A G3 grade steel ball grinding liquid and preparation method thereof

By rationally formulating and adjusting the ratio of oleic acid and diethylene glycol in the grinding fluid, a protective film is formed, which solves the problem that the existing grinding fluid cannot meet the requirements for fine grinding of G3 grade steel balls, and achieves high-quality lubrication and lubrication of the steel ball surface. Protection ensures G3 level processing effect.

CN115160985BActive Publication Date: 2024-10-11NANTONG SK SEIKO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210902947.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-10-11
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

The existing grinding fluids on the market cannot meet the strict requirements required during the fine grinding process of G3 grade steel balls, and cannot effectively lubricate and protect the surface of the steel balls, resulting in the steel balls not being able to achieve the required accuracy and quality after grinding.

Method used

Use a grinding fluid containing pH adjusters, lubricants, viscosity adjusters, emulsifiers, moisturizers, defoaming agents, rust inhibitors and bactericides to form a suitable protective film by adjusting the ratio of oleic acid and diethylene glycol , and prepare the grinding fluid through specific stirring steps to ensure the performance of the grinding fluid.

Benefits of technology

The grinding fluid can effectively protect the surface of the steel ball, reduce the single particle diameter, batch diameter variation and spherical error, improve the surface roughness, and ensure that the steel ball reaches the G3 quality standard after grinding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

A G3-grade steel ball grinding liquid and a preparation method thereof are provided. The grinding liquid is prepared by mixing 8% to 10% of a pH regulator, 21% to 27% of a lubricant, 3% to 5% of a viscosity regulator, 2% to 3% of an emulsifier, 1% to 2% of a moisturizer, 0.5% to 1% of a defoamer, 0.5% to 1% of a rust inhibitor, 0.2% to 1% of a bactericide, and the balance is 55% to 66% of deionized water. The grinding liquid has good film-forming property and good protection for the surface of the steel ball. After grinding, the variation of the diameter of a single steel ball can be less than 0.08um, the variation of the batch diameter can be less than 0.1um, the spherical error can be less than 0.08um, and the surface roughness can be less than 0.01um.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding liquid, in particular to a G3 grade steel ball grinding liquid and a preparation method thereof. Background Art

[0002] Steel balls are important components in bearings, especially in micro precision bearings. The quality of the steel ball surface directly affects the performance of the bearings. Generally speaking, steel balls need to go through cold heading, polishing, soft grinding, heat treatment, hard grinding, rough grinding and fine grinding steps. Among them, fine grinding is the most important step in steel ball processing, which determines the final quality of the steel ball. During the fine grinding process, grinding fluid is generally required to play a role in lubrication and grinding assistance, so that the steel ball can finally reach the required precision.

[0003] At present, the grades of steel balls are divided into G3, G5, G10, G16, G20...G100, G500, etc. Among them, the requirements for G3 grade steel balls are the most stringent, and the grinding fluids currently available on the market cannot meet the existing requirements. Therefore, it is necessary to develop a grinding fluid that can make the steel balls reach G3 grade after fine grinding. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a G3 grade steel ball grinding liquid and a preparation method thereof in view of the deficiencies of the above-mentioned prior art.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0006] A G3 grade steel ball grinding liquid comprises the following components by mass percentage:

[0007] 8%~10% PH regulator, 21%~27% lubricant, 3%~5% viscosity regulator, 2%~3% emulsifier, 1%~2% humectant, 0.5%~1% defoaming agent, 0.5%~1% rust inhibitor, 0.2%~1% bactericide, and the balance is 55%~66% deionized water.

[0008] Furthermore, the lubricant is 9% to 12% oleic acid and 12 to 15% diethylene glycol. Oleic acid and diethylene glycol play a lubricating role in the grinding liquid. Oleic acid is oily and diethylene glycol is water-based. By adjusting the ratio, a suitable protective film is formed on the surface of the steel ball. Usually, diethylene glycol is 1.2 to 1.3 times that of oleic acid.

[0009] Furthermore, the pH regulator is triethanolamine, which is used to adjust the pH value of the grinding liquid to ensure that the pH value of the grinding liquid is between 9 and 10.

[0010] Furthermore, the viscosity regulator is borate, which adjusts the overall viscosity of the grinding liquid and is used to control the fluidity of the steel balls during the grinding process. When the borate is lower than 3%, the viscosity of the grinding liquid is low, and the steel balls have a large impact on each other during the grinding process, which can easily cause damage to the surface of the steel balls. When the borate is higher than 5%, the grinding liquid is viscous as a whole, the fluidity of the steel balls in the grinding liquid is weakened, and normal grinding cannot be performed.

[0011] Furthermore, the emulsifier is fatty amine polyoxyethylene ether, and the emulsifier is used to promote the dissolution of oleic acid in deionized water.

[0012] Furthermore, the moisturizing agent is glycerin, and the moisturizing agent is used to lock the protective film on the surface of the steel ball.

[0013] Furthermore, the defoaming agent is silicone, and the defoaming agent eliminates a large amount of foam generated during the grinding process.

[0014] Furthermore, the rust inhibitor is benzotriazole, which prevents the steel ball from rusting.

[0015] Furthermore, the bactericide is a morpholine derivative, which prevents bacteria from growing and the grinding liquid from deteriorating.

[0016] A method for preparing a G3-grade steel ball grinding liquid comprises the following steps:

[0017] First, deionized water is heated to 60°C, oleic acid and fatty amine polyoxyethylene ether are added, and the mixture is rapidly stirred for 10 minutes. Then, triethanolamine is added to the resulting solution, and the mixture is rapidly stirred for 10 minutes. Subsequently, diethylene glycol, borate, glycerol, benzotriazole, and morpholine derivatives are successively added to the solution, and the mixture is stirred at medium speed for 30 minutes. Finally, silicone is added to the solution, and the mixture is slowly stirred for 10 minutes to obtain a grinding liquid.

[0018] Compared with the prior art, the grinding liquid of the present invention has good film-forming property on the surface of the steel ball under the same equipment and has good protection for the surface of the steel ball. After grinding, the variation of the diameter of a single steel ball can be less than 0.08um, the variation of the batch diameter can be less than 0.1um, the spherical error can be less than 0.08um, and the surface roughness can be less than 0.01um. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention will be described clearly and completely below.

[0020] Embodiment 1:

[0021] First, deionized water was heated to 60°C, 9% oleic acid and 1.3% fatty amine polyoxyethylene ether were added, and the mixture was stirred rapidly for 10 minutes. Then, 8.5% triethanolamine was added, and the mixture was stirred rapidly for 10 minutes. Subsequently, 11% diethylene glycol, 4% borate, 1.5% glycerol, 0.8% benzotriazole, and 0.5% morpholine derivative were added in sequence, and the mixture was stirred at medium speed for 30 minutes. Finally, 0.6% silicone was added to the solution, and the mixture was stirred slowly for 10 minutes to obtain the grinding liquid.

[0022] Embodiment 2:

[0023] Heat deionized water to 60°C, add 10% oleic acid and 1.5% fatty amine polyoxyethylene ether, stir rapidly for 10 minutes, then add 9% triethanolamine, stir rapidly for 10 minutes, then add 12% diethylene glycol, 3.8% borate, 1.5% glycerol, 0.8% benzotriazole, 0.5% morpholine derivative in sequence, stir at medium speed for 30 minutes, finally add 0.7% silicone to the solution, stir slowly for 10 minutes to obtain the grinding liquid.

[0024] Embodiment 3:

[0025] Heat deionized water to 60°C, add 11% oleic acid and 1.5% fatty amine polyoxyethylene ether, stir rapidly for 10 minutes, then add 9.5% triethanolamine, stir rapidly for 10 minutes, then add 13.5% diethylene glycol, 3.8% borate, 1.8% glycerol, 0.7% benzotriazole, 0.4% morpholine derivative in sequence, stir at medium speed for 30 minutes, finally add 0.7% silicone to the solution, stir slowly for 10 minutes to obtain the grinding liquid.

[0026] Embodiment 4:

[0027] Heat deionized water to 60°C, add 12% oleic acid and 2% fatty amine polyoxyethylene ether, stir rapidly for 10 minutes, then add 10% triethanolamine, stir rapidly for 10 minutes, then add 14.5% diethylene glycol, 3.5% borate, 1.5% glycerol, 0.7% benzotriazole, 0.5% morpholine derivative in sequence, stir at medium speed for 30 minutes, finally add 0.8% silicone to the solution, stir slowly for 10 minutes to obtain the grinding liquid.

[0028] Comparative Example 1:

[0029] Heat deionized water to 60°C, add 15% diethylene glycol, 4% borate, 2% glycerol, 0.8% benzotriazole, and 0.5% morpholine derivative in sequence, stir at medium speed for 30 minutes, then add 1% silicone, stir at slow speed for 10 minutes to prepare the grinding liquid.

[0030] Comparative Example 2:

[0031] Heat deionized water to 60°C, add 12% oleic acid and 2% fatty amine polyoxyethylene ether, stir rapidly for 10 minutes, then add 10% triethanolamine, stir rapidly for 10 minutes, then add 3.5% borate, 2% glycerol, 0.7% benzotriazole, 0.5% morpholine derivative in sequence, stir at medium speed for 30 minutes, finally add 1% silicone to the solution, stir slowly for 10 minutes to obtain the grinding liquid.

[0032] As shown in Table 1, the performance results of the embodiments and the comparative examples are

[0033]

[0034] Table 1

[0035] It can be seen that by adjusting the ratio of oleic acid and diethylene glycol in the grinding liquid, the grinding liquid can have good film-forming properties, ensuring that the steel ball can meet the G3 grade requirements after grinding.

[0036] The present invention is not limited to the described embodiments. Those skilled in the art may make some modifications or changes without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined in the claims.

Claims

1. A G3 grade steel ball grinding fluid, Features: The components are as follows by mass percentage: 8%~10% PH regulator, 21%~27% lubricant, 3%~5% viscosity regulator, 2%~3% emulsifier, 1%~2% moisturizer, 0.5%~1% defoamer, 0.5%~1% rust inhibitor, 0.2%~1% bactericide, and the balance is 55%~66% deionized water; The lubricant is 9% to 12% oleic acid and 12% to 15% diethylene glycol, and the amount of diethylene glycol is 1.2 to 1.3 times that of oleic acid; The pH regulator is triethanolamine; The viscosity modifier is a borate ester; The emulsifier is fatty amine polyoxyethylene ether; The moisturizing agent is glycerin; The defoaming agent is silicone; The rust inhibitor is benzotriazole; The bactericide is a morpholine derivative.

2. A method for preparing a G3 grade steel ball grinding liquid according to claim 1, Features: The following steps are involved: S1. Heat deionized water to 60°C, add oleic acid and fatty amine polyoxyethylene ether, and stir rapidly for 10 minutes; S2. Add triethanolamine to the solution of S1 and stir rapidly for 10 minutes; S3, add diethylene glycol, borate, glycerol, benzotriazole, and morpholine derivative to the solution of S2 in sequence, and stir at medium speed for 30 minutes; S4. Add silicone to the solution of S3 and stir slowly for 10 minutes to obtain a grinding liquid.