Adhesive sheet and its use

By using an adhesive layer of surfactants and polyoxyalkylene backbone compounds in the adhesive sheet, an adhesive sheet with good peeling under high adhesion force is achieved, solving the problem of easy damage to the adhered object when peeling the adhesive sheet in the prior art. It is suitable for bonding and peeling of a variety of materials.

CN115151619BActive Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202180017400.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-28
Filing Date
2021-02-24
Publication Date
2024-10-01
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

Existing adhesive sheets struggle to achieve good peelability while maintaining high adhesive strength, especially without damaging or deforming the adhered material during peeling, particularly for low-strength or brittle materials.

Method used

It employs an adhesive layer containing surfactants and polyoxyalkylene backbone compounds, which has good water-based liquid peelability, balancing adhesion reliability and peel removal. It is designed with low water peel force and appropriate elongation to prevent tearing and is suitable for various peeling methods.

Benefits of technology

It achieves a balance between high adhesion and good peelability without damaging the adhered materials, and is suitable for peeling various materials, especially rigid and brittle materials. It reduces the strength requirements of the adhesive sheet and expands the range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115151619B_ABST
    Figure CN115151619B_ABST
Patent Text Reader

Abstract

The present invention provides an adhesive sheet that can take into account both bonding reliability and peeling removability, and can be peeled off in various peeling methods without deforming or damaging the adherend. The adhesive sheet provided by the present invention has an adhesive layer. The water peeling force of the above-mentioned adhesive sheet is less than 2N / 10mm. In addition, the stress of the above-mentioned adhesive sheet at 100% elongation is less than 30MPa, and the product of the fracture stress σf [MPa] and the fracture strain εf [%] (σf×εf) ​​is greater than 250.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive sheet, a method for peeling an adhesive sheet, and a method for separating two adherends joined by an adhesive sheet. This application claims priority based on Japanese Patent Application No. 2020-34310 filed on February 28, 2020, the entire contents of which are incorporated herein by reference. Background Art

[0002] Generally, adhesives (also called pressure-sensitive adhesives. The same applies hereinafter) have the following properties: they are in a soft solid (viscoelastic) state in a temperature range near room temperature and are easily bonded to an adherend under pressure. By utilizing such properties, adhesives are widely used in various fields in the form of an adhesive sheet with a support having an adhesive layer on a support, or in the form of an adhesive sheet without a support. As technical documents related to adhesive sheets, Patent Documents 1 to 2 can be cited. Patent Document 2 is a document related to an adhesive sheet with a substrate that can be stretched and peeled.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-23656

[0006] Patent Document 2: Japanese Patent Application Publication No. 2016-8288 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Depending on the purpose, various properties are required for adhesives. Among these properties, it is sometimes difficult to achieve at a high level at the same time, for example, there is a tendency for another property to decrease when one property is to be improved. As an example of a property that is in a relationship that is difficult to achieve at the same time, the adhesion to the adherend and the peeling removal property can be cited. For example, after the adhesive sheet is used to fix the adherend, when the adhesive sheet is peeled off from the adherend, in order to prevent damage and deformation of the adherend, contrary to the above-mentioned fixing, it is required that the peeling force of the adhesive sheet from the adherend (that is, the adhesion to the adherend) be suppressed to be lower. For example, in the case of a brittle or thin adherend, it is not easy to realize an adhesive sheet with both good peeling removal property and high adhesion.

[0009] The adhesive sheet with good peeling and removal properties can be preferably used for various purposes as an adhesive sheet with excellent reprocessability, reusability and repairability. The so-called reprocessing here, for example, refers to peeling off the adhesive sheet from the adherend when the adhesive sheet is pasted to the adherend and causing adhesive damage (position deviation, generation of wrinkles or bubbles, involvement of foreign matter, etc.), peeling off the adhesive sheet from the adherend when an undesirable condition is observed in the adherend after pasting the adhesive sheet (also referred to as disassembly), typically refers to re-attaching the adhesive sheet using the peeled old adhesive sheet or a new adhesive sheet. In addition, the so-called reusable refers to making the adherend peeled off from the adhesive sheet into a state that can be reused, including reuse here. Products with components fixed with adhesive sheets are delivered to users. After the end of the product life, as long as the components can be disassembled and reused without damage to the components and without residual adhesive sheets, it is meaningful from the perspectives of effective use of resources and reduction of environmental load. In addition, the so-called repairable means that when a component fails during use of the product, the component can be replaced, repaired or inspected. As long as the component fixed with the adhesive sheet can be peeled off and removed, the component can be replaced, repaired or inspected, which is beneficial to reducing the cost of the product user and reducing the environmental load.

[0010] In view of the above-mentioned problems, the inventors of the present application proposed in Patent Document 1 a novel adhesive sheet (water-peelable adhesive sheet) that can be easily peeled off using aqueous liquids such as water and has improved water-resistant reliability during bonding. The present invention relates to an improvement of the above-mentioned water-peelable adhesive sheet, and the purpose is to provide an adhesive sheet that can take into account both bonding reliability and peeling and removal properties, and can be peeled off in various peeling methods such as peeling off from a low-strength rigid adherend such as a glass plate after bonding without deforming or damaging the adherend. Another object of the present invention is to provide a novel peeling method and adherend separation method using an adhesive sheet.

[0011] Means for solving problems

[0012] According to the present specification, an adhesive sheet having an adhesive layer is provided. The first aspect of the adhesive sheet has a water peeling force of 2 N / 10 mm or less, and the water peeling force is measured according to 10.4.1 Method 1 of JIS Z0237:2009: 180° peeling force relative to a test plate, specifically, at a test temperature of 23°C using a tensile tester at a tensile speed of 300 mm / min and a peeling angle of 180 degrees, after the adhesive surface of the adhesive layer is attached to the surface of an alkaline glass plate produced by a float process as an adherend and the contact angle with distilled water is 5 to 10 degrees, and after 1 day at room temperature, 20 μL of distilled water is dripped onto the adherend, and the distilled water is allowed to enter one end of the interface between the adhesive surface and the adherend. In addition, the stress at 100% elongation of the adhesive sheet is less than 30 MPa, and the product of the fracture stress σf [MPa] and the fracture strain εf [%] (σf×εf) ​​is 250 or more. The stress at 100% elongation, the fracture stress σf, and the fracture strain εf are measured by a tensile test conducted at a tensile speed of 100 mm / min.

[0013] In addition, in the second aspect of the adhesive sheet having an adhesive layer provided by the present specification, the adhesive layer contains at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton. In addition, the stress at 100% elongation of the adhesive sheet is less than 30 MPa, and the product of the fracture stress σf [MPa] and the fracture strain εf [%] (σf × εf) is greater than 250. The stress at 100% elongation, the fracture stress σf, and the fracture strain εf are measured by a tensile test performed at a tensile speed of 100 mm / min.

[0014] According to the adhesive sheet of the above structure, since the water peeling force is limited to less than 2N / 10mm (the first mode), or the adhesive layer contains at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton (hereinafter also referred to as a "water peeling agent") (the second mode), the peeling property of aqueous liquids such as water is good, and both bonding reliability and peeling removal property can be taken into account. In addition, the stress of the above adhesive sheet at 100% elongation is less than 30MPa. With respect to the stretching in the sheet surface direction of the adhesive sheet (the direction orthogonal to the thickness direction of the adhesive sheet), the resistance to the initial stretching is relatively small, and it can be stretched with a smaller force. Therefore, when the adhesive sheet attached to the adherend is stretched, in the initial stage of its stretching, the gap near the bonding interface with the adherend generated by the elongation of the adhesive sheet can be utilized to allow the aqueous liquid to enter the peeling front with the adherend, and good water peeling property can be achieved. The so-called "peeling front" here refers to the position where the above adhesive sheet begins to leave the above adherend when the adhesive sheet is peeled from the adherend. In addition, since the product of the above-mentioned breaking stress σf and the breaking strain εf (σf×εf) ​​is greater than 250, the elongation and strength of the adhesive sheet are balanced. Relative to the elongation of the adhesive sheet, the strength is relatively greater than the specified value, and no tearing occurs during the stretching during peeling, allowing good peeling and removal.

[0015] The advantages of the adhesive sheet of the above-mentioned structure are as follows (this is not a restrictive explanation). First, first, according to the above-mentioned adhesive sheet, it is possible to improve the stripping and removal properties. Specifically, the above-mentioned adhesive sheet can utilize its elongation and water stripping properties to peel off the adhesive sheet without forcing the adherend to be deformed or damaged because it has both elongation and water stripping properties. For example, in the mode of joining two adherends, the two adherends are formed by rigid materials, and at least one of the adherends is formed by brittle materials (such as hard and brittle materials). By stretching the adhesive sheet of the above-mentioned structure, water stripping is performed, and the adhesive sheet can be peeled off without forcing the adherend to be deformed or damaged. Specifically, when the above-mentioned two adherends are formed by rigid materials, when stripping and removing, due to the rigidity of the adherend, it is impossible to peel it off at a stripping angle greater than 0° such as 90°, and it is difficult to make an aqueous liquid enter the stripping front that becomes the starting point of water stripping. According to the adhesive sheet disclosed herein, by stretching the adhesive sheet in the pulling direction, a gap is generated at the peeling front, and an aqueous liquid is supplied therein, so that no load such as deformation is applied to the adherend, and water peeling (pulling water peeling) can be performed. That is, peeling and removal from a rigid body (such as rigid body reprocessing) can be achieved. For example, even in the case where the adherend is a low-strength rigid adherend such as a thin-walled glass plate, it has bonding reliability based on sufficient bonding strength when bonded and fixed, and it can also be peeled without damaging the adherend during peeling.

[0016] Second, since the adhesive sheet can be peeled off in the pulling direction, it can be removed from the adherend even in a peeling method with a limited peeling angle. For example, when the adherend is a component, it is sometimes difficult to stretch the adhesive sheet of the fixed component along an angle that is not parallel to the bonding surface (e.g., 90°, 180° direction). Even in such a usage mode, according to the adhesive sheet disclosed herein, the adhesive sheet can be peeled off by stretching the adhesive sheet along an angle less than 90° relative to its bonding surface (e.g., a direction parallel to the bonding surface).

[0017] Third, it is possible to prevent the stretch-peel adhesive sheet from tearing when stretched. In the past, it was necessary to use a material with a strength that could withstand the tensile force that depends on the adhesive force of the adhesive sheet, but the adhesive sheet disclosed herein has water-peelability, so the bonding strength with the adherend can be significantly reduced by using the above-mentioned aqueous liquid. Therefore, when the adhesive sheet is stretched and peeled, it is possible to prevent the adhesive sheet from tearing due to the bonding strength with the adherend, at least the risk can be greatly reduced. This can be a particularly advantageous feature in, for example, the peeling of a large-area adherend bonded with a large adhesive force as a whole, which can greatly reduce the bonding strength with the adherend that is the cause of tearing.

[0018] The adhesive sheet does not tear during the stretching and peeling, which is a particularly important feature in the method of, for example, performing the stretching and peeling from two adherends. Specifically, if the adhesive sheet used to join two adherends is to be pulled out between the two adherends and the adhesive sheet tears during stretching, the adhesive sheet returns to the middle of the above-mentioned two adherends due to its elasticity, and it is sometimes difficult to take out the end of the adhesive sheet held during the stretching and peeling. The adhesive sheet disclosed herein has a reduced peeling force during the stretching and peeling based on water peelability, so even if the strength of the adhesive sheet is not improved, more specifically, even if the strength of the adhesive sheet is relatively low corresponding to its elongation, it is not easy to have the above-mentioned undesirable situation. This can be an ideal feature in the use of the adhesive force required to be above the specified value during the joining.

[0019] Fourth, as mentioned above, the bonding strength with the adherend during peeling and removal can be significantly reduced, which means that the strength of the adhesive sheet used in the stretching and peeling can be reduced. For example, the adhesive sheet can be thinned. In addition, it is also possible to expect the increase in the freedom of choice of adhesive sheet material, design, and the expansion of the applicable position of the adhesive sheet of the stretching and peeling type.

[0020] In some preferred embodiments, the normal peel strength of the adhesive sheet is 2.5 N / 10 mm or more and 15 N / 10 mm or less, and the normal peel strength is measured after one day at room temperature according to 10.4.1 Method 1 of JIS Z0237:2009: 180° peeling strength relative to a test plate after the adhesive surface of the adhesive layer is attached to the surface of an alkaline glass plate produced by a float process as an adherend with a contact angle of 5 to 10 degrees with distilled water, specifically, at a test temperature of 23° C. using a tensile tester at a tensile speed of 300 mm / min and a peeling angle of 180 degrees. According to the adhesive sheet satisfying the above characteristics (normal adhesive strength characteristics), both high adhesive reliability based on the adhesive strength to the adherend and peeling and removability based on water peelability can be achieved.

[0021] In some preferred embodiments, the adhesive layer is formed by an adhesive composition containing a partial acrylic polymer, a crosslinking agent, and a photopolymerization initiator. The adhesive sheet formed by the adhesive composition of the above composition can satisfactorily achieve the effects brought about by the technology disclosed herein. For example, in a configuration in which the adhesive sheet is substantially formed only by the adhesive layer, the adhesive of the above composition can become an adhesive that satisfactorily meets the required properties.

[0022] In some preferred embodiments, the HLB (Hydrophile-Lipophile Balance) of the surfactant is not less than 10 and not more than 20. By using a surfactant having an HLB of 10 to 20 as the water-release agent, the water-release property of the pressure-sensitive adhesive sheet is further improved.

[0023] The adhesive layer may be formed from a water-dispersible adhesive composition, a solvent-based adhesive composition, an active energy ray-curable adhesive composition, or a hot melt adhesive composition. In the configuration using an adhesive formed from the above adhesive composition, the effects of the technology disclosed herein can be achieved.

[0024] As the adhesive layer, an acrylic adhesive layer can be used. By using an acrylic adhesive, it is easy to obtain a highly reliable adhesive force. In addition, for example, by using a water stripping agent in the acrylic adhesive, it is possible to maintain the adhesive properties of the acrylic adhesive and achieve the target water stripping property at the same time. In the structure having an adhesive layer formed of an acrylic adhesive, the effect brought by the technology disclosed herein can be satisfactorily achieved.

[0025] Some preferred adhesive sheets are double-sided adhesive sheets (double-sided adhesive sheets). In the double-sided adhesive sheet, the adhesive layer constitutes the bonding surface of at least one of the double-sided adhesive sheets. The effect of the technology disclosed herein can be particularly satisfactorily exerted in the form of a double-sided adhesive sheet. For example, when the adherends on each side of the double-sided adhesive sheet are formed of rigid materials, the bonding state of the adherends can be released without forcing the adherends to deform or break. That is, good peeling and removal properties from rigid bodies (such as rigid body reprocessing properties) can be exerted.

[0026] In addition, some forms of adhesive sheets may have a first adhesive layer and a second adhesive layer as the aforementioned adhesive layer, and an intermediate layer disposed between the first adhesive layer and the second adhesive layer. In such a configuration, the effects brought about by the technology disclosed herein can be satisfactorily achieved. In the above configuration, the adhesive layer can be formed by, for example, any one of a water-dispersible adhesive composition, a solvent-based adhesive composition, an active energy ray-curable adhesive composition, and a hot-melt adhesive composition, for example, an adhesive layer formed by a water-dispersible adhesive composition can be preferably used.

[0027] In some embodiments, the intermediate layer may be formed of a material including acrylic resin, polyurethane resin, urethane (meth) acrylate polymer, polyolefin resin, polyvinyl chloride resin, silicone, rubber or elastomer. According to the configuration of the intermediate layer using the above-mentioned materials, the adhesive force and water peelability based on the adhesive layer and the target mechanical properties (specifically, the product of stress at 100% elongation, breaking stress and breaking strain) can be satisfactorily balanced.

[0028] In addition, according to this specification, a stripping method for an elongated adhesive sheet attached to an adherend can be provided. The method includes a process (stripping process) of stretching and stripping the aforementioned adhesive sheet in a direction less than 90° relative to the bonding surface of the aforementioned adherend. And, the process of stripping the aforementioned adhesive sheet is implemented in a state where an aqueous liquid is present at the exposed portion of the stripping of the bonding interface between the aforementioned adherend and the aforementioned adhesive sheet. According to the above method, the adhesive sheet can be stripped from the adherend using the above aqueous liquid. That is, when adhesively fixed, the adhesive sheet can achieve high reliability of bonding, and on the other hand, it can be well stripped from the adherend when stripped. More specifically, the adhesive sheet has elongation, so in the initial stage of stretching the adhesive sheet in the above stripping process, the gap near the bonding interface with the adherend generated by the elongation of the adhesive sheet can be used to allow the aqueous liquid to enter the stripping portion of the bonding interface, and based on the water stripping thus performed, good stripping and removal can be achieved. It should be noted that the adhesive sheet stripped by the stripping method disclosed herein typically includes an adhesive layer. The PSA sheet may be, for example, any PSA sheet disclosed herein.

[0029] In addition, according to this specification, a method for separating two adherends joined by an elongated adhesive sheet is provided. Typically, the method includes a process of stretching the adhesive sheet in a direction of pulling from between the two adherends using the elongation of the adhesive sheet. Furthermore, the process of stretching the adhesive sheet is implemented in a state where an aqueous liquid is present at a portion of the adhesive interface between at least one of the two adherends and the adhesive sheet that is exposed to peeling. According to the above method, the adhesive sheet can be peeled off from the two adherends using the aqueous liquid, so even when the two adherends are formed of rigid materials or brittle materials, the two adherends can be separated without forcing the adherends to deform or destroy. That is, when adhesively fixed, the adhesive sheet can achieve high-reliability bonding, and on the other hand, when the bonding state is to be released, the adherends can be separated and removed well. More specifically, the adhesive sheet has elongation, so in the initial stage of stretching the adhesive sheet in the stretching process, the gap near the bonding interface with the adherend caused by the elongation of the adhesive sheet can be used to allow the aqueous liquid to enter the peeling portion of the bonding interface, and based on the water peeling performed thereby, the two adherends to which the adhesive sheet is pasted can be separated. It should be noted that the adhesive sheet used in the separation method disclosed herein typically includes an adhesive layer. The above-mentioned adhesive sheet can be, for example, any adhesive sheet disclosed herein (typically a double-sided adhesive sheet).

[0030] In addition, in the above-mentioned peeling method and separation method, the part of the bonding interface between the adherend and the pressure-sensitive adhesive sheet that is exposed to peeling is also called "peeling front".

[0031] Furthermore, any suitable combination of the above-mentioned elements may also be included in the scope of the invention for which patent protection is sought through this patent application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] [ Figure 1 ] is a cross-sectional view schematically showing the structure of an adhesive sheet according to one embodiment.

[0033] [ Figure 2 ] is a cross-sectional view schematically showing the structure of a pressure-sensitive adhesive sheet according to another embodiment.

[0034] [ Figure 3 ] is a cross-sectional view schematically showing the structure of a pressure-sensitive adhesive sheet according to another embodiment. DETAILED DESCRIPTION

[0035] The preferred embodiments of the present invention are described below. It should be noted that matters necessary for implementing the present invention, except for those specifically mentioned in this specification, can be understood by those skilled in the art based on the teachings on the implementation of the invention recorded in this specification and the technical common sense at the time of application. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in this field. In addition, in the following drawings, parts and portions that play the same role are sometimes marked with the same symbols for description, and repeated descriptions are sometimes omitted or simplified. In addition, the embodiments described in the drawings are illustrated for the purpose of clearly explaining the present invention, and do not necessarily accurately represent the actual size or reduction ratio provided.

[0036] <Configuration Example of Pressure-Sensitive Adhesive Sheet>

[0037] The adhesive sheet disclosed herein may have, for example, Figure 1 The cross-sectional structure schematically shown in FIG. The adhesive sheet 1 is constituted as a double-sided adhesive sheet without a support body formed by an adhesive layer 10. Figure 1 As shown, the double-sided adhesive sheet 1 without a support can be in the form of an adhesive sheet 50 with a release liner before use (before being attached to an adherend). In one embodiment, the adhesive sheet 1 can be in the form of a adhesive sheet 50 with a release liner, wherein each surface 10A, 10B of the adhesive layer 10 is protected by a release liner 31, 32 whose at least the adhesive layer side is a releasable surface (release surface). Alternatively, it can also be in the form of: the back side (the surface opposite to the adhesive side) of the release liner 31 is the release surface, and the adhesive surface 10B is abutted against the back side of the release liner 31, thereby protecting the adhesive surfaces 10A, 10B.

[0038] like Figure 2 As shown, the adhesive sheet disclosed herein can be configured as a single-sided adhesive sheet 2, which includes: an adhesive layer 10, one surface 10A of which is a bonding surface to be attached to an adherend; and a support (support layer) 20, which is laminated on the other surface 10B of the adhesive layer 10. The adhesive layer 10 is fixedly bonded to one surface 20A of the support 20. Figure 2 In the example shown, the adhesive layer 10 has a single-layer structure. The adhesive sheet 2 before use (before being attached to an adherend) may be, for example, Figure 2 As shown in the figure, the adhesive surface 10A is protected by a release liner 30 whose at least the adhesive layer side becomes a releasable surface (release surface), and the adhesive sheet 50 with a release liner is in the form of a release liner. Alternatively, it can also be in the form of: the second surface 20B (the surface on the opposite side to the first surface 20A, also referred to as the back side) of the support body 20 becomes the release surface, and the adhesive surface 10A is abutted against the second surface 20B of the support body 20. The adhesive surface 10A is thus protected.

[0039] The adhesive sheet disclosed herein may be constituted as, for example Figure 3A double-sided adhesive sheet (double-sided adhesive sheet) 3 having an intermediate layer 25 is shown. Figure 3 The adhesive sheet 3 shown has the following structure: adhesive layers 11 and 12 are provided on each side of the intermediate layer 25 (all non-peelable), and one of the adhesive layers (first adhesive layer) 11 is protected by a release liner 30 whose double sides become release surfaces. Such an adhesive sheet 3 can be configured as follows: by rolling up the adhesive sheet 3, the other adhesive layer (second adhesive layer) 12 is brought into contact with the back side of the release liner 30, so that the adhesive layer 12 is also protected by the release liner 30. Alternatively, the adhesive sheet can also have the following structure: each adhesive layer is protected by two release liners, at least one side of which is the release surface.

[0040] The release liner is not particularly limited, and for example, a release liner having a release treatment on the surface of a liner substrate such as a resin film or paper, or a release liner formed of a low-adhesive material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin-based resin (polyethylene, polypropylene, etc.) can be used. In the above release treatment, for example, a release treatment agent such as a silicone-based or long-chain alkyl-based release agent can be used. In some embodiments, a release-treated resin film can be preferably used as the release liner.

[0041] The adhesive layer of the adhesive sheet disclosed herein is not limited to Figure 1 or Figure 2 The single-layer structure as shown in the example of the constitution may further include one or more adhesive layers (additional adhesive layers) of the same or different compositions. Figure 3 In the adhesive sheet having an intermediate layer shown, the intermediate layer may be an adhesive layer. In this case, the adhesive sheet may have at least three adhesive layers, namely, a first adhesive layer constituting the surface of the adhesive sheet, a second adhesive layer, and an adhesive layer as an intermediate layer.

[0042] In addition, the adhesive sheet disclosed herein can be peeled off by utilizing its elongation, so a wing can be set at the end of the adhesive sheet. By holding the wing and stretching the adhesive sheet, the peeling operability can be improved. The shape of the wing is not particularly limited, and is preferably a shape (such as a rectangle) that can be held with a finger. Such an adhesive sheet can be a shape with a long side direction such as a band. For example, by arranging a wing at one end of the long side direction of the adhesive sheet in advance, the adhesive sheet can be easily stretched and peeled off.

[0043] <Characteristics of Adhesive Sheet>

[0044] (Water peel strength)

[0045] Some forms of adhesive sheets are characterized in that the water peeling force is less than 2N / 10mm (typically less than 2.0N / 10mm). Adhesive sheets that meet this feature have good water peelability and can be peeled off from adherends using aqueous liquids such as water. In this way, according to the adhesive sheet whose water peeling force is limited to less than the specified value, the load applied to the adherend when the adhesive sheet is peeled off can be reduced. This is particularly meaningful in adhesive sheets that are attached to, for example, thin adherends, brittle adherends, adherends that are easily deformed (elongated, bent, twisted, etc.), adherends with thin films that are easily damaged on the surface, etc. The water peeling force can be less than about 1.5N / 10mm, can be less than about 1.2N / 10mm, or can be less than 1.0N / 10mm. In some preferred embodiments, the water peeling force is preferably less than about 0.7N / 10mm, more preferably less than about 0.5N / 10mm, and further preferably less than 0.3N / 10mm, for example, less than about 0.2N / 10mm. The lower limit of the water peeling force is 0.0N / 10mm or more (for example, more than 0.0N / 10mm), and can be about 0.1N / 10mm or more. The water peeling force can be specifically measured by the method described in the embodiments described later. The water peeling force can be adjusted by appropriately selecting the type of adhesive and the component containing the adhesive (typically a water peeling agent, etc.) based on the contents described in this specification. It should be noted that the adhesive sheet disclosed in this specification includes a method that does not limit the water peeling force. In such a method, the adhesive sheet is not limited to an adhesive sheet having the above-mentioned characteristics.

[0046] In addition, from the perspective of improving the peeling and removal properties including reprocessability, reusability, and repairability, the following adhesive sheets are preferred: adhesive sheets that can be peeled off from the adherend without leaving adhesive residue on the adherend in the measurement of water peeling force. That is, adhesive sheets with excellent non-slurry residue are preferred. Whether the adhesive residue is left on the adherend can be determined by visually observing the adherend after peeling the adhesive sheet, for example.

[0047] (Normal peeling force)

[0048] As described above, the adhesive sheet disclosed herein can be peeled off and removed well based on water stripping properties when peeled off. On the other hand, it has sufficient adhesive force when bonded and fixed to the adherend. Although not particularly limited, the above-mentioned normal peeling force of the adhesive sheet disclosed herein can exceed 2.0N / 10mm. From the viewpoint of obtaining high bonding reliability, the above-mentioned normal peeling force is preferably about 2.5N / 10mm or more, more preferably about 3.5N / 10mm or more, and further preferably about 4.5N / 10mm or more. Some forms of adhesive sheets can present a normal peeling force of about 5.5N / 10mm or more (for example, about 6.5N / 10mm or more). The upper limit of the above-mentioned normal peeling force is not particularly limited, for example, it can be less than 25N / 10mm, it can be less than 20N / 10mm, it can also be less than 15N / 10mm or less than 10N / 10mm. The above-mentioned normal peeling force can be specifically measured by the method described in the embodiments described later. The above-mentioned normal peeling force can be adjusted by appropriately selecting the type of adhesive and the component containing the adhesive based on the content recorded in this specification.

[0049] (Water peeling force reduction rate)

[0050] For some preferred adhesive sheets, the water peeling force reduction rate obtained by the ratio (N1 / N0) of the water peeling force N1 to the normal peeling force N0 can be about 40% or more (for example, about 50% or more). For adhesive sheets with a large water peeling force reduction rate, they have sufficient adhesion when attached to the adherend, and at the same time, when peeled off, they can significantly reduce the load applied to the adherend when peeled off by using an aqueous liquid such as water. By utilizing this property, for example, it is possible to take into account the positional displacement of the adhesive sheet attached to the adherend, the performance of suppressing floating, and good peeling and removal properties. In some embodiments, it is appropriate for the water peeling force reduction rate to be 60% or more, preferably 65% ​​or more, for example, 70% or more, 75% or more, 80% or more, or 85% or more. In some embodiments, the water peeling force reduction rate is 90% or more, for example, 95% or more, and further 98% or more (typically 99% or more). The upper limit of the water peeling force reduction rate is 100% in principle, and is, for example, less than 100%.

[0051] The water peeling force reduction rate can be calculated by the formula: water peeling force reduction rate [%] = (1-(N1 / N0)) × 100.

[0052] (Stress at 100% elongation)

[0053] One of the characteristics of the adhesive sheet disclosed herein is that the stress is less than 30MPa when the above-mentioned 100% elongation. For an adhesive sheet that meets this characteristic, the resistance to the initial stretching is suppressed in terms of the stretching of the sheet surface direction of the adhesive sheet (the direction orthogonal to the thickness direction of the adhesive sheet), and it can be stretched with a smaller force. Therefore, when the adhesive sheet attached to the adherend is stretched, in the initial stage of its stretching, the gap near the bonding interface with the adherend generated by the elongation of the adhesive sheet is used to easily allow the aqueous liquid to enter the peeling front with the adherend, and it is easy to achieve good water peelability. It is appropriate that the stress is less than 15MPa when the above-mentioned 100% elongation, for example, it can also be less than 10MPa. In some ways, the stress of the adhesive sheet is preferably less than 7MPa when the 100% elongation is less than 5MPa, and more preferably less than 3MPa. In some preferred ways, the stress of the adhesive sheet is less than 1.0MPa when the 100% elongation is more preferably less than 0.7MPa, more preferably less than 0.5MPa, and particularly preferably less than 0.3MPa. The stress at 100% elongation may be 0.20 MPa or less. The lower limit of the stress at 100% elongation is not particularly limited, but from the perspectives of adhesion workability and tear prevention of the adhesive sheet, a stress of 0.01 MPa or more is appropriate, for example, 0.05 MPa or more, or 0.10 MPa or more.

[0054] (Stress at 500% elongation)

[0055] Although not particularly limited, the stress at 500% elongation of the adhesive sheet disclosed herein may be 50MPa or less (e.g., 30MPa or less). Adhesive sheets that satisfy this characteristic tend to have excellent stretching removal properties. It is appropriate that the stress at 500% elongation is 15MPa or less, for example, it may be 10MPa or less. In some embodiments, the stress at 500% elongation of the adhesive sheet is preferably 7MPa or less, more preferably 5MPa or less, and further preferably 3MPa or less. In some preferred embodiments, the stress at 500% elongation of the adhesive sheet is 1.0MPa or less, more preferably 0.7MPa or less, and further preferably 0.5MPa or less. The stress at 500% elongation may be 0.30MPa or less. The lower limit of the stress at 500% elongation is not particularly limited. From the perspectives of the pasting operability of the adhesive sheet and the prevention of tearing, it is appropriate to be 0.05MPa or more, for example, it may be 0.10MPa or more, or 0.50MPa or more.

[0056] (Elongation strength characteristics)

[0057] The adhesive sheet disclosed herein is characterized in that the product of the fracture stress σf [MPa] and the fracture strain εf [%] measured by the tensile test under the condition of a tensile speed of 100 mm / min (σf×εf) ​​is 250 or more. The elongation and strength of the adhesive sheet satisfying this feature are balanced, and the strength is relatively greater than the specified value relative to the elongation of the adhesive sheet during peeling, so that no tearing occurs during the stretching during peeling, and good peeling and removal can be achieved. The above-mentioned σf×εf (elongation strength characteristic) is preferably 300 or more, more preferably 400 or more, and further preferably 500 or more, for example, 800 or more, and may be 1200 or more. Such an adhesive sheet has better elongation and strength, and has a tendency that it is not easy to be damaged by tearing when removing the adhesive sheet, and has excellent tensile removability. It also has a tendency to be excellent in processability. The upper limit of the above (σf×εf) ​​is not particularly limited. From the viewpoints of tear prevention, workability, and operability, it may be less than 100,000, and 50,000 or less is appropriate, and may be 30,000 or less, 15,000 or less, 7,000 or less, or 4,000 or less (e.g., 2,000 or less). The adhesive sheet disclosed herein can be peeled off under a small load by utilizing water peelability during peeling and removal, so even if the above elongation strength characteristics are not excessively improved, in other words, even if the above σf×εf is a lower value in the range of 250 or more, good peeling and removal can be achieved.

[0058] In some embodiments, the above σf×εf (elongation strength property) may be less than 10000, and is appropriately 7000 or less. From the viewpoint of taking into account the adhesive properties (adhesive force, etc.), it is preferably 3000 or less, more preferably 2000 or less, further preferably 1000 or less, particularly preferably 700 or less, and may be 500 or less, or 400 or less. The above σf×εf is preferably used in the unsupported adhesive sheet.

[0059] In some other embodiments, the above σf×εf (elongation strength characteristic) is preferably 300 or more, more preferably 1000 or more, further preferably 3000 or more, and can be 5000 or more, or 10000 or more (e.g. 20000 or more, further 30000 or more). Such an adhesive sheet can exhibit better elongation and strength. The above σf×εf is preferably used in an adhesive sheet having a support layer and an intermediate layer.

[0060] (fracture stress σf)

[0061] The above-mentioned fracture stress σf of the adhesive sheet disclosed herein is not particularly limited as long as it satisfies the above-mentioned σf×εf. In some ways, from the viewpoint of preventing tearing during stretching, the fracture stress σf of the adhesive sheet can be 0.10MPa or more, 0.20MPa or more (for example, 0.30MPa or more) is appropriate, can be 0.50MPa or more, can be 0.80MPa or more, can be 1.00MPa or more, and can also be 1.20MPa or more (for example, 1.50MPa or more). The adhesive sheet having the above-mentioned fracture stress σf has a tendency to be excellent in processability. In some other ways, the above-mentioned fracture stress σf can be 0.7MPa or more, 1.0MPa or more is appropriate, preferably 1.5MPa or more, can be 2.0MPa or more, can be 3.0MPa or more, can be 10MPa or more, and can also be 20MPa or more (for example, 25MPa or more). The upper limit of the breaking stress σf of the adhesive sheet can be less than 200MPa, less than 150MPa is appropriate, less than 100MPa, or less than 30MPa. In some ways, the breaking stress σf of the adhesive sheet can be less than 50MPa, and from the perspective of obtaining suitable elongation, it is appropriate to be less than 15MPa, less than 8MPa, or less than 6MPa (for example, less than 5MPa). In some other ways, from the perspective of taking into account the adhesive properties (adhesion, etc.), the above-mentioned breaking stress σf can be, for example, less than 3.00MPa, less than 2.00MPa, less than 1.20MPa, less than 1.00MPa, less than 0.80MPa, or less than 0.60MPa. According to the technology disclosed herein, the adhesive sheet can be peeled off under a small load by utilizing water peelability when peeling and removing, so the above-mentioned breaking strength σf will not be excessively increased. In other words, it is possible to prevent tearing and other undesirable situations caused by insufficient strength by having a structure with a lower breaking stress σf.

[0062] (Fracturing strain εf)

[0063] The breaking strain εf (elongation at break) of the adhesive sheet disclosed herein is not particularly limited as long as it satisfies the above σf×εf. In some embodiments, from the perspective of obtaining an elongation suitable for water peelability, the breaking strain εf of the adhesive sheet may be 150% or more, 250% or more (e.g., 280% or more) is appropriate, preferably 300% or more, more preferably 400% or more, further preferably 500% or more, 600% or more, 800% or more, or 1000% or more (e.g., 1500% or more). The upper limit of the above-mentioned breaking strain εf is not particularly limited, and from the perspective of having suitable strength, good tear resistance, workability, and operability, for example, it may be 2000% or less, 1200% or less, 1000% or less, 900% or less, or 800% or less (e.g., 700% or less).

[0064] The above mechanical properties of the adhesive sheet (stress at 100% elongation, stress at 500% elongation, fracture stress σf and fracture strain εf) are measured by a tensile test performed at a tensile speed of 100 mm / min. Specifically, the method described in the embodiments described below can be used for measurement. The above mechanical properties can be set and adjusted by appropriately selecting the adhesive material, the adhesive-containing component (e.g., the molecular design of the base polymer, the crosslinking agent, etc.), the support, the material type of the intermediate layer, the molding method, etc. based on the contents described in this specification.

[0065] (Haze value)

[0066] In the technology disclosed herein, the haze value of the adhesive sheet is not particularly limited. In some embodiments, it is appropriate for the haze value of the adhesive sheet to be about 10% or less, and it can be about 5% or less (for example, about 3% or less). The above haze value is preferably 1.0% or less. Such a highly transparent adhesive sheet is suitable for optical uses requiring high light transmittance. The haze value of the adhesive sheet may be less than 1.0%, less than 0.7%, and less than 0.5% (for example, 0 to 0.5%). These haze values ​​associated with the adhesive sheet may also be preferably applied to the haze values ​​of the adhesive layer in the technology disclosed herein. The haze value can be adjusted, for example, by selecting the composition and thickness of the adhesive layer.

[0067] The "haze value" here refers to the ratio of diffuse transmitted light to total transmitted light when the object to be measured is irradiated with visible light. It is also called haze value. The haze value can be expressed by the following formula.

[0068] Th[%]=Td / Tt×100

[0069] In the above formula, Th is the haze value [%], Td is the scattered light transmittance, and Tt is the total light transmittance. The haze value can be measured by attaching the adhesive surface of the adhesive sheet to a single surface of an alkaline glass having a haze value of 0.1% to form a laminate of the adhesive sheet and the alkaline glass, and then using a haze meter (e.g., the product name "MR-100" manufactured by Murakami Color Technology Research Institute). When measuring, the alkaline glass to which the adhesive sheet is attached is arranged in such a way that the adhesive sheet becomes the light source side. Since the haze value of the alkaline glass is 0.1%, the value after subtracting 0.1% from the measured value is used as the haze value [%] of the adhesive layer.

[0070] <Adhesive Layer>

[0071] The adhesive sheet disclosed herein has an adhesive layer. The above-mentioned adhesive layer can be an adhesive layer composed of the following adhesive, and the adhesive is selected from various known adhesives such as acrylic adhesives, rubber adhesives (natural rubber, synthetic rubber, their mixed systems, etc.), silicone adhesives, polyester adhesives, polyurethane adhesives, polyether adhesives, polyamide adhesives, fluorine adhesives, etc. One or more adhesives. Here, the so-called acrylic adhesive refers to an adhesive with an acrylic polymer as the main component (base polymer). The same meaning applies to rubber adhesives and other adhesives.

[0072] It should be noted that the so-called "base polymer" of the adhesive refers to the main component of the rubber-like polymer contained in the adhesive, and no limiting interpretation is given otherwise. The so-called rubber-like polymer refers to a polymer that exhibits rubber elasticity in a temperature range near room temperature. In addition, in this specification, the so-called "main component" refers to the component that is contained in the largest proportion among the components contained on a weight basis. Therefore, for example, when the adhesive layer is composed of three or more components, the content of the main component in the adhesive layer can be 34% by weight or more.

[0073] In addition, in this specification, the so-called "acrylic polymer" refers to a polymer derived from a monomer component containing an acrylic monomer in an amount of more than 50% by weight, and is also called an acrylic polymer. The so-called acrylic monomer mentioned above refers to a monomer derived from a monomer having at least one (meth)acryloyl group in one molecule. In addition, in this specification, the so-called "(meth)acryloyl" refers to both acryloyl and methacryloyl. Similarly, "(meth)acrylate" refers to both acrylate and methacrylate, and "(meth)acrylic-" refers to both acrylic- and methacrylic-, respectively.

[0074] (Acrylic adhesive)

[0075] In some embodiments, an acrylic adhesive may be preferably used as a constituent material of the adhesive layer. Specifically, the adhesive layer disclosed herein may be an acrylic adhesive layer comprising an acrylic polymer. Acrylic adhesives have a tendency to be excellent in transparency, weather resistance, and freedom of design. Acrylic adhesives with high transparency may be preferably used in optical applications.

[0076] As the adhesive layer disclosed herein, for example, it is preferable to contain, as a base polymer, an acrylic polymer composed of the following monomer components, wherein the monomer components contain 33% by weight or more of an alkyl (meth)acrylate having a linear or branched alkyl group with 1 to 20 carbon atoms at the ester terminal. Hereinafter, the alkyl (meth)acrylate having an alkyl group with X to Y carbon atoms at the ester terminal may be expressed as “alkyl (meth)acrylate C X-Y In order to easily obtain a balance of properties, in some embodiments of the acrylic polymer, (meth)acrylic acid C 1-20 The proportion of the alkyl ester is, for example, 35% by weight or more, preferably 40% by weight or more, and may be 45% by weight or more. In some other embodiments, the (meth)acrylic acid C in the total monomer components of the acrylic polymer is 1-20 The proportion of the alkyl ester is suitably more than 50 wt %, for example, 70 wt % or more, 80 wt % or more, or 90 wt % or more. 1-20 The proportion of the alkyl ester may be, for example, 99.9% by weight or less, 99% by weight or less, or 95% by weight or less. From the viewpoint of the cohesiveness of the adhesive layer, the (meth)acrylic acid C in the acrylic polymer in some embodiments may be 99.9% by weight or less, 99% by weight or less, or 95% by weight or less. 1-20 The proportion of the alkyl ester in the total monomer component may be, for example, 85% by weight or less, 75% by weight or less, 65% by weight or less, 60% by weight or less, 55% by weight or less, or 50% by weight or less. 1-20 The adhesive having a limited ratio of the alkyl (meth)acrylate can be an adhesive having suitable elongation strength characteristics in a support-free adhesive sheet composed of an adhesive layer. 1-20 The alkyl esters may be used alone or in combination of two or more.

[0077] As (meth)acrylic acid C 1-20Specific non-limiting examples of the alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and the like.

[0078] Among these, it is preferred to use at least (meth)acrylic acid C 4-20 Alkyl esters, more preferably at least (meth) acrylic acid C 4-18 For example, it is preferred that the acrylic adhesive contains one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) as the above-mentioned monomer component, and it is particularly preferred that the acrylic adhesive contains at least 2EHA. 4-20 Other examples of alkyl esters include isononyl acrylate, n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), isostearyl acrylate (iSTA), and the like. 4-18 The alkyl esters may be used alone or in combination of two or more.

[0079] In some embodiments, among the monomer components constituting the acrylic polymer, (meth)acrylic acid C 4-18 Alkyl esters in (meth) acrylic acid C 1-20 The proportion of the alkyl ester may be 70% by weight or more. 4-18 The proportion of the alkyl ester may be, for example, 80% by weight or more, 90% by weight or more, or 95 to 100% by weight.

[0080] The monomer components constituting the above-mentioned acrylic polymer may include alkyl (meth)acrylate, and other monomers (copolymerizable monomers) that can be copolymerized with alkyl (meth)acrylate and added as needed. As copolymerizable monomers, monomers having polar groups (e.g., carboxyl groups, hydroxyl groups, rings containing nitrogen atoms, etc.) and monomers having a high glass transition temperature of the homopolymer (e.g., above 10° C.) may be preferably used. Monomers having polar groups can help introduce crosslinking points into acrylic polymers or increase the cohesive force of adhesives. Copolymerizable monomers may be used alone or in combination of two or more.

[0081] Specific non-limiting examples of the copolymerizable monomer include the following monomers.

[0082] Monomers containing a carboxyl group: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and the like.

[0083] Monomers containing anhydride groups: for example, maleic anhydride, itaconic anhydride.

[0084] Monomers containing hydroxyl groups: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0085] Monomers containing sulfonic acid groups or phosphoric acid groups: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, (meth)acrylate sulfopropyl ester, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethylacryloyl phosphate, etc.

[0086] Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl (meth)acrylate ether, allyl glycidyl ether, and glycidyl (meth)acrylate ether.

[0087] Monomers containing cyano groups: for example, acrylonitrile, methacrylonitrile, etc.

[0088] Isocyanate group-containing monomer: for example, 2-isocyanateethyl (meth)acrylate, etc.

[0089] Monomers containing amide groups: for example, (meth)acrylamide; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl) (meth)acrylamide, N,N-di(tert-butyl) (meth)acrylamide and the like N,N-dialkyl (meth)acrylamide; N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, N-n-butyl (meth)acrylamide and the like N-alkyl (meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinyl acetamide; Monomers having hydroxyl groups and amide groups, for example, N-(2-hydroxyethyl) ( N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide and the like; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl(meth)acrylamide such as N-methoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide; and N,N-dimethylaminopropyl(meth)acrylamide, N-(meth)acryloylmorpholine and the like.

[0090] Monomers containing amino groups: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate.

[0091] Monomers having an epoxy group: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.

[0092] Monomers having a ring containing a nitrogen atom: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc. (for example, lactams such as N-vinyl-2-caprolactam).

[0093] Monomers having a succinimide skeleton include, for example, N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyhexamethylenesuccinimide.

[0094] Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, etc.

[0095] Itaconimides: for example, N-methyl itaconimide, N-ethyl itaconimide, N-butyl itaconimide, N-octyl itaconimide, N-2-ethylhexyl itaconimide, N-cyclohexyl itaconimide, N-lauryl itaconimide and the like.

[0096] Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate.

[0097] Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates (alkoxyalkyl (meth)acrylates) such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; and alkoxyalkyl (meth)acrylates (for example, alkoxypolyalkylene glycol (meth)acrylates) such as methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate.

[0098] Monomers containing alkoxysilyl groups: for example, (meth)acrylates containing alkoxysilyl groups such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and the like; and vinyl compounds containing alkoxysilyl groups such as vinyltrimethoxysilane and vinyltriethoxysilane.

[0099] Vinyl esters: for example, vinyl acetate, vinyl propionate, etc.

[0100] Vinyl ethers: For example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether.

[0101] Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc.

[0102] Olefins: for example, ethylene, butadiene, isoprene, isobutylene, etc.

[0103] (Meth)acrylates having an alicyclic hydrocarbon group: for example, (meth)acrylates having an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, and adamantyl (meth)acrylate.

[0104] (Meth)acrylates having an aromatic hydrocarbon group: for example, (meth)acrylates having an aromatic hydrocarbon group, such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate.

[0105] In addition, (meth)acrylates containing heterocycles such as tetrahydrofurfuryl (meth)acrylate, (meth)acrylates containing halogen atoms such as (meth)acrylates containing vinyl chloride and fluorine atoms, (meth)acrylates containing silicon atoms such as silicone (meth)acrylate, and (meth)acrylates obtained from terpene compound derivative alcohols, etc.

[0106] When using such copolymerizable monomers, the usage amount is not particularly limited, and for example, it is appropriate to set it to more than 0.01% by weight of the overall monomer component. From the viewpoint of better exerting the use effect of the copolymerizable monomer, the usage amount of the copolymerizable monomer can be more than 0.1% by weight of the overall monomer component, and can be more than 0.5% by weight. In addition, from the viewpoint of easily obtaining the balance of adhesive properties, it is appropriate that the usage amount of the copolymerizable monomer is less than 60% by weight of the overall monomer component, and can be less than 50% by weight, or can be less than 40% by weight.

[0107] In some embodiments, the monomer components constituting the acrylic polymer may include hydroxyl-containing monomers. By using hydroxyl-containing monomers, the cohesion of the adhesive and the degree of crosslinking (for example, crosslinking based on isocyanate crosslinking agents) can be appropriately adjusted. As hydroxyl-containing monomers, the hydroxyl-containing monomers exemplified above can be used, for example, 2-hydroxyethyl acrylate (HEA) and 4-hydroxybutyl acrylate (4HBA) can be preferably used. Hydroxyl-containing monomers can be used alone or in combination of two or more.

[0108] The amount used when using a hydroxyl-containing monomer is not particularly limited, for example, it can be more than 0.01% by weight of the overall monomer component, it can be more than 0.1% by weight, it can be more than 0.5% by weight, it can be more than 1% by weight, it can be more than 5% by weight or more than 10% by weight. In some ways, the amount of the hydroxyl-containing monomer used is more than 15% by weight of the overall monomer component, it is appropriate to be more than 20% by weight, preferably more than 25% by weight, more preferably more than 30% by weight, further preferably more than 35% by weight, and particularly preferably more than 40% by weight. By using the above-mentioned range of hydroxyl-containing monomers, it is possible to satisfactorily obtain an adhesive layer with good elongation and strength balance. In addition, from the viewpoint of suppressing the water absorption of the adhesive layer, in some ways, the amount of the hydroxyl-containing monomer used is appropriate for the overall monomer component, for example, less than 50% by weight (for example, less than 45% by weight), it can be less than 30% by weight, it can be less than 25% by weight, it can be less than 20% by weight, it can be less than 10% by weight, or it can be less than 5% by weight.

[0109] In some embodiments, the monomer components constituting the acrylic polymer may include a monomer having a nitrogen atom. This can improve the cohesive force of the adhesive. As a monomer having a nitrogen atom, the monomers exemplified above can be used. As a preferred example of a monomer having a nitrogen atom, a monomer having a ring containing a nitrogen atom can be cited. As a monomer having a ring containing a nitrogen atom, the monomers exemplified above can be used, for example, N-vinyl cyclic amide represented by general formula (1) can be cited.

[0110] [Chemical formula 1]

[0111]

[0112] Here, in the general formula (1), R 1 is a divalent organic group, specifically -(CH2) n -. n is an integer of 2 to 7 (preferably 2, 3 or 4). Among them, N-vinyl-2-pyrrolidone can be preferably used. As another preferred example of a monomer having a nitrogen atom, (meth)acrylamide can be cited. The monomer having a nitrogen atom can be used alone or in combination of two or more.

[0113] There is no particular restriction on the amount of monomers with nitrogen atoms (preferably monomers with nitrogen-containing rings), for example, it can be more than 1% by weight of the overall monomer component, it can be more than 2% by weight, and it is appropriate to be more than 3% by weight. In some ways, the amount of monomers with nitrogen atoms is more than 5% by weight of the overall monomer component, it can be more than 10% by weight, it can be more than 15% by weight, or it can be more than 18% by weight. By using the above-mentioned range of monomers with nitrogen atoms, it is possible to satisfactorily obtain an adhesive layer with good elongation and strength balance. In addition, it is appropriate that the amount of monomers with nitrogen atoms is less than 40% by weight of the overall monomer component, it can be less than 35% by weight, it can be less than 30% by weight, or it can be less than 25% by weight. In some other ways, the amount of monomers with nitrogen atoms can be less than 20% by weight of the overall monomer component, it can be less than 12% by weight, it can be less than 8% by weight, or it can be less than 6% by weight.

[0114] In some embodiments, the monomer components constituting the acrylic polymer may include a (meth)acrylate containing an alicyclic hydrocarbon group. This can improve the cohesive force of the adhesive. As the (meth)acrylate containing an alicyclic hydrocarbon group, the (meth)acrylates exemplified above can be used, for example, cyclohexyl acrylate (CHA) and isobornyl acrylate can be preferably used. The (meth)acrylate containing an alicyclic hydrocarbon group can be used alone or in combination of two or more.

[0115] There is no particular limitation on the amount of (meth)acrylate containing alicyclic hydrocarbon groups used, and for example, it may be more than 1% by weight, more than 3% by weight, or more than 5% by weight of the total monomer component. In some embodiments, the amount of (meth)acrylate containing alicyclic hydrocarbon groups used may be more than 8% by weight of the total monomer component, or more than 10% by weight. It is appropriate that the upper limit of the amount of (meth)acrylate containing alicyclic hydrocarbon groups used is about 40% by weight or less, for example, it may be less than 30% by weight, or less than 25% by weight (for example, less than 15% by weight, and further less than 10% by weight).

[0116] In some embodiments, the proportion of carboxyl-containing monomers in the monomer components of the acrylic polymer can be, for example, less than 10% by weight, less than 3% by weight, or less than 1% by weight (e.g., less than 0.1% by weight). It is also possible to substantially not use carboxyl-containing monomers as monomer components of the acrylic polymer. Here, substantially not using carboxyl-containing monomers means at least not intentionally using carboxyl-containing monomers. The acrylic polymer of such a composition can become a polymer having metal corrosion resistance to adherends containing metals.

[0117] Although not particularly limited, the monomer components of the acrylic polymer may include the alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate exemplified above, or may not include them. In some embodiments, the proportion of alkoxyalkyl (meth)acrylate in the monomer components of the acrylic polymer is less than 20% by weight, and the proportion of alkoxypolyalkylene glycol (meth)acrylate is less than 20% by weight. The polymer composed of such monomers is not easy to gel and is easy to form a sheet. The proportion of alkoxyalkyl (meth)acrylate in the above monomer components is preferably less than 10% by weight, more preferably less than 3% by weight, and further preferably less than 1% by weight. For example, the above monomer components do not substantially contain alkoxyalkyl (meth)acrylate (content 0 to 0.3% by weight). Similarly, the proportion of alkoxypolyalkylene glycol (meth)acrylate in the above monomer components is preferably less than 10% by weight, more preferably less than 3% by weight, and further preferably less than 1% by weight. For example, the above monomer components do not substantially contain alkoxypolyalkylene glycol (meth)acrylate (content 0 to 0.3% by weight).

[0118] In some preferred embodiments, the acrylic polymer can be an acrylic polymer containing a monomer having an aromatic ring such as a benzene ring as a monomer component. The monomer having an aromatic ring is incorporated into the acrylic polymer by polymerization, thereby introducing an aromatic ring in, for example, a side chain of the acrylic polymer, and the pseudo cross-linking (physical cross-linking) of the aromatic rings can be utilized to satisfactorily obtain an adhesive layer that has a good balance and simultaneously improves elongation and strength. As a monomer having an aromatic ring, the monomers exemplified above can be used. As a preferred example of a monomer having an aromatic ring, (meth) acrylates having an aromatic hydrocarbon group can be cited. As a (meth) acrylate having an aromatic hydrocarbon group, the (meth) acrylates exemplified above can be used, for example, benzyl acrylate (BzA) can be preferably used. The monomer having an aromatic ring can be used alone or in combination of two or more.

[0119] The amount used when using a monomer with an aromatic ring is not particularly limited. For example, the amount of the monomer with an aromatic ring can be more than 5% by weight of the overall monomer component, and it is appropriate to be more than 10% by weight, preferably more than 15% by weight, and it can also be more than 18% by weight. In addition, the amount of the monomer with an aromatic ring is appropriate to be, for example, less than 40% by weight of the overall monomer component, and can be less than 35% by weight, can be less than 30% by weight, or can be less than 25% by weight. In some other embodiments, the amount of the monomer with an aromatic ring can be, for example, less than 20% by weight of the overall monomer component, can be less than 10% by weight, can be less than 3% by weight, or can be less than 1% by weight.

[0120] In some preferred embodiments, the acrylic polymer may be an acrylic polymer containing a macromonomer as a monomer component. The macromonomer is incorporated into the acrylic polymer by polymerization, whereby a segment derived from the macromonomer is introduced into, for example, a side chain of the acrylic polymer, and based on the aggregation of the segment, a well-balanced adhesive layer with improved elongation and strength can be obtained satisfactorily.

[0121] The macromonomer is not limited to a specific type, and suitable monomers can be used in the macromonomers that can form the following segments in the polymer through intermolecular forces such as ionic bonds, hydrogen bonds, π-π interactions, hydrophilic and hydrophobic interactions, entropy interactions, etc., and the segments can show aggregation domains (pseudo-crosslinking points) in the adhesive. Such macromonomers can be macromonomers having polymerizable reaction groups such as vinyl and (meth) acryloyl at the ends and having segments that become side chains after polymerization. The above-mentioned segments, for example, can be segments having a structure formed by arranging a plurality of repeating units obtained by polymerization of monomers, etc. In the range of cohesiveness that can achieve the target, the above-mentioned segments may have substituents such as carboxyl, hydroxyl, amino, alkoxy, or may not have such substituents. In addition, as with known polymers, groups derived from polymerization initiators may exist at the ends of the above-mentioned segments.

[0122] Preferred examples of the above-mentioned macromonomers include macromonomers having segments containing poly[alkyl (meth)acrylate] and poly[aryl (meth)acrylate], and macromonomers having segments containing a polymerized structure of an aromatic vinyl compound, such as polystyrene (PSt). The alkyl group constituting the poly[alkyl (meth)acrylate] segment may be linear or branched. The number of carbon atoms of the alkyl group is, for example, 1 to 20, preferably 1 to 8, and more preferably 1 to 4 (specifically 1, 2, 3 or 4, typically 1 or 4). In some other embodiments, the alkyl group constituting the above-mentioned poly[alkyl (meth)acrylate] segment is a cycloalkyl group, for example, a cycloalkyl group having 3 to 20 carbon atoms (for example, 3 to 12, preferably 3 to 8, typically 3 to 6). As the aryl group constituting the poly[aryl (meth)acrylate] segment, aryl groups having 6 to 18 carbon atoms may be exemplified, such as phenyl, benzyl, and naphthyl. Specific examples of the macromonomer include macromonomers having polymethyl methacrylate (PMMA) segments, polybutyl acrylate (PBA) segments, and macromonomers having polystyrene (PSt) segments. The macromonomers may be used alone or in combination of two or more.

[0123] The molecular weight of the above-mentioned macromonomer is not limited to a specific range, and a macromonomer with an appropriate molecular weight can be used within the range of an adhesive layer having a target elongation and strength. The molecular weight of the above-mentioned macromonomer can be, for example, more than 500, or more than 800. From the viewpoint of appropriately realizing cohesiveness that can take into account both elongation and strength, the above-mentioned molecular weight is preferably more than 1500, more preferably more than 3000, and further preferably more than 4500 (for example, more than 5000). From the viewpoints of ease of polymerization, compatibility, etc., the upper limit of the molecular weight of the macromonomer is, for example, less than 100000, and less than 30000 is appropriate, preferably less than 10000, and can also be less than 8000. It should be noted that the molecular weight of the macromonomer in this specification refers to the number average molecular weight (Mn) converted to standard polystyrene obtained by gel permeation chromatography (GPC).

[0124] There is no particular restriction on the amount used when using a macromonomer, for example, it can be more than 0.1% by weight of the entire monomer component, it is appropriate to be more than 1% by weight, preferably more than 3% by weight, more preferably more than 5% by weight, and it can also be more than 10% by weight (for example, more than 15% by weight). In addition, it is appropriate that the amount of the macromonomer is less than 40% by weight of the entire monomer component, it can be less than 35% by weight, it can be less than 30% by weight, or it can be less than 25% by weight. In some embodiments, the amount of the macromonomer can also be less than 20% by weight of the entire monomer component (for example, less than 12% by weight). For example, when the macromonomer has an aromatic ring, from the viewpoint of compatibility, it is sometimes better to use a macromonomer in an amount of, for example, less than 10% by weight of the entire monomer component, and then less than 5% by weight (for example, less than 3% by weight).

[0125] The composition of the monomer components constituting the acrylic polymer can be set in the following manner: based on the composition of the monomer components, the glass transition temperature Tg obtained by the Fox equation is -75°C or higher and 10°C or lower. In some embodiments, from the viewpoint of adhesive strength, it is appropriate that the Tg is 0°C or lower, preferably -10°C or lower, and may be -20°C or lower or -30°C or lower. In addition, from the viewpoint of cohesion, the Tg may be, for example, -60°C or higher, -50°C or higher, -45°C or higher or -40°C or higher.

[0126] Here, the Fox equation is a relationship equation between Tg of a copolymer and glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each monomer constituting the copolymer, as shown below.

[0127] 1 / Tg=Σ(Wi / Tgi)

[0128] It should be noted that, in the above Fox formula, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio based on weight), and Tgi represents the glass transition temperature of the homopolymer of monomer i (unit: K).

[0129] As the glass transition temperature of the homopolymer used for calculation of Tg, the value described in the known document is used. For example, regarding the monomers listed below, as the glass transition temperature of the homopolymer of the monomer, the following value is used.

[0130]

[0131] Regarding the glass transition temperature of homopolymers of monomers other than those exemplified above, the values ​​described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) were used. When a plurality of values ​​were described in the document, the highest value was adopted.

[0132] For monomers whose homopolymer glass transition temperature is not recorded in the above-mentioned Polymer Handbook, the value obtained by the following measurement method is used (see Japanese Patent Application Publication No. 2007-51271). Specifically, 100 parts by weight of monomer, 0.2 parts by weight of azobisisobutyronitrile and 200 parts by weight of ethyl acetate as a polymerization solvent are added to a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube and a reflux condenser, and stirred for 1 hour while circulating nitrogen. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and reacted for 10 hours. Then, it is cooled to room temperature to obtain a homopolymer solution with a solid content concentration of 33% by weight. Then, the homopolymer solution is cast on a release liner and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. The test sample was punched into a disc with a diameter of 7.9 mm, sandwiched between parallel plates, and a viscoelasticity tester (ARES, manufactured by Rheometrics) was used to apply shear strain at a frequency of 1 Hz. The viscoelasticity was measured using the shear mode in a temperature range of -70 to 150°C at a heating rate of 5°C / min, and the peak temperature of tanδ was taken as the Tg of the homopolymer.

[0133] When the polymerization is carried out, a known or customary thermal polymerization initiator or photopolymerization initiator may be used according to the polymerization method, polymerization mode, etc. Such polymerization initiators may be used alone or in combination of two or more.

[0134] The thermal polymerization initiator is not particularly limited, and for example, an azo polymerization initiator, a peroxide initiator, a redox initiator based on a combination of a peroxide and a reducing agent, a substituted ethane initiator, and the like can be used. More specifically, examples include azo initiators such as 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutyramidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate; persulfates such as potassium persulfate and ammonium persulfate; peroxide initiators such as benzoyl peroxide, tert-butyl hydroperoxide, and hydrogen peroxide; substituted ethane initiators such as phenyl-substituted ethane; redox initiators such as a combination of a persulfate and sodium bisulfite, and a combination of a peroxide and sodium ascorbate; and the like, but the present invention is not limited to these. In addition, thermal polymerization can be suitably performed at a temperature of about 20 to 100° C. (typically 40 to 80° C.), for example.

[0135] The photopolymerization initiator is not particularly limited, and for example, ketal-based photopolymerization initiators, acetophenone-based photopolymerization initiators, benzoin ether-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzil-based photopolymerization initiators, benzophenone-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, etc. can be used.

[0136] The amount of such a thermal polymerization initiator or photopolymerization initiator used may be a normal amount used in accordance with the polymerization method, polymerization mode, etc., and is not particularly limited. For example, about 0.001 to 5 parts by weight (typically about 0.01 to 2 parts by weight, for example about 0.01 to 1 part by weight) of the polymerization initiator may be used relative to 100 parts by weight of the monomer to be polymerized.

[0137] In the above polymerization, various chain transfer agents known in the past (which can also be considered as molecular weight regulators or polymerization degree regulators) can be used as needed. As chain transfer agents, thiols such as n-dodecyl mercaptan, tert-dodecyl mercaptan, thioglycolic acid, and α-thioglycerol can be used. Alternatively, chain transfer agents that do not contain sulfur atoms (non-sulfur chain transfer agents) can be used. Specific examples of non-sulfur chain transfer agents include: anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenes such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having benzylidene acetone, cinnamyl alcohol, cinnamaldehyde, etc.; hydroquinones such as hydroquinone and dihydroxynaphthalene; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; benzyl hydrogens such as diphenylbenzene and triphenylbenzene; and the like.

[0138] The chain transfer agent may be used alone or in combination of two or more. When a chain transfer agent is used, the amount used may be, for example, about 0.01 to 1 part by weight relative to 100 parts by weight of the monomer component. The technology disclosed herein can be suitably implemented even without using a chain transfer agent.

[0139] The molecular weight of the acrylic polymer obtained by appropriately using the above-mentioned various polymerization methods is not particularly limited and can be set within an appropriate range according to the required performance. The weight average molecular weight (Mw) of the acrylic polymer is, for example, about 10×10 4 Above (e.g. 20×10 4 From the perspective of achieving cohesive force and adhesive force in a well-balanced manner, more than 30×10 4 Some forms of acrylic polymer preferably have 40×10 4 More than (typically, about 50×10 4 Above, for example, about 55×10 4 The upper limit of the Mw of the acrylic polymer may be about 500×10 4 Below (e.g. about 150×10 4 The above Mw can be about 75×10 4 Herein, Mw refers to a value converted to standard polystyrene obtained by gel permeation chromatography (GPC). As a GPC device, for example, a model "HLC-8320GPC" (column: TSKgel GMH-H (S), manufactured by Tosoh Corporation) can be used. The above Mw can be the Mw of the acrylic polymer in either the adhesive composition or the adhesive layer.

[0140] The adhesive layer disclosed herein can be formed using an adhesive composition containing monomer components of the composition described above in the form of a polymer, an unpolymer (i.e., a polymerizable functional group is in an unreacted form), or a mixture thereof. The above-mentioned adhesive composition can be in the following various forms: a water-dispersible adhesive composition in the form of an adhesive (adhesive component) dispersed in water; a solvent-based adhesive composition in the form of an adhesive contained in an organic solvent, an active energy ray-curable adhesive composition prepared in a manner of curing the adhesive using active energy rays such as ultraviolet rays and radiation; a hot melt adhesive composition that forms an adhesive when applied in a heated molten state and cooled to near room temperature; and the like. Some forms of adhesive compositions are solvent-based adhesive compositions or solvent-free adhesive compositions. The solvent-free adhesive composition includes active energy ray-curable adhesive compositions and hot melt adhesive compositions.

[0141] Some forms of adhesive compositions may be active energy ray-curable adhesive compositions. By using active energy ray-curable adhesive compositions, it is possible to satisfactorily obtain an adhesive sheet that can exert the effects of the technology disclosed herein with a structure of an unsupported body (which may be without an intermediate layer) formed by an adhesive layer. In this specification, the so-called "active energy ray" refers to an energy ray having energy that can cause chemical reactions such as polymerization reactions, cross-linking reactions, and decomposition of initiators. Examples of active energy rays referred to herein include ultraviolet rays, visible rays, infrared rays, α rays, β rays, γ rays, electron rays, neutron rays, X-rays, and the like. As a preferred example of an active energy ray-curable adhesive composition, a photocurable adhesive composition can be cited. The photocurable adhesive composition has the following advantages: even a thick adhesive layer can be easily formed. Among them, an ultraviolet curable adhesive composition is preferred.

[0142] Typically, the photocurable adhesive composition contains at least a portion of the monomer components of the composition in the form of a polymer (which may be a portion of the monomer type or a portion of the amount). The polymerization method for forming the above-mentioned polymer is not particularly limited, and various polymerization methods known in the past can be appropriately used. For example, thermal polymerization such as solution polymerization, emulsion polymerization, and bulk polymerization (typically, carried out in the presence of a thermal polymerization initiator); photopolymerization by irradiation with light such as ultraviolet rays (typically, carried out in the presence of a photopolymerization initiator); radiation polymerization by irradiation with radiation such as β rays and γ rays; and so on. Among them, photopolymerization is preferred.

[0143] Some preferred embodiments of the photocurable adhesive composition contain a partial polymer of a monomer component (e.g., an acrylic partial polymer). Such a partial polymer is typically a mixture of a polymer from a monomer component and an unreacted monomer, and preferably is in a slurry state (a viscous liquid state). Hereinafter, a partial polymer of this nature is sometimes referred to as "monomer slurry" or simply "slurry". There is no particular limitation on the polymerization method for partially polymerizing the monomer component, and various polymerization methods such as those described above can be appropriately selected and used. From the viewpoint of efficiency and simplicity, photopolymerization can be preferably used. According to photopolymerization, the polymerization conversion rate (monomer conversion) of the monomer component can be easily controlled by polymerization conditions such as the amount of light irradiation (amount of light).

[0144] The polymerization conversion rate of the monomer mixture in the above-mentioned partial polymer is not particularly limited. The above-mentioned polymerization conversion rate can be, for example, about 70% by weight or less, preferably about 60% by weight or less. From the viewpoints of ease of preparation and coating properties of the adhesive composition containing the above-mentioned partial polymer, it is appropriate that the above-mentioned polymerization conversion rate is about 50% by weight or less, preferably about 40% by weight or less (for example, about 35% by weight or less). The lower limit of the polymerization conversion rate is not particularly limited, and typically, it is about 1% by weight or more, and about 5% by weight or more is appropriate.

[0145] The adhesive composition containing a partial polymer of a monomer component can be obtained, for example, by the following method: using an appropriate polymerization method (e.g., photopolymerization) to partially polymerize a monomer mixture containing all the monomer components used in the preparation of the adhesive composition. In addition, the adhesive composition containing a partial polymer of a monomer component can be a mixture of a partial polymer or a complete polymer of a monomer mixture containing a part of the monomer components used in the preparation of the adhesive composition, and a mixture of the remaining monomer components or their partial polymers. It should be noted that in this specification, the so-called "complete polymer" refers to a polymerization conversion rate exceeding 95% by weight.

[0146] The adhesive composition containing the above-mentioned partial polymer may be mixed with other components used as needed (e.g., photopolymerization initiator, water stripping agent described later, crosslinking agent, multifunctional monomer, acrylic oligomer, tackifying resin, silane coupling agent, etc.). The method of mixing such other components is not particularly limited, and for example, they may be contained in the above-mentioned monomer mixture in advance or added to the above-mentioned partial polymer.

[0147] Some preferred adhesive sheets have an adhesive layer formed by a water-dispersible adhesive composition. By using a water-dispersible adhesive composition, an adhesive sheet that can exert the effect of the technology disclosed herein can be obtained satisfactorily with a structure having a support layer (which can be an intermediate layer). As a representative example of a water-dispersible adhesive composition, an emulsion-type adhesive composition can be cited. Typically, an emulsion-type adhesive composition contains a polymer of a monomer component and additives used as needed. The emulsion polymerization of the monomer component is usually carried out in the presence of an emulsifier. According to the emulsion polymerization, a polymerization reaction liquid in the form of an emulsion in which the polymer of the monomer component is dispersed in water can be obtained. The water-dispersible adhesive composition for forming an adhesive layer can be suitably manufactured using the above-mentioned polymerization reaction liquid.

[0148] As emulsifiers for emulsion polymerization, there are no particular restrictions, and known anionic emulsifiers, nonionic emulsifiers, etc. can be used. Emulsifiers can be used alone or in combination of two or more. Non-limiting examples of anionic emulsifiers include sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzene sulfonate, sodium polyoxyethylene lauryl sulfate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene alkylphenyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, sodium polyoxyethylene alkyl sulfosuccinate, etc. Non-limiting examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, polyoxyethylene polyoxypropylene block polymers, etc. Emulsifiers having reactive functional groups (reactive emulsifiers) can be used. Examples of the reactive emulsifier include radical polymerizable emulsifiers having a structure in which a radical polymerizable functional group such as an acrylic group or an allyl ether group is introduced into the above-mentioned anionic emulsifier or nonionic emulsifier.

[0149] The amount of the emulsifier used in the emulsion polymerization can be, for example, 0.2 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or 1.5 parts by weight or more relative to 100 parts by weight of the monomer component. In addition, from the viewpoint of improving the water-resistant adhesive force or improving the transparency of the adhesive layer, in some embodiments, it is appropriate that the amount of the emulsifier used is 10 parts by weight or less, preferably 5 parts by weight or less, or 3 parts by weight or less relative to 100 parts by weight of the monomer component. It should be noted that the emulsifier used in the emulsion polymerization here can also function as a water stripping agent described later.

[0150] The adhesive composition involved in some embodiments may be a solvent-based adhesive composition. Solvent-based adhesive compositions typically contain a solution polymer of a monomer component, and additives (such as a peeling force enhancer) used as needed. The solvent (polymerization solvent) used in the solution polymerization can be appropriately selected from conventionally known organic solvents. For example, any one solvent selected from the following, or a mixed solvent of two or more, can be used, namely: aromatic compounds such as toluene (typically aromatic hydrocarbons); esters such as ethyl acetate and butyl acetate; aliphatic or alicyclic hydrocarbons such as hexane and cyclohexane; halogenated alkanes such as 1,2-dichloroethane; lower alcohols such as isopropanol (for example, monohydric alcohols with 1 to 4 carbon atoms); ethers such as tert-butyl methyl ether; ketones such as methyl ethyl ketone; and the like. According to the solution polymerization, a polymerization reaction liquid in the form of a polymer of a monomer component dissolved in a polymerization solvent can be obtained. The solvent-based adhesive composition disclosed herein can be suitably manufactured using the above-mentioned polymerization reaction liquid.

[0151] (Compound A)

[0152] In some preferred embodiments, the adhesive layer may be characterized by containing at least one compound A (also referred to as "water stripping agent") selected from a surfactant and a compound having a polyoxyalkylene skeleton. Thus, the peeling force can be effectively reduced by using an aqueous liquid such as water. The reason for this is not particularly limited, but it is believed that the surfactant and the compound having a polyoxyalkylene skeleton both have a hydrophilic region, which is biased on the surface of the adhesive layer, and the peeling force is effectively reduced when in contact with water. As the surfactant and the compound having a polyoxyalkylene skeleton, one or more of the known surfactants and the compound having a polyoxyalkylene skeleton can be used without particular limitation. Typically, compound A is preferably contained in the adhesive composition (and thus the adhesive layer) in a free form. As compound A, from the perspective of the preparation of the adhesive composition, a compound that is liquid at room temperature (about 25°C) can be preferably used. It should be noted that among the above-mentioned surfactants, there are compounds having a polyoxyalkylene skeleton, and of course vice versa.

[0153] The HLB of compound A (typically a surfactant) is not particularly limited, for example, it is 3 or more, about 6 or more is appropriate, and it can be 8 or more (for example, 9 or more). In some preferred embodiments, the HLB of compound A is 10 or more. As a result, there is a tendency to exhibit water stripping properties satisfactorily. The above-mentioned HLB is more preferably 11 or more, further preferably 12 or more, and particularly preferably 13 or more (for example, 14 or more or 15 or more, and further 16 or more). By including compound A having an HLB in the above-mentioned range in the adhesive layer containing an acrylic polymer, water stripping properties can be more effectively exhibited. The upper limit of the above-mentioned HLB is less than 20, for example, it can be less than 18, or it can be less than 16 (for example, less than 15).

[0154] It should be noted that the HLB in this specification is a hydrophile-lipophile balance value proposed by Griffin, which is a value indicating the affinity of a surfactant to water and oil, and a numerical value between 0 and 20 indicates the ratio of hydrophilicity to lipophilicity. The definition of HLB is as described in WC Griffin: J. Soc. Cosmetic Chemists, 1, 311 (1949); Takahashi Kotomi, Nanba Yoshiro, Koike Motoo, Kobayashi Masao, "Surfactant Handbook", 3rd edition, published by Gongxue Book Co., Ltd., November 25, 1977, p179-182, etc. The compound A having the above HLB can be selected based on the technical common sense of a person skilled in the art with reference to the above references, etc. as needed.

[0155] As the surfactant that can be used as compound A, known nonionic surfactants, anionic surfactants, cationic surfactants, etc. can be used. Among them, nonionic surfactants are preferred. The surfactants can be used alone or in combination of two or more.

[0156] Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl phenyl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, and sorbitan monooleate; polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan triisostearate, polyoxyethylene sorbitan monooleate, and polyoxyethylene sorbitan trioleate; polyoxyethylene glycerol ether fatty acid esters; polyoxyethylene-polyoxypropylene block copolymers, and the like. These nonionic surfactants may be used alone or in combination of two or more.

[0157] Examples of anionic surfactants include: alkyl sulfates such as lauryl sulfate and octadecyl sulfate; fatty acid salts; alkylbenzene sulfonates such as nonylbenzene sulfonate and dodecylbenzene sulfonate; naphthalene sulfonates such as dodecylnaphthalene sulfonate; alkyldiphenyl ether disulfonates such as dodecyldiphenyl ether disulfonates; polyoxyethylene octadecyl ether sulfates and polyoxyethylene lauryl ether sulfates; polyoxyethylene alkylphenyl ether sulfates such as polyoxyethylene lauryl phenyl ether sulfates; polyoxyethylene styrenated phenyl ether sulfates; sulfosuccinates such as lauryl sulfosuccinate and polyoxyethylene lauryl sulfosuccinate; polyoxyethylene alkyl ether phosphates; polyoxyethylene alkyl ether acetates; and the like. When the anionic surfactant forms a salt, the salt may be, for example, a metal salt (preferably a monovalent metal salt) such as a sodium salt, a potassium salt, a calcium salt, a magnesium salt, an ammonium salt, an amine salt, and the like. These anionic surfactants may be used alone or in combination of two or more.

[0158] As a compound having a polyoxyalkylene skeleton that can be used as compound A, for example, polyalkylene glycols such as polyethylene glycol (PEG) and polypropylene glycol (PPG) can be used; polyethers containing polyoxyethylene units, polyethers containing polyoxypropylene units, compounds containing oxyethylene units and oxypropylene units (the arrangement of these units can be random or block-shaped); their derivatives; and the like. In addition, compounds having a polyoxyalkylene skeleton among the above-mentioned surfactants can also be used. These can be used alone or in combination of two or more. Among them, it is preferred to use a compound containing a polyoxyethylene skeleton (also called a polyoxyethylene segment), and more preferably PEG.

[0159] The molecular weight (chemical formula weight) of the compound having a polyoxyalkylene skeleton (e.g., polyethylene glycol) is not particularly limited, and for example, less than 1000 is appropriate, and from the perspective of the preparation of the adhesive composition, it is preferably about 600 or less (e.g., 500 or less). The lower limit of the molecular weight of the compound having a polyoxyalkylene skeleton (e.g., polyethylene glycol) is not particularly limited, and a compound having a molecular weight of about 100 or more (e.g., about 200 or more, and further about 300 or more) can be preferably used.

[0160] In some embodiments, the amount of compound A used is about 3 parts by weight or less relative to 100 parts by weight of the total amount of monomer components of the polymer contained in the adhesive layer (e.g., monomer components of acrylic polymers. It can also have the same meaning as polymers or base polymers. Unless otherwise specified, the same applies below). It is appropriate to be about 2 parts by weight or less. From the perspective of optical properties such as transparency, it is preferably less than 1 part by weight, more preferably less than 0.7 parts by weight, and further preferably less than 0.5 parts by weight. By limiting the amount of compound A used, there is a tendency that the adhesive force is also easy to maintain. In addition, for compound A with an HLB of more than 10, there is a tendency that good water peelability is easily exerted even when added in small amounts. In addition, from the perspective of exerting the effect of the addition of compound A, the amount of compound A relative to 100 parts by weight of the monomer components of the above-mentioned polymer can be 0.001 parts by weight or more, for example, 0.01 parts by weight or more is appropriate, preferably 0.03 parts by weight or more (e.g., 0.1 parts by weight or more). In a composition in which water-strippability is important, the amount of the compound A may be 0.2 parts by weight or more (eg, 0.3 parts by weight or more) based on 100 parts by weight of the monomer component.

[0161] (Multifunctional monomer)

[0162] A multifunctional monomer can be used in the adhesive composition (and thus the adhesive layer) as needed. The multifunctional monomer helps to adjust the cohesive force and other purposes. When the adhesive layer is formed and after being attached to the adherend, the multifunctional monomer reacts with the above-mentioned ethylenically unsaturated group by light (such as ultraviolet light) irradiation, thereby forming a cross-linked structure with suitable flexibility. Therefore, in this specification, "multifunctional monomer" can be referred to as a cross-linking agent. For example, in the adhesive layer formed by the photocurable adhesive composition, a multifunctional monomer can be preferably used. As the multifunctional monomer, a compound having two or more ethylenically unsaturated groups can be used. One type of multifunctional monomer can be used alone, or two or more types can be used in combination.

[0163] Examples of the ethylenically unsaturated group possessed by the multifunctional monomer include, but are not limited to, acryloyl, methacryloyl, vinyl, and allyl groups. From the viewpoint of photoreactivity, preferred ethylenically unsaturated groups include acryloyl and methacryloyl. Among them, acryloyl is preferred.

[0164] As a multifunctional monomer, a compound having 2 to 10 ethylenically unsaturated groups in the molecule is preferred, a compound having 2 to 8 ethylenically unsaturated groups in the molecule is more preferred, and a compound having 2 to 6 ethylenically unsaturated groups in the molecule is further preferred. In some embodiments, as a multifunctional monomer, a compound having 4 or less (specifically 2 to 4, for example 2 or 3, preferably 2) ethylenically unsaturated groups in the molecule can be used. By using such a multifunctional monomer in which the number of ethylenically unsaturated groups is limited, it is easy to obtain an adhesive layer that takes into account both elongation and strength.

[0165] Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butanediol (meth)acrylate, and hexanediol di(meth)acrylate. Among them, trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate are suitable, and 1,6-hexanediol diacrylate is more preferred.

[0166] The amount of the multifunctional monomer used varies according to its molecular weight, number of functional groups, etc. For example, it is appropriate to use a range of about 0.01 to 3.0 parts by weight relative to 100 parts by weight of the monomer component (typically, an acrylic polymer or a monomer component of the polymer) of the polymer contained in the adhesive layer. In some embodiments, the amount of the multifunctional monomer used relative to 100 parts by weight of the above-mentioned monomer component can be, for example, 0.02 parts by weight or more, 0.1 parts by weight or more, 0.5 parts by weight or more, 1.0 parts by weight or more, or 2.0 parts by weight or more. By increasing the amount of the multifunctional monomer used, there is a tendency to obtain higher cohesion. On the other hand, from the perspective of avoiding the reduction of the adhesion between the adhesive layer and the adjacent layer due to excessive increase in cohesion, the amount of the multifunctional monomer used relative to 100 parts by weight of the above-mentioned monomer component can be, for example, 10 parts by weight or less, 5.0 parts by weight or less, or 3.0 parts by weight or less. In some embodiments, the amount of the multifunctional monomer used relative to 100 parts by weight of the above-mentioned monomer component is, for example, 1.0 parts by weight or less, preferably 0.5 parts by weight or less, more preferably 0.3 parts by weight or less, and may be 0.2 parts by weight or less. By using such a multifunctional monomer content, it is easy to obtain an adhesive layer with improved elongation, an adhesive layer with improved elongation and strength balance. Such an adhesive layer is suitable for a method in which the adhesive sheet is composed of an adhesive layer.

[0167] (Crosslinking agent)

[0168] Adhesive composition disclosed herein can be mainly for the purpose of crosslinking in the adhesive layer or the crosslinking of the adhesive layer and its adjacent surface, and contains a crosslinking agent as required. The type of crosslinking agent is not particularly limited, and can be selected from the crosslinking agents known in the past, for example, according to the composition of the adhesive composition, in the mode in which the crosslinking agent plays a suitable crosslinking function in the adhesive layer. As usable crosslinking agents, isocyanate crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, carbodiimide crosslinking agents, melamine crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, hydrazine crosslinking agents, amine crosslinking agents, etc. can be exemplified. These can be used alone, or two or more can be used in combination.

[0169] The content of the crosslinking agent (in the case of two or more crosslinking agents, it is the total amount thereof) is not particularly limited. From the viewpoint of an adhesive that can achieve good balance in adhesive properties such as adhesive force and cohesive force, the content of the crosslinking agent is preferably about 5 parts by weight or less, more preferably about 0.001 to 5 parts by weight, still more preferably about 0.001 to 4 parts by weight, and further preferably about 0.001 to 3 parts by weight, relative to 100 parts by weight of the monomer components of the polymer contained in the adhesive layer (for example, an acrylic polymer or the monomer components of the polymer). Alternatively, an adhesive composition that does not contain the above crosslinking agent may also be used. When a photocurable adhesive composition is used as the adhesive composition disclosed herein, the adhesive composition may substantially not contain a crosslinking agent such as an isocyanate-based crosslinking agent. Here, the fact that the adhesive composition substantially does not contain a crosslinking agent (typically an isocyanate-based crosslinking agent) means that the amount of the crosslinking agent relative to 100 parts by weight of the above monomer components is less than 0.05 parts by weight (for example, less than 0.01 parts by weight).

[0170] In order to make the crosslinking reaction proceed more effectively, a crosslinking catalyst may also be used. Examples of the crosslinking catalyst include metal-based crosslinking catalysts such as tetra-n-butyl titanate, tetra-isopropyl titanate, iron(III) acetylacetonate (Japanese: Narsem Second Iron), butyltin oxide, and dioctyltin dilaurate. Among them, tin-based crosslinking catalysts such as dioctyltin dilaurate are preferred. The amount of the crosslinking catalyst used is not particularly limited. The amount of the crosslinking catalyst used relative to 100 parts by weight of the monomer components of the polymer in the adhesive layer (for example, an acrylic polymer or the monomer components of the polymer) may be, for example, about 0.0001 parts by weight or more and 1 part by weight or less, may be 0.001 parts by weight or more and 0.1 part by weight or less, or may be 0.005 parts by weight or more and 0.5 part by weight or less.

[0171] In the adhesive composition used for the formation of the adhesive layer, a compound that produces keto-enol tautomerism can be contained as a crosslinking retarder as desired. For example, in an adhesive composition containing an isocyanate crosslinking agent or an adhesive composition that can be used in combination with an isocyanate crosslinking agent, a compound that produces keto-enol tautomerism can be preferably used. Thus, the effect of extending the pot life of the adhesive composition can be exerted. The compound that produces keto-enol tautomerism can be used alone or in combination of two or more. With respect to 100 parts by weight of the monomer component (for example, an acrylic polymer or a monomer component of the polymer) of the polymer forming the adhesive layer, the amount of the compound that produces keto-enol tautomerism can be, for example, 0.1 parts by weight or more and 20 parts by weight or less, 0.5 parts by weight or more and 15 parts by weight or less is appropriate, for example, 1 part by weight or more and 10 parts by weight or less, or 1 part by weight or more and 5 parts by weight or less.

[0172] (Tackifying resin)

[0173] The adhesive layer may contain a tackifying resin. Examples of the tackifying resin include rosin-based tackifying resins (including rosin derivative tackifying resins), petroleum-based tackifying resins, terpene-based tackifying resins, phenol-based tackifying resins, ketone-based tackifying resins, etc. These may be used alone or in combination of two or more.

[0174] In some embodiments of the adhesive sheet disclosed herein, as the tackifying resin, one or more selected from rosin-based tackifying resins, rosin derivative tackifying resins, and terpene phenol resins can be preferably used. Among them, rosin derivative tackifying resins are preferred, and preferred examples include rosin esters such as stabilized rosin esters and polymerized rosin esters.

[0175] The softening point of the tackifier resin is not particularly limited. From the viewpoint of suppressing the reduction of the cohesive force of the adhesive layer, it is preferred to use a tackifier resin with a softening point of 80°C or more. The softening point of the tackifier resin can be above 90°C, above 100°C, above 110°C, or above 120°C. A tackifier resin with a softening point of 130°C or above or 140°C can be used. In addition, from the viewpoint of transparency and adhesion to the adherend, a tackifier resin with a softening point of 200°C or below or 180°C or below can be preferably used. It should be noted that the softening point of the tackifier resin referred to herein can be a nominal value recorded in a document, a catalogue, etc. In the absence of a nominal value, the softening point of the tackifier resin can be determined based on the softening point test method (ring and ball method) specified in JIS K5902 or JIS K2207.

[0176] From the viewpoint of suitably exerting the use effect of tackifying resin, relative to 100 weight parts of monomer components of the polymer contained in the adhesive layer, the use amount of tackifying resin is appropriate to be more than 1 weight part, can be more than 5 weight parts, can be more than 10 weight parts, can be more than 15 weight parts, can be more than 20 weight parts, can be more than 25 weight parts. In addition, from the viewpoint of realizing the adhesion and cohesion of the adherend well in balance at the same time, the use amount of tackifying resin relative to 100 weight parts of monomer components can be, for example, less than 70 weight parts, can be less than 50 weight parts, can be less than 40 weight parts. Or, relative to 100 weight parts of the above-mentioned monomer components, the content of the above-mentioned tackifying resin in the adhesive layer is, for example, less than 10 weight parts, and further can be less than 5 weight parts. The content of the above-mentioned tackifying resin can be less than 1 weight part (for example, less than 0.5 weight part), can be less than 0.1 weight part (for 0 weight parts or less than 0.1 weight part), and the above-mentioned adhesive layer can also not substantially include tackifying resin.

[0177] (Acrylic oligomer)

[0178] In the adhesive layer disclosed herein, from the viewpoints of improving cohesion, improving adhesion to the surface adjacent to the adhesive layer (for example, the surface of the support layer, etc.), an acrylic acid oligomer may be contained. As the acrylic acid oligomer, a polymer having a Tg higher than the Tg of the above-mentioned acrylic acid polymer is preferably used. For example, in the method of utilizing ultraviolet irradiation when making the adhesive layer, acrylic acid oligomers are suitable because they are not easy to cause inhibition.

[0179] The Tg of the acrylic oligomer is not particularly limited, and may be, for example, above about 20°C and below 300°C. The Tg may be, for example, above about 30°C, above about 40°C, above about 60°C, above about 80°C, or above about 100°C. When the Tg of the acrylic oligomer becomes higher, the effect of improving the cohesive force tends to be generally better. In addition, from the viewpoints of anchoring with the support layer, impact absorption, etc., the Tg of the acrylic oligomer may be, for example, below about 250°C, below about 200°C, below about 180°C, or below about 150°C. It should be noted that the Tg of the acrylic oligomer is the same as the Tg of the acrylic polymer corresponding to the above-mentioned monomer component composition, and is a value calculated based on the Fox formula.

[0180] The Mw of acrylic acid oligomers can be typically about 1000 or more and less than about 30000, preferably about 1500 or more and less than about 10000, more preferably about 2000 or more and less than about 5000. When Mw is within the above range, it is easy to appropriately exert the effect of improving cohesion and adhesion to adjacent surfaces. With regard to the Mw of acrylic acid oligomers, gel permeation chromatography (GPC) can be utilized to measure and obtain as a value converted by standard polystyrene. Specifically, in HPLC8020 manufactured by Tosoh Corporation, 2 TSKgel GMH-H (20) are used as columns, tetrahydrofuran solvent is utilized, and measurement is performed under the condition of a flow rate of about 0.5 mL / minute.

[0181] Examples of the monomer components constituting the acrylic oligomer include the following (meth)acrylate monomers: the various (meth)acrylate monomers described above; 1-20 Alkyl esters; the above-mentioned various alicyclic hydrocarbon group-containing (meth)acrylates; the above-mentioned various aromatic hydrocarbon group-containing (meth)acrylates; (meth)acrylates obtained from terpene compound derivative alcohols; etc. These can be used alone or in combination of two or more.

[0182] Preferred acrylic oligomers include, for example, homopolymers of dicyclopentanyl methacrylate (DCPMA), cyclohexyl methacrylate (CHMA), isobornyl methacrylate (IBXMA), isobornyl acrylate (IBXA), dicyclopentanyl acrylate (DCPA), 1-adamantyl methacrylate (ADMA), and 1-adamantyl acrylate (ADA); copolymers of DCPMA and MMA, copolymers of DCPMA and IBXMA, copolymers of ADA and methyl methacrylate (MMA), copolymers of CHMA and isobutyl methacrylate (IBMA), copolymers of CHMA and IBXMA, copolymers of CHMA and acryloylmorpholine (ACMO), copolymers of CHMA and diethylacrylamide (DEAA), and copolymers of CHMA and AA.

[0183] Acrylic acid oligomers can be formed by polymerizing the monomer components constituting the acrylic acid oligomers. The polymerization method and polymerization mode are not particularly limited, and various polymerization methods known in the past (e.g., solution polymerization, emulsion polymerization, bulk polymerization, photopolymerization, radiation polymerization, etc.) can be used in an appropriate manner. The type of polymerization initiator (e.g., azo polymerization initiator) that can be used as needed is roughly as exemplified for the synthesis of acrylic acid polymers, and the amount of polymerization initiator and the amount of chain transfer agent (e.g., mercaptan) that can be used are appropriately set in a manner to obtain the desired molecular weight based on technical common sense, and therefore detailed description is omitted.

[0184] When the adhesive layer contains an acrylic oligomer, the content thereof may be, for example, 0.01 parts by weight or more relative to 100 parts by weight of the above-mentioned base polymer (typically an acrylic polymer), and may be 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.2 parts by weight or more from the viewpoint of obtaining a higher effect. In addition, from the viewpoint of compatibility with the base polymer, it is appropriate that the content of the above-mentioned acrylic oligomer is less than 50 parts by weight, preferably less than 30 parts by weight, more preferably less than 25 parts by weight, for example less than 10 parts by weight, less than 5 parts by weight, or less than 1 part by weight.

[0185] (Silane coupling agent)

[0186] The adhesive layer disclosed herein may also contain a silane coupling agent. In the method of containing a silane coupling agent, the silane coupling agent is preferably contained in the adhesive composition (and thus the adhesive layer) in a free form. One silane coupling agent can be used alone, or two or more silane coupling agents can be used in combination. The amount of silane coupling agent contained in the adhesive layer disclosed herein can be set in a manner to obtain the desired effect of use, without particular limitation. In addition, the technology disclosed herein can be implemented in a manner using an adhesive composition that does not substantially contain a silane coupling agent. By limiting the use of a silane coupling agent or not using a silane coupling agent, the adhesive force can be suppressed from increasing over time, and good water removability can be easily obtained.

[0187] (Photopolymerization Initiator)

[0188] The adhesive layer of the adhesive sheet disclosed herein may contain a photopolymerization initiator as required for the purpose of improving or imparting photocurability. As the photopolymerization initiator, the same as the photopolymerization initiator exemplified as the photopolymerization initiator that can be used in the synthesis of acrylic polymers, ketal photopolymerization initiators, acetophenone photopolymerization initiators, benzoin ether photopolymerization initiators, acylphosphine oxide photopolymerization initiators, α-acetone alcohol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzyl photopolymerization initiators, benzophenone photopolymerization initiators, thioxanthone photopolymerization initiators, etc. can be used. One type of photopolymerization initiator can be used alone, or two or more types can be used in combination as appropriate.

[0189] The content of the photopolymerization initiator in the adhesive layer is not particularly limited and can be set in a manner that appropriately exerts the desired effect. In some embodiments, the content of the photopolymerization initiator can be, for example, about 0.005 parts by weight or more, 0.01 parts by weight or more is appropriate, and 0.05 parts by weight or more is also appropriate relative to 100 parts by weight of the acrylic polymer. By increasing the content of the photopolymerization initiator, the photocurability of the adhesive layer is improved. In addition, the content of the photopolymerization initiator relative to 100 parts by weight of the acrylic polymer is appropriate to be 5 parts by weight or less, preferably 1 part by weight or less, and can be 0.5 parts by weight or less, and can also be 0.1 parts by weight or less. From the viewpoint of improving the storage stability of the adhesive sheet (for example, stability against light degradation), it is advantageous if the content of the photopolymerization initiator is not too much.

[0190] Typically, the adhesive layer containing a photopolymerization initiator can be formed using the adhesive composition containing the photopolymerization initiator (e.g., a solvent-based adhesive composition). The adhesive composition containing a photopolymerization initiator can be prepared, for example, by mixing the other components used in the composition with the photopolymerization initiator. In addition, when an acrylic polymer synthesized (photopolymerized) in the presence of a photopolymerization initiator is used to prepare the adhesive composition, the residue (unreacted product) of the photopolymerization initiator used when synthesizing the acrylic polymer can be used as part or all of the photopolymerization initiator contained in the adhesive layer. The same is true for the case of using an acrylic oligomer synthesized in the presence of a photopolymerization initiator as an acrylic oligomer used as needed. From the perspective of ease of preparation management, in some embodiments, the adhesive layer can be formed using an adhesive composition prepared by newly adding the above-mentioned amount of photopolymerization initiator to other constituent components.

[0191] (Other ingredients)

[0192] The adhesive layer disclosed herein may contain various additives commonly used in the field of adhesives such as viscosity modifiers (e.g., thickeners), leveling agents, plasticizers, fillers, colorants such as pigments and dyes, stabilizers, preservatives, and anti-aging agents as other optional components as needed. Such various additives may be conventionally used, and since they are not particularly characterized in the present invention, detailed descriptions thereof are omitted.

[0193] In the technology disclosed herein, the amount of components other than the base polymer (suitably an acrylic polymer) in the adhesive layer can be limited. In the technology disclosed herein, the amount of components other than the base polymer in the adhesive layer is, for example, about 30% by weight or less, about 15% by weight or less is appropriate, preferably about 12% by weight or less (for example, about 10% by weight or less). The adhesive layer of such a composition is easy to meet the specified optical properties (such as transparency) and can be preferably used for optical purposes. In some ways, the amount of components other than the base polymer in the adhesive layer can be about 5% by weight or less, about 3% by weight or less, or about 1.5% by weight or less (for example, about 1% by weight or less). The composition in which the amount of components other than the base polymer (such as an acrylic polymer) is limited in this way can be preferably used for a photocurable adhesive composition.

[0194] (Formation of Adhesive Layer)

[0195] The adhesive layer constituting the adhesive sheet disclosed herein may be a cured layer of an adhesive composition. That is, the adhesive layer may be formed in the following manner: after the adhesive composition is imparted (e.g., applied) to an appropriate surface, a curing treatment is appropriately implemented. In the case of performing two or more curing treatments (drying, crosslinking, polymerization, etc.), they may be performed simultaneously or in multiple stages.

[0196] In the adhesive composition using the partial polymer of monomer components (acrylic polymer slurry), typically, as the above-mentioned curing treatment, a final copolymerization reaction is carried out. That is, the partial polymer is supplied to a further copolymerization reaction to form a complete polymer. For example, if it is a photocurable adhesive composition, light irradiation is implemented. As required, curing treatments such as crosslinking and drying can be implemented. For example, in the case where it is necessary to dry in the form of a photocurable adhesive composition (for example, in the case of a photocurable adhesive composition in which the partial polymer of the monomer components is dissolved in the form of an organic solvent), light curing can be carried out after the composition is dried.

[0197] In the adhesive composition using a fully polymerized product, typically, as the above-mentioned curing treatment, drying (heat drying), crosslinking and the like are performed as required. In the case of a solvent-based adhesive composition to which photocurability (photocrosslinkability) is imparted by the addition of a multifunctional monomer, photocuring can be performed after the composition is dried. Here, the so-called drying of the above-mentioned composition can be after the adhesive sheet obtained by the above-mentioned drying is attached to the adherend. The adhesive sheet disclosed herein can be used in the following manner: by using a method including a step of photocuring it after being attached to the adherend, the adhesive sheet is attached to the above-mentioned adherend.

[0198] The adhesive layer of the multilayer structure of more than two layers can be made by laminating a preformed adhesive layer. Alternatively, an adhesive composition can be applied to the preformed first adhesive layer, and the adhesive composition can be cured to form a second adhesive layer. When the adhesive layer of the adhesive sheet used in a pasting mode of laminating to an adherend and then photocuring is a multilayer structure, the above-mentioned adhesive layer to be photocured can be a partial layer (e.g., a layer) included in the above-mentioned multilayer structure, or it can be all layers.

[0199] The coating of the adhesive composition can be carried out using a conventional coating machine such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a rod coater, a knife coater, a spray coater, etc. For the adhesive sheet having a support layer, as a method for providing the adhesive layer on the support layer, a direct method of directly applying the adhesive composition to the support layer to form the adhesive layer can be used, and a transfer method of transferring the adhesive layer formed on the release surface to the support layer can also be used.

[0200] (Thickness of adhesive layer)

[0201] The thickness of the adhesive layer is not particularly limited, and for example, it can be about 3 μm to 2000 μm. From the perspective of step tracking and adhesion to the adherend, in some embodiments, the thickness of the adhesive layer can be, for example, 5 μm or more, and 10 μm or more is appropriate, preferably 20 μm or more, and more preferably 30 μm or more. In some embodiments, the thickness of the adhesive layer can be 50 μm or more, can exceed 50 μm, can be 70 μm or more, can be 100 μm or more, and can be 120 μm or more. In addition, from the perspective of preventing the occurrence of slurry residue caused by cohesive failure of the adhesive layer, in some embodiments, the thickness of the adhesive layer can be, for example, less than 1000 μm, less than 700 μm, less than 500 μm, less than 300 μm, and further less than 200 μm or less than 170 μm. As for the technology disclosed herein, it can also be appropriately implemented in the form of an adhesive sheet in which the thickness of the adhesive layer can be 130 μm or less, 90 μm or less, or 60 μm or less (for example, 40 μm or less). According to the technology disclosed herein, the adhesive sheet can be peeled off under a small load by utilizing water peelability when peeling and removing, so that even if the thickness of the adhesive layer is limited, it is possible to prevent the occurrence of undesirable conditions such as tearing due to insufficient strength. As for the adhesive sheet disclosed herein, when each side of the intermediate layer has an adhesive layer, the thickness of the two adhesive layers can be the same or different.

[0202] <Middle Layer>

[0203] Some forms of adhesive sheets can be adhesive sheets having an intermediate layer between the first and second adhesive layers disposed on the surface constituting the adhesive sheet. In the technology disclosed herein, the intermediate layer is not particularly limited, and can be a support (support layer) that supports the adhesive layer as described later, or a viscoelastic layer (which can be an adhesive) disposed on the back of the above-mentioned adhesive layer disclosed herein. By having an intermediate layer, an adhesive sheet that can satisfactorily exert the effect brought by the technology disclosed herein can be obtained.

[0204] (Stress at 100% elongation of the middle layer)

[0205] In the mode in which the adhesive sheet has an intermediate layer, it is appropriate that the stress of the intermediate layer at 100% elongation is less than 30MPa. Thus, the stress of the adhesive sheet at 100% elongation can be less than 30MPa. It is appropriate that the stress at 100% elongation is 15MPa or less, for example, it can also be 10MPa or less. In some modes, the stress at 100% elongation of the intermediate layer is preferably 7MPa or less, more preferably 5MPa or less, and further preferably 3MPa or less. In some preferred modes, the stress at 100% elongation of the intermediate layer is 1.0MPa or less, can be 0.7MPa or less, can be 0.5MPa or less, can be 0.3MPa or less, and can also be 0.20MPa or less. The lower limit of the stress at 100% elongation is not particularly limited. From the perspective of the pasting operability of the adhesive sheet and the prevention of tearing, it is appropriate to be 0.01MPa or more, for example, it can be 0.05MPa or more, and it can also be 0.10MPa or more.

[0206] (Stress at 500% elongation of the middle layer)

[0207] Although not particularly limited, the stress of the middle layer at 500% elongation can be 50MPa or less (for example, 30MPa or less). An adhesive sheet having such an intermediate layer tends to have excellent stretching removability. It is appropriate that the stress at 500% elongation is 15MPa or less, for example, it can also be 10MPa or less. In some embodiments, the stress of the middle layer at 500% elongation is preferably 7MPa or less, can be 5MPa or less, or can be 3MPa or less (for example, 1.0MPa or less). The lower limit of the stress at 500% elongation is not particularly limited. From the perspective of the adhesive sheet's pasting operability and tear prevention, it is appropriate to be 0.05MPa or more, for example, it can be 0.10MPa or more, or 0.50MPa or more.

[0208] (fracture stress σf of the middle layer)

[0209] In the technology disclosed herein, from the perspective of preventing tearing during stretching, the fracture stress σf of the intermediate layer can be 0.10MPa or more, 0.20MPa or more (for example, 0.30MPa or more) is appropriate, can be 0.50MPa or more, can be 0.80MPa or more, can be 1.00MPa or more, and can also be 1.20MPa or more (for example, 1.50MPa or more). The adhesive sheet having the intermediate layer with the above-mentioned fracture stress σf has a tendency to be excellent in processability. In some embodiments, the above-mentioned fracture stress σf can be 2.0MPa or more, can be 3.0MPa or more, can be 10MPa or more, and can also be 20MPa or more (for example, 25MPa or more). The upper limit of the fracture stress σf of the intermediate layer is not particularly limited, and can be 200MPa or less, and 150MPa or less is appropriate, can be 100MPa or less, and can also be 30MPa or less. In some embodiments, the breaking stress σf of the adhesive sheet can be 50MPa or less. From the perspective of obtaining suitable elongation, it is appropriate to be 15MPa or less. It can be 8MPa or less, or 6MPa or less (for example, 5MPa or less). In some embodiments, the above-mentioned breaking stress σf can be 3.00MPa or less, or 2.00MPa or less. According to the technology disclosed herein, the adhesive sheet can be peeled off under a small load by utilizing water peelability when peeling and removing, so that the above-mentioned breaking strength σf can be prevented without excessively increasing it. In other words, it can prevent tearing and other undesirable conditions caused by insufficient strength by having a structure with a lower breaking stress σf.

[0210] (fracture strain εf of the middle layer)

[0211] In the technology disclosed herein, from the viewpoint of making the water-peelable property have suitable elongation, the fracture strain εf (elongation at fracture) of the intermediate layer may be 150% or more, 250% or more (e.g., 280% or more) is appropriate, preferably 300% or more, more preferably 400% or more, further preferably 500% or more, 600% or more, 800% or more, or 1000% or more (e.g., 1500% or more). The upper limit of the fracture strain εf is not particularly limited, and from the viewpoint of having suitable strength, good tear resistance, workability, and operability, for example, it may be 2000% or less, 1200% or less, 1000% or less, 900% or less, or 800% or less.

[0212] The above mechanical properties of the intermediate layer (stress at 100% elongation, stress at 500% elongation, fracture stress σf and fracture strain εf) are measured by a tensile test performed at a tensile speed of 100 mm / min. Specifically, the mechanical properties of the adhesive sheet are measured in the same manner as the method for measuring the mechanical properties (tensile test) described in the examples described later. The above mechanical properties can be set and adjusted by appropriately selecting the type of intermediate layer material, the molding method, etc. based on the contents described in this specification.

[0213] As the middle layer, various materials of the adhesive sheet that can realize the display of the specified mechanical properties can be used. As the above-mentioned middle layer, for example, a resin film can be preferably used. As the above-mentioned middle layer, an elongated fabric or non-woven fabric can be used. The above-mentioned resin film can be a non-foamed resin film, a rubber film, a foam film, etc. Among them, preferably a non-foamed resin film and a rubber film, more preferably a non-foamed resin film. The non-foamed resin film does not substantially have bubbles (holes) that can become a weakness in terms of mechanical strength, and has a tendency to be excellent in mechanical strength such as tensile strength compared to the foam. In addition, the non-foamed resin film is also excellent in terms of processability, dimensional stability, thickness accuracy, economy (cost), etc.

[0214] It should be noted that the "resin film" in this specification is a substantially non-porous film, which is different from the concept of so-called non-woven fabrics and fabrics (i.e., does not include the concept of non-woven fabrics and fabrics). In addition, the so-called non-foamed resin film refers to a resin film that has not been intentionally treated to form a foamed body. Specifically, the non-foamed resin film can be a resin film with a foaming ratio of less than 1.1 times (for example, less than 1.05 times, typically less than 1.01 times).

[0215] Preferred examples of resin materials constituting the resin film that can become the intermediate layer include acrylic resins such as acrylic copolymers; polyurethane resins such as ether polyurethane, ester polyurethane, and carbonate polyurethane; urethane (meth) acrylate polymers; polyolefin resins such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-butylene copolymer; polyester resins such as polybutylene terephthalate (PBT); polycarbonate resins; vinyl chloride resins (PVC) such as soft polyvinyl chloride; silicones such as silicone rubber; and the like. The above-mentioned resin materials can be styrene copolymers (typically styrene elastomers) such as styrene butadiene copolymers, styrene isoprene copolymers, styrene ethylene butene copolymers, styrene ethylene propylene copolymers, styrene butadiene styrene copolymers, and styrene isoprene styrene copolymers, and acrylic rubbers. The above-mentioned resin materials can be used alone or in combination of two or more. It should be noted that the above-mentioned resin materials contain substances generally referred to as rubber and thermoplastic elastomers.

[0216] In some preferred embodiments, the middle layer is formed by an acrylic resin. By using an acrylic resin, it is easy to obtain an middle layer with high transparency and suitable for optical purposes. For example, an acrylic block copolymer having a hard segment (A) and a soft segment (B) in one molecule can be preferably used. The so-called hard segment (A) refers to a relatively hard block in the structure of the acrylic block copolymer in terms of the relationship with the soft segment (B) in the acrylic copolymer. In addition, the so-called soft segment (B) refers to a relatively soft block in the structure of the acrylic block copolymer in terms of the relationship with the hard segment (A). One acrylic block copolymer can be used alone, or two or more can be used in combination.

[0217] As the acrylic block copolymer, an acrylic block copolymer having at least one acrylate block (hereinafter also referred to as Ac block) and at least one methacrylate block (hereinafter also referred to as MAc block) can be preferably used. For example, a block copolymer having a structure in which Ac blocks and MAc blocks are alternately arranged is preferred.

[0218] Examples of the alkyl acrylate constituting the Ac block include alkyl acrylates having an alkyl group with carbon atoms of 1 to 20 (preferably 4 to 14, for example 6 to 12). Examples include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate (2EHA), nonyl acrylate, isononyl acrylate, decyl acrylate, dodecyl acrylate, stearyl acrylate, etc. These may be used alone or in combination of two or more.

[0219] Examples of the alkyl methacrylate constituting the MAc block include alkyl methacrylates having an alkyl group with 1 to 20 carbon atoms (preferably 1 to 14). Specific examples thereof include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-heptyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, isononyl methacrylate, decyl methacrylate, dodecyl methacrylate, and stearyl methacrylate. These may be used alone or in combination of two or more.

[0220] The acrylic block copolymer may be an AB type, ABA type, ABAB type, ABABA type or the like, in which A blocks (hard segments (A)) of polymers having a hard structure with excellent cohesion and elasticity and B blocks (soft segments (B)) of polymers having a soft structure with excellent viscosity are alternately arranged.

[0221] As the hard segment (A), the MAc block as described above can be preferably used. As the soft segment (B), the Ac block as described above can be preferably used. In some preferred embodiments, the acrylic block copolymer is a triblock copolymer of the structure of MAc block-Ac block-MAc block (ABA type). For example, a triblock copolymer in which two MAc blocks have substantially the same monomer composition can be preferably used.

[0222] The weight ratio of the hard segment (A) to the soft segment (B) contained in the acrylic block copolymer is not particularly limited. For example, the weight ratio (A / B) of the hard segment (A) / soft segment (B) may be in the range of 4 / 96 to 90 / 10, and the range of 7 / 93 to 70 / 30 is appropriate, and the range of 10 / 90 to 50 / 50 (e.g., 15 / 85 to 40 / 60) is preferred.

[0223] In the technology disclosed herein, the weight average molecular weight (Mw) of the acrylic block copolymer is not particularly limited, and for example, a block copolymer having a Mw of 3×10 4 ~30×10 4 The acrylic block copolymer preferably has a Mw of 3.5×10 4 ~25×10 4 The range is about 4×10 4 ~20×10 4 (For example, 4.5×10 4 ~15×10 4 ). By making the Mw of the acrylic block copolymer an appropriate range, it is easy to obtain the target elongation and strength. It should be noted that the Mw of the acrylic block copolymer referred to herein is a value calculated in terms of polystyrene obtained by GPC measurement of a sample prepared by dissolving the copolymer in tetrahydrofuran (THF). Specifically, the above-mentioned GPC measurement can be implemented, for example, using "HLC-8120GPC" manufactured by Tosoh Corporation as a GPC measurement device.

[0224] The acrylic block copolymer as described above can be synthesized by a known method (for example, see Japanese Patent Application Publication No. 2001-234146, Japanese Patent Application Publication No. 11-323072), or can be purchased and used as a commercial product. Examples of the commercial products include the trade names "KURARITY LA" series and "KURARITY LK" series manufactured by KURARAY CO., LTD, and the trade name "NABSTAR" manufactured by Kaneka Corporation. As a method for synthesizing the acrylic block copolymer, a method using a living polymerization method can be preferably adopted.

[0225] In some other embodiments, the acrylic resin layer that can be used as the intermediate layer can be formed by the same method as the adhesive layer formed by the acrylic adhesive. Using the material that can be used for the above-mentioned adhesive layer, an intermediate layer with a predetermined elongation and strength can be formed. The details are the same as those of the adhesive layer, so repeated description is omitted.

[0226] In some other preferred embodiments, the middle layer is formed by a polyurethane resin film. The so-called polyurethane resin film here refers to a resin film containing polyurethane as the main component of the resin component (the component with the highest mixing ratio, typically a component contained in excess of 50% by weight. The same below). Typically, the polyurethane resin film is composed of a material that does not substantially exhibit a yield point, and is a film material for an adhesive sheet that is easy to achieve a specified breaking strength and elongation. In addition, since the polyurethane resin film can achieve good physical properties even without adding additives such as plasticizers, it can also be a preferred middle layer material in terms of preventing the seepage of the above-mentioned additives.

[0227] The proportion of polyurethane in the resin components contained in the polyurethane resin film is preferably 70% by weight or more (for example, 80% by weight or more, typically 90% by weight or more and 100% by weight or less). The polyurethane resin film disclosed herein can be a film formed by a polymer blend of polyurethane and other resins. The above-mentioned other resins can be, for example, one or more of acrylic resins, polyolefins, polyesters, polycarbonates, etc. Alternatively, the technology disclosed herein can also be implemented in a manner using an intermediate layer that does not substantially contain a resin component other than polyurethane. It should be noted that the above-mentioned polyurethane is a polymer compound that can be synthesized by polyaddition reaction of polyols (such as diols) and polyisocyanates (such as diisocyanates) in an appropriate ratio. It should be noted that the NCO / OH ratio of the polyurethane can be appropriately set to obtain the desired mechanical properties.

[0228] The polyurethane resin as described above can be used by molding a resin synthesized by a known method into a film, or can be used by purchasing a commercial product. Examples of the commercial products include the product name "ESMER URS" series manufactured by Nihon Matai Co., Ltd., polyurethane resins and polyurethane resin films that can be purchased from KURABO INDUSTRIES LTD.

[0229] In some other preferred embodiments, the intermediate layer is formed by a resin film containing a carbamate (meth) acrylate polymer. As the carbamate (meth) acrylate polymer disclosed herein, a polymer containing a structural unit derived from a carbamate (meth) acrylate can be used. The so-called carbamate (meth) acrylate here refers to a compound having a carbamate bond and a (meth) acryloyl group in one molecule, and the compound can be used without particular limitation. One type of carbamate (meth) acrylate can be used alone, or two or more types can be used in combination. The carbamate (meth) acrylate preferably has two or more carbamate bonds and two or more (meth) acryloyl groups. The number of (meth) acryloyl groups possessed by the carbamate (meth) acrylate is preferably 2 to 5, and more preferably 2 to 3. For example, a carbamate (meth) acrylate having two (meth) acryloyl groups can be preferably used. In addition, the carbamate (meth) acrylate is preferably a carbamate acrylate. The term “urethane acrylate” herein refers to a urethane acrylate in which the ratio of the number of acryloyl groups among the (meth)acryloyl groups contained in the urethane (meth)acrylate exceeds 50%.

[0230] The urethane (meth) acrylate polymer can be synthesized by a known method. As the urethane (meth) acrylate, various commercially available urethane (meth) acrylates can be used. For example, the trade name "UV-3300B" manufactured by Nippon Synthetic Chemical Industry Co., Ltd., the trade name "BEAMSET505A-6" manufactured by Arakawa Chemical Industries, Ltd., etc. can be preferably used.

[0231] In some other preferred embodiments, the middle layer is formed by a PVC-based resin film. The above-mentioned PVC-based resin film is made by molding a PVC-based resin composition (molding material) containing a PVC-based resin into a film shape. The so-called PVC-based resin composition here refers to a resin composition in which the main component (i.e., more than 50% by weight) among the resin components (polymer components) is a PVC-based resin (typically PVC). About 80% by weight or more (more preferably about 90% by weight or more) of the total amount of the resin components contained in the PVC-based resin composition is preferably a PVC-based resin. It is also possible that the resin components are substantially all PVC. Based on the PVC-based resin composition, a PVC-based resin film showing physical properties suitable for the middle layer can be formed.

[0232] In some other embodiments, the middle layer is formed by an organosilicon film. As the material of the organosilicon film, an organosilicon rubber is preferred. The organosilicon rubber is a polysiloxane having a cross-linked structure and rubber-like properties. The organosilicon rubber can be prepared by reacting a polysiloxane as a precursor of the organosilicon rubber. For example, the organosilicon rubber can be an organosilicon rubber formed by reacting an organosilicon rubber precursor containing an alkenyl-containing polyorganosiloxane and an organohydrogenpolysiloxane using a catalyst or the like. As the organosilicon, an organosilicon synthesized by a known method can be used, or a commercially available product can be used. Various commercially available organosilicon rubbers can be used. For example, the product name "KEIJU" series manufactured by Mitsubishi Chemical Corporation can be preferably used.

[0233] In some embodiments, the middle layer can be a layer formed by a polyolefin resin. As a polyolefin resin, one polyolefin can be used alone or in combination with two or more polyolefins. The polyolefin can be, for example, a homopolymer of an α-olefin, a copolymer of two or more α-olefins, a copolymer of one or more α-olefins and other vinyl monomers, etc. As a specific example, polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene rubber (EPR) and other ethylene-propylene copolymers, ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, ethylene-ethyl acrylate copolymers, etc. can be cited. Low-density (LD) polyolefins and high-density (HD) polyolefins can be used.

[0234] In some other embodiments, the middle layer can be a layer formed by an elastic system resin film. The elastic system resin film here refers to a resin film having an elastomer layer. The above-mentioned elastomer layer may contain any appropriate resin within the range of the elongation and strength that can achieve the target. As examples of such resins, olefin elastomers, styrene elastomers, etc. can be cited. Preferably, the elastomer layer contains an olefin elastomer. By making the elastomer layer contain an olefin elastomer, an elastic system resin film showing physical properties suitable for being the middle layer of the adhesive sheet disclosed herein can be formed. As a specific example of a suitable olefin elastomer, an α-olefin elastomer can be cited. As preferred α-olefin elastomers, ethylene elastomers, propylene elastomers and 1-butene elastomers can be cited.

[0235] The α-olefin elastomer can be purchased from a commercial product, such as the "TAFMER" series manufactured by Mitsui Chemicals and the "Vistamaxx" series manufactured by Exxon Mobil. An appropriate α-olefin elastomer can be selected from these products and used.

[0236] In some other embodiments, the middle layer may be a foam film formed of a foam of a plastic material (plastic foam). Specific examples of plastic foams include: polyolefin resin foams; polyester resin foams; polyvinyl chloride resin foams; vinyl acetate resin foams; polyphenylene sulfide resin foams; amide resin foams such as aliphatic polyamide (nylon) resin foams and fully aromatic polyamide (aramid) resin foams; polyimide resin foams; polyetheretherketone (PEEK) foams; styrene resin foams such as polystyrene foams; urethane resin foams such as polyurethane resin foams; and the like. In addition, as the plastic foam, rubber resin foams such as polychloroprene rubber foams may also be used.

[0237] As a preferred foam, a polyolefin resin foam (hereinafter also referred to as "PO foam") can be exemplified. As the plastic material constituting the PO foam (i.e., the polyolefin resin), various known or customary polyolefin resins can be used without particular limitation. For example, polyethylene such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, etc. can be cited. As an example of LLDPE, linear low-density polyethylene of the Ziegler-Natta catalyst system, linear low-density polyethylene of the metallocene catalyst system, etc. can be cited. The polyolefin resins can be used alone or in combination of two or more. In some embodiments, a PO foam substantially composed of a foam of a polyethylene resin or a polypropylene resin can be preferably used. The polyethylene resin herein refers to a resin with ethylene as the main monomer (i.e., the main component among monomers), and may include ethylene-propylene copolymers and ethylene-vinyl acetate copolymers in which the copolymerization ratio of ethylene exceeds 50% by weight, in addition to HDPE, LDPE, and LLDPE. Similarly, the polypropylene resin refers to a resin with propylene as the main monomer. Among them, polyethylene foam is preferred.

[0238] The method for producing the polyolefin foam as described above is not particularly limited, and various known methods can be appropriately adopted. For example, it can be produced by a method including a molding process, a crosslinking process and a foaming process of the corresponding polyolefin resin. In addition, an extension process can be included as required. As a method for crosslinking the polyolefin foam, for example, a chemical crosslinking method using an organic peroxide or the like, or an ionizing radiation crosslinking method irradiated with ionizing radiation, etc., can be cited, and the above methods can be used in combination. As the above-mentioned ionizing radiation, electron beams, α rays, β rays, γ rays, etc. can be cited. The dose of ionizing radiation is not particularly limited, and an appropriate irradiation dose can be set in consideration of the target physical properties (such as degree of crosslinking), etc.

[0239] The intermediate layer (e.g., resin film) may also be mixed with various additives such as fillers (inorganic fillers, organic fillers, etc.), colorants (pigments, dyes), anti-aging agents, antioxidants, ultraviolet absorbers, antistatic agents, lubricants, plasticizers, stabilizers, etc. as needed. For example, when a soft PVC resin film is used as the intermediate layer, the amount of plasticizer mixed is about 20 to 100 parts by weight (more preferably about 30 to 70 parts by weight) relative to 100 parts by weight of the PVC resin. The mixing ratio of various additives is usually less than 30% by weight (e.g., less than 20% by weight, typically less than 10% by weight).

[0240] The surface of the intermediate layer (e.g., resin film) may be subjected to previously known surface treatments such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, and application of a primer. Such a surface treatment may be a treatment for improving the adhesion between the intermediate layer and the adhesive layer, in other words, the anchoring of the adhesive layer to the intermediate layer. The composition of the primer is not particularly limited and can be appropriately selected from known primers. The coating thickness of the primer is not particularly limited, and a range of 0.01 μm to 1 μm is appropriate, preferably 0.1 μm to 1 μm. It should be noted that when the intermediate layer is a polyurethane resin film, due to its high surface energy, good anchoring can be obtained even without the above-mentioned surface treatment.

[0241] The intermediate layer may be a single layer structure, or a multilayer structure of 2 layers, 3 layers or more. For example, the intermediate layer may be substantially composed of the above-mentioned resin film. In addition to the above-mentioned resin film, the above-mentioned intermediate layer also includes an auxiliary layer. As examples of the above-mentioned auxiliary layer, an optical property adjustment layer (such as a coloring layer, an anti-reflection layer), a printing layer for giving the adhesive sheet a desired appearance, a laminating layer, an antistatic layer, a primer layer, a peeling layer and other surface treatment layers can be cited.

[0242] The manufacturing method of the intermediate layer is not particularly limited as long as it appropriately adopts the film forming method known in the past. When using resin film as the intermediate layer, for example, extrusion molding, inflation molding, T-die casting molding, calendering roll molding, etc., can be appropriately adopted. Common film forming methods known in the past.

[0243] The thickness of the intermediate layer is not particularly limited and can be appropriately selected according to the purpose. The thickness of the intermediate layer is, for example, 10 μm or more, 20 μm or more (for example, 30 μm or more) is appropriate, preferably 50 μm or more, more preferably 70 μm or more, and can also be 100 μm or more (for example, 120 μm or more). The intermediate layer with the above thickness can become a layer that is less likely to tear and has excellent stretch removal properties. The thickness of the intermediate layer can be 1000 μm or less, 500 μm or less is appropriate, preferably 300 μm or less, more preferably 200 μm or less (for example, 150 μm or less), and can also be 120 μm or less (for example, 80 μm or less). According to the technology disclosed herein, the adhesive sheet can be peeled off under a small load by utilizing water peelability when peeling and removing, so even if the thickness of the intermediate layer is limited, it can prevent the undesirable conditions such as tearing caused by insufficient strength. In addition, reducing the thickness of the intermediate layer is advantageous in terms of filmization, miniaturization, lightweighting, and resource saving of the adhesive sheet.

[0244] <Support layer>

[0245] In the case where the adhesive sheet is single-sided adhesive, the adhesive sheet may be an adhesive sheet having a support (support layer) for supporting the adhesive layer. The support layer is basically the same as the above-mentioned intermediate layer except that it is laminated on the adhesive layer to form the back of the adhesive sheet. The usable materials, formation methods, composition (thickness, etc.), properties (such as mechanical properties), etc. may also be the range that the intermediate layer can adopt, so repeated description is omitted here.

[0246] It should be noted that the surface of the support layer that is opposite to the side bonded to the adhesive layer (hereinafter also referred to as the back side) can be subjected to a peeling treatment, a peeling treatment, an antistatic treatment, or other previously known surface treatments as needed. For example, by surface treating the back side of the support layer with a peeling agent, the unwinding force of the adhesive sheet wound into a roll can be reduced. As the peeling agent, a silicone peeling agent, a long-chain alkyl peeling agent, an olefin peeling agent, a fluorine peeling agent, a fatty acid amide peeling agent, molybdenum sulfide, silica powder, etc. can be used.

[0247] <Additional Adhesive Layer>

[0248] In the adhesive sheet disclosed herein, in addition to the above-mentioned adhesive layer, other adhesive layers may also be configured. Such an adhesive sheet may be an adhesive sheet in which the adhesive layer disclosed herein constitutes one surface (adhesive surface) of the adhesive sheet and other adhesive layers constitute the other surface (adhesive surface) of the adhesive sheet. As examples of the above-mentioned adhesive sheet, there can be cited: a double-sided adhesive sheet without a support body having a multilayer structure formed by stacking two layers of adhesive layers; a double-sided adhesive sheet in which each surface of the intermediate layer is respectively configured with an adhesive layer. The adhesive layer that can be additionally configured can be an adhesive layer composed of one or more adhesives selected from the following known various adhesives, such as acrylic adhesives, rubber adhesives (natural rubber, synthetic rubber, their mixed systems, etc.), silicone adhesives, polyester adhesives, polyurethane adhesives, polyether adhesives, polyamide adhesives, fluorine adhesives, etc. From the perspective of transparency, weather resistance, etc., in some methods, as the constituent material of the additional adhesive layer, an acrylic adhesive can be preferably used. Regarding other matters about the additional adhesive layer, the same structure as the above-mentioned adhesive layer can be adopted, or an appropriate structure can be adopted according to the application and purpose based on known or commonly used technologies and technical common sense, so detailed description is omitted here.

[0249] <Total Thickness of Adhesive Sheet>

[0250] The total thickness of the adhesive sheet disclosed herein (including an adhesive layer, an intermediate layer and a support layer, excluding a release liner) is not particularly limited, and may be 3 μm or more, 5 μm or more, and 10 μm or more is appropriate. From the perspective of the adhesion of the step difference tracking property and the like to the adherend, it is preferably 20 μm or more, and more preferably 30 μm or more. In some embodiments, the thickness of the adhesive sheet may be 50 μm or more, may be more than 50 μm, may be 70 μm or more, may be 100 μm or more, or may be 120 μm or more. An adhesive sheet having the above-mentioned thickness may become an adhesive sheet that is less prone to tearing and has excellent stretching removal properties. The upper limit of the total thickness of the adhesive sheet is, for example, 5 mm or less, may be 3 mm or less, or may be 1 mm or less. In some preferred embodiments, the thickness of the adhesive sheet is 500 μm or less, preferably 300 μm or less, more preferably 200 μm or less (e.g., 150 μm or less), or 120 μm or less (e.g., 80 μm or less). According to the technology disclosed in this article, the adhesive sheet can be peeled off under a light load by utilizing the water peeling property during peeling and removal, so even if the structure is a thin-walled structure with relatively low strength, it is possible to prevent the undesirable situation caused by insufficient strength such as tearing. In addition, reducing the thickness of the adhesive sheet is advantageous in terms of thin film, miniaturization, light weight, resource saving, etc.

[0251] <Purpose>

[0252] The purpose of the adhesive sheet disclosed herein is not particularly limited and can be used for various purposes. The adhesive sheet disclosed herein can be preferably used for various purposes that need to be reprocessed, reusable, and repairable because it can take into account both bonding reliability and peeling removal, and can contribute to improving the yield rate of products, improving production efficiency, effectively utilizing resources, reducing environmental load, and reducing the cost of users. The above-mentioned adhesive sheet can be used in the mode of pasting one of its surfaces (adhesive surface) on the adherend, and can also be used for pasting its two sides (adhesive surface) on the adherend. Wherein, it can be preferably used for the purpose of joining 2 adherends. In such a use form, the adhesive sheet can maintain a high reliability bonding state when the adherend is joined, and can utilize elongation and water peeling when peeling and removing to remove from the adherend when the load on the adherend is small, specifically, without forcing the adherend to be deformed or damaged. Remove from the adherend. More specifically, for example, when the adherend contains brittle materials, by utilizing the elongation and water peeling of the adhesive sheet, the joining state of the adherend can be released without destroying the brittle adherend. For example, even when the adherend is a low-strength rigid adherend such as a thin-walled glass plate, sufficient adhesive strength provides bonding reliability during bonding and the adherend can be peeled off without damaging the adherend.

[0253] As an example of suitable use, optical use can be cited. The adhesive sheet disclosed herein can not damage the optical properties, so while taking into account the bonding reliability and peeling removal, the special feature can be used to fix, join, shape, decorate, protect, support and other uses of the optical component by being pasted on the optical components constituting various portable devices (portable devices), automobiles, home appliances, etc. The material constituting at least the surface of the above-mentioned optical component can be, for example: glass such as alkaline glass plate and alkali-free glass; metal materials such as stainless steel (SUS) and aluminum; ceramic materials such as alumina and silica; resin materials such as acrylic resin, ABS resin, polycarbonate resin, polystyrene resin, transparent polyimide resin; and so on. The adhesive sheet disclosed herein can be pasted on the coating surface of coatings such as acrylic, polyester, alkyd resin, melamine, polyurethane, acid epoxy cross-linking, or their composite systems (such as acrylic melamine, alkyd melamine) and the plated surface of galvanized steel sheets. Preferred examples of adherends include inorganic materials such as the above-mentioned glass, the above-mentioned ceramic materials, and the above-mentioned metal materials. The adhesive sheet disclosed herein can be, for example, a constituent element of an optical component with an adhesive sheet, wherein the optical component comprises an optical component having at least a portion of its surface made of such a material and the above-mentioned adhesive sheet, and the adhesive surface of the above-mentioned adhesive sheet is bonded to the surface of the above-mentioned optical component.

[0254] Optical applications of the technology disclosed herein include, for example, bonding optical components (optical component bonding), manufacturing products using the optical components (optical products), etc. As the optical adhesive sheet used in such applications, the adhesive sheet disclosed herein can be preferably used.

[0255] The so-called optical component is a component having optical properties (e.g., polarization, light refraction, light scattering, light reflection, light transmittance, light absorption, light diffraction, optical rotation, visual recognition, etc.). As the above-mentioned optical component, as long as it is a component with optical properties, it is not particularly limited, for example, components constituting devices (optical devices) such as display devices (image display devices) and input devices or components used by these devices can be cited, for example, polarizing plates, wavelength plates, phase difference plates, optical compensation films, brightness enhancement films, light guide plates, reflective films, anti-reflective films, hard coating (HC) films, impact absorption films, anti-fouling films, photochromic films, dimming films, transparent conductive films (ITO films), design films, decorative films, surface protection plates, prisms, lenses, color filters, transparent substrates, and components stacked with them (sometimes collectively referred to as "functional films"), etc. It should be noted that the above-mentioned "plate" and "film" each include forms such as plate, film, and sheet. For example, "polarizing film" includes "polarizing plate", "polarizer", and the like.

[0256] As the above-mentioned display device, for example, a liquid crystal display device, an organic EL (electroluminescent) display device, a PDP (plasma display panel), an electronic paper, etc. can be cited. In particular, in the case of a foldable display device or a vehicle-mounted display device containing expensive components, the technology disclosed herein can be preferably applied. In addition, as the above-mentioned input device, a touch panel, etc. can be cited.

[0257] The optical components are not particularly limited, and examples thereof include components formed of glass, acrylic resin, polycarbonate, polyethylene terephthalate, metal thin film, etc. (e.g., sheet-shaped, film-shaped, plate-shaped components), etc. It should be noted that the "optical components" in this specification also include components that perform the functions of decoration and protection while maintaining the visual recognizability of display devices and input devices (design films, decorative films, surface protection films, etc.).

[0258] The adhesive sheet disclosed herein has high adhesive reliability and good peeling and removal properties, and therefore can be preferably used as an adhesive sheet for electronic devices (preferably portable electronic devices) that require high adhesive reliability during use and require smooth removal of constituent components when they are repaired, replaced, inspected, or reused. For example, in mobile phones, smart phones, tablet computers, laptop computers, various wearable devices (for example, wrist-worn types worn on the wrist like a watch, modular types worn on a part of the body with clips, straps, etc., glasses-wearing types including glasses-type (monocular type, binocular type. Also including head-worn types), clothing types such as those installed in the form of accessories on shirts, socks, hats, etc., ear-worn types worn on the ears like headphones, etc.), digital cameras, digital video cameras, audio equipment (portable music players, IC recorders, etc.), calculators (calculators, etc.), mobile game devices, electronic dictionaries, electronic notebooks, In portable electronic devices such as e-books, in-vehicle information devices, mobile radios, mobile televisions, mobile printers, mobile scanners, and mobile modems, it can be suitably used for fixing the protective panel (lens) that protects the display, fixing the key module components, fixing the antenna assembly, fixing the rim sheet, fixing the decorative panel, fixing the battery, fixing various other components (circuit substrates, various panel components, buttons, lighting device components, internal camera components, heat dissipation materials, graphite sheets), fixing logos (design characters), various designs and other identification objects (including various logos), etc. It should be noted that the so-called "portable (or mobile)" in this specification not only means that it can be carried, but also means that it has a level of portability that an individual (a standard adult) can move relatively easily.

[0259] The adhesive sheet disclosed herein is suitable as an adhesive sheet used for the purpose of fixing batteries (including primary batteries and secondary batteries, such as polymer batteries) in electronic devices (typically portable electronic devices). Batteries are usually arranged in a location to be disassembled when repairing, replacing, inspecting components (including batteries) of electronic devices, etc. Therefore, the adhesive sheet used to fix the battery needs to be removed more frequently. By applying the above-mentioned adhesive sheet in this use, the function of fixing the battery can be well exerted, and when the battery at the end of its service life is disassembled, the removal method based on water peeling using stretching can be used to easily perform the disassembly. According to the adhesive sheet disclosed herein, the above-mentioned removal method can be used to suppress the deformation of the battery and remove the adhesive sheet well.

[0260] In addition, the adhesive sheet disclosed herein is suitable for the purpose of laminating brittle materials such as glass (typically hard and brittle materials). For example, in the use of fixing two adherends and in the mode in which at least one of the adherends is formed by brittle materials such as glass materials, the adhesive sheet disclosed herein can be preferably used. With regard to hard and brittle materials such as glass, it is sometimes impossible to withstand the force when peeling off the adhesive sheet attached to it and breakage occurs, but by using the adhesive sheet disclosed herein, the adhesive sheet can be peeled off and removed without damaging the adherends such as glass. Specifically, the fixed use of glass materials such as windshields and window glasses of automobiles can be cited; the use of glass materials being laminated to each other in window glasses, antibacterial glass, etc. composed of glass plates of multilayer structures. In addition, the fixing of glass parts (lenses, etc.) in frames and panels having glass plates, and the lamination of glass plates to each other are also suitable uses of the adhesive sheet disclosed herein.

[0261] The size of the glass plate as an adherend is not limited to a specific range, and the thickness of the glass plate can be, for example, 0.1 to 5 mm (e.g., 0.5 to 2 mm). The length of the glass plate is, for example, 5 mm to 1 m (e.g., 50 mm or more, further 100 mm or more and 500 mm or less). The adhesive sheet disclosed herein can be preferably used for applications that are bonded to glass plates of such sizes. It should be noted that the length of the glass plate refers to the length of the portion having the maximum length in the surface direction of the glass plate.

[0262] In addition, the adhesive sheet disclosed herein is also suitable as an adhesive sheet for fixing replaced articles (interior decoration items such as hooks and mirrors, building materials, etc.) or parts (adhered objects, fixed objects, adhered objects, etc.) after being attached to walls, pillars, furniture, home appliances, glass surfaces, etc. and used for a predetermined period of time. In this application, the adhesive sheet performs a good fixing function in fixing the articles, etc., and can be peeled off and removed by water peeling when the articles, etc. are disassembled.

[0263] <Articles or components with adhesive sheets>

[0264] The adhesive sheet disclosed herein may be a constituent element of an article or component with an adhesive sheet formed by joining an article or component to one surface. In such an article or component with an adhesive sheet, the other surface of the adhesive sheet may be in a form protected by a release liner. Alternatively, the adhesive sheet may be a constituent element of an article or component formed by joining an object to its two sides. Such an article or component may be in the form of a laminate, which has an object A, an object B, and an adhesive sheet for joining the object A and the object B. As the above-mentioned article and component, the above-mentioned article and the article that can become the constituent component may be cited. The same is true for the object. In some embodiments, the adhesive sheet may be a constituent element of an optical component with an adhesive sheet formed by joining an optical component to the surface of an adhesive layer. As the above-mentioned optical component, it is preferred that the surface to which the adhesive sheet is pasted is a component with a non-absorbent smooth surface. Examples of the above-mentioned optical component are as described above. It should be noted that the surface of the above-mentioned component to which the adhesive sheet is attached may be hydrophilized. As a hydrophilic treatment, for example, a corona treatment, a plasma treatment, a hydrophilic coating treatment with a hydrophilic coating layer, and the like may be cited to help improve hydrophilicity.

[0265] <Peeling method>

[0266] In addition, according to this specification, a method for peeling an adhesive sheet attached to an adherend from the adherend is provided. The method may include a water stripping step, in which, at the peeling front of the adhesive sheet from the adherend, in a state where an aqueous liquid exists at the interface between the adherend and the adhesive sheet, the adhesive sheet is peeled from the adherend while allowing the aqueous liquid to enter the interface following the movement of the peeling front. The peeling front referred to herein refers to the part where the adhesive sheet begins to separate from the adherend when the adhesive sheet is peeled from the adherend. According to the water stripping step, the aqueous liquid can be effectively used to peel the adhesive sheet from the adherend. The peeling method can be satisfactorily implemented, for example, in a manner in which any adhesive sheet disclosed herein is peeled from an adherend.

[0267] As the aqueous liquid used in the above-mentioned stripping method, a liquid containing a small amount of additives as needed in water or a mixed solvent with water as the main component can be used. As a solvent other than water constituting the above-mentioned mixed solvent, a lower alcohol (such as ethanol), a lower ketone (such as acetone), etc. that can be uniformly mixed with water can be used. As the above-mentioned additive, a known surfactant, etc. can be used. From the viewpoint of avoiding contamination of the adherend, in some ways, it is preferred to use an aqueous liquid that does not substantially contain additives. From the viewpoint of environmental hygiene, it is particularly preferred to use water as the aqueous liquid. As water, there is no particular limitation, and considering the purity required according to the purpose, the ease of obtaining, etc., for example, distilled water, ion exchange water, tap water, etc. can be used.

[0268] In some embodiments, the above-mentioned stripping method can be preferably carried out in the following manner: for example, similarly to the determination of water stripping force described later, an aqueous liquid is supplied to the interface between the adhesive sheet attached to the adherend and the adherend, so that the aqueous liquid enters the interface between the adhesive sheet and the adherend, and then the adhesive sheet is stripped without supplying new water (i.e., only using the aqueous liquid supplied to the adherend before the start of stripping). It should be noted that if the water entering the interface between the adhesive sheet and the adherend following the movement of the stripping front dries up halfway through the water stripping process, water can be intermittently or continuously added after the start of the water stripping process. For example, in the case where the adherend is hygroscopic and the aqueous liquid is easily retained on the surface of the adherend or the adhesive surface after stripping, it is preferred to adopt a method of adding water after the start of the water stripping process.

[0269] The amount of the aqueous liquid supplied before the start of peeling is not particularly limited as long as it can introduce the above-mentioned aqueous liquid from the outside of the sticking range of the adhesive sheet to the interface between the adhesive sheet and the adherend. The amount of the above-mentioned aqueous liquid can be, for example, more than 5 μL, more than 10 μL is appropriate, and can be more than 20 μL. In addition, the upper limit of the amount of the above-mentioned aqueous liquid is not particularly limited. In some ways, from the perspective of improving operability, the amount of the above-mentioned aqueous liquid can be, for example, less than 10 mL, less than 5 mL, less than 1 mL, less than 0.5 mL, less than 0.1 mL, or less than 0.05 mL. By reducing the amount of the above-mentioned aqueous liquid, the operation of removing the above-mentioned aqueous liquid by drying, wiping off, etc. after peeling the adhesive sheet can be omitted or simplified.

[0270] Typically, the adhesive sheet peeled by the above-mentioned peeling method is an elongated adhesive sheet comprising an adhesive layer. The so-called elongated adhesive sheet here refers to an adhesive sheet with a stress of less than 30MPa when the above-mentioned 100% elongation, and preferably can be an adhesive sheet with a fracture strain εf of more than 300%. The above-mentioned adhesive sheet is, for example, preferably any adhesive sheet disclosed herein. Therefore, the above-mentioned peeling method is suitable as a peeling method for any adhesive sheet disclosed herein. According to the elongated adhesive sheet as described above, it is possible to dramatically improve the entry of an aqueous liquid into the interface between the adhesive sheet and the above-mentioned adherend. Specifically, the adhesive sheet has elongation, so in the above-mentioned peeling process, for example, by holding one end of the adhesive sheet (which can be a wing) and stretching the adhesive sheet, a gap is generated near the bonding interface with the above-mentioned adherend due to the elongation of the adhesive sheet at the beginning of the stretching. Therefore, there is no need to use special operations such as tools such as a utility knife, and it is possible to supply an aqueous liquid to the gap generated near the bonding interface with the above-mentioned adherend, so that the aqueous liquid enters the peeling portion of the bonding interface, thereby enabling water peeling.

[0271] The peeling angle of the adhesive sheet is not particularly limited. For example, the adhesive sheet can be peeled off from the adherend at an appropriate peeling angle in the range of 0 ° to 180 ° relative to the bonding surface with the adherend. In the mode of peeling off the adhesive sheet joining two adherends from the adherend, the peeling angle of the adhesive sheet can be, for example, less than 90 ° (0 ° to less than 90 °) relative to the bonding surface with an adherend. The adhesive sheet disclosed herein has elongation, so by stretching at an angle less than 90 °, the adhesive sheet can be peeled off using its elongation. Such a peeling form is also referred to as stretching peeling and stretching removal. In the mode of releasing the bonding state of two adherends joined by the adhesive sheet, it is also referred to as pull-out peeling and pull-out removal. In such a peeling method, specifically, in the initial stage of the stretching of the adhesive sheet, by supplying an aqueous liquid to the gap generated by the elongation of the adhesive sheet, in other words, by performing the peeling operation in a state where an aqueous liquid exists at the exposed part of the adhesive interface between the adherend and the adhesive sheet, the adhesive sheet can be peeled off from the adherend smoothly with a small load on the adherend by utilizing the elongation and water peeling properties of the adhesive sheet. This is particularly advantageous in that two adherends are separated without forcing the adherends to deform or break when they are made of rigid or brittle materials.

[0272] The peeling angle (typically the stretching peeling angle) of the adhesive sheet can be 0° to less than 45° (e.g., 0° to less than 30°, and further 0° to less than 15°). In addition, due to the peripheral structure of the bonding portion of the adhesive sheet, the adhesive sheet disclosed herein can also cope well with the method of stretching the adhesive sheet at an angle that is not parallel to the bonding surface (e.g., an angle of 45° to 90°, for example, an angle of more than 45° and less than 90°).

[0273] The water stripping process involved in some methods can be preferably implemented in a manner that allows the above-mentioned stripping front to move at a speed of more than 10 mm / minute. In terms of moving the stripping front at a speed of more than 10 mm / minute, for example, under the condition that the stripping angle is 180 degrees, it is equivalent to stripping the adhesive sheet at a tensile speed of more than 20 mm / minute. The speed at which the above-mentioned stripping front moves can be, for example, more than 25 mm / minute, more than 50 mm / minute, more than 150 mm / minute, more than 300 mm / minute, or more than 500 mm / minute. According to the stripping method disclosed herein, while the above-mentioned aqueous liquid enters the above-mentioned interface, the above-mentioned adhesive sheet is stripped from the above-mentioned adherend, thereby, even at such a faster stripping speed, good water stripping properties can be exerted. The upper limit of the speed at which the stripping front moves is not particularly limited. The speed at which the above-mentioned stripping front moves can be, for example, less than 1000 mm / minute.

[0274] The peeling method disclosed herein can be preferably applied to the peeling of an adhesive sheet adhered to a non-water-absorbing smooth surface such as a glass plate, a metal plate, a resin plate, etc. In addition, the peeling method disclosed herein can be preferably used as a method for peeling an adhesive sheet from any of the above-mentioned optical components. Among them, it is suitable as a method for peeling an adhesive sheet adhered to a glass plate such as an alkali glass or an alkali-free glass.

[0275] <Separation method>

[0276] In addition, the technology disclosed herein includes a method for separating two adherends joined by an elongated adhesive sheet. The method includes a process of stretching the adhesive sheet in the direction of pulling from between the above-mentioned two adherends using the elongation of the adhesive sheet. In addition, the process of stretching the adhesive sheet is implemented in a state where an aqueous liquid is present at the exposed part of the peeling of the bonding interface between at least one of the above-mentioned two adherends and the aforementioned adhesive sheet. According to the method, the adhesive sheet can be pulled from the two adherends by water peeling using the above-mentioned aqueous liquid. Therefore, even when the two adherends are formed by rigid materials or brittle materials, the two adherends can be separated without forcing the adherends to deform or destroy. The above-mentioned separation method can be a method for releasing the joining of the adherends and a method for disassembling the adherends. As for the details of these methods, as with the above-mentioned peeling method, the contents recorded in the above-mentioned peeling method can be adopted, so repeated descriptions are omitted.

[0277] It should be noted that the matters disclosed by this specification include the following aspects.

[0278] [1] An adhesive sheet having an adhesive layer, wherein:

[0279] The water peeling force of the adhesive sheet is 2 N / 10 mm or less, and the water peeling force is measured by a tensile tester at a test temperature of 23°C, a tensile speed of 300 mm / min, and a peeling angle of 180°, according to 10.4.1 method 1 of JIS Z0237:2009, after the adhesive surface of the adhesive layer is attached to the surface of an alkaline glass plate produced by a float process as an adherend and the contact angle with distilled water is 5 to 10 degrees, and 20 μL of distilled water is dripped onto the adherend after 1 day at room temperature, so that the distilled water enters one end of the interface between the adhesive surface and the adherend.

[0280] The stress at 100% elongation of the aforementioned adhesive sheet is less than 30 MPa, and the product of the breaking stress σf [MPa] and the breaking strain εf [%] (σf×εf) ​​is greater than 250, wherein the aforementioned stress at 100% elongation, the aforementioned breaking stress σf and the aforementioned breaking strain εf are measured by a tensile test carried out under the condition of a tensile speed of 100 mm / min.

[0281] [2] An adhesive sheet having an adhesive layer,

[0282] The adhesive layer comprises at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton,

[0283] The stress at 100% elongation of the aforementioned adhesive sheet is less than 30 MPa, and the product of the breaking stress σf [MPa] and the breaking strain εf [%] (σf×εf) ​​is greater than 250, wherein the aforementioned stress at 100% elongation, the aforementioned breaking stress σf and the aforementioned breaking strain εf are measured by a tensile test carried out under the condition of a tensile speed of 100 mm / min.

[0284] [3] The adhesive sheet according to [1] or [2] above, having a normal peel strength of 2.5 N / 10 mm or more and 15 N / 10 mm or less, the normal peel strength being measured at room temperature for one day in accordance with JIS Z0237:2009, 10.4.1, method 1: 180° peel strength relative to a test plate, using a tensile testing machine at a test temperature of 23°C, at a tensile speed of 300 mm / min and a peel angle of 180 degrees, after the adhesive surface of the adhesive layer is attached to an alkaline glass plate produced by a float process as an adherend with a contact angle with distilled water of 5 to 10 degrees.

[0285] [4] The pressure-sensitive adhesive sheet according to any one of [1] to [3] above, wherein the pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition containing an acrylic partial polymer, a crosslinking agent, and a photopolymerization initiator.

[0286] [5] The pressure-sensitive adhesive sheet according to any one of [1] to [4] above, wherein the HLB of the surfactant is 10 or more and 20 or less.

[0287] [6] The PSA sheet according to any one of [1] to [5] above, wherein the PSA layer is formed from a water-dispersible PSA composition, a solvent-based PSA composition, an active energy ray-curable PSA composition, or a hot-melt PSA composition.

[0288] [7] The pressure-sensitive adhesive sheet according to any one of [1] to [6] above, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer.

[0289] [8] The PSA sheet according to any one of [1] to [7] above, which is a double-sided adhesive sheet.

[0290] The pressure-sensitive adhesive layer constitutes at least one adhesive surface of the pressure-sensitive adhesive sheet.

[0291] [9] The pressure-sensitive adhesive sheet according to [8] above, comprising a first pressure-sensitive adhesive layer and a second pressure-sensitive adhesive layer as the pressure-sensitive adhesive layer, and further comprising an intermediate layer disposed between the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer.

[0292]

[10] The adhesive sheet as described in [9] above, wherein the intermediate layer is formed of a material including acrylic resin, polyurethane resin, urethane (meth)acrylate polymer, polyolefin resin, polyvinyl chloride resin, silicone, rubber or elastomer.

[0293]

[11] The pressure-sensitive adhesive sheet according to any one of [1] to

[10] above, wherein the content of the compound is less than 1 part by weight based on 100 parts by weight of the base polymer contained in the pressure-sensitive adhesive layer.

[0294]

[12] The pressure-sensitive adhesive sheet according to any one of [1] to

[11] above, which is used for optical applications.

[0295]

[13] The pressure-sensitive adhesive sheet according to any one of [1] to

[12] above, wherein the pressure-sensitive adhesive layer has a thickness of 10 μm to 200 μm.

[0296]

[14] The pressure-sensitive adhesive sheet according to any one of [1] to

[13] above, wherein the water peel strength reduction rate is 60% or more.

[0297]

[15] The pressure-sensitive adhesive sheet according to any one of [1] to

[14] above, wherein the haze value is less than 0.7%.

[0298]

[16] An optical member with a pressure-sensitive adhesive sheet, comprising the pressure-sensitive adhesive sheet according to any one of [1] to

[15] above, and an optical member bonded to one surface of the pressure-sensitive adhesive sheet.

[0299]

[17] A method for peeling a pressure-sensitive adhesive sheet, the method comprising peeling a stretchable pressure-sensitive adhesive sheet adhered to an adherend,

[0300] The peeling method comprises the step of peeling the adhesive sheet by stretching it in a direction less than 90° with respect to the bonding surface with the adherend,

[0301] The step of peeling the pressure-sensitive adhesive sheet is performed in a state where an aqueous liquid is present at a portion of the bonding interface between the adherend and the pressure-sensitive adhesive sheet that is exposed to peeling.

[0302]

[18] The peeling method according to

[17] above, wherein the pressure-sensitive adhesive sheet is the pressure-sensitive adhesive sheet according to any one of [1] to

[15] above.

[0303]

[19] A method for separating two adherends, the method comprising separating two adherends joined via an extensible pressure-sensitive adhesive sheet.

[0304] The separation method comprises the step of utilizing the elongation of the adhesive sheet to stretch the adhesive sheet in a direction of pulling the adhesive sheet away from between the two adherends.

[0305] The step of stretching the pressure-sensitive adhesive sheet is performed in a state where an aqueous liquid is present at a portion of the adhesive interface between at least one of the two adherends and the pressure-sensitive adhesive sheet that is exposed to peeling.

[0306]

[20] The separation method according to

[19] above, wherein the pressure-sensitive adhesive sheet is the pressure-sensitive adhesive sheet described in any one of [1] to

[15] above.

[0307] Example

[0308] Hereinafter, some embodiments related to the present invention will be described, but the present invention is not intended to be limited to the contents shown in these embodiments. It should be noted that, unless otherwise specified, in the following description, "parts" and "%" are based on weight.

[0309] <Evaluation method>

[0310] [Normal peeling force]

[0311] The release liner covering one surface of the adhesive layer (double-sided adhesive sheet without support) was peeled off from the adhesive sheet, and a 25 μm thick polyethylene terephthalate (PET) film was laminated on the exposed adhesive surface for mounting. The film was cut into a size of 20 mm wide and 100 mm long to prepare a test piece.

[0312] Under the environment of 23 ℃ and 50% RH, the release liner covering the other surface of the above-mentioned adhesive layer is peeled off from the above-mentioned test piece, and a 2kg rubber roller is reciprocated once so that the exposed adhesive surface is pressed against the alkaline glass plate as the adherend. It is subjected to autoclave treatment (50 ℃, 0.5MPa, 15 minutes). Then, under the environment of 23 ℃ and 50% RH, a tensile testing machine is used to measure the peel strength of the test piece from the adherend under the conditions of a tensile speed of 300mm / minute and a peeling angle of 180 degrees (wherein, until the following water peeling force is measured, that is, until distilled water is supplied to the peeling interface). The measurement is carried out 3 times, and their average value is converted into a value (unit: N / 10mm) relative to a width of 10mm, and this value is used as the normal peeling force [N / 10mm]. The above-mentioned normal peeling force is measured in a manner that the peeling of the test piece attached to the adherend is carried out from bottom to top. As the adherend, an alkaline glass plate (product name "MICRO SLIDE GLASS S200423", manufactured by Matsunami Glass Industries, Ltd.) can be used. As a tensile tester, a universal tensile compression tester (device name "tensile compression tester, TCM-1kNB", manufactured by Minebea) or a substitute thereof can be used. It should be noted that when the measurement object is a single-sided adhesive sheet, the above-mentioned PET film backing is not required.

[0313] [Water peel strength]

[0314] In the measurement of the normal peeling force, in the measurement of the peeling strength of the test piece from the adherend, 20 μL of distilled water was supplied to the portion where the test piece began to separate from the adherend (peeling front), and the peeling strength after the distilled water supply was measured. The water peeling force was measured for each normal peeling force measurement (i.e., 3 times), and their average value was converted into a value relative to a width of 10 mm (unit: N / 10 mm), and this value was taken as the water peeling force [N / 10 mm].

[0315] It should be noted that, with respect to the measurement of water peeling force, the normal peeling force and the water peeling force can be measured continuously for each test piece, or different test pieces can be used for the normal peeling force and the water peeling force. For example, in the case where it is difficult to prepare a test piece of sufficient length for continuous measurement, it is possible to use different test pieces for measurement. With respect to the adherend, the tensile testing machine, and other matters, it is basically the same as the measurement of normal peeling force.

[0316] It should be noted that in the measurements of the normal peel force and the water peel force, an alkaline glass plate produced by a float process was used as an adherend, and the contact angle of the surface of the adhered test piece with distilled water was 5 to 10 degrees. As such an adherend, an alkaline glass plate manufactured by Matsunami Glass Industries Co., Ltd. can be used, but the present invention is not limited thereto, and an alkaline glass plate other than or in addition to the alkaline glass plate manufactured by Matsunami Glass Industries Co., Ltd. can also be used.

[0317] The contact angle of the alkaline glass plate was measured by the following method. That is, the contact angle was measured by the drop method using a contact angle meter (manufactured by Kyowa Interface Science Co., Ltd., trade name "DMo-501 model", control box "DMC-2", control and analysis software "FAMAS (version 5.0.30)") under a measurement atmosphere of 23°C and 50% RH. The amount of distilled water added was 2 μL, and the contact angle was calculated by the θ / 2 method based on the image after 5 seconds of addition (implemented with N5).

[0318] [Tensile test]

[0319] Prepare a test piece made of 3cm wide x 5cm long by cutting the adhesive sheet with a release film, peel off the release film, roll up the long side, and make a rod-shaped test piece with a length of 3cm. Under the conditions of 23°C and 50% RH, use a tensile testing machine to perform the tensile test on the test piece under the conditions of a chuck distance of 10mm and a tensile speed of 100mm / min, and measure the stress at 100% elongation [MPa], the stress at 500% elongation [MPa], the fracture stress σf [MPa] and the fracture strain εf [%]. The stress at 100% elongation [MPa] and the stress at 500% elongation [MPa] are respectively the load [N] measured when the test piece is elongated by 100% and 500% in the above tensile test divided by the cross-sectional area [mm 2 The breaking stress σf [MPa] is the load [N] at the time of breaking of the test piece in the above tensile test divided by the cross-sectional area [mm 2 ] and the breaking strain εf[%] is the elongation [%] of the test piece when it breaks. As a tensile testing machine, a universal tensile-compression testing machine (device name "tensile-compression testing machine, TCM-1kNB" manufactured by Minebea) or its equivalent can be used.

[0320] It should be noted that when the PSA sheet to be measured cannot be rolled into a rod shape, an object obtained by punching the PSA sheet into a No. 1 dumbbell shape (10 mm wide according to JIS K 6251) is used as a test piece, and the same tensile test as above is carried out to measure the stress at 100% elongation [MPa], the stress at 500% elongation [MPa], the breaking stress σf [MPa] and the breaking strain εf [%].

[0321] [Rigid body reprocessability]

[0322] (1) 1.5cm×5cm pasting evaluation

[0323] The adhesive sheet (double-sided adhesive sheet) was cut into 1.5 cm wide, and alkali-free glass (Corning, product name "Eagle XG", thickness 0.7 mm) as the adherend was pasted on both sides of the 1.5 cm × 5 cm area. Specifically, under an environment of 23 ° C and 50% RH, the surface of the adhesive sheet was exposed, the adherend was pasted with an area of ​​1.5 cm × 5 cm, and a 2 kg rubber roller was pressed back and forth once. This operation was performed on each side of the adhesive sheet. At this time, a 1 cm long portion at one end of the long side direction of the adhesive sheet was left in an unpasted state extending from the two adherends pasted to the adhesive sheet, and used as a wing. After being placed in an environment of 23°C and 50% RH for 30 minutes, water was supplied to the vicinity of the bonding interface between the adherend and the adhesive sheet (specifically, a drop of water (about 20 μL) was dripped near the interface of each surface of the adhesive sheet using a glass pipette), and the adhesive sheet was pulled by hand from the above two adherends, and peeled off from the above adherends at a nearly constant speed over 15 seconds. The reprocessability at this time was evaluated using the following criteria.

[0324] G: The peeling can be completed.

[0325] P: Peeling was not smooth and could not be completed within 15 seconds, or the adhesive sheet was torn during peeling.

[0326] (2) 3cm×5cm pasting evaluation

[0327] The adhesive sheet (double-sided adhesive sheet) was cut into 3 cm width, and non-alkali glass as an adherend was attached to both sides of the 3 cm×5 cm area. The rest was evaluated in the same manner as the above 1.5 cm×5 cm attachment evaluation, and the reprocessability was evaluated.

[0328] It should be noted that the larger the bonding area, the greater the resistance during stretching, and the easier it is for the PSA sheet to tear. Therefore, this evaluation method is an evaluation under stricter conditions than the evaluation method (1) above.

[0329] <Example 1>

[0330] (Preparation of Adhesive Composition)

[0331] 100 parts of a monomer mixture containing 54.9% of n-butyl acrylate (BA), 11.5% of cyclohexyl acrylate (CHA), 22.1% of 4-hydroxybutyl acrylate (4HBA), 7.4% of hydroxyethyl acrylate (HEA), and 4.1% of N-vinyl-2-pyrrolidone (NVP) were mixed with 0.3 parts of a photopolymerization initiator (manufactured by IGM Resins, trade name "Omnirad 651", 2,2-dimethoxy-1,2-diphenylethane-1-one), and photopolymerization was performed by pulse irradiation with ultraviolet rays in a nitrogen atmosphere until the viscosity (BH viscometer, No. 5 rotor, 10 rpm, measurement temperature: 30°C) reached about 15 Pa·s, thereby preparing a monomer syrup containing a partial polymer of the above-mentioned monomer mixture (polymerization rate: about 8%). To 100 parts of the monomer slurry, 0.15 parts of dipentaerythritol hexaacrylate (DPHA) as a multifunctional monomer (crosslinking agent) and 0.3 parts of a surfactant (polyoxyethylene sorbitan monolaurate, HLB 16.7, trade name "RHEODOL TW-L120", manufactured by Kao Corporation) were added, uniformly mixed, and then degassed to prepare the ultraviolet curable adhesive composition of this example.

[0332] (Manufacturing of adhesive sheet)

[0333] The adhesive composition obtained in the above was applied to the release surface of a release film R1 (MRF#38 manufactured by Mitsubishi Resins Corporation, product name, 38 μm thick), covered with a release film R2 (MRE#25 manufactured by Mitsubishi Resins Corporation, product name, 25 μm thick) to block air, and cured by ultraviolet irradiation to form an adhesive layer with a thickness of 150 μm. The ultraviolet irradiation was performed using a black light lamp at an illumination of 4 mW / cm 2 (Measured using an industrial UV inspector (manufactured by TOPCON, trade name "UVR-T1") with a peak sensitivity wavelength of about 350 nm) and irradiated for 180 seconds. In this way, the adhesive sheet of this example (an adhesive sheet formed only by an adhesive layer) was obtained. The adhesive sheet of this example was protected on its adherend surface by release films R1 and R2. It should be noted that the release films R1 and R2 are both release liners with one side of the PET film being the release surface (silicone release treated surface).

[0334] <Example 2>

[0335] Except for the monomer composition shown in Table 1, a monomer syrup was prepared in the same manner as in Example 1, and 0.1 parts of 1,6-hexanediol diacrylate (HDDA) as a multifunctional monomer and 0.3 parts of a surfactant (polyoxyethylene sorbitan monolaurate, HLB 16.7, trade name "RHEODOL TW-L120", manufactured by Kao Corporation) were added to 100 parts of the obtained monomer syrup, and the mixture was uniformly mixed and then degassed to prepare the ultraviolet curable adhesive composition of this example. The adhesive sheet of this example was obtained in the same manner as in Example 1 except that the obtained adhesive composition was used.

[0336] <Examples 3 to 4, Examples 6 to 10, Examples 12 to 13>

[0337] Except for the monomer composition shown in Table 1, the adhesive composition was prepared in the same manner as in Example 2 to obtain the adhesive sheet of each example. It should be noted that in Table 1, BzA is benzyl acrylate, AA-6 is a macromonomer manufactured by Toagosei Co., Ltd. (trade name "AA-6", a macromonomer having a methyl methacrylate segment, number average molecular weight Mn6000), AS-6 is a macromonomer manufactured by Toagosei Co., Ltd. (trade name "AS-6", a macromonomer having a styrene segment, number average molecular weight Mn6000), and "EBECRYL 3703" is a trade name "EBECRYL 3703" manufactured by Daicel Allnex (amine-modified bisphenol A type epoxy acrylate, average molecular weight 850).

[0338] <Example 5>

[0339] A PSA sheet of this example was obtained by preparing a PSA composition in the same manner as in Example 4 except that trimethylolpropane triacrylate (TMPTA) was used instead of HDDA as the multifunctional monomer.

[0340] <Example 11>

[0341] Except that the monomer composition is set as shown in Table 1, a monomer slurry is prepared in the same manner as in Example 1, and 0.12 parts of DPHA as a multifunctional monomer and 0.4 parts of 3-glycidoxypropyltrimethoxysilane (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.) are added to 100 parts of the obtained monomer slurry, and the mixture is uniformly mixed, and then degassed to prepare the ultraviolet curable adhesive composition of this example. Except that the obtained adhesive composition is used, the adhesive sheet of this example is obtained in the same manner as in Example 1.

[0342] <Example 14>

[0343] (Preparation of Adhesive Layer)

[0344] The adhesive composition obtained in Example 1 was applied to the release surface of a release film R1 (MRF#38, manufactured by Mitsubishi Resins Corporation, with a thickness of 38 μm), covered with a release film R2 (MRE#25, manufactured by Mitsubishi Resins Corporation, with a thickness of 25 μm) to block air, and cured by ultraviolet irradiation to form an adhesive layer with a thickness of 50 μm. The ultraviolet irradiation was performed using a black light lamp at an illumination of 4 mW / cm 2 (Measured using an industrial UV tester (manufactured by TOPCON, trade name "UVR-T1") with a peak sensitivity wavelength of about 350 nm) and irradiated for 180 seconds. In this way, two adhesive layers were prepared, each side of which was protected by two release films. It should be noted that the ultraviolet curing adhesive used in this example is recorded as U-1 in Table 2.

[0345] (Production of acrylic polymer film)

[0346] The acrylic block copolymer A (manufactured by KURARAY CO., LTD, trade name "KURARITY LA3320", a triblock copolymer of polyMMA block-polyBA block-polyMMA block. MMA is methyl methacrylate and BA is n-butyl acrylate) is dissolved in toluene in a concentration of 30%. The obtained polymer solution is applied to the release surface of the release film R1 (manufactured by Mitsubishi Resins Corporation, product name "MRF#38", thickness 38μm), and dried at 130°C for 3 minutes to form an acrylic polymer layer with a thickness of 50μm. The release film R2 (manufactured by Mitsubishi Resins Corporation, product name "MRE#38", thickness 38μm) is attached to the exposed surface of the acrylic polymer layer. In this way, an acrylic polymer film A1 is produced with each side protected by two release films.

[0347] (Manufacturing of adhesive sheet)

[0348] The release film R2 covering the adhesive layer obtained in the above is peeled off, and the adhesive layer is bonded to each side of the acrylic polymer film A1. Specifically, the release film covering one side of the acrylic polymer film A1 is peeled off, and the above-mentioned adhesive layer is bonded to the exposed side of the acrylic polymer film A1, and the same operation is also performed on the other side of the acrylic polymer film A1, so that the two sides of the acrylic polymer film A1 are bonded with adhesive layers. In this way, an adhesive sheet (double-sided adhesive sheet with an intermediate layer) having an adhesive layer on both sides of the acrylic polymer film A1 as an intermediate layer is obtained. The adhesive sheet of this example is protected by the release film R1 and the bonding surface with the adherend.

[0349] <Example 15>

[0350] The acrylic polymer layer formed in the same manner as in Example 14 was laminated to produce an acrylic polymer film A2 having a thickness of 150 μm. A pressure-sensitive adhesive sheet of this example was obtained in the same manner as in Example 14 except that this acrylic polymer film A2 was used.

[0351] <Example 16>

[0352] A PSA sheet of this example was obtained in the same manner as in Example 14 except that the thickness of each PSA layer was changed to 100 μm.

[0353] <Example 17>

[0354] An acrylic block copolymer B (manufactured by KURARAY CO., LTD., trade name "KURARITY LA2250", a triblock copolymer of polyMMA block-polyBA block-polyMMA block) was dissolved in toluene to a concentration of 30%. An acrylic polymer film B1 having a thickness of 150 μm was prepared in the same manner as in Example 15 except that the polymer solution was used. The obtained acrylic polymer film B1 was used to obtain the adhesive sheet of this example.

[0355] <Example 18>

[0356] (Preparation of Adhesive Composition)

[0357] 85 parts of 2-ethylhexyl acrylate (2EHA), 13 parts of methyl acrylate (MA), 1.2 parts of acrylic acid (AA), 0.8 parts of methacrylic acid (MAA), 0.02 parts of 3-methacryloxypropyltrimethoxysilane (trade name "KBM-503", manufactured by Shin-Etsu Chemical Co., Ltd.), 0.048 parts of tert-dodecyl mercaptan as a chain transfer agent, and 2.0 parts of an emulsifier (LATEMUL E-118B manufactured by Kao Corporation) were mixed and emulsified in 100 parts of ion-exchanged water to prepare an aqueous emulsion of a monomer mixture (monomer emulsion).

[0358] The monomer emulsion was added to a reaction vessel equipped with a condenser, a nitrogen inlet tube, a thermometer and a stirring device, and stirred at room temperature for more than 1 hour while introducing nitrogen. Next, the system was heated to 60°C, 0.1 parts of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate (VA-057 manufactured by Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator, and the mixture was reacted at 60°C for 6 hours to obtain an aqueous dispersion of an acrylic polymer. After the system was cooled to room temperature, 30 parts of a tackifier resin emulsion (trade name "SUPER ESTER E-865NT" manufactured by Arakawa Chemical Industries, Ltd., an aqueous dispersion of polymerized rosin ester with a softening point of 160°C) was added in terms of solid content. Furthermore, 10% ammonia water as a pH adjuster and polyacrylic acid (aqueous solution with a non-volatile content of 36%) as a thickener were used to adjust the pH to about 7.5 and the viscosity to about 9 Pa·s, thereby preparing an emulsion-type adhesive composition.

[0359] (Manufacturing of adhesive sheet)

[0360] The emulsion adhesive composition obtained above was applied to a release film R1 (manufactured by Mitsubishi Resins Corporation, product name "MRF#38", thickness 38μm), and dried at 120°C for 3 minutes to form an adhesive layer with a thickness of 25μm. Two adhesive layers with release films were prepared and bonded to each side of an acrylic polymer film A2 with a thickness of 150μm made in the same manner as in Example 15. In this way, an adhesive sheet having an adhesive layer on both sides of the acrylic polymer film A2 as an intermediate layer was obtained. The release film R1 was used to protect the adhesive sheet of this example from being attached to the adherend. It should be noted that in Table 2, the emulsion adhesive used in this example is recorded as E-1.

[0361] <Example 19>

[0362] An acrylic polymer film B2 having a thickness of 50 μm was prepared by the same method as in Example 17 using an acrylic block copolymer B (manufactured by KURARAY CO., LTD., trade name “KURARITY LA2250”) (a triblock copolymer of polyMMA block-polyBA block-polyMMA block). A pressure-sensitive adhesive sheet of this example was obtained in the same manner as in Example 18 except that this acrylic polymer film B2 was used.

[0363] <Example 20>

[0364] As the intermediate layer, a thermoplastic polyurethane film A having a thickness of 150 μm (manufactured by Nihon Matai Co., Ltd., product name “ESMER URS PX98”) was used. Otherwise, the same procedure as in Example 18 was carried out to obtain a pressure-sensitive adhesive sheet of this example.

[0365] <Example 21>

[0366] As the intermediate layer, a polyurethane film B (manufactured by KURABO INDUSTRIES LTD., trade name "Kurangile") having a thickness of 50 μm was used. Otherwise, the same procedure as in Example 18 was carried out to obtain a pressure-sensitive adhesive sheet of this example.

[0367] <Example 22>

[0368] As the intermediate layer, a 100 μm thick silicone rubber film (manufactured by Mitsubishi Chemical Corporation, product name “KEIJU CF-100-5A”) was used. Otherwise, the same procedure as in Example 18 was carried out to obtain a pressure-sensitive adhesive sheet of this example.

[0369] <Example 23>

[0370] As the intermediate layer, a PET film having a thickness of 50 μm (manufactured by Toray Industries, Ltd., product name “Lumirror S10”) was used. Otherwise, the same procedure as in Example 14 was carried out to obtain a pressure-sensitive adhesive sheet of this example.

[0371] <Example 24>

[0372] The acrylic block copolymer A (KURARAY CO., LTD, trade name "KURARITY LA3320", a triblock copolymer of polyMMA block-polyBA block-polyMMA block) was dissolved in toluene in a concentration of 30%. The obtained polymer solution was applied to the release surface of the release film R1 (Mitsubishi Resins Corporation, product name "MRF#38", thickness 38μm), and dried at 130°C for 3 minutes to form an acrylic adhesive layer with a thickness of 250μm. The release film R2 (Mitsubishi Resins Corporation, product name "MRE#38", thickness 38μm) was attached to the exposed surface of the acrylic adhesive layer. In this way, the adhesive sheet of this example was obtained. The release films R1 and R2 were used to protect the adhesive surface of the adhesive sheet of this example with the adherend. It should be noted that the acrylic adhesive used in this example is recorded as H-1 in Table 2.

[0373] <Example 25>

[0374] Instead of acrylic block copolymer A, acrylic block copolymer B (KURARAY CO., LTD., trade name "KURARITY LA2250", a triblock copolymer of polyMMA block-polyBA block-polyMMA block) was used. In the same manner as in Example 24, an acrylic adhesive layer with a thickness of 250 μm was formed to obtain an adhesive sheet of this example. The adhesive sheet of this example was protected on the adherend surface by release films R1 and R2. It should be noted that in Table 2, the acrylic adhesive used in this example is recorded as H-2.

[0375] <Performance Evaluation>

[0376] The normal peel strength [N / 10 mm], water peel strength [N / 10 mm], stress at 100% elongation [MPa], stress at 500% elongation [MPa], breaking stress σf [MPa], and breaking strain εf [%] of the obtained PSA sheet were measured. The results are shown in Tables 1 and 2.

[0377] [Table 1]

[0378]

[0379] [Table 2]

[0380]

[0381] Examples 1 to 13 shown in Table 1 all use a single-layer adhesive sheet, among which the evaluation results of the rigid body reprocessability of 1.5 cm × 5 cm adhesive sheets of Examples 1 to 10 are qualified. The water peeling force of the adhesive sheets of the above examples is less than 2N / 10mm, the stress at 100% elongation is less than 30MPa, and the product of the breaking stress σf [MPa] and the breaking strain εf [%], that is, σf×εf (elongation strength characteristics) is 250 or more. In addition, the adhesive layer of each of the above examples contains a surfactant. In addition, Examples 2 to 10, whose elongation strength characteristics (σf×εf) ​​are more than 300, show more excellent rigid body reprocessability. In addition, the normal peeling force of the adhesive sheets of Examples 1 to 10 is more than 2.5N / 10mm. On the other hand, the evaluation results of the rigid body reprocessability of the adhesive sheets of Examples 11 to 13 are unqualified. In Example 11, the water peeling force is greater than 2N / 10mm, the adhesive layer does not contain a surfactant, and the elongation strength characteristics (σf×εf) ​​are less than 250. The water peeling force of the adhesive sheet of Example 12 was 2N / 10mm or less, and the adhesive layer contained a surfactant, but the elongation strength property (σf×εf) ​​was less than 250. The water peeling force of the adhesive sheet of Example 13 was 2N / 10mm or less, and the adhesive layer contained a surfactant, but could not be 100% elongated. The elongation strength property (σf×εf) ​​was less than 250.

[0382] If the results of Table 1 are observed more specifically, it is confirmed by the comparison of, for example, Examples 4, 6 and 12 that by increasing the amount of hydroxyl-containing monomers (specifically HEA, 4HBA), the fracture stress is increased while the fracture strain is not reduced but improved. In addition, it is confirmed by the comparison of Examples 3 and 12 that by increasing the amount of nitrogen-containing monomers (specifically NVP), the fracture stress and fracture strain are significantly increased. Example 11 is a system using different crosslinking agents (multifunctional monomers), but in this example, the effect of the small amount of nitrogen-containing monomers is confirmed (fracture strain reduction). In Example 2, by increasing the amount of hydroxyl-containing monomers and nitrogen-containing monomers, compared with Example 12, improved fracture stress and fracture strain are shown. In addition, the comparison of Examples 1 and 12, and the comparison of Examples 4 and 5 show that the fracture stress and fracture strain can be improved by selecting the type of crosslinking agent (multifunctional monomer) and adjusting the amount of crosslinking agent. In addition, it was confirmed that the use of benzyl acrylate and macromonomers in Examples 7 to 10 can improve the breaking stress and breaking strain, or can adjust both in a well-balanced manner. It is believed that the structure of the monomers exerts cohesiveness without impairing the flexibility of the adhesive layer, thereby achieving improved breaking stress and breaking strain.

[0383] The above Examples 1 to 10 all have good normal peeling force and water peeling properties. Therefore, it can be seen that when designing the adhesive layer, by adjusting the types of monomers such as monomers containing polar groups, the types of cross-linking agents, and their amounts, the specified peeling characteristics can be maintained, and the ideal 100% elongation stress can be achieved, thereby obtaining improved elongation strength characteristics (σf×εf).

[0384] In addition, as shown in Table 2, in Examples 14 to 22 using a laminated adhesive sheet with an intermediate layer, excellent rigid body reprocessing properties can also be obtained. These examples have water peelability, and the stress is less than 30MPa at 100% elongation, and the elongation strength characteristics (σf×εf) ​​are 250 or more. In addition, it is confirmed that in Examples 14 to 17, although an adhesive (adhesive of Example 1) that failed to obtain good results in the rigid body reprocessing properties of 3cm×5cm pasted in the case of a single adhesive layer was used, the elongation strength characteristics (σf×εf) ​​were improved by providing an intermediate layer, and excellent rigid body reprocessing properties can be obtained. In addition, the normal peel force of the adhesive sheet of Examples 14 to 22 is 2.5N / 10mm or more. On the other hand, in Example 23, which is configured with a PET film as an intermediate layer, although the elongation strength characteristics (σf×εf) ​​show a high value, it is difficult to stretch to a stress of 30MPa or more at 100% elongation, so water cannot enter the bonding interface and rigid body reprocessing properties cannot be obtained. In addition, the single-layer PSA sheets of Examples 24 and 25 using the intermediate layer material as the PSA layer did not have water releasability, and thus did not obtain rigid body reprocessability.

[0385] From the above results, it can be seen that the adhesive sheet with a water peeling force of 2N / 10mm or less, or an adhesive layer containing at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton, and a stress of less than 30MPa at 100% elongation, and σf×εf of 250 or more, has good peeling properties using aqueous liquids such as water, and can take into account both bonding reliability and peeling and removal properties. Specifically, it can be seen that the adhesive sheet according to the above structure can be stretched with a smaller force to exhibit good water peeling properties, and no tearing occurs during the stretching during peeling, thereby achieving good peeling and removal properties.

[0386] Although the specific examples of the present invention have been described in detail above, these are only examples and do not limit the scope of the claims. The technology described in the scope of the claims includes various modifications and substitutions of the specific examples described above.

[0387] Description of Reference Numerals

[0388] 1, 2, 3 adhesive sheet

[0389] 10 Adhesive layer

[0390] 11. First adhesive layer

[0391] 12 Second adhesive layer

[0392] 10A One surface (bonding surface)

[0393] 10B Another surface

[0394] 20 Support body (support layer)

[0395] 20A Side 1

[0396] 20B Second side (back side)

[0397] 25 Middle Layer

[0398] 30, 31, 32 Release liner

[0399] 50 Adhesive sheet with release liner

Claims

1. An adhesive sheet having an adhesive layer, wherein: The adhesive layer is formed of an adhesive composition, The adhesive composition contains a monomer component constituting an acrylic polymer, a multifunctional monomer, and at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton. Among the monomer components constituting the acrylic polymer, (meth)acrylic acid C 1-20 The proportion of alkyl esters is 35% by weight or more and 50% by weight or less, the proportion of hydroxyl-containing monomers is 20% by weight or more and 45% by weight or less, the proportion of monomers having nitrogen atoms is 1% by weight or more and 20% by weight or less, and the proportion of alicyclic hydrocarbon group-containing (meth)acrylates is 8% by weight or more and 40% by weight or less, The amount of the multifunctional monomer used is 0.01 to 0.1 parts by weight relative to 100 parts by weight of the monomer component. The multifunctional monomer is selected from trimethylolpropane tri(meth)acrylate or 1,6-hexanediol diacrylate, The water peeling force of the adhesive sheet is 2N / 10mm or less, and the water peeling force is measured by a tensile tester at a test temperature of 23°C, a tensile speed of 300mm / min, and a peeling angle of 180°, according to 10.4.1 method 1 of JIS Z0237:2009, after the adhesive surface of the adhesive layer is attached to the surface of an alkaline glass plate produced by a float process as an adherend and the contact angle with distilled water is 5 to 10 degrees, and 20μL of distilled water is dripped onto the adherend and the distilled water is allowed to enter one end of the interface between the adhesive surface and the adherend. The stress at 100% elongation of the adhesive sheet is less than 30 MPa, and the product of the breaking stress σf [MPa] and the breaking strain εf [%] (σf×εf) ​​is greater than 300, wherein the stress at 100% elongation, the breaking stress σf and the breaking strain εf are measured by a tensile test conducted at a tensile speed of 100 mm / min.

2. The adhesive sheet according to claim 1, which has a normal peel strength of 2.5 N / 10 mm or more and 15 N / 10 mm or less, the normal peel strength being measured at a test temperature of 23°C using a tensile tester at a tensile speed of 300 mm / min and a peel angle of 180 degrees after the adhesive surface of the adhesive layer is attached to an alkaline glass plate produced by a float process as an adherend and the contact angle with distilled water is 5 to 10 degrees and the test piece is left at room temperature for one day, in accordance with 10.4.1 Method 1 of JIS Z0237:2009: 180° peel adhesion relative to a test plate.

3. An adhesive sheet having an adhesive layer, The adhesive layer is formed of an adhesive composition, The adhesive composition contains a monomer component constituting an acrylic polymer, a multifunctional monomer, and at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton. Among the monomer components constituting the acrylic polymer, (meth)acrylic acid C 1-20 The proportion of alkyl esters is 35% by weight or more and 50% by weight or less, the proportion of hydroxyl-containing monomers is 20% by weight or more and 45% by weight or less, the proportion of monomers having nitrogen atoms is 1% by weight or more and 20% by weight or less, and the proportion of alicyclic hydrocarbon group-containing (meth)acrylates is 8% by weight or more and 40% by weight or less, The amount of the multifunctional monomer used is 0.01 to 0.1 parts by weight relative to 100 parts by weight of the monomer component. The multifunctional monomer is selected from trimethylolpropane tri(meth)acrylate or 1,6-hexanediol diacrylate, The stress of the adhesive sheet at 100% elongation is less than 30 MPa, and the product of the fracture stress σf [MPa] and the fracture strain εf [%] (σf×εf) ​​is greater than 300, wherein: The stress at 100% elongation, the fracture stress σf, and the fracture strain εf are measured by a tensile test performed at a tensile speed of 100 mm / min.

4. The adhesive sheet according to claim 3, wherein The adhesive layer is formed of an adhesive composition containing an acrylic partial polymer, a crosslinking agent, and a photopolymerization initiator.

5. The adhesive sheet according to claim 3 or 4, wherein The HLB of the surfactant is 10 or more and 20 or less.

6. The adhesive sheet according to any one of claims 1 to 3, wherein The adhesive layer is formed of a water-dispersible adhesive composition, a solvent-based adhesive composition, an active energy ray-curable adhesive composition, or a hot-melt adhesive composition.

7. The pressure-sensitive adhesive sheet according to any one of claims 1 to 3, which is a double-sided pressure-sensitive adhesive sheet. The adhesive layer constitutes at least one adhesive surface of the adhesive sheet. 8 . The pressure-sensitive adhesive sheet according to claim 7 , comprising a first pressure-sensitive adhesive layer and a second pressure-sensitive adhesive layer as the pressure-sensitive adhesive layer, and further comprising an intermediate layer disposed between the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer.

9. The adhesive sheet according to claim 8, wherein The intermediate layer is formed of a material including acrylic resin, polyurethane resin, urethane (meth)acrylate polymer, polyolefin resin, polyvinyl chloride resin, silicone, rubber or elastomer.

10. A method for peeling an adhesive sheet, which is a method for peeling an elongate adhesive sheet adhered to an adherend. The adhesive sheet is an adhesive sheet having an adhesive layer, The adhesive layer is formed of an adhesive composition, The adhesive composition contains a monomer component constituting an acrylic polymer, a multifunctional monomer, and at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton. Among the monomer components constituting the acrylic polymer, (meth)acrylic acid C 1-20 The proportion of alkyl esters is 35% by weight or more and 50% by weight or less, the proportion of hydroxyl-containing monomers is 20% by weight or more and 45% by weight or less, the proportion of monomers having nitrogen atoms is 1% by weight or more and 20% by weight or less, and the proportion of alicyclic hydrocarbon group-containing (meth)acrylates is 8% by weight or more and 40% by weight or less, The amount of the multifunctional monomer used is 0.01 to 0.1 parts by weight relative to 100 parts by weight of the monomer component. The multifunctional monomer is selected from trimethylolpropane tri(meth)acrylate or 1,6-hexanediol diacrylate, The peeling method includes the step of peeling the adhesive sheet by stretching it in a direction less than 90° with respect to the adhesive surface with respect to the adherend, The step of peeling the adhesive sheet is carried out in a state where an aqueous liquid is present at a portion of the adhesive interface between the adherend and the adhesive sheet that is exposed to peeling. The product of the breaking stress σf [MPa] and the breaking strain εf [%] (σf×εf) ​​of the adhesive sheet is 300 or more, wherein The fracture stress σf and the fracture strain εf are measured by a tensile test performed under the condition of a tensile speed of 100 mm / min.

11. A method for separating two adherends, the method comprising separating two adherends joined by an extensible adhesive sheet. The adhesive sheet is an adhesive sheet having an adhesive layer, The adhesive layer is formed of an adhesive composition, The adhesive composition contains a monomer component constituting an acrylic polymer, a multifunctional monomer, and at least one compound selected from a surfactant and a compound having a polyoxyalkylene skeleton. Among the monomer components constituting the acrylic polymer, (meth)acrylic acid C 1-20 The proportion of alkyl esters is 35% by weight or more and 50% by weight or less, the proportion of hydroxyl-containing monomers is 20% by weight or more and 45% by weight or less, the proportion of monomers having nitrogen atoms is 1% by weight or more and 20% by weight or less, and the proportion of alicyclic hydrocarbon group-containing (meth)acrylates is 8% by weight or more and 40% by weight or less, The amount of the multifunctional monomer used is 0.01 to 0.1 parts by weight relative to 100 parts by weight of the monomer component. The multifunctional monomer is selected from trimethylolpropane tri(meth)acrylate or 1,6-hexanediol diacrylate, The separation method includes the step of stretching the adhesive sheet in a direction of pulling it away from between the two adherends. The step of stretching the adhesive sheet is performed in a state where an aqueous liquid is present at a portion of the adhesive interface between at least one of the two adherends and the adhesive sheet that is exposed to peeling. The product of the breaking stress σf [MPa] and the breaking strain εf [%] (σf×εf) ​​of the adhesive sheet is 300 or more, wherein The fracture stress σf and the fracture strain εf are measured by a tensile test performed under the condition of a tensile speed of 100 mm / min.

Citation Information

Patent Citations

  • Block copolymer composition and its use as pressure-sensitive adhesive

    JP1999323072A

  • Pressure-sensitive adhesive composition, pressure- sensitive adhesive sheet using the same, and their production method

    JP2001234146A

  • Adhesive composition, pressure sensitive adhesive double coated tape, adhesion method and portable electronic device

    JP2007051271A

  • Adhesive sheet and method for peeling adhesive sheet

    JP2020023656A

  • Optical device, measurement device, robot, electronic apparatus, mobile body, and shape forming device

    JP2020034310A