A method for replenishing sodium in positive electrode of sodium ion battery and sodium ion battery
By using a composite sodium supplementation agent of sodium manganate and ferrous sulfate in the cathode material of the sodium-ion battery, and using sand grinding dispersion and spray granulation technology, the problems of low Coulombic efficiency and high sodium supplementation cost of the sodium-ion battery are solved, and achieved The preparation of efficient and low-cost cathode materials for sodium-ion batteries improves the first charge and discharge performance and cycle stability of the battery.
Patent Information
- Application Number
- CN202210902348.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-29
AI Technical Summary
The first Coulombic efficiency of sodium-ion batteries is low, and the existing sodium supplementation method has high process costs, which limits the development and promotion of sodium-ion batteries.
Sodium manganate is used as the cathode sodium replenishing agent. After mixing with ferrous sulfate and conductive agent in deionized water, a composite sodium replenishing agent is prepared through sanding dispersion and spray granulation technology to form a stable cathode material to ensure high voltage It does not cause structural changes and improves the processing performance and electrical properties of the material.
It achieves the first Coulombic efficiency improvement of sodium-ion batteries, reduces production costs, is simple and safe to operate, and is suitable for mass production.
Smart Images

Figure CN115241432B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sodium ion batteries, and in particular to a method for replenishing sodium at a positive electrode of a sodium ion battery and a sodium ion battery. Background Art
[0002] The goals of carbon peak and carbon neutrality require rapid development of new energy, especially energy storage lithium-ion batteries. However, due to the scarcity of resources such as lithium and cobalt, it is difficult to effectively reduce the cost of lithium-ion batteries. The working principle of sodium-ion batteries is similar to that of lithium batteries, and sodium resources are abundant and low-cost, which is of great significance for the development of sodium-ion batteries. The negative electrode of sodium-ion batteries generally uses soft carbon or hard carbon materials, which have the problem of low first coulomb efficiency, affecting the battery energy density.
[0003] At present, in addition to improving the coulombic efficiency by modifying the process of negative electrode materials, the problem of low coulombic efficiency of batteries can be improved by supplementing sodium in sodium ion batteries. For the selection of sodium supplement materials, it is first required to provide sodium ions during the charge and discharge process, and the charge and discharge material structure does not affect the physical changes of the electrode. At the same time, the electrochemical properties are stable, the environment is stable, and the processability is good. However, the existing sodium supplementation methods have the problem of high process costs.
[0004] Based on this, there is an urgent need to develop a sodium supplement material and method that meets the requirements to improve the low initial coulombic efficiency of the battery while taking into account the low cost requirements, so as to facilitate the development and promotion of sodium ion batteries. Summary of the invention
[0005] The purpose of the present invention is to provide a method which uses a simple operation and low cost method to directly supplement sodium to the positive electrode material, and also improves the problem of low initial coulombic efficiency of the full battery.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] A method for replenishing sodium in a positive electrode of a sodium ion battery, characterized in that it comprises the following steps:
[0008] S1: Mix the positive electrode sodium supplement agent with solvent A, and fully grind and disperse them in a sand mill to obtain slurry B;
[0009] S2: Mix ferrous sulfate and sodium sulfate with deionized water, then add a conductive agent and stir to obtain slurry A, which is then mixed with slurry B and then spray granulated to obtain a positive electrode material precursor;
[0010] S3: calcining the cathode material precursor in a nitrogen atmosphere to obtain a cathode material Na having a composite sodium supplement x Fe y (SO4) z .
[0011] As a preferred embodiment, the positive electrode sodium supplement is Na r MnO2, wherein r=0.8~1.1; solvent A is one or a combination of deionized water, ethanol, ether, N-methylpyrrolidone (NMP), and acetone;.
[0012] Preferably, the mass ratio of the sodium supplement to the solvent A is in the range of 1:2 to 1:10.
[0013] Preferably, the mass ratio of the ferrous sulfate, sodium sulfate, conductive agent, deionized water and slurry B is 75:20~30:20~100:200~300:20~60.
[0014] Preferably, the mass ratio of the positive electrode sodium supplement in the positive electrode material precursor is in the range of 1%-10%.
[0015] As a preferred embodiment, 1 <x≤10,1<y≤10,z=x / 2+y。
[0016] Preferably, in step S3, the calcination temperature is 300-400°C, the holding time is 5-20h, and after cooling, a positive electrode material having a composite sodium supplement is obtained.
[0017] Preferably, the conductive agent in step S2 is a carbon nanotube aqueous solution with a solid content of 3.0% to 6.0%.
[0018] A sodium ion battery comprises a positive electrode material prepared by the above-mentioned sodium ion battery positive electrode sodium replenishment method.
[0019] Compared with the prior art, the present invention has the following advantages and positive effects:
[0020] The present invention utilizes the characteristic that sodium manganate itself can release higher energy under high voltage as a positive electrode material, and can supplement the sodium ion loss caused by SEI film or other side reactions during the first charge. At the same time, the phase change itself under high voltage will not cause a large change in volume, nor will it affect the ion or electron conduction impedance. Therefore, in the process of sodium manganate supplementing sodium, there will be no risk of structural collapse caused by large structural changes, and the structure is stable. By adding sodium manganate as a sodium supplementing agent during the preparation of sodium ferrous sulfate positive electrode material, sodium ferrous sulfate can be coated on the surface of sodium manganate by sand milling dispersion and then spray granulation, thereby inhibiting the sodium dissolution and manganese dissolution of sodium manganate, and improving the material processing performance and electrical properties; the sodium ion battery positive electrode sodium supplementation technology provided by the present invention is safe and stable, with low production process cost and easy operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0022] Figure 1 This is a flow chart of the method for replenishing sodium at the positive electrode of the present invention;
[0023] Figure 2 It is the full-electric first charge and discharge curve of the positive electrode material to the hard carbon negative electrode in the comparative example;
[0024] Figure 3 This is a SEM image of the sodium ferrous sulfate positive electrode material of the composite sodium supplement in Example 1;
[0025] Figure 4 The first full charge and discharge curve of the positive electrode material to the hard carbon negative electrode in Example 1;
[0026] Figure 5 This is the first full charge and discharge curve of the positive electrode material on the hard carbon negative electrode in Example 2. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as limiting the present invention; the terms "first", "second", and "third" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance. In addition, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0029] like Figure 1-Figure 5 As shown,
[0030] Embodiment 1:
[0031] Preparation of slurry B: Weigh 16.8 g of sodium manganate material, add it into 40 g of anhydrous ethanol and stir it mechanically for 30 min, then add the mixed slurry into a sand mill and grind it for 1 h.
[0032] Preparation of precursor: 150g of ferrous sulfate and 46g of sodium sulfate were dissolved in 550g of deionized water, and then added into 160g of a 5% solid content carbon nanotube aqueous solution, and mechanically stirred for 30min to obtain slurry A. The mixed solution was then mixed with slurry B and granulated directly by spray drying.
[0033] Preparation of positive electrode material: The granulated precursor is sintered in a nitrogen atmosphere, the temperature is raised to 400°C, kept at this temperature for 10 hours, and the positive electrode material is obtained after cooling.
[0034] Battery assembly and testing: positive electrode material, SP, PVDF were weighed in a mass ratio of 90:5:5, a certain amount of NMP was added for high-speed dispersion, and then the coating was roller pressed. After drying, φ14mm positive electrode sheets were cut and matched with φ16mm hard carbon negative electrode sheets. The electrolyte was NaPF6+EC+PC+EMC system, and the button-charged full battery was assembled for testing. The first charge and discharge capacity was as follows: Figure 4 As shown, the first charge and discharge capacities are 97 mAh / g and 92 mAh / g respectively, the first coulombic efficiency is above 94.8%, and the capacity retention rate is greater than 92.7% after the battery is cycled 50 times.
[0035] Embodiment 2:
[0036] Preparation of slurry B: Weigh 16.8 g of sodium manganate material, add it into 40 g of NMP and stir it mechanically for 30 min, then add the mixed slurry into a sand mill and grind it for 1 h.
[0037] Preparation of precursor: 150g of ferrous sulfate and 46g of sodium sulfate were dissolved in 550g of deionized water, and then added to 160g of a 5% solid content carbon nanotube aqueous solution to obtain slurry A, which was mechanically stirred for 30 minutes. The mixed solution was then mixed with slurry B and granulated directly by spray drying.
[0038] Preparation of positive electrode material: The granulated precursor is sintered in a nitrogen atmosphere, the temperature is raised to 400°C, kept at this temperature for 10 hours, and the positive electrode material is obtained after cooling.
[0039] Battery assembly and testing: positive electrode material, SP, PVDF were weighed in a mass ratio of 90:5:5, a certain amount of NMP was added for high-speed dispersion, and then the coating was roller pressed. After drying, φ14mm positive electrode sheets were cut and matched with φ16mm hard carbon negative electrode sheets. The electrolyte was NaPF6+EC+PC+EMC system, and the button-charged full battery was assembled for testing. The first charge and discharge capacity was as follows: Figure 4 As shown, the first charge and discharge capacities are 100mAh / g and 97mAh / g respectively, the first coulombic efficiency is above 97%, and the capacity retention rate is greater than 93.1% after the battery is cycled 50 times, which has excellent first coulombic efficiency and cycle stability.
[0040] Comparative Example 1:
[0041] Preparation of positive electrode material: 150g of ferrous sulfate and 46g of sodium sulfate were dissolved in 550g of deionized water, and then 160g of carbon nanotube aqueous solution with a solid content of 5% was added; the above slurry was mechanically stirred and dispersed for 2 hours, and then granulated by spray drying. The granulated precursor was sintered in a nitrogen atmosphere, heated to 400℃, kept warm for 10h, and cooled to obtain the positive electrode material.
[0042] Battery assembly and testing: positive electrode material, SP, PVDF were weighed in a mass ratio of 90:5:5, a certain amount of NMP was added for high-speed dispersion, and then the coating was roller pressed. After drying, φ14mm positive electrode sheets were cut and matched with φ16mm hard carbon negative electrode sheets. The electrolyte was NaPF6+EC+PC+EMC system, and the button-charged full battery was assembled for testing. The first charge and discharge capacity was as follows: Figure 2 As shown, the first charge and discharge capacities are 90 mAh / g and 85 mAh / g respectively, the first coulombic efficiency is above 94.4%, and the capacity retention rate is greater than 93.3% after the battery is cycled 50 times.
[0043] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work, any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention.
Claims
1. A method for replenishing sodium in a positive electrode of a sodium ion battery, characterized in that: The following steps are involved: S1: Mix the positive electrode sodium supplement agent with solvent A, and fully grind and disperse them in a sand mill to obtain slurry B; S2: Mix ferrous sulfate and sodium sulfate with deionized water, then add a conductive agent and stir to obtain slurry A, which is then mixed with slurry B and then spray granulated to obtain a positive electrode material precursor; S3: calcining the cathode material precursor in a nitrogen atmosphere to obtain a cathode material Na having a composite sodium supplement x Fe y (SO4) z ; The positive electrode sodium supplement is Na r MnO2, wherein r=0.8-1.1; solvent A is one or a combination of deionized water, ethanol, ether, N-methylpyrrolidone, and acetone.
2. The method for replenishing sodium in the positive electrode of a sodium ion battery according to claim 1, characterized in that: The mass ratio of the sodium supplement agent to the solvent A is in the range of 1:2 to 1:
10.
3. The method for replenishing sodium in the positive electrode of a sodium ion battery according to claim 1, characterized in that: The mass ratio of the ferrous sulfate, sodium sulfate, conductive agent, deionized water and slurry B is 75:20-30:20-100:200-300:20-60.
4. The method for replenishing sodium in the positive electrode of a sodium ion battery according to claim 1, characterized in that: The mass ratio of the positive electrode sodium supplement in the positive electrode material precursor is in the range of 1%-10%.
5. The method for replenishing sodium in the positive electrode of a sodium ion battery according to claim 1, characterized in that: 1 of them <x≤10,1<y≤10,z=x / 2+y。 6. The method for replenishing sodium in the positive electrode of a sodium ion battery according to claim 1, characterized in that: In step S3, the calcination temperature is 300-400° C., and the holding time is 5-20 hours. After cooling, a positive electrode material having a composite sodium supplement is obtained.
7. The method for replenishing sodium in the positive electrode of a sodium ion battery according to claim 1, characterized in that: In the step S2, the conductive agent is a carbon nanotube aqueous solution with a solid content of 3.0% to 6%.
8. A sodium ion battery, characterized in that: It comprises a positive electrode material prepared by the positive electrode sodium replenishment method for a sodium ion battery according to any one of claims 1 to 7.
Citation Information
Patent Citations
Sodium-rich transition metal oxide composite sodium-supplementing positive electrode active material, positive electrode material, positive electrode, preparation of positive electrode and application of positive electrode in sodium-ion battery
CN111293290A
Positive electrode material for sodium ion battery and sodium ion battery comprising positive electrode material
CN113130896A