Recovery method of iron phosphate waste
Patent Information
- Application Number
- CN202411204505.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art has failed to effectively recycle and process floor-standing waste in iron phosphate production lines, intercepting waste in basket filters and unqualified iron phosphate waste, resulting in waste of resources and environmental pollution.
By stirring and dissolving the iron phosphate waste with phosphoric acid, adding oxidant and ferrous sulfate purification liquid, controlling the pH value and temperature, filtration and washing multiple times, and finally roasting at high temperature to obtain battery-grade iron phosphate without crystallization water.
实现了磷酸铁废料的有效回收,减少了危险废弃物,降低了生产成本,并与现有生产线高度重合,不需另建回收生产线。
Smart Images

Figure CN119038510A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste material recycling, and in particular relates to a method for recycling iron phosphate waste. Background Art
[0002] The continuous development of new energy is an important foundation for the sustainable development of human society. With the advancement of science and technology, people's demand for mobile energy is becoming stronger and stronger, especially the demand for pure electric vehicles is increasing with the intensification of the oil and environmental crisis. Compared with traditional secondary batteries, lithium iron phosphate batteries have unique advantages such as high energy density, high power density, low self-discharge rate, high operating voltage, long cycle life, no memory effect, green and pollution-free, and have rapidly developed into one of the most advanced and important secondary batteries.
[0003] As the main raw material for preparing lithium iron phosphate, iron phosphate has an important influence on the physical and chemical properties of lithium iron phosphate. During the production process of iron phosphate, various floor wastes, intercepted wastes in basket filters, and unqualified iron phosphate wastes are generated. The existing recycling technology mainly focuses on the recycling of iron phosphate wastes after lithium iron phosphate slag extraction, and there are few studies on the recycling of various floor wastes in iron phosphate production lines, intercepted wastes in basket filters, and unqualified iron phosphate wastes produced. With the increase in the production capacity of iron phosphate enterprises, if iron phosphate waste is treated as solid waste and is not properly recycled and disposed of, it will not only waste resources, but also cause serious pollution to the environment. Therefore, how to properly recycle and treat iron phosphate waste is an urgent problem to be solved. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for recovering waste ferric phosphate.
[0005] To achieve the above object, the present invention adopts the following technical scheme: a method for recycling iron phosphate waste, characterized in that the specific steps are as follows: Step 1: adding phosphoric acid to the collected iron phosphate waste and stirring until completely dissolved, controlling the temperature to be 50°C-100°C; adding water to dilute to a certain pH value, filtering to obtain an acidic solution, then adding an oxidant to the acidic solution, stirring and mixing evenly to obtain a clear and transparent solution; Step 2: Add a certain amount of purified ferrous sulfate solution as a primer into the reactor, then slowly add the clear transparent solution in step 1 into the primer, stir evenly, and obtain a mixed solution; Step 3: slowly add the alkaline solution to the above mixed solution, adjust the slurry pH to 1.8-2.8, control the reaction temperature to ≤60°C, control the reaction time to 0.5h-3h, stir and react to obtain a yellow slurry; Step 4: Filter the yellow slurry and wash it with desalted water to obtain a filter cake; Step 5: adding desalted water to a filter cake, dispersing the filter cake evenly to form a slurry, adding phosphoric acid to adjust the pH value of the slurry to 1-1.8, and aging the slurry; Step 6: Filter the aged slurry to obtain a second-stage filter cake, wash it with desalted water, and then dry it at a temperature of 60°C-300°C to obtain iron phosphate containing crystal water, namely FePO 4 ·2H 2 O, and then calcined at a high temperature of 300℃ to 800℃ to obtain battery-grade iron phosphate without crystal water, namely FePO 4 .
[0006] Furthermore, in step 1, the mass ratio of the iron phosphate waste to phosphoric acid is 1:(1-6); the dilution pH is 0.5-1.5; and the oxidant is one of hydrogen peroxide and nitric acid or a mixture of the two in any proportion.
[0007] Furthermore, in step 2, the concentration of the ferrous sulfate purification solution is 15%-22%, and the stoichiometric ratio of the amount of ferrous sulfate purification solution added to the amount of phosphoric acid added in step 1 is 1:1.
[0008] Furthermore, in step 3, the alkaline solution is any one of ammonia water, sodium hydroxide solution, and potassium hydroxide solution, or a mixture of several of them in any proportion; and the stirring speed is 250 r / min-600 r / min.
[0009] Furthermore, in step 3, the slurry pH is 2-2.5, the reaction temperature is 25°C-50°C, and the reaction time is 0.5h-1.5h.
[0010] Further, in step 4, the product is washed with desalted water until the conductivity of the washing water is 1 mS / cm-9 mS / cm.
[0011] Furthermore, in step 5, phosphoric acid is added at a concentration of 85%; the aging temperature is controlled at 70°C-100°C, and the aging time is controlled at 0.5-6h.
[0012] Furthermore, in step 6, washing with desalted water until the conductivity is 100 μS / cm-800 μS / cm; drying time is 1-6 hours; and roasting time is 1-6 hours.
[0013] The beneficial effects of the present invention are: 1. The iron phosphate waste is dissolved with phosphoric acid, and no new impurity elements are introduced. In addition, the ferrous sulfate purification liquid is additionally added in a stoichiometric ratio with phosphoric acid in the present invention, so that phosphoric acid is not wasted.
[0014] 2. The iron phosphate waste recovery production line can be highly overlapped with the existing production line, and there is no need to build a separate iron phosphate recovery production line.
[0015] 3. Reduce hazardous waste, lower the production cost of battery-grade iron phosphate, and improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a SEM image of the iron phosphate sample obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0017] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0018] Example 1 A method for recycling iron phosphate waste, the specific steps are as follows: 1. Weigh 100 g of waste iron phosphate, add 200 g of 85% phosphoric acid at a solid-liquid ratio of 1:2, react at 80 ° C until the waste iron phosphate is completely dissolved, dilute with water to a pH of 1.0, filter to obtain an acidic solution, add 107 g of hydrogen peroxide, stir and mix evenly to obtain a clear and transparent solution.
[0019] 2. Add 1211 gg of purified ferrous sulfate solution into the reactor, slowly add the clear and transparent solution in step 1 into the purified ferrous sulfate solution, stir evenly, and obtain a mixed solution.
[0020] 3. Slowly add ammonia water to the mixture, adjust the pH to 2.7, and stir the mixture at room temperature and 600 r / min for 30 min to obtain a yellow slurry.
[0021] 4. Filter the yellow slurry, add desalted water to wash until the conductivity of the washing water is 4mS / cm, and obtain a filter cake.
[0022] 5. Add desalted water to the first filter cake and disperse evenly to form a slurry. Add 85% phosphoric acid to adjust the pH value of the slurry to 1.5. Heat to 80°C, 300r / min, react for 2h to obtain the second stage slurry.
[0023] 6. Filter the above-mentioned second-stage slurry, add desalted water for washing, and wash until the conductivity of the washing water is 500μS / cm to obtain the second-stage filter cake; dry the second-stage filter cake at 100℃ for 5h to obtain FePO 4 ·2H 2 O; calcined at 550°C for 4.0 hours to obtain an iron phosphate sample.
[0024] The iron phosphate samples were tested and the results are shown in Table 1, which meet the requirements of battery-grade iron phosphate standards.
[0025] SEM images Figure 1 .
[0026] Example 2 A method for recycling iron phosphate waste, the specific steps are as follows: 1. Weigh 100 g of waste iron phosphate, add 150 g of 85% phosphoric acid at a solid-liquid ratio of 1:1.5, react at 90 ° C until the waste iron phosphate is completely dissolved, dilute with water to a pH of 1.5, filter to obtain an acidic solution, add 80.36 g of hydrogen peroxide, stir and mix evenly to obtain a clear and transparent solution.
[0027] 2. Add 910 g of purified ferrous sulfate solution to the reactor, slowly add the clear and transparent solution in step 1 to the purified ferrous sulfate solution, stir evenly, and obtain a mixed solution.
[0028] 3. Slowly add ammonia water to the mixture, adjust the pH to 2.0, stir and react at room temperature and 400 r / min for 1 h to obtain a yellow slurry.
[0029] 4. Filter the yellow slurry, add desalted water to wash until the conductivity of the washing water is 3mS / cm, and obtain a filter cake.
[0030] 5. Add desalted water to the first filter cake and disperse it evenly to form a slurry. Add 85% phosphoric acid to adjust the pH value of the slurry to 1.5. Heat to 90°C, 500r / min, react for 1h to obtain the second stage slurry.
[0031] 6. Filter the above-mentioned second-stage slurry, add desalted water for washing, and wash until the conductivity of the washing water is 300μS / cm to obtain the second-stage filter cake. Dry the second-stage filter cake at 200℃ for 2h to obtain FePO 4 ·2H 2 O; calcined at 600°C for 2.0 hours to obtain an iron phosphate sample.
[0032] The iron phosphate samples were tested and the results are shown in Table 1, which meet the requirements of battery-grade iron phosphate standards.
[0033] Example 3 A method for recycling iron phosphate waste, the specific steps are as follows: 1. Weigh 100 g of waste iron phosphate, add 300 g of 85% phosphoric acid, react at 70 ° C until the waste iron phosphate is completely dissolved, dilute with water to a pH of 0.8, filter to obtain an acidic solution, add 160.7 g of hydrogen peroxide, stir and mix evenly to obtain a clear and transparent solution; 2. Add 1820 g of purified ferrous sulfate solution into the reactor, slowly add the clear transparent solution in step 1 into the purified ferrous sulfate solution, stir evenly, and obtain a mixed solution.
[0034] 3. Slowly add sodium hydroxide solution to the mixture, adjust the pH to 2.5, and stir the mixture at room temperature and 600 r / min for 1 h to obtain a yellow slurry.
[0035] 4. Filter the yellow slurry, add desalted water to wash until the conductivity of the washing water is 4mS / cm, and obtain a filter cake; 5. Add desalted water to the first filter cake and disperse the filter cake evenly to form a slurry. Add 85% phosphoric acid to adjust the pH value of the slurry to 1.4, heat to 80°C, 300r / min, react for 2h to obtain the second stage slurry; 6. Filter the above-mentioned second-stage slurry, add deionized water to wash until the conductivity of the washing water is 500μS / cm, and obtain the second-stage filter cake; dry the second-stage filter cake at 150℃ for 3h to obtain FePO 4 ·2H 2 O; calcined at 650°C for 1.5 hours to obtain an iron phosphate sample.
[0036] The iron phosphate samples were tested, and the results are shown in Table 1, which meet the requirements of battery-grade iron phosphate standards.
[0037] Table 1 It can be seen from Table 1 that the iron phosphate samples prepared in the above three embodiments meet the implementation standards of battery-grade iron phosphate in various indicators.
[0038] The above embodiments are only preferred embodiments of the present invention and are not limitations of the technical solutions of the present invention. Any technical solution that can be implemented on the basis of the above embodiments without creative work should be deemed to fall within the scope of protection of the patent of the present invention.
Claims
1. A method for recovering iron phosphate waste, characterized in that: The specific steps are as follows: Step 1: adding phosphoric acid to the collected iron phosphate waste and stirring until completely dissolved, controlling the temperature to be 50°C-100°C; adding water to dilute to a certain pH value, filtering to obtain an acidic solution, then adding an oxidant to the acidic solution, stirring and mixing evenly to obtain a clear and transparent solution; Step 2: Add a certain amount of purified ferrous sulfate solution as a primer into the reactor, then slowly add the clear transparent solution in step 1 into the primer, stir evenly, and obtain a mixed solution; Step 3: slowly add the alkaline solution to the above mixed solution, adjust the slurry pH to 1.8-2.8, control the reaction temperature to ≤60°C, control the reaction time to 0.5h-3h, stir and react to obtain a yellow slurry; Step 4: Filter the yellow slurry and wash it with desalted water to obtain a filter cake; Step 5: adding desalted water to a filter cake, dispersing the filter cake evenly to form a slurry, adding phosphoric acid to adjust the pH value of the slurry to 1-1.8, and aging the slurry; Step 6: Filter the aged slurry to obtain a second-stage filter cake, wash it with desalted water, dry it at 60°C-300°C to obtain iron phosphate containing crystal water, i.e., FePO4·2H2O, and then calcine it at a high temperature of 300°C-800°C to obtain battery-grade iron phosphate without crystal water, i.e., FePO4.
2. A method for recycling iron phosphate waste as claimed in claim 1, characterized in that: In step 1, the mass ratio of the iron phosphate waste to phosphoric acid is 1: (1-6); the dilution pH is 0.5-1.5; and the oxidant is one of hydrogen peroxide and nitric acid or a mixture of the two in any proportion.
3. The method for recycling waste iron phosphate according to claim 1, characterized in that: In step 2, the concentration of the ferrous sulfate purification solution is 15%-22%, and the stoichiometric ratio of the amount of ferrous sulfate purification solution added to the amount of phosphoric acid added in step 1 is 1:
1.
4. A method for recycling iron phosphate waste as claimed in claim 1, characterized in that: In step 3, the alkaline solution is any one of ammonia water, sodium hydroxide solution, and potassium hydroxide solution, or a mixture of several of them in any proportion; the stirring speed is 250 r / min-600 r / min.
5. The method for recycling waste iron phosphate according to claim 1, characterized in that: In step 3, the pH of the slurry is 2-2.5, the reaction temperature is 25°C-50°C, and the reaction time is 0.5h-1.5h.
6. The method for recycling waste iron phosphate according to claim 1, characterized in that: In step 4, the product is washed with desalted water until the conductivity of the washing water is 1 mS / cm-9 mS / cm.
7. The method for recycling waste iron phosphate according to claim 1, characterized in that: In step 5, phosphoric acid is added at a concentration of 85%; the aging temperature is controlled at 70°C-100°C, and the aging time is controlled at 0.5-6h.
8. The method for recycling waste iron phosphate according to claim 1, characterized in that: In step 6, washing with desalted water until the conductivity is 100 μS / cm-800 μS / cm; drying time is 1-6 hours; and roasting time is 1-6 hours.
Citation Information
Patent Citations
Method for regenerating iron phosphate waste
CN110683528A
Method for preparing battery-grade iron phosphate by using waste lithium iron phosphate lithium extraction slag
CN118324104A