Decorative and protective coating compositions for metal, glass and plastic

By using a coating composition containing an inorganic-organic hybrid material containing titanium alkoxide, the adhesion and chemical resistance problems caused by complex pretreatment and powder coating layer thickness in the prior art are solved, and high adhesion, resistance and durability are achieved. Decorative coating that is corrosive and has broad tint capabilities, replacing the expensive anodizing process.

CN115175970BActive Publication Date: 2024-10-01EPG F SARL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180014961.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-20
Filing Date
2021-02-18
Publication Date
2024-10-01
Estimated Expiration
2041-02-18

AI Technical Summary

Technical Problem

Existing technologies for producing decorative and protective coatings on metal, glass and plastic substrates require complex and expensive pre-treatment steps and thick powder coating layers, resulting in reduced adhesion, chemical resistance and scratch resistance The rubability is insufficient, and the anodizing process is limited to color variety and uniformity.

Method used

Coating compositions using inorganic-organic hybrid materials containing titanium alkoxides, applied by wet chemical methods and thermally cured, including partially hydrolyzed alkoxysilanes, metal alkoxides, oligomeric alcohols, polyisocyanates and colorants to replace traditional powder coating and anodizing processes.

Benefits of technology

It achieves a decorative coating that provides high adhesion, corrosion resistance, UV stability, abrasion resistance, a wide color range, and good color uniformity without the need for a pretreatment layer, replacing expensive anodization. processes and complex pre-processing steps.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A coating composition, comprising: I. an inorganic-organic hybrid material, prepared from the following ingredients: A1. one or more partially hydrolyzed alkoxysilanes of formula (Ia), (R 1 O) n S i 2 3‑n R 3 (Ia) A2. Optionally one or more partially hydrolyzed alkoxysilanes of formula (Ib), (R 4 O) n S i 5 4‑n (Ib) B1. One or more metal alkoxides of formula (IIa), Ti(OR 6 )4(IIa)B2. Optionally one or more metal alkoxides of formula (IIb), M +(4‑m) (OR 7 ) 4‑m (IIb) wherein the symbols and numbers are as defined in the specification, and wherein the molar ratio of Si in components A1 and A2 to Ti in component B1 is 1-20:1; C. one or more oligomeric or polymeric polyols; D. one or more blocked, optionally modified polyisocyanates; and E. optionally one or more monomers, oligomers and / or polymers having one or more free epoxy groups; II. optionally one or more colorants and III. optionally one or more auxiliaries, which are particularly suitable for decorative and protective coatings for metal, glass and plastic substrates.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to an inorganic-organic coating composition, in particular a coating composition for metal, glass and plastic substrates, a method for coating a substrate with the coating composition of the present invention, and a substrate coated with the coating composition of the present invention.

[0002] Various processes are known in the prior art for producing decorative and / or protective surfaces for metal, glass and plastic substrates, such as powder coatings, in particular anodic layers for aluminium materials.

[0003] Powder coatings usually require several pretreatment steps. In addition to removing surface residues (paint, grease), these steps also include cleaning and applying several conversion coatings. The purpose of these coatings is to achieve a better match between surface and paint. Cleaning liquids based on ethanol or acetone evaporate at room temperature and do not leave any residue on the surface. Some base materials require pretreatment to control corrosion. Inadequate surface preparation can lead to reduced adhesion and even to spontaneous detachment or pits in the paint film. Typical processes in the field of powder coatings are phosphating of steel, coloring of galvanized steel, chroming and anodizing of aluminum. The thickness of the powder coating layer produced is usually between 60 and 120 μm. Depending on the specific application and the surface characteristics, the layer thickness can also be above or below this range.

[0004] Sometimes complex pretreatment steps are cost-intensive and should therefore be avoided. However, if pretreatment is not done correctly, there is a risk of loss of adhesion, which can result in rejects. Other disadvantages of powder coatings in the functional decorative sector are the relatively high layer thicknesses, which can lead to a plastic-like appearance and can impair the haptics. In addition, powder coatings for certain areas of application do not have adequate chemical and corrosion resistance as well as adequate scratch and abrasion resistance.

[0005] For aluminum and its alloys, the process often used to produce colored surfaces is the anodizing process. Depending on the production conditions and the aluminum alloy, the anodized layer is varied. Ordinary anodized coating is carried out at room temperature in a sulfuric acid electrolyte at a current density of 1.5A / dm2. Compared with the untreated surface, the anodized surface is transparent, which can protect the aluminum from corrosion and scratches to a certain extent. Hard anodized layers are carried out at a temperature of about 0°C in a mixed sulfuric acid electrolyte with a high current density of 2-5A / dm2. Compared with ordinary anodizing, they are characterized by particularly enhanced wear resistance and scratch resistance. The third technology is the Glossel anodizing technology. In this case, the metal is polished by electrolytic polishing before ordinary anodizing and then anodized in a sulfuric acid electrolyte. The anodized layer has a porous structure; dyes or other substances can optionally be embedded in these pores. The opening of the pores can be closed by compression in hot water. In this way, aluminum oxide hydrate (boehmite) is formed in the pores. Anodizing improves corrosion resistance compared to bright aluminum (aluminum itself), but one disadvantage of the anodized layer is its lack of pH stability (between pH 4 and 9). Of course, at pH values ​​outside this range, both bright aluminum and the anodized layer must be protected with a coating. There are several ways to produce colored anodized aluminum.

[0006] In the case of coloring with organic dyes, the anodized aluminum is immersed in a hot dye solution and then rinsed off. Coloring by this technology, the dye molecules mainly accumulate in the upper area of ​​the pores of the anodized layer and form bonds with the oxide layer. The greater the amount of dye in the solution, the greater the extent to which they accumulate in the oxide layer. In the case of inorganic dyes, after anodizing, the aluminum is neutralized in a dye bath (metal salt solution), rinsed and dyed. The ions in the solution accumulate in the pores of the anodized layer and become solid.

[0007] Electrolytic coloring is carried out under alternating voltage. The electrolyte contains colored metal salts. The duration of electrolysis depends on the desired color depth. The metal ions penetrate deeply into the pores of the layer. Due to absorption and scattering effects, the pores that are not filled with metal produce a color that is affected by light.

[0008] For decorative coloring of aluminum materials, the anodizing process is limited to a limited variety of colors, the main disadvantages are that not all types of aluminum can be colored by this method, and the above methods usually do not produce uniform coloring. In addition, not all aluminum alloys and semi-finished products can be colored using these expensive and inconvenient methods.

[0009] In order to avoid these problems of the known methods, which are the main methods still used today, proposals have been made to use hybrid materials, namely inorganic-organic sol-gel materials.

[0010] DE 10 2007 003761 A1 discloses a material and a method for coating substrates having heterogeneous surface properties using epoxide-functional or isocyanate-functional alkoxysilanes.

[0011] DE 43 38 361 A1 discloses a process for preparing compositions based on silanes containing epoxy groups. The coating compositions disclosed include nanoparticles as necessary.

[0012] DE 10 2012 022731 discloses a highly wear-resistant anti-lime layer having high chemical resistance.

[0013] DE 10 2013 017217 A1 discloses coated optical moldings.

[0014] WO 2017 / 067666 discloses a method for producing a coated light metal substrate, in particular an aluminum substrate, comprising the following steps: a) wet-chemically applying a coating composition to the light metal substrate and b) thermally curing the coating, wherein the coating composition comprises a sol-gel material and, if necessary, a complexing agent selected from 1,3-dicarbonyl compounds is added.

[0015] Although this prior art coating system has achieved good results, there is still room for improvement in view of the various different requirements placed on such coating systems:

[0016] Coating systems and methods for producing coatings that can be used must be suitable for producing creative decorative surfaces as an alternative to powder coating, especially anodic layers for aluminum and its alloys. They should be able to be applied without pretreatment layers or primers, and they should be able to conceal traces of pretreatment operations, such as sanding operations. For specific applications, the materials should be stable to hand sweat and UV radiation and should have high scratch and wear stability. They should also have high corrosion resistance; a wide range of color tinting should be possible without losing the above properties, and a high degree of color uniformity must be ensured.

[0017] The present invention surprisingly found that a coating composition comprising a specific inorganic-organic hybrid material can largely meet the above requirements, said specific inorganic-organic hybrid material comprising at least one titanium alkoxide.

[0018] Therefore, one subject of the present invention is a coating composition comprising

[0019] I. An inorganic-organic hybrid material, prepared by the following composition

[0020] A1. one or more partially hydrolyzed alkoxysilanes of formula (Ia),

[0021] (R 1 O) n S i 2 3-n R 3 (Ia)

[0022] in:

[0023] R 1 is C1-C6 alkyl or C1-C 10 Aryl,

[0024] R 2 is C1-C4 alkyl, C2-C4 alkenyl or C2-C4-alkynyl, C6-C 10 Aryl, C6-C 10 Arylalkyl or C6-C 10 Alkaryl,

[0025] R 3 is an epoxy functional group, and

[0026] n is 1, 2 or 3;

[0027] A2. optionally one or more partially hydrolyzed alkoxysilanes of formula (Ib),

[0028] (R 4 O) n S i 5 4-n (Ib)

[0029] in:

[0030] R 4 It is C1-C6 alkyl or C6-C 10 Aryl,

[0031] R 5 It is C1-C 10 Alkyl, C2-C4 alkenyl or C2-C4 alkynyl, C6-C 10 Aryl, C6-C 10 Arylalkyl or C6-C 10 Alkaryl, said group being optionally substituted by one or more, preferably one, amino group, and

[0032] n is 1, 2, 3 or 4;

[0033] B1 one or more metal alkoxides of formula (IIa),

[0034] Ti(OR 6 )4 (IIa)

[0035] in:

[0036] R 6 It is C1-C6 alkyl or C6-C 10 Aryl;

[0037] B2 optionally one or more metal alkoxides of formula (IIb),

[0038] M +(4-m) (OR 7 ) 4-m (IIb)

[0039] in:

[0040] M is a metal of the main group or transition group 3 or 4, except Ti, whose EN < 1.5,

[0041] R 7 is a C1-C6 alkyl group, or a C6-C 10 Aryl, and

[0042] m is 0 or 1, preferably 1,

[0043] The molar ratio of Si in components A1 and A2 to Ti in component B1 is 1-20:1;

[0044] C. One or more oligomeric alcohols or polymeric polyols

[0045] D. one or more blocked, optionally modified polyisocyanates; and

[0046] E. optionally one or more monomers, oligomers and / or polymers having one or more, preferably at least two, free epoxy groups;

[0047] II. Optional one or more colorants and

[0048] III. Optional one or more adjuvants.

[0049] Another subject of the present invention is a method for producing a coated substrate, comprising the following steps:

[0050] a) wet-chemically applying the coating composition of the invention to a substrate, and

[0051] b) Thermally curing coating compositions.

[0052] A further subject matter of the present invention is the use of the coating composition of the invention for coating substrates, preferably for coating metal, glass and plastic substrates, more preferably light metal substrates, very particularly aluminum substrates.

[0053] Likewise, the present invention provides substrates, preferably metal, glass and plastic substrates, more preferably light metal substrates, very particularly aluminum substrates, coated with the coating composition of the invention.

[0054] Coated substrates, especially decorative metal, plastic and glass substrates, produced using the coating compositions of the invention combine an excellent visual appearance with very good corrosion resistance, UV stability and scratch resistance.

[0055] By using a titanium component, a high hydrolysis rate of the alkoxysilane can be achieved (e.g., compared to the use of aluminum alkoxides). Due to the tetravalent nature of titanium compared to the trivalent nature of aluminum, a higher densification can be achieved in the final product. Another effect of using a titanium compound is a lower water content after the reaction and a lower haze of the coating.

[0056] The invention thus expands the possibilities of avoiding or replacing expensive anodizing processes, the use of alternative alloys and the use of milling, casting, die casting and sheet materials. Furthermore, the coating material of the invention is distinguished by improved process stability.

[0057] In particular, the present invention can obtain a coating having the following performance characteristics:

[0058] - Adhesion: Cross-cut (DIN EN ISO 2409) GT: 0;

[0059] - Adhesion after boiling test: (residence time in boiling DIN water 2 hours) GT: 1;

[0060] -Corrosion resistance: NSS-Test (DIN EN ISO 9227) 240h;

[0061] -UV aging:

[0062] - SUN test, in-house (DIN EN ISO 4892-2 method B6) 250 hours;

[0063] - SUN test, external (DIN EN ISO 4892-2 method A2) 500 hours;

[0064] -Abrasion resistance:

[0065] -Abrasion test (DIN EN ISO 60068-2-70) 50 000 times <20 mm 2 ;

[0066] -Hand sweat test 40 000 cycles;

[0067] - Tribometer test, successful 20 000 and 50 000 cycles with cotton cloth (no loss of gloss or color change);

[0068] -Surface hardness:

[0069] - Scratch resistance (DIN EN ISO 1518): 8 to 10N.

[0070] The coating composition of the present invention, i.e. I. inorganic-organic hybrid material, II. optionally one or more colorants, and III. optionally, one or more auxiliaries, may further comprise a diluent consisting of a moiety produced by synthesis and derived from partial hydrolysis of alcohol, and optionally also one or more further diluents. The coating composition of the present invention preferably consists of components I to III and a diluent containing a moiety produced by synthesis and derived from partial hydrolysis of alcohol, and optionally one or more additional diluents.

[0071] The inorganic-organic hybrid material is a block prepolymer prepared in situ, which is formed by condensation of hydrolyzable alkoxysilanes. It is obtained from the following components: A1, one or more partially hydrolyzed alkoxysilanes of formula (Ia); A2, optionally one or more partially hydrolyzed alkoxysilanes of formula (Ib); B1, one or more metal alkoxides of formula (IIa); B2, optionally one or more metal alkoxides of formula (IIb); C, one or more oligomeric or polymeric polyols; D, one or more blocked, optionally modified polyisocyanates; and E, optionally one or more monomers, oligomers and / or polymers, which have one or more, preferably at least two free epoxy groups.

[0072] Component A1

[0073] In the formula (Ia) of the partially hydrolyzed alkoxysilane, the symbols and numbers preferably have the following definitions:

[0074] R 1 Preferred are methyl, ethyl, propyl or butyl, the latter two groups are straight chain or branched, preferably straight chain, more preferably methyl or ethyl.

[0075] n is preferably 2 or 3, preferably 3.

[0076] R 2 Preferred is C1-C4 alkyl, more particularly methyl or ethyl.

[0077] R 3Preferred are epoxyalkyl groups, the alkyl groups of which may be interrupted by one or more heteroatoms, such as oxygen or nitrogen. The alkyl groups may also be substituted by one or more substituents, such as hydroxyl, amino, carboxyl or aryl. The alkyl groups may be linear, branched and / or cyclic. Preferred alkyl groups contain 1 to 20, in particular 1 to 10 carbon atoms outside the oxirane ring. More preferably, the alkyl groups are interrupted by oxygen atoms. Particularly preferred epoxy functional groups are glycidyloxypropyl groups.

[0078] Examples of suitable epoxy-modified alkoxysilanes include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3,4-epoxybutyltrimethoxysilane, 3,4-epoxybutyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-glycidoxypropyldimethylethoxysilane, 3-glycidoxypropyldimethylmethoxysilane, 3-glycidoxypropylmethyldiethoxysilane and 3-glycidoxypropylmethyldimethoxysilane.

[0079] "Partially hydrolyzed" in the context of the present invention means that the ratio of unhydrolyzed groups to hydrolyzed groups (ie, ROR ratio) is from 0.33 to 0.8.

[0080] The preferred molar ratio for partial hydrolysis is as follows: the ratio of silane of general formula (Ia) to water is generally 7.5:1 to 1:1.5, preferably 5:1 to 1:1, and more preferably the ratio is 1:1.

[0081] The partial hydrolysis can be carried out with acidic or alkaline catalysis or in a neutral medium. Acidic catalysis is preferred, in which case one or more acids are used, examples being hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid and organic acids such as acetic acid. In a preferred embodiment, the partial hydrolysis is carried out at least partially with phosphoric acid. The coatings produced therewith are characterized by high corrosion resistance and the absence of discoloration and blistering problems.

[0082] The epoxy functional groups do not hydrolyze under conditions that hydrolyze the functionalized alkoxysilane moieties.

[0083] Component A1 comprises one or more, preferably 1, 2 or 3, or 1 or 2, more particularly 1, alkoxysilane of the formula (Ia).

[0084] Component A2

[0085] The hybrid material comprises optionally one or more alkoxysilanes of formula (Ib) as component A2. In a preferred embodiment, the hybrid material comprises 1, 2, 3, 4 or 5, more preferably 1 to 4, alkoxysilanes of formula (Ib). In another preferred embodiment, the hybrid material does not comprise (zero) alkoxysilanes of formula (Ib).

[0086] The symbols and numbers in formula (Ib) preferably have the following definitions:

[0087] R 4 Preferred are methyl, ethyl, propyl or butyl, the latter two groups are straight chain or branched, preferably straight chain, more preferably methyl or ethyl.

[0088] R 5 It is C1-C8 alkyl, C6-C 10 Aryl, C6-C 10 Arylalkyl or C6-C 10 Alkaryl, said group is optionally substituted by one or more, preferably one, amino group.

[0089] n is preferably 3 or 4.

[0090] R 4 More preferred is a methyl group or an ethyl group.

[0091] R 5 More preferred is a methyl group, a hexyl group, a phenyl group or a 3-aminopropyl group.

[0092] More preferably, n is 3 or 4.

[0093] Particularly preferred alkoxysilanes of the formula (Ib) are tetraethoxysilane, methyltriethoxysilane, hexyltriethoxysilane, phenyltriethoxysilane and 3-aminopropyltriethoxysilane.

[0094] If alkoxysilanes of formula (Ib) are used, they are present in a mixture with alkoxysilanes of formula (Ia), so that for the partial hydrolysis the above statements regarding component A1 still apply. In this case, the above molar ratios refer to the sum of the alkoxysilanes of formula (Ia) and (Ib).

[0095] The inorganic fraction of the coating composition of the invention can be advantageously increased by adding the alkoxysilanes of component A2. The use of compounds such as hexyltriethoxysilane and phenyltriethoxysilane leads to increased hydrophobicity, improved corrosion control and, in the latter case, also increased UV stability.

[0096] Component B1

[0097] Component B1 of the hybrid material of the present invention comprises one or more titanium alkoxides of formula (IIa),

[0098] Ti(OR 6 )4 (IIa),

[0099] Where R 6 It is C1-C6 alkyl or C6-C 10 Aryl.

[0100] R 6 Preferred is a C1-C6 alkyl group, and more preferred is an n-butyl group.

[0101] The molar ratio of Si in components A1 and A2 to Ti in component B1 is 1-20:1, preferably 3-10:1, more preferably 4-8:1, very preferably 4.5-5.5:1.

[0102] The use of titanium alkoxides in component B1 has a significant effect, for example, the alkoxides can be added to the system without the need for additional stabilizing ligands. Ligands which have a stabilizing effect on metal alkoxides are known; here, chelate-forming ligands are usually used. However, a particular advantage of the present invention is that no stabilizers, in particular no chelating agents, need to be added to the coating composition.

[0103] Therefore, in a preferred embodiment, the coating composition of the invention comprises no complexing agents for stabilizing the metal alkoxides of formula (IIa) and (IIb), more preferably no chelating agents, particularly preferably no 1,3-dicarbonyl compounds.

[0104] However, if complexing agents are to be added which have a stabilizing effect on the metal alkoxide, 1,3-dicarbonyl compounds such as β-diketones and β-ketoesters are particularly suitable. Examples are ethyl acetoacetate, allyl acetoacetate, methacryloyloxyethyl acetoacetate, 3-acetyl-6-trimethoxysilylhexane-2-one, 2,2,6,6-tetramethyl-3,5-heptanedione, butyl acetate, ethyl benzoylacetate. Preferred complexing agents are β-diketones and β-ketoesters, more preferably acetylacetone (pentane-2,4-dione) and ethyl acetoacetate (ethyl 3-oxobutyrate), especially ethyl acetoacetate.

[0105] A preferred molar ratio of metal alkoxide of formula (IIa) and optionally (IIb) to complexing agent has proven to be 0.9:1.1, very preferably 1:1. If desired, the metal alkoxide complex can preferably be prepared at low temperatures, such as between -10°C and 0°C, more preferably in an ice bath at 0°C. The complexing agent is preferably added to the initial charge of metal alkoxide in the absence of air. Stirring is then preferably carried out, preferably for 8 to 48 hours, particularly preferably for 24 hours.

[0106] Component B2

[0107] The hybrid material optionally comprises one or more metal alkoxides of the formula (IIb) as component B2.

[0108] In a preferred embodiment, the hybrid material comprises one or more, preferably 1, 2 or 3, more preferably 1 or 2, metal alkoxides of formula (IIb). In another preferred embodiment, the hybrid material contains no (zero) metal alkoxide of formula (IIb).

[0109] Suitable metals M in formula (IIb) are metals of the main group and transition groups 3 and 4 of the Periodic Table of the chemical elements other than Ti, having an electronegativity <1.5 (according to the Pauling method); preferably Al, Zr and B. Particularly preferred is Al.

[0110] In formula (IIb), n is 0 or 1, preferably 1. X is preferably a group OR 7 .OR 7 Preferably C 1-6 Alkoxy or C 6-10 Aryloxy. Preferred groups OR 7 The preferred radicals are methoxy, ethoxy, propoxy and butoxy. Particularly preferred are ethoxy and sec-butoxy.

[0111] Particularly preferred compounds of formula (IIb) are aluminum alkoxides, more particularly aluminum tri-sec-butylate (aluminum tri-sec-butanolate).

[0112] If the hybrid material comprises a metal alkoxide of the formula (IIb), the molar ratio of Ti in component B1 to metal alkoxide B2 is at least 1:1.

[0113] With regard to the addition of complexing agents to the metal alkoxides in component B2, the above statements concerning component B1 apply analogously, which means that the coating composition of the invention preferably contains no stabilizing complexing agents, more preferably no chelating agents, particularly preferably no 1,3-dicarbonyl compounds.

[0114] Component C

[0115] Suitable as component C are oligomeric or polymeric polyols, for example polyvinyl alcohol (e.g. or other oligomers or polymers with free OH groups, such as polyesters and polyethers with OH groups, or polyacrylates with diols or polyols as alcohol component.

[0116] As component C, it is possible with preference to use polyester polyols, polyether polyols, polyether ester polyols, polycarbonate polyols, polyether carbonate polyols, polybutadiene derivatives, derivatives based on polysiloxanes, and mixtures thereof.

[0117] Suitable polyester polyols can be polycondensates of diols and optionally triols and tetraols and dicarboxylic acids and optionally tricarboxylic acids and tetracarboxylic acids or hydroxycarboxylic acids or lactones. Instead of free polycarboxylic acids, the corresponding polycarboxylic anhydrides or corresponding polycarboxylic acid esters of lower alcohols can also be used to prepare polyesters.

[0118] The polyester polyols are prepared in a conventional manner by polycondensation of aliphatic and / or aromatic polycarboxylic acids having 4 to 16 carbon atoms, which may optionally also be their anhydrides, and optionally their low molecular weight esters, including cyclic esters. Examples of suitable alcohols are ethylene glycol, butanediol, diethylene glycol, triethylene glycol, polyalkylene glycols such as polyethylene glycol, and 1,2-propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol and isomers, neopentyl glycol or neopentyl glycol hydroxypivalate, or mixtures thereof, preferably 1,6-hexanediol and its isomers, 1,4-butanediol, neopentyl glycol and neopentyl glycol hydroxypivalate. Furthermore, polyols such as trimethylolpropane, glycerol, erythritol, pentaerythritol, trimethylolbenzene or trishydroxyethyl isocyanurate or mixtures thereof can also be used. Particular preference is given to using diols, very preferably 1,4-butanediol and 1,6-hexanediol, very preferably 1,6-hexanediol.

[0119] As dicarboxylic acids according to the invention, for example phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexanedicarboxylic acid, adipic acid, azelaic acid, sebacic acid, glutaric acid, tetrachlorophthalic acid, maleic acid, fumaric acid, itaconic acid, malonic acid, suberic acid, 2-methylsuccinic acid, 3,3-diethylglutaric acid and / or 2,2-dimethylsuccinic acid may be used. The corresponding anhydrides may also be used as acid sources.

[0120] Furthermore, monocarboxylic acids such as benzoic acid and hexanecarboxylic acid can also be used.

[0121] Suitable compounds are available, for example, from Covestro as Branded commercially available products are particularly preferred D651 MDA / X, a branched polyester polyol. Also preferred is 1380 BT, a trifunctional polypropylene ether polyol.

[0122] The amount of component C is generally 5 to 25% by weight, based on the entire coating composition.

[0123] In the preparation of the coating composition of the present invention, the oligomer or polymer is usually diluted with a diluent, examples of which are one or more solvents, such as alcohols, glycols, esters and / or aromatic solvents. A preferred example is a glycol monoether acetate, such as propylene glycol monomethyl ether acetate (PGMEA, 1-methoxy-2-propyl acetate).

[0124] Component D

[0125] Suitable as component D according to the invention are blocked polyisocyanates based on, for example, 1,4-diisocyanatobutylene glycol, 1,6-diisocyanatohexamethylene (HDI), isophorone diisocyanate (IPDI), 2,2,4 and / or 2,4,4-trimethylhexamethylene diisocyanate, isomeric bis(4,4′-isocyanatocyclohexyl)methane (H12-MDI) or mixtures thereof with any desired isomer content, cyclohexylene 1,4-diisocyanate, 4-isocyanatomethyloctane-1,8-diisocyanate (nonane triisocyanate), isocyanatomethyloctane-1,8-diisocyanate (isocyanatomethyloctane-2,4-diisocyanate), isocyanatomethyloctane-2,8-diisocyanate (isocyanatomethyloctane-3,4-diisocyanate), isocyanatomethyloctane-3,8-diisocyanate (isocyanatomethyloctane-3,8-diisocyanate), isocyanatomethyloctane-4,4 ... Phenyl 1,4-diisocyanate, toluene 2,4- and / or 2,6-diisocyanate (TDI), naphthylene 1,5-diisocyanate, diphenylmethane 2,2'- and / or 2,4'- and / or 4,4'-diisocyanate (MDI), 1,3- and / or 1,4-bis(2-isocyanatopropyl-2-yl)benzene (TMXDI), 1,3-bis(isocyanatomethyl)benzene (XDI), 2,6-diisocyanatohexanoic acid alkyl esters with an alkyl group having 1 to 8 carbon atoms (lysine diisocyanate), and mixtures thereof. Suitable structural units of component D further include modifications, such as compounds containing allophanate, uretdione, carbamate, isocyanurate, biuret, iminooxadiazinedione or oxadiazinedione structures, based on the diisocyanates, as well as polycyclic compounds, such as polymeric MDI (pMDI), and combinations of all these compounds.

[0126] Particular preference is given to using blocked diisocyanates based on HDI and IPDI.

[0127] The isocyanate groups are partially or completely blocked and cannot react directly with the isocyanate-reactive groups. This ensures that the reaction only takes place at a certain temperature (blocking temperature). Typical blocking agents are known from the prior art and are selected from those which can be cleaved from the isocyanate groups in a temperature range between 60 and 220° C. (depending on the compound) before the diisocyanate can react with the isocyanate-reactive groups. Examples of typical blocking agents are caprolactam, methyl ethyl ketoxime, pyrazoles such as 3,5-dimethyl-2-pyrazole or 1-pyrazole, triazoles such as 1,2,4-triazole, diisopropylamine, diethyl malonate, diethylamine, phenol or its derivatives or imidazole.

[0128] Corresponding blocked isocyanates are commercially available, for example from Covestro as Particularly preferred are blocked polyisocyanates based on isophorone diisocyanate and hexamethylene diisocyanate, such as those commercially available from Covestro. PL 340 and 350.

[0129] The preferred modified polyisocyanate is uretdione, for example, Evonik Corporation sells Trade name: Commercially available product.

[0130] The amount of component D is generally 5 to 20% by weight, based on the entire coating composition.

[0131] Component E

[0132] As component E, the hybrid material optionally comprises one or more, preferably one, monomers, oligomers and / or polymers having one or more, preferably at least two, free epoxy groups.

[0133] Preferred E are di- and triglycidyl ethers and esters. Particularly preferred are 4,4'-isopropylidene diphenol diglycidyl ether (bisphenol A diglycidyl ether BPADGE), 1,2-cyclohexanedicarboxylic acid diglycidyl ester, 3,4-epoxycyclohexylmethyl ester 3,4-epoxycyclohexanecarboxylate, neopentyl glycol diglycidyl ether, trimethylolpropane triglycidyl ether and tris(4-hydroxyphenyl)methane triglycidyl ether, especially 4,4'-isopropylidene diphenol diglycidyl ether.

[0134] In a preferred embodiment, the hybrid material comprises one or more, preferably one monomer, oligomer and / or polymer having at least two free epoxy groups. In this case, the amount of component E is generally 5 to 25, preferably 10 to 20 mol %, based on the amount of component A1.

[0135] In a further preferred embodiment, the hybrid material, preferably the entire coating composition, comprises no monomers, oligomers or polymers having one or more free epoxy groups.

[0136] In a preferred embodiment, the hybrid material of the present invention is prepared from the following components:

[0137] A1. one or more (preferably 1) partially hydrolyzed alkoxysilanes of formula (Ia), preferably 3-glycidyloxypropyltrimethoxysilane;

[0138] A2. one or more (preferably 2 to 5) partially hydrolyzed alkoxysilanes of formula (Ib);

[0139] B1. A metal alkoxide of formula (IIa), preferably tetra-n-butyl titanate;

[0140] C. one or more (preferably 1) oligomeric or polymeric polyols, preferably branched polyesters and / or polyethers containing hydroxyl groups, more preferably branched polyesters containing hydroxyl groups;

[0141] D. one or more (preferably 1) blocked, optionally modified polyisocyanates, preferably blocked aliphatic polyisocyanates based on isophorone diisocyanate; and

[0142] E. Optionally one or more (preferably 1) monomers, oligomers and / or polymers having one or more, preferably at least two, free epoxy groups, preferably di- and / or triglycidyl ethers and / or esters, more preferably 4,4'-isopropylidene diphenol diglycidyl ether.

[0143] Here, a preferred embodiment is one in which component E consists of one or more (preferably 1) monomers, oligomers and / or polymers having one or more, preferably at least two, free epoxy groups, preferably di- and / or triglycidyl ethers and / or esters, more preferably 4,4'-isopropylidene diphenol diglycidyl ether.

[0144] Additionally preferred are those embodiments described which do not contain component E.

[0145] In this embodiment, component A2 preferably comprises at least one trialkoxysilane (n=3), preferably at least one trialkoxysilane wherein R 5 is a C1-C8 alkyl group, preferably a methyl group or a hexyl group, a phenyl group or a 3-aminopropyl group, more preferably at least three different trialkoxysilane groups, wherein R 5 In each case it is C1-C8-alkyl, preferably methyl or hexyl, phenyl or 3-aminopropyl.

[0146] In another preferred embodiment, component A2 comprises at least one tetraalkoxysilane (n=4), preferably tetraethoxysilane; and at least one trialkoxysilane (n=3), preferably at least one wherein R 5 is a C1-C8 alkyl group, preferably a methyl group, a hexyl group, a phenyl group or a 3-aminopropyl group; more preferably at least three different trialkoxysilanes, wherein R 5 In each case it is C1-C8-alkyl, preferably methyl or hexyl, phenyl or 3-aminopropyl.

[0147] II. Colorants

[0148] In addition to the hybrid material, the coating composition of the present invention optionally comprises one or more colorants.

[0149] In a preferred embodiment, the coating composition of the present invention comprises one or more, preferably 1 to 3, colorants.

[0150] In another preferred embodiment, the coating composition of the present invention contains no colorant.

[0151] The colorants added to achieve different color effects in the coating composition of the present invention can be pigments (organic and inorganic, colored inorganic ions or colored complexes, effect pigments) or soluble dyes. Representative examples of the various pigments available on the market are products from BASF SE, including the effect pigment Black Olive TM >, mica-based effect pigments, Pearlescent pigments, borosilicate based Pigments, Glaciers TM Frost white pigment, black graphite pigment, Mica-based effect pigments, Royal mica-based effect pigments, Pearlescent pigments, Pearlescent pigments, Glossy pigments, Vacuum metallized aluminum pigments, aluminum pigment pastes, such as Hydrolan, Effect pigments, Brilliant effect pigments, Santa FeTM color effect pigments or other pigments such as Chromaflow white, color and gold pigments, Timrex KS4, 200 and 299 or inclusive KS4, 200, mica effect pigments such as Royal Gold 323, carbon black pigments such as 200PWD, carbon black pigment pastes and lustrous copper such as 532. Metal complex dyes, such as cobalt complexes of anionic chromium and azo dyes. Examples of cations are sodium or substituted ammonium ions. Substituted soluble phthalocyanines also belong to this class.

[0152] Examples of organic azo pigments are: monoazo yellow and monoazo orange, naphthol, naphthol AS, azo lakes, benzimidazolone and organometallic complexes.

[0153] Examples of organic polycyclic pigments are: phthalocyanines, quinacridones, perylenes and perrenones, thioindigos, anthraquinones, dioxazines, isoindolinones and isoindolines, diketopyrrolopyrroles (DPP), triarylcarboniums and quinophthalones. Examples of inorganic pigments are: iron oxides, chromium oxide greens, ultramarine, Prussian blue, phthalocyanine greens, various mixed metal oxides, bismuth vanadates, manganese oxide (MnO). Examples of dyes include anthraquinone dyes, azo dyes, dioxazine dyes, indigo dyes, nitro and nitroso dyes, phthalocyanine dyes, sulfur dyes and triphenylmethane dyes. Specific examples are Congo red, methyl orange, rhodamine B or methyl red.

[0154] The amount of colorant required for 50 ml of coating solution depends on the desired color intensity and ranges from 0.1 to 20 g, preferably 1 to 15 g, more preferably 2 to 12 g.

[0155] The amount of colorant II is generally 0.1 to 40% by weight, based on the entire coating composition.

[0156] III.Adjuvant

[0157] The coating composition of the present invention optionally comprises one or more adjuvants.

[0158] In a preferred embodiment, the coating composition of the invention comprises one or more, preferably 1 to 10, auxiliaries. In this case, the amount of auxiliaries is generally 0.1 to 10% by weight, preferably 1 to 5% by weight, based on the entire coating composition.

[0159] In another preferred embodiment, the coating composition according to the invention contains no adjuvants.

[0160] Preferred auxiliaries are dispersants for one or more colorants and additives for adjusting the rheology, in particular wetting aids and flow control aids, such as those sold by the company Byk in a variety of different specifications. An example of a dispersant is Tego Dispers 670; an example of a rheological additive is Tego Glide 100. In addition, to increase the UV stability, UV stabilizers such as Eversorb 40, Eversorb 81 and / or Eversorb 95 can be added.

[0161] Other possible additives are nanoparticles (e.g. SiO2, TiO2, Al2O3, AlOOH, ZnO, B2O3, ZrO2, talc, mica) to produce mechanical and optical properties, which can be used in amounts of 0.1 to 40% by weight, based on the entire coating composition.

[0162] Besides the alcohol fraction originating from partial hydrolysis, synthetically produced, the coating composition of the invention optionally comprises one or more further diluents. The amount of diluent (alcohol and any other diluents), based on the entire coating composition, is generally 20 to 80% by weight.

[0163] The individual components of the coating composition of the present invention are usually already in a diluent. For example, in the production process of the coating composition of the present invention, the oligomer or polymer is usually used in a diluent, such as one or more solvents, such as alcohols, glycols, esters and / or aromatic solvents. A preferred example is a glycol monoether acetate, such as propylene glycol monomethyl ether acetate (PGMEA, 1-methoxy-2-propyl acetate).

[0164] Furthermore, for the production of coating solutions, commercial solvents are usually added to the base solution consisting of components I to III to establish a suitable viscosity; these commercial solvents are described in coating technical manuals. Examples of such solvents are fatty alcohols, fatty esters, alcohols containing alkoxy groups such as 1-methoxy-2-propanol, ketones, including their substitutions, for example butyl acetate or xylene or mixtures thereof.

[0165] The amount of the solvent added per 50 ml of the coating composition is 5-200 ml, preferably 10-100 ml, more preferably 10-20 ml.

[0166] The coating composition of the invention is advantageously produced in a plurality of stages.

[0167] First, a partial hydrolyzate (i.e., starting components A1 and optionally A2) is prepared. The partial hydrolysis can be carried out under acidic or alkaline catalysis or in a neutral medium. Acidic catalysis is preferred, in which case one or more acids are used, such as hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid or an organic acid such as acetic acid. In a preferred embodiment, the partial hydrolysis is at least partially carried out with phosphoric acid.

[0168] In a preferred embodiment, the partial hydrolyzate is prepared by mixing alkoxysilane (Ia and optionally Ib) with water, wherein the molar ratio of alkoxysilane (Ia and optionally Ib) to water is 7.5:1-1:1.5, preferably 5:1-1:1, more preferably 1:1, and vigorously stirring (preferably at room temperature). The stirring time is preferably 8 to 16 hours, more preferably 12 hours.

[0169] The base solution is prepared by reacting starting components A1 and optionally A2 with components B1 and optionally B2. This is generally carried out by mixing at a temperature preferably between -10°C and 0°C, particularly preferably in an ice bath at 0°C.

[0170] The mixing is preferably carried out by adding the metal alkoxide solution of components B1 and optionally B2 to the main hydrolyzate of alkoxysilane (A1 and optionally A2) under stirring, wherein the molar ratio of the two is 0.1:1-1:1, preferably 0.2:1-0.7:1, more particularly 0.3:1-0.6:1.

[0171] The stirring time, ie, the duration of uniform mixing, is generally 1 to 3 hours, preferably 1 to 2 hours, more preferably 90 minutes.

[0172] In order to complete the reaction, 3 to 100 ml, preferably 3 to 50 ml, more preferably 4 to 4.5 ml of distilled water is added dropwise to every 50 ml of the reaction solution, and then stirred for 1 to 5 hours, preferably 2 hours (basic solution).

[0173] To the resulting mixture of components A1 and optionally A2 and components B1 and optionally B2, an oligomeric or polymeric polyol, such as polyvinyl alcohol or polyester alcohol, is added as component C. The molar ratio of alkoxysilane (Ia and optionally Ib) to polyol is generally 2:1-1:2.

[0174] The coating composition comprises a blocked, optionally modified isocyanate as component D. Component D is generally added to the solution of components A, B and C with stirring.

[0175] The ratio of free hydroxyl groups to NCO groups in the polyols here is generally from 5:1 to 1:1, preferably from 2.5:1 to 1:1, more particularly from 1.2:1 to 1:1.

[0176] Optionally, the mixture can be admixed with one or more monomers, oligomers and / or polymers having at least two free epoxy groups as component E.

[0177] The reaction is completed by subsequent stirring, usually for 1 to 3 hours.

[0178] To produce the coating solution, commercial solvents are usually also added as diluents to the base solution to obtain the appropriate viscosity; these commercial solvents are described in coating technical manuals. Examples of such solvents are fatty alcohols, fatty esters, alcohols containing alkoxy groups such as 1-methoxy-2-propanol, ketones, including their substitutions such as butyl acetate or xylene, or mixtures thereof.

[0179] The amount of the diluent added per 50 ml of the coating composition is 5-200 ml, preferably 10-100 ml, more preferably 10-20 ml.

[0180] The base solution is optionally also admixed with auxiliaries III, examples of which are commercial additives for adapting the rheology, in particular wetting aids and flow control aids.

[0181] Furthermore, in order to achieve various color effects, the base solution is optionally admixed with colorants II, for example pigments (organic and inorganic, colored inorganic ions or colored complexes, effect pigments) or soluble dyes.

[0182] The method of the present invention for producing a coated substrate comprises the following steps:

[0183] a) wet-chemically coating the coating composition of the invention onto a substrate, and

[0184] b) Thermal curing of the coating composition.

[0185] The wet chemical application of the coating composition (step a)) can be carried out by conventional wet-chemical coating techniques known to those skilled in the art, for example, spraying, electrostatic spraying, dipping, pouring, spin coating, roller coating, spreading, blade coating or curtain coating. Printing methods such as screen printing can also be used. Spraying is preferred, for example, for application to bright anodized decorative strips.

[0186] The coating composition applied to the substrate is generally cured C (step b)) at a temperature of 80 to 240° C., preferably 120 to 230° C., more preferably 150 to 220° C., very preferably 180 to 210° C., more particularly 170 to 190° C.). If the curing comprises a first drying step, this step is generally carried out at a temperature of 80 to 120° C., and then further curing is generally carried out at a temperature of 160 to 240° C.

[0187] Curing can be accomplished by any suitable heat supply (ambient temperature, infrared radiation, microwave radiation). In the case of conventional heat supply, for example in an oven, the curing time is 2 to 120 minutes, more preferably 5 to 15 minutes, more particularly 12 minutes (at a temperature of 180 to 210°C).

[0188] Microwave curing is carried out using standard commercial equipment and the curing time is generally 5 to 20 minutes, more preferably 5 to 15 minutes.

[0189] For anodized surfaces, temperatures up to about 160° C. and curing times of about 1 hour are generally used. Thermal consolidation by IR or NIR radiation is also optionally possible.

[0190] The film thickness obtained by the process of the present invention is typically in the range of 3 to 15 μm.

[0191] Substrate

[0192] The coating compositions of the present invention and the methods of the present invention are used to produce decorative and protective coatings on surfaces and substrates. According to the present invention, the term "substrate" includes surfaces. Preferred are metal, glass and plastic substrates. Particularly preferred substrates include aluminum and its alloys, anodized aluminum, carbon steel, steel and its alloys, stainless steel, copper alloys, brass alloys and bronze. In another embodiment, the substrate may also be made of glass or plastic.

[0193] Preferred substrates are light metal substrates. Light metals in the sense of the present invention are substrates with a density of less than 5 g / cm 3Metals and alloys thereof. Preference is given to Al, Mg and Ti and their alloys; particular preference is given to Al and its alloys, in particular those with the elements Mn, Mg, Cu, Si, Ni, Zn and Be. The definition of aluminum alloys is in accordance with EN 573-3 / 4.

[0194] In another preferred embodiment, the substrate is a non-anodized aluminum substrate.

[0195] In another embodiment, the substrate is an anodized aluminum substrate.

[0196] The substrate coated with the coating composition of the invention can be a semi-finished product, such as a plate, sheet, tube, rod or wire, a structural component or a finished product. For example, it can be used for factory equipment, tools, household appliances such as irons, electrical components, switches, machines, vehicle and aircraft parts, especially automotive parts, luggage items such as suitcases, housings, production equipment, building facings, heat exchangers or parts thereof.

[0197] The coatings are particularly suitable for metal substrates, such as aluminum substrates, such as metal housings for electronic devices, parts for optical instruments, interior and exterior parts for vehicles, parts in mechanical engineering and plant construction, engines, parts for medical devices, parts for household appliances, other electrical appliances and turbines, household appliances, building cladding parts, elevator parts, conveyor parts, furniture parts, handles, seat parts, in particular for parts for vehicles and aircraft, garden tools, agricultural machinery, accessories, engine parts and general production plant equipment. In addition, they can also be used in the decorative field, such as fashion jewelry.

[0198] The present invention is further illustrated by the following examples, which do not have any limiting effect on the present invention. Example:

[0199] Example 1

[0200] Basecoat:

[0201] 244 mmol of 3-glycidyloxypropyltriethoxysilane was stirred with 6.60 g of 1M phosphoric acid and cooled to 10° C. Then 50 mmol of n-butyl titanate (titanium tetra-n-butoxide) was added, stirred and further cooled to 10° C. 220 mmol of water was added dropwise and further stirred.

[0202] 500 mmol of propylene glycol monomethyl ether acetate (PGMEA), 191 mmol of a hydroxyl-containing branched polyester (Desmophen D651 MPA / X) and 51 mmol of a blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340 BA / SN) were subsequently added, followed by stirring.

[0203] Silver paint production:

[0204] 244 mmol of 3-glycidyloxypropyltriethoxysilane was stirred with 6.60 g of 1M phosphoric acid and cooled to 10° C. Then 50 mmol of n-butyl titanate was added, stirred and further cooled to 10° C. 220 mmol of water was added dropwise and further stirred.

[0205] Then, 500 mmol of PGMEA, 191 mmol of a hydroxyl-containing branched polyester (Desmophen D651MPA / X) and 51 mmol of a blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340BA / SN) were added, followed by stirring. 100.0 g of PGMEA, 5.0 g of a surface additive and a rheological additive (Tego Dispers 6700 and Glide 100), 8.3 g of an aluminum color paste (Hydrolan STAPA S2100), 20.8 g of a mother-of-pearl pigment (Magnapearl 3100) and 8.0 g of a yellow-white pigment paste were added, followed by stirring.

[0206] The coating composition from Example 1 was applied by robotic spraying to non-anodized, pre-cleaned aluminum parts. The film thickness obtained was 12 μm. The coating was cured at a temperature of 160° C. in a forced-air oven for 60 minutes without pre-drying. The silver film obtained met the desired requirements.

[0207] Example 2

[0208] Preparation of primer:

[0209] 132 mmol of 3-glycidyloxypropyltriethoxysilane, 101 mmol of methyltrimethoxysilane, 31 mmol of tetraethoxysilane, 39 mmol of phenyltriethoxysilane and 13 mmol of hexyltrimethoxysilane were added, and 5.79 g of 1M phosphoric acid was added, stirred and mixed, and cooled to 10°C.

[0210] Then, 63 mmol of n-butyl titanate was added, and the mixture was further stirred and cooled to 10°C. 463 mmol of water was added dropwise to the mixture, and the mixture was further stirred. Subsequently, 624 mmol of PGMEA, 104 mmol of a hydroxyl-containing branched polyester (Desmophen D651 MPA / X), 28 mmol of a blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340BA / SN), 18 mmol of 4,4'-isopropyldiphenol diglycidyl ether, 10 mmol of 3-glycidyloxypropyltriethoxysilane and 5 mmol of 3-aminopropyltriethoxysilane were added, and the mixture was then stirred.

[0211] Production of bronze paint:

[0212] 132 mmol of 3-glycidyloxypropyltriethoxysilane, 101 mmol of methyltrimethoxysilane, 31 mmol of tetraethoxysilane, 39 mmol of phenyltriethoxysilane and 13 mmol of hexyltrimethoxysilane were added, and 5.79 g of 1M phosphoric acid was added, stirred and mixed, and cooled to 10°C.

[0213] Then, 63 mmol of n-butyl titanate was added, and the mixture was further stirred and cooled to 10°C. 463 mmol of water was added dropwise to the mixture, and the mixture was further stirred. Subsequently, 624 mmol of PGMEA, 104 mmol of a hydroxyl-containing branched polyester (Desmophen D651 MPA / X), 28 mmol of a blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340BA / SN), 18 mmol of 4,4'-isopropyldiphenol diglycidyl ether, 10 mmol of 3-glycidyloxypropyltriethoxysilane and 5 mmol of 3-aminopropyltriethoxysilane were added, and the mixture was then stirred.

[0214] Then 38.0 g of PGMEA, 5.5 g of surface and rheology additives (Tego Dispers 6700 and Glide 100), 22.63 g of mica effect pigment (Royal Gold 323), 1.13 g of carbon black pigment (200 PWD) were added and the mixture was then stirred.

[0215] Example 3

[0216] To 103mmol 3-glycidyloxypropyltriethoxysilane were added 79mmol methyltrimethoxysilane, 24mmol tetraethoxysilane, 31mmol phenyltriethoxysilane and 11mmol hexyltrimethoxysilane, 4.53g 1M phosphoric acid, and the mixture was stirred and cooled to 10°C.

[0217] Thereafter, 49 mmol of n-butyl titanate was added, the mixture was further stirred and cooled to 10° C. 363 mmol of water was further added dropwise to the mixture, followed by stirring. 470 mmol of acetone, 282 mmol of isopropylidene glycerol, 54.2 g of a hydroxyl-containing branched polyester (Plusodur V730S), 66 mmol of a blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340 BA / SN), 14 mmol of 4,4′-isopropylidene diphenol diglycidyl ether, 8 mmol of 3-glycidyloxypropyltriethoxysilane and 4 mmol of 3-aminopropyltriethoxysilane were then added, and the mixture was further stirred.

[0218] Production of high-gloss black paint:

[0219] To 103mmol 3-glycidyloxypropyltriethoxysilane were added 79mmol methyltrimethoxysilane, 24mmol tetraethoxysilane, 31mmol phenyltriethoxysilane and 11mmol hexyltrimethoxysilane, 4.53g 1M phosphoric acid, and the mixture was stirred and cooled to 10°C.

[0220] Thereafter, 49 mmol of n-butyl titanate was added, further stirred and cooled to 10° C. Further, 363 mmol of water was added dropwise to the mixture, followed by stirring.

[0221] Then 470 mmol acetone, 282 mmol isopropylidene glycerol, 54.2 g hydroxyl-containing branched polyester (Plusodur V730S), 66 mmol blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340 BA / SN), 14 mmol 4,4'-isopropylidene diphenol diglycidyl ether, 8 mmol 3-glycidyloxypropyltriethoxysilane and 4 mmol 3-aminopropyltriethoxysilane were added, and the mixture was further stirred. Then 50.0 g acetone, 69.0 g isopropylidene glycerol, 4.0 g surface additives and rheological additives (Tego Dispers 6700 and Glide 100) and 30.0 g carbon black pigment paste were added, and the mixture was then stirred.

[0222] Example 4

[0223] To 173 mmol of 3-glycidyloxypropyltriethoxysilane were added 133 mmol of methyltrimethoxysilane, 40 mmol of tetraethoxysilane, 51 mmol of phenyltriethoxysilane and 18 mmol of hexyltrimethoxysilane. 7.59 g of 1M phosphoric acid was added, followed by stirring and cooling to 10° C. Thereafter, 82 mmol of n-butyl titanate was added, further stirred and cooled to 10° C. 606 mmol of water was added dropwise to the mixture, followed by stirring.

[0224] Subsequently, 434 mmol of PGMEA, 19.33 g of trifunctional polypropylene ether polyol (Desmophen D1380BT), 28 mmol of blocked aliphatic polyisocyanate based on isophorone diisocyanate (Desmodur PL340 BA / SN), 24 mmol of 4,4'-isopropyldiphenol diglycidyl ether, 14 mmol of 3-glycidyloxypropyltriethoxysilane and 7 mmol of 3-aminopropyltriethoxysilane were added and further stirred.

Claims

1. A coating composition comprising I. An inorganic-organic hybrid material, prepared from the following ingredients A1. one or more partially hydrolyzed alkoxysilanes of formula (Ia), (R 1 O) n SiR 2 3-n R 3 (Ia) in: R 1 It is C 1 -C 6 Alkyl or C 1 -C 10 Aryl, R 2 It is C 1 -C 4 Alkyl, C 2 -C 4 Alkenyl or C 2 -C 4 -Alkynyl, C 6 -C 10 Aryl, C 6 - C 10 Arylalkyl or C 6 -C 10 Alkaryl, R 3 is an epoxy functional group, and n is 1, 2 or 3; A2. optionally one or more partially hydrolyzed alkoxysilanes of formula (Ib), (R 4 O) n SiR 5 4-n (Ib) in: R 4 It is C 1 -C 6 Alkyl or C 6 -C 10 Aryl, R 5 It is C 1 -C 10 Alkyl, C 2 -C 4 Alkenyl or C 2 -C 4 Alkynyl, C 6 -C 10 Aryl, C 6 -C 10 Arylalkyl or C 6 -C 10 Alkaryl, the R 5 The group is optionally substituted with one or more amino groups, and n is 1, 2, 3 or 4; B1. one or more metal alkoxides of formula (IIa), Ti(OR 6 ) 4 (IIa) in: R 6 It is C 1 -C 6 Alkyl or C 6 -C 10 Aryl; B2. optionally one or more metal alkoxides of formula (IIb), M+ (4-m) (OR 7 ) 4-m (IIb) in: M is Al, Zr or B, R 7 It is C 1 -C 6 Alkyl, or C 6 -C 10 Aryl, and m is 0 or 1, The molar ratio of Si in components A1 and A2 to Ti in component B1 is 1-20:1; C. one or more polymeric polyols; D. one or more blocked polyisocyanates; and E. optionally one or more monomers and / or polymers having one or more free epoxy groups; II. Optional one or more colorants and III. Optional one or more adjuvants.

2. The coating composition according to claim 1, wherein in formula (Ia): R 1 It is C 1 -C 4 alkyl, R 3 is 3-glycidyloxypropyl, and n is 3.

3. A coating composition according to claim 1 or 2, wherein component C is one or more oligomeric polyols.

4. The coating composition according to claim 1 or 2, wherein the D component is one or more modified blocked polyisocyanates.

5. A coating composition according to claim 1 or 2, wherein the E component is optionally one or more monomers and / or oligomers having one or more free epoxy groups.

6. The coating composition according to claim 1 or 2, wherein the one or more partially hydrolyzed alkoxysilanes of formula (Ia) are 3-glycidoxypropyltrimethoxysilane and / or 3-glycidoxypropyltriethoxysilane.

7. The coating composition according to any one of claims 1 or 2, wherein one or more compounds of formula (Ib) are not optional but essential.

8. According to the claim 7 A coating composition wherein the one or more compounds of formula (Ib) are selected from tetraethoxysilane, methyltriethoxysilane, hexyltriethoxysilane, phenyltriethoxysilane, aminopropyltriethoxysilane, and mixtures of two or more thereof.

9. The coating composition according to any one of claims 1 or 2, wherein the partial hydrolysis of the compound of formula (Ia), or the compound of (Ia) and the compound of formula (Ib), is carried out in an acidic medium.

10. The coating composition according to any one of claims 1 or 2, in, The one or more metal alkoxides of formula (IIa) is titanium tetra-n-butoxide.

11. The coating composition according to any one of claims 1 or 2, wherein in formula (IIb): M is Al, Zr or B; R 7 It is C 1 -C 6 Alkyl, and m is 0 or 1.

12. The coating composition according to any one of claims 1 or 2, wherein component E comprises one or more di- or tri-glycidyl ethers or di- or tri-glycidyl esters.

13. The coating composition according to any one of claims 1 or 2, wherein component C used comprises a branched polyester polyol.

14. The coating composition according to claim 1, wherein component D used comprises one or more blocked polyisocyanates based on isophorone diisocyanate or hexamethylene diisocyanate.

15. A method for producing a coated substrate, The following steps are involved: a) applying the coating composition according to any one of claims 1 to 11 wet-chemically to a substrate, and b) thermally curing the coating composition.

16. The method according to claim 15, in, The heat curing time is in the range of 2 minutes to 2 hours.

17. The method according to claim 15 or 16, wherein the thermal curing in step b) is carried out at a temperature in the range of 80 to 240°C.

18. The method according to any one of claims 15 or 16, in, The substrates are metal, glass and plastic substrates.

19. The method according to claim 15, in, The substrate is an aluminum substrate.

20. A coated substrate, wherein the coating composition according to any one of claims 1 to 14 is coated on the substrate.

21. The coated substrate according to claim 20, wherein the substrate is metal, glass or plastic.

22. A coated substrate according to claim 21, wherein the substrate is aluminium.

23. Use of a coating composition according to any one of claims 1 to 14 for coating a substrate.

24. The use according to claim 23, wherein the substrate is metal, glass and plastic.

25. Use according to claim 23, wherein the substrate is aluminum.