Pre-lithiated binary topological structure phosphorus / carbon composite material and its preparation method and application

The binary topology phosphorus/carbon composite material formed through pre-lithiation treatment solves the problems of high-rate charge-discharge cycle stability and low first Coulomb efficiency of lithium-ion battery phosphorus-based composite materials, achieving efficient electrochemical performance improvement. .

CN115188936BActive Publication Date: 2024-10-18TIANJIN UNIV +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210661740.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-27
Publication Date
2024-10-18
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

Phosphorus-based composite anode materials for lithium-ion batteries have deficiencies in high-rate charge-discharge cycle stability and first Coulombic efficiency, resulting in safety hazards and performance limitations.

Method used

A pre-lithiated binary topology phosphorus/carbon composite material is designed. The phosphorus source is coated with a coating material and carbonized at high temperature, and then lithiated to form a lithiated x-dimensional phosphorus/y-dimensional carbon structure, which is optimized Improve the conductivity and structural stability of the material.

Benefits of technology

It improves the first Coulomb efficiency and high-rate charge and discharge performance of phosphorus-based anode materials, enhances the conductivity and cycle stability of the material, and achieves high theoretical specific capacity and improved safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115188936B_ABST
    Figure CN115188936B_ABST
Patent Text Reader

Abstract

The present invention relates to a pre-lithiated binary topological structure phosphorus / carbon composite material, a preparation method and an application thereof. The present invention provides a pre-lithiated binary topological structure phosphorus / carbon composite material, which is lithiated x-dimensional phosphorus / y-dimensional carbon, wherein x and y are both integers, and 0≤x<3, 1≤y≤3. The present invention also provides a method for preparing the pre-lithiated binary topological structure phosphorus / carbon composite material: (a) mixing a phosphorus source and a lithium source, and performing a lithiation treatment on the phosphorus source with a lithium source to obtain a lithium phosphide material; (b) mixing and heating the lithium phosphide material obtained in step (a) and a carbon-based material to obtain a pre-lithiated binary topological structure phosphorus / carbon composite material. The pre-lithiated binary topological structure phosphorus / carbon composite material prepared by the present invention has a high theoretical specific capacity and a relatively high electrical conductivity, and also ensures a high first coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the parent application with application number 201911376368.7, invention name “Pre-lithiation binary topological structure phosphorus / carbon composite material and preparation method and application” and application date December 27, 2019. Technical Field

[0002] The invention belongs to the field of lithium ion battery electrode materials, and in particular relates to a pre-lithiated binary topological structure phosphorus / carbon composite material and a preparation method and application thereof. Background Art

[0003] Lithium-ion batteries stand out among many secondary battery systems due to their high energy density, and have successfully occupied the portable electronic device market in just over two decades. However, with the rise of some new energy storage devices such as power batteries and fixed energy storage power stations, new requirements have been put forward for the development of secondary batteries. Power batteries not only require high energy density, but also high rate performance and safety performance. However, graphite, the main negative electrode material of lithium-ion batteries currently commercialized, has a low electrode potential and is prone to form "lithium dendrites" at high current density, thus posing a safety hazard. A spinel structure Li with "zero strain" 4 Ti 5 O 12 Due to its high electrode potential (1.5V vs Li / Li + ), it is not easy to form "lithium dendrites" during the charge and discharge process, and its high safety performance has attracted widespread attention. However, its low theoretical specific capacity (175mAh / g) limits its widespread application in lithium-ion batteries. As an emerging negative electrode material, phosphorus has the advantages of low price, abundant reserves, environmental friendliness, and high specific capacity, and has gradually developed into the focus of negative electrode research. In addition, compared with silicon (0.4V vs Li / Li + ), graphite (0.1Vvs Li / Li + ) negative electrode, which has a higher electrode potential (0.7Vvs Li / Li + ), which is conducive to achieving the safety of power batteries under high-rate charge and discharge conditions. However, the poor conductivity of phosphorus and the large volume change during charge and discharge limit the development of phosphorus.

[0004] Phosphorus has many allotropes: white phosphorus, amorphous red phosphorus, purple phosphorus, fibrous phosphorus, black phosphorus, and blue phosphorus. Among them, the application of amorphous red phosphorus, purple phosphorus, black phosphorus, and blue phosphorus in lithium-ion battery negative electrode materials has been confirmed experimentally or theoretically. In recent years, in order to give full play to the advantages of phosphorus' high theoretical specific capacity, researchers have conducted a lot of scientific research, mainly focusing on the composite of red phosphorus or black phosphorus with carbon-based materials with good conductivity. According to the different dimensions (D) and bonding methods of phosphorus and carbon, a variety of phosphorus / carbon binary topological structures can be formed. For example, Liu Cheng et al. introduced the phosphorus-carbon binary topological structure in “Design of phosphorus-carbon binary topological structure and its application in energy storage” (Energy Storage Science and Technology, Volume 7, Issue 6), including the binary topological structures of red phosphorus / carbon 0D / 0D, 0D / 1D, 1D / 1D, 0D / 2D, 2D / 2D, 0D / 3D and the binary topological structures of black phosphorus / carbon 0D / 0D, 0D / 1D, 2D / 2D. In Chinese Patent Publication No. CN109148870A, the surface oxidation and freeze-drying treatment were carried out. The graphite and nanotubes are used as the base material, mixed with red phosphorus solid powder and sealed in a tube, and calcined at high temperature to effectively fill the red phosphorus into the interlayer spacing of the base material, forming a 0D (red phosphorus) / 2D (carbon) structure. These phosphorus-carbon binary topological structures can effectively improve the conductivity of the electrode material, alleviate the structural collapse and pulverization problems caused by volume changes during lithium ion charging and discharging, and improve the cycle stability of the phosphorus negative electrode, but its first coulombic efficiency is low, and the high-rate charge and discharge performance needs to be further improved. Summary of the invention

[0005] In response to the current technical problems of high-rate charge and discharge cycle stability and low first coulombic efficiency of phosphorus-based composite negative electrode materials for lithium-ion batteries, the inventors of the present invention have designed a phosphorus-carbon binary topological structure and modification method with a confinement effect after long-term research, aiming to improve the first coulombic efficiency and high-rate charge and discharge performance of phosphorus-based negative electrode materials.

[0006] To this end, the present invention provides the following first set of technical solutions.

[0007] A pre-lithiated binary topological structure phosphorus / carbon composite material is lithiated x-dimensional phosphorus / y-dimensional carbon, wherein x and y are both integers, and 0≤x<3, 1≤y≤3.

[0008] Preferably, according to the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, the phosphorus is amorphous red phosphorus, purple phosphorus, fibrous phosphorus, black phosphorus or blue phosphorus.

[0009] Preferably, according to the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, the carbon is a one-dimensional tubular carbon-based material, a two-dimensional layered carbon-based material or a three-dimensional porous carbon material.

[0010] The present invention also provides a method for preparing the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, which comprises the following steps:

[0011] (a) coating a phosphorus source with a coating material, and then carbonizing it at high temperature to obtain a binary topological structure of x-dimensional phosphorus / y-dimensional carbon, wherein x and y are both integers, and 0≤x<3, 1≤y≤3;

[0012] (b) treating the binary topological structure x-dimensional phosphorus / y-dimensional carbon obtained in step (a) with a lithium source.

[0013] Preferably, according to the above preparation method, the coating material is a substance that forms a carbon or nitrogen-doped carbon-based material after pyrolysis.

[0014] Preferably, according to the above preparation method, the coating material is an organic amine compound.

[0015] Preferably, according to the above preparation method, the coating material is dopamine.

[0016] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis.

[0017] Preferably, according to the above preparation method, the phosphorus source is a phosphorus oxide compound.

[0018] Preferably, according to the above preparation method, the phosphorus source is phosphorus pentoxide.

[0019] Preferably, according to the above preparation method, the carbonization temperature is 300-1000°C.

[0020] Preferably, according to the above preparation method, the carbonization temperature is 350-800°C.

[0021] Preferably, according to the above preparation method, the carbonization temperature is 500-700°C.

[0022] Preferably, according to the above preparation method, the mass ratio of lithium to phosphorus in the lithium source and phosphorus source is 1:1-1:200.

[0023] Preferably, according to the above preparation method, the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic composite solution.

[0024] Preferably, according to the above preparation method, the lithiation treatment temperature is 180-400°C.

[0025] Preferably, according to the above preparation method, the phosphorus source and the coating material have an elemental mass ratio of phosphorus to carbon of 3:1-30:1.

[0026] The present invention also provides a second method for preparing the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, which comprises the following steps:

[0027] (a) placing a phosphorus source and a carbon-based material in two heating temperature zones of a tubular furnace chamber and heating them to obtain a binary topological structure of x-dimensional phosphorus / y-dimensional carbon, wherein x and y are both integers, and 0≤x<3, 1≤y≤3;

[0028] (b) treating the binary topological structure x-dimensional phosphorus / y-dimensional carbon obtained in step (a) with a lithium source.

[0029] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis.

[0030] Preferably, according to the above preparation method, the phosphorus source is red phosphorus.

[0031] Preferably, according to the above preparation method, the carbon-based material is graphite, expanded graphite, graphitic acid or porous carbon.

[0032] Preferably, according to the above preparation method, the phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 3:1-30:1.

[0033] Preferably, according to the above preparation method, the heating temperature of the phosphorus source is 400-500°C, and the heating temperature of the carbon-based material is 200-350°C.

[0034] Preferably, according to the above preparation method, the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic composite solution.

[0035] Preferably, according to the above preparation method, the lithiation treatment temperature is 180-400°C.

[0036] Preferably, according to the above preparation method, the mass ratio of lithium to phosphorus in the lithium source and phosphorus source is 1:1-1:200.

[0037] The present invention also provides a third method for preparing the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, which comprises the following steps:

[0038] (a) mixing a carbon-based material and a lithium source, and performing a lithiation treatment on the carbon-based material with the lithium source to obtain a lithiated carbon-based material;

[0039] (b) mixing and heating the lithiated carbon-based material obtained in step (a) and a phosphorus source to obtain a pre-lithiated binary topological structure phosphorus / carbon composite material.

[0040] Preferably, according to the above preparation method, the carbon-based material is graphite, expanded graphite or porous carbon.

[0041] Preferably, according to the above preparation method, the carbon-based material is expanded graphite.

[0042] Preferably, according to the above preparation method, the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic composite solution.

[0043] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis.

[0044] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus.

[0045] Preferably, according to the above preparation method, the phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:2-10:1.

[0046] Preferably, according to the above preparation method, the mass ratio of lithium to phosphorus in the lithium source and phosphorus source is 1:1-1:200.

[0047] Preferably, according to the above preparation method, the lithiation treatment temperature is 200-800°C.

[0048] Preferably, according to the above preparation method, the lithiation treatment temperature is 200-500°C.

[0049] Preferably, according to the above preparation method, the heating temperature in step (b) is 200-400°C.

[0050] Preferably, according to the above preparation method, the heating time in step (b) is 1-4 hr.

[0051] The present invention also provides a fourth method for preparing the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, which comprises the following steps:

[0052] (a) mixing a phosphorus source and a lithium source, and subjecting the phosphorus source to lithiation with the lithium source to obtain a lithium phosphide material;

[0053] (b) mixing and heating the lithium phosphide material and the carbon-based material obtained in step (a) to obtain a pre-lithiation binary topological structure phosphorus / carbon composite material.

[0054] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis.

[0055] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus.

[0056] Preferably, according to the above preparation method, the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic composite solution.

[0057] Preferably, according to the above preparation method, the lithium source is lithium foil.

[0058] Preferably, according to the above preparation method, the mass ratio of lithium to phosphorus in the lithium source and phosphorus source is 1:1-1:200.

[0059] Preferably, according to the above preparation method, the lithiation treatment temperature is 200-800°C.

[0060] Preferably, according to the above preparation method, the lithiation treatment temperature is 200-400°C.

[0061] Preferably, according to the above preparation method, the heating temperature in step (b) is 200-400°C.

[0062] Preferably, according to the above preparation method, the heating time in step (b) is 1-4 hr.

[0063] Preferably, according to the above preparation method, the carbon-based material is expanded graphite or graphitic acid.

[0064] Preferably, according to the above preparation method, the carbon-based material is expanded graphite.

[0065] Preferably, according to the above preparation method, the phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-20:1.

[0066] The present invention also provides a fifth method for preparing the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material, which comprises the following steps:

[0067] (a) The phosphorus source and the conductive carbon material are directly mixed by ball milling or hand milling.

[0068] (b) mixing the phosphorus-carbon composite material obtained in step (a) with a lithium source and heating them to obtain a pre-lithiated binary topological structure phosphorus / carbon composite material.

[0069] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis.

[0070] Preferably, according to the above preparation method, the phosphorus source is elemental phosphorus.

[0071] Preferably, according to the above preparation method, the carbon-based material is graphite, porous carbon, activated carbon, or carbon nanotubes.

[0072] Preferably, according to the above preparation method, the carbon-based material is carbon nanotubes.

[0073] Preferably, according to the above preparation method, the phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-15:1.

[0074] Preferably, according to the above preparation method, the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic composite solution.

[0075] Preferably, according to the above preparation method, the lithium source is lithium foil.

[0076] Preferably, according to the above preparation method, the mass ratio of lithium to phosphorus in the lithium source and phosphorus source is 1:1-1:200.

[0077] Preferably, according to the above preparation method, the lithiation treatment temperature is 200-800°C.

[0078] Preferably, according to the above preparation method, the lithiation treatment temperature is 300-500°C.

[0079] The present invention also provides a lithium ion battery negative electrode, the active material of which is the above-mentioned pre-lithiation binary topological structure phosphorus / carbon composite material.

[0080] The present invention also provides a lithium ion battery, which comprises the above lithium ion battery negative electrode.

[0081] In addition, in order to solve the above-mentioned problems in the prior art, the present invention also provides the following second set of technical solutions.

[0082] 1. A method for preparing a pre-lithiated binary topological structure phosphorus / carbon composite material, wherein the pre-lithiated binary topological structure phosphorus / carbon composite material is lithiated x-dimensional phosphorus / y-dimensional carbon, wherein x and y are both integers, and 0≤x<3, 1≤y≤3; the preparation method comprises the following steps:

[0083] (a) mixing a phosphorus source and a lithium source, and subjecting the phosphorus source to lithiation with the lithium source to obtain a lithium phosphide material;

[0084] (b) mixing and heating the lithium phosphide material and the carbon-based material obtained in step (a) to obtain a pre-lithiation binary topological structure phosphorus / carbon composite material.

[0085] 2. The preparation method according to technical solution 1, wherein the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis; preferably, the phosphorus source is elemental phosphorus.

[0086] 3. The preparation method according to technical solution 1 or 2, wherein the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic complex solution; preferably, the lithium source is lithium foil.

[0087] 4. The preparation method according to any one of technical solutions 1-3, wherein the mass ratio of lithium to phosphorus in the lithium source and the phosphorus source is 1:1-1:200.

[0088] 5. The preparation method according to any one of technical solutions 1-4, wherein the lithiation treatment temperature is 200-800°C; preferably, the lithiation treatment temperature is 200-400°C.

[0089] 6. The preparation method according to any one of technical solutions 1 to 5, wherein the carbon-based material is expanded graphite or graphitic acid; preferably, the carbon-based material is expanded graphite.

[0090] 7. A preparation method according to any one of technical solutions 1-6, wherein the phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-20:1.

[0091] 8. The preparation method described in any one of technical solutions 1-7 can produce a pre-lithiation binary topological structure phosphorus / carbon composite material.

[0092] 9. A pre-lithiation binary topological structure phosphorus / carbon composite material according to technical solution 8, wherein the phosphorus is amorphous red phosphorus, purple phosphorus, fibrous phosphorus, black phosphorus or blue phosphorus.

[0093] 10. A pre-lithiation binary topological structure phosphorus / carbon composite material according to technical solution 8, wherein the carbon is a one-dimensional tubular carbon-based material, a two-dimensional layered carbon-based material or a three-dimensional porous carbon material.

[0094] 11. A lithium-ion battery negative electrode, wherein the active material is a pre-lithiated binary topological structure phosphorus / carbon composite material prepared by the method described in any one of technical solutions 1 to 7 or a pre-lithiated binary topological structure phosphorus / carbon composite material described in any one of technical solutions 8 to 10.

[0095] 12. A lithium ion battery comprising the lithium ion battery negative electrode described in technical solution 11.

[0096] The beneficial effects of the present invention are as follows: (1) Compared with the binary topological structure phosphorus / carbon composite material, the pre-lithiation binary topological structure phosphorus / carbon composite material prepared by the present invention has a high theoretical specific capacity and a relatively high conductivity. (2) During the pre-lithiation process, the elemental phosphorus and the surface of the carbon substrate material form materials such as lithium phosphide, lithium oxide or lithium nitride with high ionic conductivity, thereby optimizing the SEI film composition. (3) Compared with the binary topological structure phosphorus / carbon composite material, the pre-lithiation is equivalent to a lithium replenishment process for the negative electrode, thereby ensuring a high initial coulombic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0097] Figure 1 This is a TEM image (200,000 times) of the binary topological structure phosphorus / carbon composite material in Example 1 of the present application;

[0098] Figure 2 This is the XRD pattern of the pre-lithiation binary topological structure phosphorus / carbon composite material obtained in Example 3 of the present application;

[0099] Figure 3 This is a SEM image (50,000 times) of the pre-lithiation binary topological structure phosphorus / carbon composite material obtained in Example 3 of the present application;

[0100] Figure 4 This is a SEM image (30,000 times) of the pre-lithiation binary topological structure phosphorus / carbon composite material obtained in Example 4 of the present application;

[0101] Figure 5 This is a schematic diagram of the pre-lithiation binary topological structure phosphorus / carbon composite material obtained in Example 7 of the present application. DETAILED DESCRIPTION

[0102] The present invention first provides a pre-lithiation binary topological structure phosphorus / carbon composite material, which is lithiated x-dimensional phosphorus / y-dimensional carbon, wherein x and y are both integers, and 0≤x<3, 1≤y≤3. The phosphorus includes amorphous red phosphorus, purple phosphorus, fibrous phosphorus, black phosphorus, and blue phosphorus. The carbon includes a one-dimensional tubular carbon-based material, a two-dimensional layered carbon-based material, or a three-dimensional porous carbon material.

[0103] The present invention also provides four preparation methods for the pre-lithiation binary topological structure phosphorus / carbon composite material: (1) first confine elemental phosphorus in a carbon-based material, and then perform a lithiation treatment. (2) first perform a lithiation treatment on the carbon-based material, and then confine phosphorus in the carbon-based material. (3) first perform a lithiation treatment on phosphorus, and then confine it in the carbon-based material. (4) first directly mix the phosphorus source and the conductive carbon material by ball milling or hand milling, and then perform a lithiation treatment. In the preparation method (1), the method of confining elemental phosphorus in a carbon-based material to form a phosphorus-carbon binary topological structure includes two methods: (I) a "top-down" method, that is, first coating the phosphorus source and then performing high-temperature carbonization; (II) a "bottom-up" method, that is, introducing elemental phosphorus into the carbon-based material.

[0104] In the above method, the lithium source used for lithiation treatment is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic composite solution. The phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis. The carbon-based material is graphite, expanded graphite, graphitic acid or porous carbon.

[0105] In method (1) (I), the ratio of the lithium source to the phosphorus source is 1:1-1:200 in terms of the mass ratio of lithium to phosphorus, and the mass ratio of the phosphorus source to the coating material is 3:1-30:1 in terms of the mass ratio of phosphorus to carbon. The temperature of the lithiation treatment is 180-400°C. The coating material is a material that forms a carbon- or nitrogen-doped carbon-based material after pyrolysis; the carbonization temperature is 300-1000°C.

[0106] Preferably, the phosphorus source is a phosphorus oxide compound, the coating material is one or more organic amine compounds, and the carbonization temperature is 350-800°C.

[0107] More preferably, the phosphorus source is P 2 O 5 Or red phosphorus, the coating material is dopamine, and the carbonization temperature is 500-700℃.

[0108] In method (1)(II), a phosphorus source and a carbon-based material are placed in two heating temperature zones of the same tubular furnace chamber and heated. The phosphorus source is heated at 400-500°C and the carbon-based material is heated at 200-350°C. The two react to obtain a binary topological structure of x-dimensional phosphorus / y-dimensional carbon, which is then lithiated with a lithium source at a lithiation treatment temperature of 180-400°C.

[0109] In method (2), the carbon-based material is graphite, expanded graphite or porous carbon; the lithiation treatment temperature is 200-800°C; and the phosphorus source is elemental phosphorus and a compound of elemental phosphorus or phosphorus oxide that can be formed after pyrolysis.

[0110] Preferably, the carbon-based material is expanded graphite; the lithiation temperature is 200-500° C.; and the phosphorus source is elemental phosphorus.

[0111] In method (3), the phosphorus source is elemental phosphorus, the lithiation temperature is 200-800° C., and the carbon-based material is expanded graphite or graphitic acid.

[0112] Preferably, the lithium source is lithium foil; the usage ratio of the lithium source to the phosphorus source is 1:1-1:200 in terms of the mass ratio of lithium to phosphorus element; the temperature of the lithiation treatment is 200-400° C.; and the carbon-based material is expanded graphite.

[0113] In method (4), the phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis, preferably elemental phosphorus; the carbon-based material is graphite, porous carbon, activated carbon, carbon nanotubes, preferably carbon nanotubes; the lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic complex solution, preferably lithium foil; the phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-15:1, and the lithium source and the phosphorus source have an elemental mass ratio of lithium to phosphorus of 1:1-1:200; the lithiation treatment temperature is 200-800°C, preferably 300-500°C.

[0114] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments and drawings. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0115] The instrument models and parameter conditions used in the following examples are as follows:

[0116] XRD: Bruker D8-Focus X-ray diffractometer was used with a test range of 20-70° and a scan rate of 5° / min;

[0117] TEM: JEM-2100 transmission electron microscope (TEM) was used;

[0118] SEM: Hitachi S-4800 scanning electron microscope (SEM) was used.

[0119] Example 1

[0120] Take 1g of red phosphorus in a 250mL four-necked flask, add 150mL of 2mg / mL dopamine solution (the solvent is tris(hydroxymethyl)aminomethane buffer (Tris-HCl)), stir at room temperature for 72h, filter and dry. The obtained sample is placed in a tube furnace and calcined at 500℃ for 3h under an inert atmosphere to obtain a binary topological structure of 0D phosphorus / 3D carbon, such as Figure 1 As shown, in the composite material, the carbon formed by pyrolysis is coated on the surface of phosphorus. 0.5g of 0D phosphorus / 3D carbon was mixed with 0.02g of lithium foil in an iron crucible, heated at 300℃ for 1h in a glove box, cooled naturally and fully ground, and heated at 300℃ for 1h to obtain a binary topological structure of pre-lithiated 0D phosphorus / 3D carbon.

[0121] The composite material obtained in this example was used as the active material, and the weight ratio of the composite material to the conductive carbon black (SP) and the adhesive polyvinylidene fluoride (PVDF) was 80:10:10, and pressed onto a nickel foam substrate with a diameter of 12 mm. Metal lithium was used as the negative electrode, and a Cegard2300 microporous polypropylene membrane with a diameter of 16 mm was used as the separator. The assembled battery was a CR2032 button cell.

[0122] Cycle test: When testing with the blue power test system, the temperature is room temperature, constant current charging and discharging is adopted, the voltage control range is 0.01~3V, and constant current charging and discharging is carried out at a current density of 100mA / g.

[0123] The charge (discharge) specific capacity = charge (discharge) capacity / mass of active material. The above capacity test process is repeated to obtain the n-time capacity retention rate = the n-th discharge specific capacity / the first discharge specific capacity.

[0124] High rate test: When testing with the blue power test system, the temperature is room temperature, constant current charging and discharging is adopted, the voltage control range is 0.01~3V, and constant current charging and discharging is carried out at a current density of 1000mA / g.

[0125] Example 2

[0126] Take 1g of red phosphorus in a 250mL four-necked flask, add 150mL of 2mg / mL dopamine solution (the solvent is tris(hydroxymethyl)aminomethane buffer (Tris-HCl)), stir for 72h, filter and dry. The obtained sample is placed in a tube furnace and calcined at 600℃ for 3h under an inert atmosphere to obtain a binary topological structure of 0D phosphorus / 3D carbon. Take 0.5g of 0D phosphorus / 3D carbon and mix it with 0.02g of lithium foil and place it in an iron crucible, heat it at 300℃ for 1h in a glove box, cool it naturally and grind it thoroughly, and heat it at 300℃ for 1h to obtain a binary topological structure of pre-lithiated 0D phosphorus / 3D carbon.

[0127] The composite prepared in this example is used as the active material, and the battery is assembled according to the raw materials and assembly process in Example 1. The first discharge specific capacity is reduced, while the rate performance, cycle stability and reversible capacity are improved. It is speculated that the reason may be that as the temperature rises, the phosphorus evaporated from the carbon core increases, the phosphorus in the composite material decreases, and the specific capacity decreases. As the temperature rises, the graphitization degree of the carbon material increases, which is conducive to the improvement of the conductivity of the material.

[0128] Example 3

[0129] 0.9 g of black phosphorus and 0.3 g of carbon nanotubes were mixed by ball milling, placed in an iron crucible, 0.6 g of lithium foil was added, heated at 300 °C in a glove box for 1.5 h, cooled naturally and fully ground, and heated at 500 °C for 1 h to obtain a binary topological structure of pre-lithiated 0D phosphorus / 1D carbon.

[0130] Figure 2 This is the XRD diagram of the binary topological structure of pre-lithiation 0D phosphorus / 1D carbon. After pre-lithiation, the phosphorus in the composite material is converted into lithium phosphide Li x P(x=1,3). Figure 3 This is an SEM image of the binary topological structure of pre-lithiation 0D phosphorus / 1D carbon. It can be seen from the figure that the composite material after lithiation still presents a 0D / 1D binary topological structure, and the surface of the carbon nanotube becomes rough, which may be due to the formation of lithium phosphide particles on the surface of the carbon nanotube.

[0131] The composite prepared in this embodiment is used as the active material, and a battery is assembled according to the raw materials and assembly process in Example 1. At a current density of 100 mA / g, the discharge capacity in the first week can reach 1847.8, and the coulomb efficiency in the first week can reach 87.2%. When the current density reaches 1000 mA / g, after 1000 cycles, the discharge capacity can still reach 667.3 mAh / g.

[0132] Example 4

[0133] Take 1g of red phosphorus and 1g of expanded graphite and place them in two heating zones of the tubular furnace chamber, heat the red phosphorus at 450°C, and the temperature of the expanded graphite zone is 300°C. After reacting for 4h, the binary topological structure of 0D phosphorus / 2D carbon is obtained. Take 0.5g of 0D phosphorus / 2D carbon and 0.02g of lithium foil and mix them in an iron crucible. Heat them at 300°C for 1h in a glove box. After natural cooling, grind them thoroughly and heat them at 300°C for 1h to obtain the binary topological structure of pre-lithiated 0D phosphorus / 2D carbon ( Figure 4 ).

[0134] The composite prepared in this example is used as the active material, and the rate performance of the battery is greatly improved by assembling the battery according to the raw materials and assembly process in Example 1. It is speculated that the reason may be that the rich functional groups between the expanded graphite layers react with P to form a stable chemical force.

[0135] Example 5

[0136] 0.5 g of expanded graphite was mixed with 0.02 g of lithium foil, placed in an iron crucible, and calcined at 300°C for 2 h in a glove box to obtain lithiated expanded graphite. 0.5 g of red phosphorus was added and mixed, and then heated at 300°C for 2 h to obtain a binary topological structure of pre-lithiated 0D phosphorus / 2D carbon.

[0137] Using the composite prepared in this example as the active material, a battery was assembled according to the raw materials and assembly process in Example 1. The discharge capacity in the first week could reach 1698.6 mAh / g, the capacity retention rate could reach 84.7% after 100 cycles, and the discharge capacity could still reach 512.4 mAh / g after 1000 cycles at a current density of 1000 mA / g.

[0138] Example 6

[0139] 0.5 g of red phosphorus was mixed with 0.02 g of lithium foil, placed in an iron crucible, calcined at 300 ° C for 2 h in a glove box, and then calcined at 450 ° C for 2 h to obtain lithium phosphide material. 0.5 g of expanded graphite was added and mixed, and then heated at 300 ° C for 3 h to obtain a binary topological structure of pre-lithiated 0D phosphorus / 2D carbon.

[0140] The composite prepared in this example was used as the active material, and a battery was assembled according to the raw materials and assembly process in Example 1. Compared with Example 4, the specific capacity, rate performance and cycle stability thereof were all decreased.

[0141] Example 7

[0142] Take 1.0g P 2 O 5In a four-necked flask, add 120 mL of 0.1 mol / L hydrochloric acid, add 480 μL of aniline, stir for 0.5 h, add 80 mL of 1% ammonium persulfate dropwise, stir at 600 rpm for 24 h in an ice-water bath to obtain polyaniline-coated P 2 O 5 The composite material was placed in a tube furnace and calcined at 400°C for 3h to obtain. 0.5g of carbon-coated phosphorus porous composite material was placed in an iron crucible, 0.05g of lithium foil was added, and heated at 300°C for 1.5h in a glove box. After natural cooling, it was fully ground and heated at 400°C for 1h to obtain a binary topological structure of pre-lithiated 0D phosphorus / 3D carbon ( Figure 5 ).

[0143] The composite prepared in this embodiment is used as the active material, and a battery is assembled according to the raw materials and assembly process in Example 1. At a current density of 100 mA / g, the first-week discharge specific capacity can reach 1804.3, and the first-week coulomb efficiency can reach 86.1%. When the current density reaches 1000 mA / g, the first discharge specific capacity can reach 782.6 mAh / g. After 1000 cycles, the discharge specific capacity can still reach 645.2 mAh / g.

[0144] Comparative Example 1

[0145] The preparation method of the binary topological structure of 0D phosphorus / 3D carbon is the same as that of Example 1, except that a lithiation step is added in Example 1, while there is no lithiation step in Comparative Example 1. The first discharge specific capacity obtained in Comparative Example 1 at a current density of 100 mA / g can reach 1912.5 mAh / g, but the first cycle coulombic efficiency is only 52.4%. When the current density is 1000 mA / g, after 1000 cycles, the discharge specific capacity can only be maintained at 289.8 mAh / g.

[0146] Comparative Example 2

[0147] The preparation method of the binary topological structure of 0D phosphorus / 2D carbon is the same as that of Example 4, except that a lithiation step is added to Example 4, while there is no lithiation step in Comparative Example 2. When the current density is 100 mA / g for charging and discharging, the first-week specific capacity obtained in Comparative Example 2 is 1816.8 mAh / g, the first-week coulombic efficiency is 61.2%, and the capacity retention rate is 50.3% after 100 cycles. When the current density is 1000 mA / g, the discharge specific capacity is 312.5 mAh / g after 1000 cycles.

[0148] Table 1 Electrochemical performance of each lithium battery in the embodiment

[0149]

[0150] It can be seen from Table 1 that when the composite material prepared by the method of the present invention is used as the active material, the first coulombic efficiency and high-rate charge and discharge performance of the phosphorus-based negative electrode material can be significantly improved.

[0151] The above is a detailed introduction of the present invention in combination with the embodiments and drawings. The above embodiments are only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the ideas and principles of the present invention, there will be changes in the specific implementation methods and application scopes, and these changes should be included in the protection scope of the present invention.

Claims

1. A method for preparing a pre-lithiated binary topological structure phosphorus / carbon composite material, wherein the pre-lithiated binary topological structure phosphorus / carbon composite material is lithiated x-dimensional phosphorus / y-dimensional carbon, in, x and y are both integers, and 0≤x<3, 1≤y≤3; the preparation method comprises the following steps: (a) mixing a phosphorus source and a lithium source, and performing a lithiation treatment on the phosphorus source with the lithium source to obtain a lithium phosphide material; (b) The lithium phosphide material and the carbon-based material obtained in step (a) are mixed and heated to obtain a pre-lithiation binary topological structure phosphorus / carbon composite material.

2. The preparation method according to claim 1, in, The phosphorus source is elemental phosphorus or a compound that can form a stable elemental phosphorus after pyrolysis.

3. The preparation method according to claim 2, in, The phosphorus source is elemental phosphorus.

4. The preparation method according to claim 1, in, The lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic complex solution.

5. The preparation method according to claim 4, in, The lithium source is lithium foil.

6. The preparation method according to claim 2, in, The lithium source is lithium foil, lithium powder, molten lithium, inorganic lithium salt or Li-organic complex solution.

7. The preparation method according to any one of claims 1 to 6, in, The lithium source and the phosphorus source have an elemental mass ratio of lithium to phosphorus of 1:1-1:

200.

8. The preparation method according to any one of claims 1 to 6, in, The lithiation treatment temperature is 200-800°C.

9. The preparation method according to claim 8, in, The lithiation treatment temperature is 200-400°C.

10. The preparation method according to claim 7, in, The lithiation treatment temperature is 200-800°C.

11. The preparation method according to any one of claims 1 to 6, in, The carbon-based material is expanded graphite or graphitic acid.

12. The preparation method according to claim 11, in, The carbon-based material is expanded graphite.

13. The preparation method according to claim 7, in, The carbon-based material is expanded graphite or graphitic acid.

14. The preparation method according to claim 8, in, The carbon-based material is expanded graphite or graphitic acid.

15. The preparation method according to any one of claims 1 to 6, in, The phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-20:

1.

16. The preparation method according to claim 7, in, The phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-20:

1.

17. The preparation method according to claim 8, in, The phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-20:

1.

18. The preparation method according to claim 11, in, The phosphorus source and the carbon source have an elemental mass ratio of phosphorus to carbon of 1:1-20:

1.

19. The preparation method according to any one of claims 1 to 18 obtains a pre-lithiated binary topological structure phosphorus / carbon composite material.

20. The pre-lithiation binary topological structure phosphorus / carbon composite material according to claim 19, in, The phosphorus is amorphous red phosphorus, violet phosphorus, black phosphorus or blue phosphorus.

21. The pre-lithiated binary topological structure phosphorus / carbon composite material according to claim 19 or 20, in, The carbon is a one-dimensional tubular carbon-based material, a two-dimensional layered carbon-based material, or a three-dimensional porous carbon material.

22. A lithium-ion battery negative electrode, wherein the active material is a pre-lithiated binary topological structure phosphorus / carbon composite material prepared by the method described in any one of claims 1 to 18 or a pre-lithiated binary topological structure phosphorus / carbon composite material described in any one of claims 19 to 21.

23. A lithium ion battery comprising the lithium ion battery negative electrode according to claim 22.

Citation Information

Patent Citations

  • A preparation method of a high-performance carbon-phosphorus composite negative electrode material

    CN109148870A

  • Manufacturing method of film layer-structure pre-lithiation silicon carbon negative electrode

    CN110071264A

  • Silicon-carbon negative electrode pre-lithiation method

    CN110071265A