacquer 42 can be varnished green and the embossed structure 44 can produce a curved view of an emblem as a pattern. The two patterns can also be recognizable from different viewing directions. From Figure 2 It can be seen that feature areas 30 , 40 with different color effects produced by embossing lacquer layers 32 , 42 and different patterns produced by embossing structures 34 , 44 are arranged directly adjacent to each other in register without gaps or overlaps.
[0063] Reference now Figure 3 and Figure 4 The basic principle of an advantageous production of the characteristic layer 24 of the security element 20 is explained in more detail, Figure 3 and Figure 4 Four intermediate steps in the production of the security element 20 are respectively shown in (a) to (d).
[0064] refer to Figure 3 (a), firstly, a carrier film 22, such as a transparent, colorless PET film, is provided, and thermoplastic embossing lacquers 32, 42 of the desired color effects are applied to the desired feature areas 30, 40, respectively. Here, the thermoplastic embossing lacquers 32, 42 are coordinated with each other so that in addition to different colors, they also have different softening temperatures and can therefore be embossed at different temperatures. For example, the thermoplastic embossing lacquers 42 can already be embossed at a lower temperature T2, while the thermoplastic embossing lacquers 32 can only be embossed at a higher temperature T1>T2.
[0065] Then, in a first embossing step, which is performed at a higher temperature T1, the two embossing lacquers 32, 42 are provided with a first embossing structure 34 by means of a first embossing mold 50, such as in Figure 3 As shown in (b).
[0066] The carrier film with the embossed feature layer is then cooled to a lower temperature T2 and demolded, and the embossing lacquer 32 in the feature area 30 with the embossed structure 34 is thereby cured, while the embossing lacquer 42 remains still deformable. Therefore, the embossing lacquer 42 still flows partially or completely after demolding and at best does not completely form the first embossed structure, as in Figure 3 As shown by reference numeral 34' in (c).
[0067] exist Figure 3 (c) also shows a second embossing mold 52 for the second embossing step, with which a second embossing structure 44 is embossed at a lower temperature T2 into the still deformable embossing lacquer layer 42 of the feature region 40. The embossed structure 34 of the feature region 30 has already solidified and is no longer significantly affected by the second embossing step, in particular due to the measures described in more detail below.
[0068] After the second embossing step, the carrier film with the twice embossed feature layer is cooled to a temperature T<T2, for example to room temperature, and the embossing lacquer 42 in the feature region 40 is thereby also cured.
[0069] In this way, as in Figure 3 As shown in (d), a feature layer 24 having the desired double embossed structures 34, 44 in register with the feature areas 30, 40 is obtained. The feature layer 24 can then be metallized, as shown in FIG. Figure 2As shown, or it can be different in different ways Figure 3 The intermediate product of (d) is further processed into the desired security element.
[0070] exist Figure 4 In the design scheme, the thermoplastic embossing lacquer 32 and the UV embossing lacquer 42 are used instead of two thermoplastic embossing lacquers with different softening temperatures. Figure 4 In the embodiment of the present invention, the thermoplastic embossing lacquer is first embossed and then the UV embossing lacquer. Even though UV embossing lacquer is generally easier to emboss than thermoplastic embossing lacquer, when using suitable embossing lacquer and / or under suitable conditions, it is also possible to use the following method: Figure 4 Imprinting sequence shown.
[0071] refer to Figure 4 (a) A carrier film 22, for example a transparent, colorless PET film, is provided and coated or coated with a thermoplastic embossing lacquer 32 in the feature area 30 and with a UV embossing lacquer 42 in the feature area 40, the thermoplastic embossing lacquer and the UV embossing lacquer each having the desired different color effects.
[0072] Then, in a first embossing step, the first embossing structure 34 is embossed by the first embossing mold 50 under embossing conditions in which the thermoplastic embossing varnish 32 can be embossed, such as Figure 4 (b) The imprinting conditions may include, for example, a temperature T1 of 120° C. and a relatively high imprinting pressure.
[0073] The carrier film with the embossed feature layer is then cooled to a lower temperature T2<T1 and demolded, and the embossing varnish 32 in the feature region 30 is thereby cured. For example, the lower temperature T2 may be T2=30° C. The UV embossing varnish 42 is not embossed under the embossing conditions of the first embossing step, so that after the first embossing step, the embossing varnish 32 provided with the embossed structure 34 is present in the feature region 30, and the UV embossing varnish 42 that is not embossed is present in the feature region 40, as shown in FIG. Figure 4 (c) as shown.
[0074] exist Figure 4 (c) also shows a second embossing tool 52, by means of which the second embossing structure 44 is pressed into the UV-curable embossing lacquer layer 42 of the feature region 40 at a lower temperature T2 and UV radiation 54. By hardening the embossing lacquer layer 42 by means of radiation from UV-LEDs, the heat input into the thermoplastic layer 32 can be minimized. Due to the lower temperature in the second embossing step and due to the measures described in more detail below, the already cured embossed structure 34 of the feature region 30 is not significantly affected by the second embossing step.
[0075] After the second embossing step and UV curing, the embossing lacquer 42 is also cured in the feature area 40, so that Figure 3 As shown in , a feature layer 24 is obtained, which has the desired dual embossed structures 34, 44 in register with the feature areas 30, 40, as shown in 4(d).
[0076] In combination Figure 3 and 4 In the described embodiment, the two embossing lacquer layers 32, 42 are already present on the carrier film in the first embossing step. However, it is also possible to apply the layer to be embossed subsequently only after the layer to be embossed first has been embossed. In this case, it is also important that the embossed structure of the first embossed layer remains unchanged under the embossing conditions of the subsequently embossed layer. This usually requires special measures, which are now referred to in detail in the following examples. Figures 5 to 7 Elaborate in more detail.
[0077] One possibility for ensuring that the embossed structure of the first embossed layer is not destroyed or damaged by the subsequent embossing step is to use a flexible embossing mold for the second embossing.
[0078] This is based on Figure 5 The design scheme is illustrated, wherein the feature layer 24 is similar to Figure 4 By way of example, on the one hand, it comprises feature regions 30 with thermoplastic embossing lacquer 32 and on the other hand, it comprises feature regions 40 with UV embossing lacquer 42. The structures 34 and 44 to be embossed respectively have structure dimensions L1 and L2 of 50 μm to 150 μm in the plane. The structure height is usually in the order of magnitude of a few micrometers.
[0079] exist Figure 5 In a variant of the invention, the UV embossing lacquer 42 is first provided with the desired second embossing structure 44 and then hardened, as in Figure 5 (a). The thermoplastic embossing lacquer 32 can also be embossed, or as in Figure 5 As shown in (a), the thermoplastic embossing lacquer can remain free of embossed structures by flowing.
[0080] The first embossing structure 34 is now pressed in with the aid of a flexible embossing mold 60, which has the desired embossing structure 34 on its surface. The flexible embossing mold 60 is formed, for example, from silicone rubber and deforms due to a pressure tip on a length scale λ of a few micrometers. During embossing, the feature area 40 with the already hardened UV embossing lacquer 42 acts to produce a corresponding deformation 62 of the flexible embossing mold 60, so that on the one hand the already hardened embossing lacquer area 42 is not damaged, but on the other hand the embossing lacquer 32 can be embossed with the embossing structure 34 in the feature area 30, as in Figure 5As shown in (b).
[0081] Since the transition region 64 in which the shape of the imprinting mold 60 changes significantly has a size of the order of magnitude λ<<L1, L2, that is, the transition region 64 is significantly smaller than the structural size of the imprinting structures 34, 44, the possibly smaller, defective or even non-existent imprinting structure in the transition region 64 has no significant effect on the overall quality of the imprinting structure 34 in the feature region 30.
[0082] Thus, after the thermoplastic embossing lacquer 32 has cooled and the flexible embossing mold 60 has been demoulded, the feature layer 24 is provided with the desired registered double embossing structures 34, 44 in the feature regions 30, 40, as in Figure 5 As shown in (c).
[0083] refer to Figure 6 Another possibility is to use a hard embossing mold 70 in combination with a soft embossing top roller 72 and a suitable carrier film 74 in the security element.
[0084] In this design, Figure 6 The original situation shown in (a) corresponds largely to Figure 5 The original situation of (a), i.e., a feature layer 24 is present on a suitable carrier film 74, which will be described in more detail below, wherein a thermoplastic embossing lacquer 32 is applied in the feature area 30 and a UV embossing lacquer 42 is applied in the feature area 40. In this case, the UV embossing lacquer 42 has already been provided with the desired embossed structure 44 in a first embossing step. Here, the structures 34, 44 to be embossed also have structure sizes L1 and L2 in the plane between 50 μm and 150 μm.
[0085] In order to emboss the embossed structure 34 in the second embossing step, Figure 6 In the method, a hard stamping mold 70 is used, which can be made of nickel, for example. The hard stamping mold 70 is particularly suitable for stamping thermoplastic lacquer 32, but is not suitable for stamping thermoplastic lacquer 32. Figure 5 Compared with the flexible stamping mold 60 of the design scheme, the hard stamping mold has a poor ability to compensate for the height difference.
[0086] In order to still ensure that the already embossed and hardened lacquer area 42 is not deformed or damaged in the second embossing step, use is made of the fact that embossing always requires a counterpressure, which is usually applied by the embossing top roller 72. As a special feature, Figure 6 In the method, a relatively soft embossing top pressing roller 72 is used, which is made of an elastomer with a hardness of less than 90 Shore hardness, especially less than 85 Shore hardness.
[0087] As in Figure 6As schematically shown in (b), in the second embossing step, the already hardened UV embossing lacquer area 42 is pressed together with the carrier film 74 into the soft embossing top roller 72 by the hard embossing mold 70 far enough to enable the thermoplastic embossing lacquer 32 to be embossed without damaging or destroying the UV embossing lacquer area 42.
[0088] After the thermoplastic embossing lacquer 32 has cooled and been demolded, the feature layer 24 is thus provided with the desired registered double embossing structures 34, 44 in the feature regions 30, 40, as in Figure 6 As shown in (c).
[0089] As an alternative or in addition to the use of a soft embossing embossing roller 72, the embossing roller can also be provided with a structured surface which locally limits the deformation of the embossing roller. For example, the surface can be divided into sections with λ c Individual honeycombs have a characteristic size of ≈25 μm, so that, for example, with structural sizes L1 , L2 =100 μm of the embossed structures 34 , 44 , it can be expected that a plurality, in particular 9 honeycomb segments can each exert their ideal embossing pressure, while adjacent segments are greatly deformed.
[0090] Returning to the advantageous properties of the carrier film 74, said carrier film must be sufficiently easily deformed under the embossing conditions of the second embossing step to allow the embossing roller 72 to be deformed in the second embossing step. Figure 6 Height compensation shown in (b).
[0091] For this purpose, for example, a very thin carrier film 74 can be used, the thickness of which is preferably less than 23 μm, in particular less than 19 μm and particularly preferably between 6 μm and 15 μm. Alternatively or in addition, the carrier film 74 can also be adapted to the embossing conditions by virtue of the glass transition temperature T g The embossing conditions of the second embossing step are exceeded and the film is therefore particularly susceptible to deformation.
[0092] Another possibility for ensuring that the firstly embossed layer is not destroyed or damaged under the embossing conditions of the subsequently embossed layer is to provide a compensation layer 80 in the layer structure of the security element itself.
[0093] To illustrate, Figure 7 The layer structure of the security element to be produced is shown, wherein a compensation layer 80 is arranged between the carrier film 22 and the feature layer 24, said compensation layer being flexible at least under the embossing conditions of the second embossing and preferably having elastic properties. If it is provided that the optical effect of the security element is observed from the side of the embossing lacquer layer 32, 42 and therefore also through the compensation layer, the compensation layer is preferably transparent and designed with a low scattering effect. In particular, the compensation layer 80 can be formed, for example, from silicone rubber.
[0094] exist Figure 7 The original situation shown in (a) corresponds largely to Figure 6 The starting situation of (a), in particular the feature layer 24 contains in the feature region 30 a thermoplastic embossing lacquer 32 and in the feature region 40 a UV embossing lacquer 42 which has already been provided with the desired embossing structure 44 in a first embossing step.
[0095] The embossed structure 34 can then be embossed in a second embossing step using a hard embossing mold 70 which is particularly suitable for embossing the thermoplastic lacquer 32. Figure 7 (b), the second embossing step of the thermoplastic lacquer 32 is carried out at an elevated temperature, at which the compensation layer 80 is elastic, so that the already hardened UV embossing lacquer area 42 is locally pressed into the compensation layer 80 by the hard embossing mold 70. This prevents the embossed structure 44 from being deformed or damaged and at the same time enables the embossing of the embossing lacquer layer 32.
[0096] In order to sufficiently press in the UV embossing lacquer area 42, the layer thickness of the compensation layer 80 should be slightly greater than the height difference to be compensated, which is usually between 2 and 15 μm in the case of a typical embossed microstructure 44. The compensation layer 80 can also advantageously be deformed in such a way that when the UV embossing lacquer area 42 is pressed in, the thermoplastic embossing lacquer area 32 is simultaneously pressed slightly upwards and thus facilitates the second embossing. This deformation can be carried out in particular while maintaining the volume.
[0097] After the second embossing step has been completed and the thermoplastic embossing lacquer 32 has cooled and been demolded, the elastic compensation layer 80 has been deformed back to its original state, so that the produced feature layer 24 is provided with the desired registered double embossing structures 34, 44 in the feature regions 30, 40, as shown in FIG. Figure 7 As shown in (c).
[0098] In the embodiments described so far, it is assumed that there are already registered embossing lacquer areas on the carrier film in the feature areas 30, 40. Some advantageous possibilities for applying two or more different embossing lacquers side by side without register fluctuations in the feature layer and therefore ideally without unintentional gaps or overlaps are now described below.
[0099] First of all, a variant using the phenomenon of surface energy or surface tension is described here. Depending on the material of the carrier film used, it may be necessary to first provide the carrier film with a coating having a suitable surface energy. Further layers may be required for this purpose, such as a primer layer or a release layer for subsequent detachment. Corona treatment, plasma treatment or flame treatment of the film can also contribute to sufficient adhesion. In the following description, it is assumed that the carrier 90 mentioned is or includes a suitable carrier film and may have been pretreated accordingly or provided with further layers in order to provide a surface energy suitable for the respective method.
[0100] exist Figure 8 In the method variant shown, the carrier 90 is first printed in the feature region 40 by any method with a embossable, hydrophilic formulation 42 after drying, which has the desired color or transparency in the feature region 40. In the embodiment described, the formulation is a UV embossing lacquer 42, which after printing is embossed with an associated embossing structure 44 in the feature region 40 and is finally cured by UV crosslinking, as in Figure 8 Here, the characteristic region 30 is initially uncoated and represents an area having a hydrophobic surface.
[0101] Then the carrier film provided with UV embossing lacquer is wetted inline or in a separate process with a wetting agent 92. Here, only the characteristic areas 40 of the hydrophilic coating receive the wetting agent 92, while the hydrophobic characteristic areas 30 remain free of the wetting agent, as in Figure 8 As shown in (b).
[0102] A second embossing lacquer layer of the thermoplastic embossing lacquer 32 is then applied to the carrier film, for which purpose in the present exemplary embodiment a printing cylinder 94 is used, on which the embossing lacquer layer 32 is provided over the entire surface, as in Figure 8 In order to achieve that the embossing lacquer 32 is applied only in the gaps 30 between the already coated areas 40 , the surface of the printing cylinder 94 is provided with compressible elements 96 .
[0103] The compressible element 96 is deformed during the printing process of the embossing lacquer layer 32 by the pressure tip generated by the already hardened UV lacquer layer 42, as in Figure 8 As shown in (c), the embossing lacquer 32 is therefore in contact with the carrier 90 in the feature areas 30 without protrusions and is transferred there without damaging the already existing embossed structure 44. Although the UV embossing lacquer 42 of the feature areas 40 is also in contact with the embossing lacquer layer 32 during printing, due to the previously applied wetting agent 92, the UV embossing lacquer is ink-repellent (farbabweisend) and therefore does not accept the embossing lacquer 32.
[0104] In this way, the thermoplastic embossing lacquer 32 is deposited only in the characteristic areas 30 during the printing step, such as in Figure 8 (d). The already embossed and hardened UV embossing lacquer 42 is present in the feature area 40. Then, for example, Figures 5 to 7 The intermediate product thus obtained is further processed as described, and in this case the desired embossing structure can also be provided for the embossing lacquer layer 32. Instead of thermoplastic embossing lacquer, other UV embossing lacquers can also be used, which can also have the same curing properties as the first embossing lacquer, since the first embossing lacquer is already cured during the printing of the other embossing lacquer.
[0105] exist Fig. 9 In a method variant of , a soft pressure roller 98 with a Shore hardness of less than 90, in particular less than 85, is used instead of the compressible element in the printing cylinder.
[0106] exist Fig. 9 The original situation shown in (a) essentially corresponds to Figure 8 The original situation and a carrier 90 which has been coated in the feature areas 40 with a UV embossing lacquer 42 which becomes hydrophilic after hardening are shown. The UV embossing lacquer 42 is embossed with the desired embossing structure 44 and hardened by UV crosslinking. The carrier film coated in this way is then wetted with a wetting agent 92 inline or in a separate process, wherein only the hydrophilically coated feature areas 40 receive the wetting agent 92, while the uncoated feature areas 30 remain free of the wetting agent.
[0107] Then, a second embossing lacquer layer of thermoplastic embossing lacquer 32 is provided over the entire surface of the printing cylinder 94. The soft embossing roller 98 provides the counterpressure for the printing step, but due to its relatively low hardness of less than 90 or less than 85 Shore A, it can be deformed locally by the pressure tip. Fig. 9 As schematically shown in (b), when printing the embossing lacquer layer 32, the already hardened UV embossing lacquer area 42 is lightly pressed into the soft top pressure roller 98 together with the carrier film 90 by the printing roller 94, so that the thermoplastic embossing lacquer 32 in the feature area 30 contacts the carrier film 90 and is transferred there without damaging the existing embossing structure 44.
[0108] Although the UV embossing lacquer areas 42 are also in contact with the embossing lacquer layer 32, they are ink-repellent due to the applied wetting agent 92 and therefore do not accept the embossing lacquer 32. Thus, a design with unembossed thermoplastic embossing lacquer 32 in the feature areas 30 and embossed, hardened UV embossing lacquer 42 in the feature areas 40 is produced by the printing step, which can be further processed as described above. Instead of thermoplastic embossing lacquer, other UV embossing lacquers can also be used here, which, since the first embossing lacquer has already cured when printing the other embossing lacquer, can also have the same curing properties as the first embossing lacquer.
[0109] In this variant, the carrier film 90 must be sufficiently deformable under the printing conditions of the second embossing lacquer 32 to allow the embossing roller 98 to achieve the desired effect. Fig. 9 (b) shows a height compensation. For this purpose, for example, a very thin carrier film 90 can be used (preferably with a thickness of less than 23 μm, in particular 19 μm, in particular a thickness between 6 μm and 15 μm) and / or a carrier film 90 with a low glass transition temperature can be used, which is exceeded by the printing conditions of the second embossing lacquer, so that the film is particularly easy to deform.
[0110] Another possibility is to provide the compensation layer 80 in the layer structure of the security element itself. Fig.10 In the layer structure of the security element to be produced, a compensation layer 80 is arranged on the carrier film 22 , which compensation layer is flexible at least under the printing conditions of the embossing lacquer layer 32 and preferably has elastic properties.
[0111] exist Fig.10 The original state shown in (a) corresponds to Fig. 9 (a) shows the original state and a carrier film 22 with an applied compensation layer 80, for example made of silicone rubber, which is coated in the feature area 40 with a hydrophilic UV embossing lacquer 42 after hardening. The compensation layer can also be provided with a thin cover layer to make it easier to apply the embossing lacquer layers 32, 42 and / or to provide a suitable surface energy. The UV embossing lacquer 42 is embossed with the desired embossed structure 44 and hardened by UV crosslinking. The carrier film coated in this way is then wetted with a wetting agent 92 inline or in a separate process, wherein only the hydrophilically coated feature area 40 receives the wetting agent 92, while the uncoated feature area 30 remains free of the wetting agent.
[0112] Then, a second embossing lacquer layer of thermoplastic embossing lacquer 32 is provided on the printing cylinder 94 over the entire surface. Fig.10As shown in (b), the compensation layer 80 is elastic under the printing conditions of the thermoplastic lacquer 32, so that the already hardened UV embossing lacquer areas 42 are locally pressed into the compensation layer 80 by the printing cylinder 94. This prevents the embossed structure 44 from being deformed or damaged and allows the embossing lacquer layer 32 to be applied without problems precisely in the gaps 30 between the UV embossing lacquer areas 42.
[0113] In order to be able to emboss the UV embossing lacquer regions 42 sufficiently far, the layer thickness of the compensation layer 80 should be slightly greater than the height difference to be compensated, which is typically between 2 and 15 μm.
[0114] Although the UV embossing lacquer areas 42 are also in contact with the embossing lacquer layer 32 , they are ink-repellent due to the applied wetting agent 92 and therefore do not accept the embossing lacquer 32 .
[0115] After the printing step is completed, the elastic compensation layer 80 is deformed back to its original shape, thereby forming Fig.10 The desired design shown in (c), which has unembossed thermoplastic embossing lacquer 32 in the feature area 30 and embossed, hardened UV embossing lacquer 42 in the feature area 40, can be further processed as described above.
[0116] If a particularly high-resolution structuring of the UV embossing lacquer layer 42 is to be achieved in the described embodiment, then instead of Figures 8 to 10 In the exemplary embodiment of FIG. 4 , the embossing lacquer layer is printed in a structured manner; the embossing lacquer layer 42 can also be applied in a residue-free embossing process, as is described in principle in patent specification EP 3 230 795 B1.
[0117] In order to be able to successfully carry out such high-resolution, residue-free embossing, the surface energy of the carrier, the embossing tool used and the surface tension of the embossing lacquer must be matched to one another.
[0118] refer to Fig.11 (a), in which a UV embossing lacquer 42 is first applied to the entire surface of a carrier 90. A structured embossing mold 100 comprises mold areas 102, 104 with different height levels, the shape and size of which correspond to the feature area 30 (convex mold area 102) or 40 (concave mold area 104). The desired embossing structure 44 of the feature area 40 is arranged in the concave mold area 104, which is away from the layer 42 to be embossed in the next embossing step.
[0119] When the structured embossing mold 100 approaches the full-surface and not yet hardened embossing lacquer layer 42, the protruding regions 102, due to their geometry, reduce the layer thickness of the embossing lacquer 42 present there by squeezing out. More precisely, due to the wetting properties of the embossing lacquer 42, the peeling coefficient, i.e., the interface energy between the carrier 90 and the embossing lacquer 42 and between the embossing lacquer 42 and the structured embossing mold 100, becomes negative, so that the embossing lacquer 42 is withdrawn from the feature region 30 below the protruding mold region 102 into the feature region 40 below the recessed mold region 104.
[0120] This tendency to wetting and dewetting depends not only on the surface energy but also on the layer thickness. Thus, in the feature region 30, the protruding mold region 102 of the embossing mold 100 locally causes a residue-free dewetting of the embossing lacquer 42 when approaching. The embossing lacquer 42 collected in the feature region 40 is embossed there by the embossing structure 44 arranged in the recessed mold region 104.
[0121] After the embossing lacquer 42 has hardened, the carrier film 90 therefore contains the desired high-resolution structure with embossed, hardened UV lacquer areas 42 and the still uncoated feature areas 30 located therebetween, as in Fig.11 (b). Then, for example, it is possible to Figures 8 to 10 Further processing was performed as described.
[0122] According to other method variants which also use the phenomena of surface energy or surface tension, reference is made to Fig.12 (a), first a layer of a first embossing lacquer 32 is printed onto a carrier 90, the first embossing lacquer having a particularly low surface energy after it has dried or crosslinked. The printed first embossing lacquer 32 is embossed and dried or hardened. The first embossing lacquer 32 is applied in a structured manner, so that there are feature areas 30 with the first embossing lacquer and feature areas 40 that have not yet been coated and do not have embossing lacquer. It has proven to be advantageous to provide approximately half of the total area to be coated with the first embossing lacquer 32.
[0123] Then a second embossing lacquer formulation 42 with low viscosity and high surface tension is applied over the entire surface. Fig.12 The case of an intermediate step is shown in (a). The second embossing lacquer formulation 42 can be a UV embossing lacquer, in particular a water-thinnable formulation, which possibly still has to be physically dried before embossing.
[0124] Due to its low viscosity and high surface tension, the second formulation 42 dewets the first embossing lacquer 32 having a lower surface energy, as in Fig.12 As shown by arrow 110 in (a), after dewetting, Fig.12(b) is the case shown in Figure 2. In the case of complete dewetting, Fig.12 As shown in (b), the application of the second embossing lacquer formulation 42 can also be repeated several times, so that the material with high surface tension accumulates continuously in the feature area 40 until a sufficient amount of second embossing lacquer 42 is present there for the desired second embossing.
[0125] In addition to the described use of surface energy and surface tension phenomena, there is also an advantageous possibility based on layer stripping for applying two or more different embossing lacquer layers next to each other without register fluctuations, now in combination with Fig.13 and 14 The feasibility is described in more detail.
[0126] First reference Fig.13 , a first layer made of a first thermoplastic embossing lacquer 42 having a desired first color is applied in a structured manner to the carrier film 22 and dried. The first embossing lacquer 42 is applied in a structured manner in the pattern of the feature area 40, but the applied layer thickness d1 is greater than the layer thickness d0 actually required in the end, as in Fig.13 As shown in (a).
[0127] A second layer of a second thermoplastic embossing lacquer 32 having the desired second color is then applied over the entire surface. Fig.13 As shown in (b), the second embossing varnish 32 is advantageously applied with a layer thickness d2>d1, but in principle it is sufficient to apply the second embossing varnish with a layer thickness d2>d0. The application of the second embossing varnish 32 can also be carried out in multiple steps and in combination with a wiping or scraping step in each case, so that the layer thickness of the second embossing varnish 32 on the first applied embossing varnish area 42 is kept small.
[0128] After the second embossing lacquer 32 has cured or physically dried, the formed structure is mechanically stripped to the desired layer thickness d0, for example by milling 120 a layer region 122 that protrudes beyond the layer thickness d0. If the milling cutter 120 is set to the desired target layer thickness, then in the simplest case milling can be performed to this target layer thickness at which the two embossing lacquers 32, 42 are exposed in the feature regions 30, 40 arranged exactly side by side, as in Fig.13 As shown in (c).
[0129] Fine-tuning and feedback of the milling step 120 can be performed by means of the milling removal, ie the material removed from the layer region 122. Fig.13As shown in (b), during the milling process, initially only the material of the second embossing lacquer 32 at the higher level is removed in the still small layer removal 124, and only in the case of a larger layer removal is the material of the first embossing lacquer 42 also removed. The desired removal depth can therefore be controlled by spectral inspection or, if necessary, simply by checking the color of the milled removal. This ensures that the excess second embossing lacquer 32 present on the first embossing lacquer area 42 is completely removed and reliably reaches the first embossing lacquer area 42. Fig.13 The final position is shown in (c).
[0130] exist Fig.14 In other embodiments, two different embossing lacquers are used to produce the feature layer 24 , one of which is soluble in the stripping medium and the other is insoluble.
[0131] First reference Fig.14 (a), UV embossing lacquer 42 of a first color is first applied in a structured manner in feature areas 40 on the carrier film 22. The UV embossing lacquer 42 is usually embossed with the desired embossed structure 44 and hardened. The feature areas 30 located between the embossing lacquer areas 42 are ideally kept completely uncoated.
[0132] A thermoplastic embossing lacquer 32 having a second color is then provided for which there is a suitable stripping medium, by means of which the dried embossing lacquer 32 can be removed at a well-defined stripping rate, but which does not dissolve the UV embossing lacquer 42 .
[0133] As in Fig.14 As shown in FIG. 2( b), the second layer is applied over the entire surface of the carrier film 22 using this embossing lacquer 32. Application can be achieved, for example, in flexographic printing (or flexographic printing), wherein the flexographic sleeve presses a significant portion of the embossing lacquer 32 under high pressure into the recesses 130 between the already hardened UV embossing lacquer areas 42, and only relatively little ink remains on the embossing lacquer areas 42.
[0134] The embossing lacquer 32 is still liquid immediately after being applied, so that the excess can be wiped off or scraped off the printed film and thus removed in particular from the already hardened embossing lacquer areas 42. After the embossing lacquer 32 has been physically dried, the recesses 130 between the already hardened UV embossing lacquer areas 42 are partially filled, as in Fig.14 As shown in (b). On the embossing lacquer area 42 there is usually also a thin tint film 132 consisting of embossing lacquer material.
[0135] The embossing lacquer 32 is applied repeatedly and excess material is removed until the recess 130 is fully filled or even overfilled, as in Fig.14(c). The repetition improves the relationship between the filling degree of the recess 130 and the undesired color tone 132 of the embossing lacquer area 42. It can be proposed to change the color concentration of the embossing lacquer 32 during the step-by-step filling process, in particular to change to lower and lower color concentrations, because when wiping or scraping off, the color tone of the corresponding penultimate application step is also reduced and the proportion of undesired color on the embossing lacquer area 42 is thus reduced.
[0136] After the final repeated application and wiping or scraping off, the thermoplastic embossing lacquer 32 is physically dried, thus forming a Fig.14 The situation shown in (c).
[0137] The embossing lacquer 32 is then subjected to a development step by means of an associated stripping medium. The stripping medium can be aqueous, have a defined pH value or can also be solvent-based. It may be necessary to expose the embossing lacquer 32 before stripping.
[0138] The stripping process is stopped, for example by rinsing with another medium, as soon as the embossing lacquer 32 has been stripped sufficiently by the stripping medium to expose the embossing lacquer areas 42. The hardened UV embossing lacquer 42 is not stripped by the stripping medium of the embossing lacquer 32, so that the exposure is carried out with high selectivity.
[0139] After the stripping step is completed, the desired structure is present on the carrier film 22, which has feature areas 40 with an embossed UV embossing lacquer layer 42 of a first color and feature areas 30 located between the feature areas 40, which have a thermoplastic embossing lacquer layer 32 of a second color that has not yet been embossed, as in Fig.14 Further processing can be carried out, for example, according to the working steps already described.
[0140] Replacement of UV embossing paint 42, Fig.14 Other thermoplastic embossing lacquers can also be used in the working step. The thermoplastic embossing lacquers may be insoluble in the stripping medium of the embossing lacquers 32 from the outset, or they may contain a crosslinking agent which makes them insoluble in the stripping medium of the embossing lacquers 32, but whose crosslinking reaction has not yet proceeded to such an extent at the time of the first embossing that embossing would be prevented. Such crosslinking agents may be isocyanates, wherein the use of aliphatic isocyanates leads to a slower reaction if embossing is to be carried out with a certain time delay after the coating step.
[0141] The first embossing lacquer layer 42 can be applied by applying the desired pattern to the feature area 40 in a structured manner. However, in particular in the case of UV embossing lacquer, it is also possible to first apply the embossing lacquer layer over the entire surface and then structure it as desired. Advantageous possibilities for this, in particular for structuring UV embossing lacquer layers with high resolution, have already been described above. If a thermoplastic embossing lacquer is applied as the first embossing lacquer layer, pressure at elevated temperature or pressure from the melt may be required in order to successfully achieve fine structuring with sufficient layer thickness.
[0142] Before and / or after embossing the first embossing lacquer layer 42, a further method step may be provided, with which the embossing lacquer is converted into a stable and / or embossable form. This may be, for example, an exposure step or an annealing step. A wet chemical treatment may also be provided, in which the embossing lacquer is contacted with a liquid medium in order to induce hardening or crosslinking.
[0143] List of Reference Numerals
[0144] 10 Banknotes
[0145] 12 Anti-counterfeiting elements
[0146] 14 Observer
[0147] 20 Anti-counterfeiting elements
[0148] 22 Carrier film
[0149] 24 Feature Layer
[0150] 30 Feature Area
[0151] 32 Embossed paint layer
[0152] 34 Imprinted structure
[0153] 34' Incompletely formed embossed structure
[0154] 40 Feature Area
[0155] 42 Embossed paint layer
[0156] 44 Imprinted structure
[0157] 50, 52 Imprinting mold
[0158] 60 Flexible Imprinting Mold
[0159] 62 Deformation
[0160] 64 Transition Zone
[0161] 70 Hard embossing mold
[0162] 72 Soft top roller
[0163] 74 Carrier film
[0164] 80 Compensation layer
[0165] 90 Carrier
[0166] 92 Wetting agent
[0167] 94 Printing Cylinders
[0168] 96 Compressible elements
[0169] 98 Soft top roller
[0170] 100 Structured embossing molds
[0171] 102 Protruding mold area
[0172] 104 Recessed mold area
[0173] 110 De-wetting
[0174] 120 Milling cutter
[0175] 130 Recess
[0176] 132 Tint Film
Claims
1. A method for producing a security element for providing security for valuables, the security element comprising a feature layer having a first feature area and a second feature area, in which different first or second embossing lacquer layers are present, wherein: In the method, - applying a hydrophilic layer of a first embossing lacquer on the carrier in the first feature region, the applied layer being embossed with an embossed structure producing the first optical effect and hardened, - providing a different second layer of embossing lacquer on the printing tool, and - in a printing step, bringing the printing tool into contact with the carrier and thereby transferring the second embossing lacquer, Therein, in the printing step, the second embossing lacquer is transferred only into the second feature regions which are not coated with the hydrophilic first embossing lacquer.
2. The method according to claim 1, characterized in that Prior to the printing step, the carrier is moistened with a first embossing lacquer layer and in the process the moistening agent is transferred exclusively to the hydrophilic first embossing lacquer layer of the first feature regions.
3. The method according to claim 1, characterized in that The different, second embossing lacquer layer is provided over the entire surface of the printing tool.
4. The method according to claim 1, characterized in that In a printing step, a layer of a second embossing lacquer is provided on a flexible printing tool, which is deformed locally by the pressure tip generated by the layer of the already hardened first embossing lacquer.
5. The method according to claim 4, characterized in that The flexible printing tool is a printing cylinder having a compressible element.
6. The method according to claim 1, characterized in that In the printing step, a second layer of embossing lacquer is provided on the printing tool and, to generate the counterpressure, a soft embossing roller is used which is deformed locally by the pressure tip generated by the already hardened first layer of embossing lacquer.
7. The method according to claim 6, characterized in that The printing tool is a hard printing cylinder.
8. The method according to claim 1, characterized in that A flexible compensation layer is arranged on the carrier, which is deformed locally during the printing step by the pressure tips generated by the already hardened first lacquer layer.
9. The method according to claim 1, characterized in that The first embossing lacquer is first applied to the entire surface of the carrier and then structured into a wetted first feature area and a dewetted second feature area by a residue-free embossing method through the approach of a structured embossing mold, and at the same time, an embossing structure that produces a first optical effect is embossed into the wetted first feature area by the structured embossing mold.
10. The method according to claim 1, characterized in that The first embossing lacquer is hardened by the action of radiation.
11. The method according to claim 10, characterized in that The first embossing lacquer is hardened by UV irradiation.
12. A method for producing a security element for providing security for valuables, the security element comprising a feature layer having a first feature area and a second feature area, in which different first or second embossing lacquer layers are present, wherein: In the method, - applying a layer of a first embossing lacquer with a lower surface energy on the carrier in the first feature region, the applied layer being embossed with an embossed structure producing the first optical effect and hardened, - applying a layer of a second, different embossing lacquer having a lower viscosity and a higher surface tension over the entire surface and causing the second embossing lacquer to dewet from the first feature areas coated with the first embossing lacquer into the second feature areas, and - Repeating the application and dewetting process in order to collect a sufficient amount of second embossing lacquer for embossing in the second feature area.
13. The method according to claim 1 or 12, characterized in that A second embossing structure is embossed into the embossing lacquer layer of the second embossing lacquer, said second embossing structure producing a second optical effect.
14. The method according to claim 13, characterized in that The second embossing structure is transferred exclusively into the second embossing lacquer layer by using a flexible embossing template, a soft embossing roller or a flexible compensating layer in the layer structure of the security element in order to transfer the second embossing structure exclusively into the second embossing lacquer layer.
15. The method according to claim 1 or 12, characterized in that Thermoplastic embossing lacquers having different softening temperatures are applied as embossing lacquers.
16. The method according to claim 1 or 12, characterized in that As one embossing lacquer a radiation-curing embossing lacquer is applied and as the other embossing lacquer a thermoplastic embossing lacquer is applied.
17. The method according to claim 16, characterized in that As one embossing lacquer a UV-curing embossing lacquer is applied and as the other embossing lacquer a thermoplastic embossing lacquer is applied.
18. The method according to claim 1 or 12, characterized in that Embossing lacquers of different colors, different transparencies and / or different brightness are applied.
19. The method according to claim 1 or 12, characterized in that The embossing lacquer layers of the first and second feature regions (30, 40) are arranged adjacent to each other without gaps and without overlap.
20. The method according to claim 1 or 12, characterized in that The first and the second embossing lacquer layer are provided with a common reflection-increasing coating.
21. The method according to claim 20, characterized in that The reflection-enhancing coating is a highly refractive or metallic coating.