Composite solid electrolyte membrane and preparation method thereof and lithium ion solid-state battery
Through the preparation method of composite solid electrolyte membrane, atomized spraying technology is used to form a high-density composite electrolyte membrane, which solves the problems of potential safety hazards of liquid electrolytes in lithium batteries and insufficient performance of pure ceramic electrolyte membranes, and achieves the same goal as high-nickel ternary or The matching of quaternary cathode materials improves battery capacity and safety performance.
Patent Information
- Application Number
- CN202211029870.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-08-25
AI Technical Summary
The organic solvent of the liquid electrolyte in existing lithium batteries causes battery safety hazards, and it is difficult to prepare pure ceramic electrolyte membranes with high density and stability to match high-nickel ternary or quaternary cathode materials, resulting in insufficient battery performance.
Using the preparation method of composite solid electrolyte membrane, through atomization spraying technology of inorganic oxide or inorganic-organic composite electrolyte slurry and polymer monomer, lithium salt and organic solvent, a high-density composite electrolyte membrane is formed to improve ionic conductivity. efficiency and battery safety performance.
The adaptation of the composite solid electrolyte membrane to the high-voltage cathode material is achieved, suppressing the generation of lithium dendrites, improving battery capacity and safety performance, and avoiding an increase in battery internal resistance.
Smart Images

Figure CN115275337B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion solid-state batteries, and in particular to a composite solid-state electrolyte membrane and a preparation method thereof, and a lithium ion solid-state battery. Background Art
[0002] In recent years, with the continuous development of electric vehicles, the market has put forward higher requirements for the comprehensive performance of lithium batteries, such as battery capacity, cycle performance and safety performance, especially safety performance, which is the key to the application of lithium batteries. However, the organic solvent electrolyte commonly used in liquid lithium batteries will produce lithium dendrites during the battery cycle, causing battery short circuit. Moreover, the organic solvent in the electrolyte is a flammable substance. After the dendrite punctures inside the battery or the external collision causes a short circuit, it is very easy to react with the decomposition products of the ternary or quaternary high-nickel positive electrode commonly used in power batteries, causing fire or even explosion.
[0003] Solid-state batteries use solid electrolytes to replace liquid electrolytes, which can fundamentally solve the safety hazards of battery combustion and explosion. Solid electrolytes can match metallic lithium, thereby greatly increasing the battery capacity. Therefore, solid-state batteries are the main direction of lithium battery development, and the core of solid-state battery development is solid electrolytes. Oxide solid electrolytes in solid electrolytes have the advantages of high ionic conductivity, stable structure, and wide electrochemical window, so they are widely used in the research and development of solid-state batteries. However, pure ceramic films are difficult to control within 100um, and have poor interfacial contact with the active components of the battery. In addition, due to the existence of internal stress, they are easy to break during the battery cycle, and large-capacity batteries cannot be prepared. Therefore, pure ceramic electrolyte membranes cannot meet the needs of power batteries. In order to solve the above problems, oxide electrolytes are usually compounded with polymer electrolytes, and the flexibility and viscoelasticity of polymers are used to improve the problems existing in oxide electrolytes.
[0004] At present, the preparation methods of oxide composite electrolyte flexible membranes mainly include coating, casting, vapor deposition, solution casting, co-extrusion, etc. These traditional preparation methods cannot prepare dense oxide films. Some use binders or polymer electrolytes to connect oxide electrolyte particles, but the binders and common polymers themselves have low conductivity, and the commonly used polymer electrolytes have a low electrochemical stability window, which is not suitable for high-nickel ternary or quaternary high-voltage positive electrode materials. Although some polymer electrolytes are relatively stable to high-nickel ternary materials, their ionic conductivity is low. Excessive content of such polymers will also have an adverse effect on battery performance.
[0005] Therefore, it is urgent to develop a method for preparing a composite solid electrolyte to prepare a highly dense composite solid electrolyte membrane that is stable to high-nickel ternary positive electrode materials. Summary of the invention
[0006] In view of the above shortcomings of the prior art, the present invention provides a composite solid electrolyte membrane and a preparation method thereof and a solid-state battery, which can be used to prepare a flexible composite oxide electrolyte membrane material with high density, and can maintain stability for positive high-nickel ternary or quaternary positive electrode materials, thereby improving the ionic conductivity of the composite membrane material and the safety performance of the battery.
[0007] To achieve the above object and other related objects, the present invention provides a method for preparing a composite solid electrolyte membrane, which comprises at least the following steps:
[0008] Preparing a first electrolyte slurry, wherein the first electrolyte slurry is an inorganic oxide electrolyte slurry or an inorganic-organic composite electrolyte slurry;
[0009] The first electrolyte slurry is coated on a substrate to form a film and dried to obtain a first electrolyte membrane;
[0010] Evenly mixing the polymer monomer, the initiator, the lithium salt and the organic solvent to prepare the second electrolyte slurry;
[0011] Applying the second electrolyte slurry on the first electrolyte membrane by atomizing spraying, and forming a second electrolyte membrane on the first electrolyte membrane after in-situ curing;
[0012] The substrate is peeled off to obtain a composite solid electrolyte membrane.
[0013] In one example of the present invention, in the inorganic oxide electrolyte slurry, the mass percentage of the oxide electrolyte is 15-35%, the mass percentage of the binder is 1-5%, and the rest is an organic solvent; in the inorganic-organic composite electrolyte slurry, the mass percentage of the oxide electrolyte is 12-25%, and the rest is a mixture of a polymer electrolyte, a lithium salt and an organic solvent, wherein the total mass of the polymer electrolyte and the lithium salt is 2-5% of the mass of the mixture, and the mass ratio of the polymer electrolyte to the lithium salt is 7:1-20:1.
[0014] In one example of the present invention, the inorganic oxide electrolyte comprises LLZO (Li7La3Zr2O 12 ), LLZAO(Li 6.25 La3Zr2Al 0.25 O 12 ), LLZTO(Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 ), LLZNO(Li7La3Zr 1.75 Nb 0.25 O 12 ), LATP(Li3Al x Ti 2-x(PO4)3), LAGP(Li 1.5 Al 0.5 Ge 1.5 (PO4)3), LZSPO(Li3Zr2Si2PO 12 ), any one of SiO2 or Al2O3 or a combination of at least two thereof.
[0015] In an example of the present invention, the organic solvent includes any one of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), acetonitrile (AN) or acetone, or a combination of at least two thereof.
[0016] In one example of the present invention, the lithium salt includes one or more combinations of lithium perchlorate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl imide), lithium tetrafluoroborate, lithium trifluoromethanesulfonate and lithium bis(oxalatoborate).
[0017] In an example of the present invention, the first electrolyte slurry is formed into a film by casting or coating, and the thickness of the first electrolyte film is 1 to 100 μm.
[0018] In one example of the present invention, when preparing the first electrolyte membrane, after the drying process is completed, a hot pressing process is also included, and the hot pressing parameters of the hot pressing process are a temperature of 40 to 80° C., a pressure of 30 to 60 MPa, and a time of 10 to 80 min.
[0019] In one example of the present invention, preparing the second electrolyte slurry includes: adding the lithium salt to the organic solvent at room temperature and mixing and stirring evenly; then adding the polymer monomer and the initiator, and magnetically stirring at room temperature for 20 to 40 minutes; wherein, in the second electrolyte slurry, the mass percentage of the polymer monomer is 5 to 15%, the mass of the initiator is 1 to 10% of the mass of the polymer monomer, and the ratio of the organic solvent to the lithium salt is 1:1 to 3:1.
[0020] In one example of the present invention, the organic solvent in the second electrolyte slurry is a carbonate or carbonate-containing organic solvent, including one or more of ethylene carbonate, diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate; the polymer monomer includes one or a combination of triethylene glycol dimethacrylate, ethylene glycol diacrylate, and polyethylene glycol monomethyl ether methacrylate; the initiator is azobisisobutyronitrile or benzoyl peroxide.
[0021] In one example of the present invention, the atomization spraying includes: injecting the second electrolyte slurry into an ultrasonic atomization generator, and spraying it onto the first electrolyte membrane after being atomized by the ultrasonic atomization generator, wherein the spraying distance is controlled at 5 to 10 cm, and 1 to 50 μm is sprayed at a speed of 1 to 2 cm / s.
[0022] Another aspect of the present invention further provides a composite solid electrolyte membrane, which is prepared by the above-mentioned preparation method.
[0023] The present invention also provides a lithium ion solid-state battery, which comprises the composite solid-state electrolyte membrane prepared by the above preparation method.
[0024] The preparation method of the composite solid electrolyte membrane of the present invention prepares a second electrolyte slurry (polymer electrolyte slurry) of a high-nickel resistant ternary or quaternary high-voltage positive electrode material, and then sprays it onto the surface of a first electrolyte membrane (inorganic oxide or inorganic-organic composite electrolyte membrane), thereby achieving effective control of the coating thickness, improving the high-voltage resistance of the electrolyte while reducing the use of polymer electrolytes and reducing the impact on the ionic conductivity of the composite solid electrolyte membrane.
[0025] The second electrolyte slurry is sprayed onto the first electrolyte membrane by atomization spraying, and the polymer molecules can penetrate into the gaps of the first electrolyte membrane, and then form a composite solid electrolyte membrane through in-situ polymerization, which improves the density and interface contact performance of the first electrolyte membrane and improves its flexibility. Due to the high density of the composite electrolyte membrane, the formation of lithium dendrites during the battery cycle can be suppressed, the safety performance of the battery can be improved, and the internal resistance of the battery will not increase significantly; in addition, the second electrolyte membrane has the characteristics of being stable to high-voltage positive electrode materials such as high-nickel ternary or quaternary materials, so that it can match high-voltage positive electrode materials and increase the capacity of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The present invention is a flow chart of the preparation method of the composite solid electrolyte membrane;
[0028] Figure 2 Flow chart of step S1 of a method for preparing a composite solid electrolyte membrane of the present invention in one embodiment;
[0029] Figure 3Flow chart of step S1 of another embodiment of the method for preparing a composite solid electrolyte membrane of the present invention;
[0030] Figure 4 The flowchart of the method for preparing the composite solid electrolyte membrane of the present invention is shown in one embodiment. DETAILED DESCRIPTION
[0031] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.
[0032] It should be noted that the terms such as "upper", "lower", "left", "right", "middle" and "one" etc. used in this specification are only for the convenience of description and are not intended to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships, without substantially changing the technical content, should also be regarded as the scope of implementation of the present invention.
[0033] The present invention provides a composite solid electrolyte membrane and a preparation method thereof and a lithium ion solid-state battery, which can achieve the adaptation of the composite solid electrolyte membrane and a high-voltage positive electrode material, avoid the increase of the internal resistance of the battery, and improve the ability of the composite solid electrolyte membrane to inhibit the growth of lithium dendrites, thereby effectively improving the capacity and safety of the battery.
[0034] See also Figure 1 The present invention provides a method for preparing a composite solid electrolyte membrane, which comprises at least the following steps:
[0035] S1, preparing a first electrolyte slurry;
[0036] S2, coating the first electrolyte slurry on a substrate, forming a film, and drying to obtain a first electrolyte membrane;
[0037] S3, uniformly mixing the polymer monomer, initiator, lithium salt and organic solvent to prepare a second electrolyte slurry;
[0038] S4, applying the second electrolyte slurry on the first electrolyte membrane by atomizing spraying, and forming a second electrolyte membrane on the first electrolyte membrane after in-situ curing;
[0039] S5. Peeling off the substrate to obtain a composite solid electrolyte membrane.
[0040] The first electrolyte slurry in step S1 is an inorganic oxide electrolyte slurry or an inorganic-organic composite electrolyte slurry.
[0041] See also Figure 1 and Figure 2 When the prepared first electrolyte slurry is an inorganic oxide slurry, step S1 specifically includes the following steps:
[0042] S11, adding an oxide electrolyte into an organic solvent and mixing and stirring to obtain an electrolyte mixture;
[0043] S12, mixing the binder and the solvent and stirring until the mixture is clear and free of bubbles, to obtain a glue solution;
[0044] S13, adding the glue prepared in step S12 to the electrolyte mixed solution dispersed in step S11 and stirring evenly, and adjusting the solid content and viscosity in the slurry by using an organic solvent and the glue to obtain an inorganic oxide slurry.
[0045] The inorganic oxide electrolyte in step S11 includes any one of LLZO, LLZAO, LLZTO, LLZNO, LATP, LAGP, LZSPO, SiO2 or Al2O3, or a combination of at least two of them, that is, the inorganic oxide electrolyte can be any one of the listed oxide types, for example, it can be LLZO or LLZAO or LLZTO or LLZNO or LATP or LAGP or LZSPO or SiO2 or Al2O3; it can also be any two or more combinations of the listed oxide types, such as a combination of LLZO and LLZAO, a combination of LATP and LAGP, a combination of LLZTO, LLZNO and LATP, a combination of LLZO, SiO2, Al2O3 and LZSPO, etc., which are not listed one by one here. When the oxide electrolyte is a combination of several components, the ratio of each component in the composition is not limited, and it can be mixed in any ratio. The inorganic oxide electrolyte includes but is not limited to the types listed above, and other inorganic oxide electrolytes with equivalent effects can also be used.
[0046] The organic solvent in step S11 is recorded as the first solvent, and the first solvent includes any one or a combination of at least two of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, acetonitrile and acetone, that is, the first solvent can be any one of the solvents listed above, such as N-methylpyrrolidone or N,N-dimethylformamide or N,N-dimethylacetamide or acetonitrile or acetone; it can also be a combination of two or more of the solvents listed above, such as a mixture of N-methylpyrrolidone and N,N-dimethylformamide or a mixture of N,N-dimethylacetamide, acetonitrile and acetone or a mixture of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, acetonitrile and acetone, etc., which are not listed one by one here. When the first solvent is a mixture of several components, the ratio of each component in the mixture is not limited, and it can be mixed in any proportion. The first solvent includes but is not limited to the types listed above, and other organic solvents with equivalent effects can also be used.
[0047] In step S11, when preparing the electrolyte mixture, a small amount of dispersant is also added to grind the oxide electrolyte solid particles to a particle size of 0.2 to 0.8 μm. For example, the particle size can be 0.2 μm, 0.4 μm, 0.6 μm or 0.8 μm, etc. Any value within the above range. By adding a dispersant, the solid particles of the oxide electrolyte can be refined, so that the electrolyte in the prepared first electrolyte slurry is evenly dispersed to obtain a uniformly distributed first electrolyte membrane. Among them, the amount of dispersant added is 0.2 to 1% of the mass of the oxide electrolyte. For example, the amount of dispersant added can be 0.2%, 0.5%, 0.7% or 1% of the mass of the oxide electrolyte, etc. Any value within the above range.
[0048] When configuring the glue in step S12, the binder can be polyvinylidene fluoride (PVDF), and the solvent can be any one or more combinations of the first solvents listed above; the concentration of PVDF in the glue is 5-10%, for example, the concentration of PVDF can be 5%, 8% or 10%; preferably, the concentration of PVDF is 10%.
[0049] The mass percentage of the oxide electrolyte in the inorganic oxide electrolyte slurry prepared in step S13 is 15-35%, for example, 15%, 25%, 30% or 35% or any value within the above range; the mass percentage of the binder is 1-5%, for example, 1%, 3% or 5% or any value within the above range; the rest is an organic solvent and a small amount of dispersant.
[0050] See also Figure 1 and Figure 3 When the prepared first electrolyte slurry is an inorganic-organic composite electrolyte slurry, step S1 specifically includes the following steps:
[0051] S101, mixing a polymer electrolyte and a lithium salt in a certain proportion, adding an organic solvent, and stirring evenly to obtain a mother solution;
[0052] S102, weighing the oxide electrolyte and the organic solvent, mixing and stirring evenly, adding them into the mother liquor and dispersing them evenly, and preparing an inorganic-organic composite electrolyte slurry.
[0053] The polymer electrolyte in step S101 includes but is not limited to any one or more of polyvinyl chloride (PVC), polyethylene oxide (PEO), polyacrylonitrile (PAN), and polyvinylidene fluoride (PVDF), that is, the polymer electrolyte can be any one of the polymer types listed above, for example, the polymer electrolyte is PVC or PEO or PAN, etc.; the polymer electrolyte can also be any two or more combinations of the types listed above, such as a composition of PVC and PEO or a composition of PAN and PVDF or a composition of PEO, PAN and PVDF, etc., which are not listed one by one here. When the polymer electrolyte is a combination of multiple components, there is no restriction on the proportion of each component in the composition, and it can be mixed in any proportion. The organic solvent can be any one or more of the first solvents listed above.
[0054] The lithium salt includes, but is not limited to, one or more of lithium perchlorate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bistrifluoromethanesulfonyl imide, lithium tetrafluoroborate, lithium trifluoromethanesulfonate and lithium dioxalate borate. That is, the lithium salt may be any one of the types listed above, such as lithium perchlorate or lithium hexafluoroarsenate or lithium hexafluorophosphate or lithium bistrifluoromethanesulfonyl imide or lithium tetrafluoroborate or lithium trifluoromethanesulfonate or lithium dioxalate borate. The lithium salt may also be a combination of any two or more of the types listed above, such as a combination of lithium perchlorate and lithium hexafluoroarsenate, or a combination of lithium hexafluorophosphate, lithium bistrifluoromethanesulfonyl imide and lithium tetrafluoroborate, or a combination of lithium hexafluorophosphate, lithium trifluoromethanesulfonate and lithium dioxalate borate. When the lithium salt is a combination of multiple types, there is no restriction on the proportion of each component in the composition, and they can be mixed in any proportion. When preparing the mother solution, the mass ratio of the polymer electrolyte to the lithium salt is 7:1 to 20:1, for example, 7:1, 10:1, 15:1 or 20:1.
[0055] In step S102, the oxide electrolyte can be selected from any one or more combinations of the oxide electrolytes listed above, which will not be repeated here. The weighing of the oxide electrolyte is carried out in a glove box, and then the weighed oxide electrolyte is placed in a sample bottle, a small amount of organic solvent is added to disperse evenly, poured into the mother liquor, and stirred and dispersed until a white emulsion is formed. This application does not limit the dispersion method, and conventional stirring methods in the art can be adopted, such as ultrasound + magnetic stirring or magnetic stirring, etc. For example, ultrasonic dispersion is performed for 5 to 10 minutes, and then the sample is sealed, heated in a water bath at 60°C, and magnetically stirred at a speed of 1000rpm for 2 hours to obtain an inorganic-organic composite electrolyte slurry. Among them, in the inorganic-organic composite electrolyte slurry, the mass percentage of the oxide electrolyte is 12 to 25%, for example, 12%, 18% or 25% any value within the above range, and the balance is polymer electrolyte, lithium salt and organic solvent, wherein the total mass of the polymer electrolyte and the lithium salt accounts for 2 to 5% of the mass of the mixed solution of the polymer electrolyte, lithium salt and organic solvent, for example, 2%, 3%, 4% or 5% any value within the above range, and the mass ratio of the polymer electrolyte to the lithium salt is 7:1 to 20:1.
[0056] See also Figure 1 , step S2 is to coat the first electrolyte slurry prepared in step S1 on a substrate, form a film, and dry it to obtain a first electrolyte membrane, wherein the substrate may be, for example, a wet or dry PP film, a PE film, etc.; the film forming method may be casting or coating, and its specific process may refer to the conventional method in the art, which will not be repeated here. Preferably, hot pressing treatment is also included after drying, and the density of the oxide can be further improved by hot pressing treatment. The hot pressing treatment specifically includes: placing the dried flexible membrane at 40 to 80°C, and pressing it for 10 to 80 minutes at a pressure of 30 to 60 MPa; wherein the hot pressing temperature may be selected from any value within the above range such as 40°C, 60°C or 80°C; the pressure may be selected from any value within the above range such as 30MPa, 40MPa, 50MPa or 60MPa; the pressing time may be selected from any value within the above range such as 10min, 30min, 50min or 80min. The parameters during hot pressing treatment can be selected within the above range according to the characteristics of the material. After the hot pressing treatment, a first electrolyte membrane with a relatively high density is obtained, and the thickness of the first electrolyte membrane is 1 to 100 μm, and further 10 to 60 μm, for example, any value within the above range such as 10 μm, 30 μm, 50 μm or 60 μm. Within this thickness range, the first electrolyte membrane can ensure the mechanical properties of the composite solid electrolyte membrane, ensure the mechanical properties of the composite solid electrolyte membrane, and reduce impedance, which is beneficial to improving battery safety and capacity.
[0057] See also Figure 1In step S3, in the second electrolyte slurry, the mass percentage of the polymer monomer is 5-15%, for example, 5%, 10% or 15%, and the initiator is 1-10% of the mass of the polymer monomer, for example, the mass of the initiator is 1%, 5% or 10% of the mass of the polymer monomer, and any value within the above range; the remainder is lithium salt and organic solvent, and the mass ratio of organic solvent to lithium salt is 1:1-3:1, for example, 1:1, 2:1 or 3:1.
[0058] Wherein, the polymer monomer includes but is not limited to one or more of triethylene glycol dimethacrylate, ethylene glycol diacrylate, and polyethylene glycol monomethyl ether methacrylate, that is, the polymer monomer can be any one of the above-listed types or a combination of any two or three. For example, the polymer monomer is triethylene glycol dimethacrylate, ethylene glycol diacrylate, or polyethylene glycol monomethyl ether methacrylate, or a combination of triethylene glycol dimethacrylate and ethylene glycol diacrylate, or a combination of ethylene glycol diacrylate and polyethylene glycol monomethyl ether methacrylate, or a combination of triethylene glycol dimethacrylate, ethylene glycol diacrylate, and polyethylene glycol monomethyl ether methacrylate. When the polymer monomer is a combination of several types, there is no restriction on the proportion of each component in the composition, and any proportion can be mixed.
[0059] The organic solvent in the second electrolyte slurry is recorded as the second solvent, and the second solvent is a carbonate or carbonate-containing organic solvent, and the second solvent includes one or more of ethylene carbonate, diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate, that is, the second solvent can be any one of the above solvents, such as ethylene carbonate or diethyl carbonate or dimethyl carbonate or methyl ethyl carbonate; it can also be any two or more combinations of the above solvents, such as a combination of ethylene carbonate and diethyl carbonate, or a combination of dimethyl carbonate and methyl ethyl carbonate, or a combination of diethyl carbonate, dimethyl carbonate and methyl ethyl carbonate. When the second solvent is a combination of several components, there is no restriction on the proportion of each component in the composition, and it can be mixed in any proportion.
[0060] The initiator is mainly used to initiate in-situ polymerization of polymer monomers, and the initiator may be azobisisobutyronitrile or benzoyl peroxide, etc.
[0061] When preparing the second electrolyte slurry, first weigh the raw materials according to the above ratio, add the lithium salt into the second solvent, and mix and stir evenly at room temperature; then add the polymer monomer and initiator, and magnetically stir at room temperature for 20 to 40 minutes to obtain the second electrolyte slurry.
[0062] See also Figure 1, step S4 applies the second electrolyte slurry prepared in step S3 to the first electrolyte membrane prepared in step S2 by atomizing spraying. The specific steps of atomizing spraying include: transferring the second electrolyte slurry to an ultrasonic atomizing generator, the ultrasonic frequency of the ultrasonic atomizing generator is 2 to 3 MHz, the atomized second electrolyte slurry reaches the nozzle through the mist outlet conduit, and then controls the spraying distance to be 5 to 10 cm, and moves forward at a speed of 1 to 2 cm / s to form a uniform thin film layer on the first electrolyte membrane. The thickness of the atomizing spray is 1 to 50 μm, such as any value within the above range such as 10 μm, 30 μm or 50 μm; preferably, the thickness of the atomizing spray is 1 to 10 μm, such as 1 μm, 5 μm or 10 μm.
[0063] In-situ curing is to place the electrolyte membrane coated with the second electrolyte slurry at 50-80°C, such as 50°C, 60°C or 80°C, and vacuum dry for 3-6 hours, such as 3 hours, 4 hours, 5 hours or 6 hours, so that the polymer monomer is polymerized in-situ to form the second electrolyte membrane, and the composite electrolyte membrane is obtained after roller pressing. Spraying is carried out by atomization spraying, and the polymer monomer can penetrate into the gaps in the first electrolyte membrane, and in-situ curing is achieved in the subsequent drying process, which improves the interface contact between the two and increases the density of the composite electrolyte.
[0064] Step S5 is to peel off the substrate to obtain the composite solid electrolyte membrane.
[0065] On the other hand, the present invention provides a composite solid electrolyte membrane, which is prepared by the above-mentioned preparation method. The composite electrolyte membrane includes a first electrolyte membrane and a second electrolyte membrane, and the second electrolyte membrane is located on the surface of the first electrolyte, wherein the first electrolyte membrane is an inorganic oxide electrolyte membrane or an inorganic-organic composite electrolyte membrane; the second electrolyte membrane is a polymer electrolyte membrane resistant to high-nickel ternary or quaternary positive electrode materials. The composite solid electrolyte membrane of the present invention has the high ionic conductivity of the inorganic oxide electrolyte and can maintain stability to the positive high-nickel ternary or quaternary positive electrode materials, thereby improving the ionic conductivity of the composite membrane material and the safety performance of the battery.
[0066] The present invention also provides a lithium ion solid-state battery, comprising a positive electrode, a negative electrode and a solid electrolyte, wherein the positive electrode comprises an oxide, a high-nickel ternary or quaternary or other high-voltage positive electrode material, the negative electrode is a carbon or silicon-carbon composite material or lithium metal, and the solid electrolyte is a composite solid electrolyte membrane of the present invention, or a composite solid electrolyte membrane prepared by the method of the present invention. Since the composite solid electrolyte in the solid-state battery has a high density, the generation of lithium dendrites in the battery during the cycle is suppressed, the safety performance of the battery is improved, and the internal resistance of the battery does not increase significantly; in addition, the second electrolyte membrane in the composite solid electrolyte membrane has the characteristics of being stable to high-nickel ternary or quaternary high-voltage positive electrode materials, so that it can match the high-voltage positive electrode material and improve the capacity of the battery.
[0067] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The preparation process of the following embodiments can be found in Figure 4 .
[0068] Example 1
[0069] Step 1: Mix and stir the PVDF binder and NMP until they are clear, uniform and free of bubbles, and prepare a glue solution with a PVDF concentration of 10%; add it to the LATP and NMP mixed solution after particle size refinement, mix and stir for 1 hour until uniform, and adjust the mass percentage of the oxide electrolyte to 25% and the mass percentage of the binder to 3% by adding the glue solution and the solvent NMP to prepare the first electrolyte slurry;
[0070] Step 2: Use a small coating machine to coat the first electrolyte slurry on the substrate, and form a 20 μm first electrolyte membrane after drying;
[0071] Step 3: Ethylene carbonate and LiFSI are mixed and stirred evenly in a mass ratio of 2:1, and then monomer triethylene glycol dimethacrylate and initiator azobisisobutyronitrile are added, and stirred at room temperature for 20 minutes to obtain a second electrolyte slurry, wherein the mass percentage of triethylene glycol dimethacrylate in the second electrolyte slurry is 8%, and the mass of azobisisobutyronitrile is 5% of the mass of triethylene glycol dimethacrylate;
[0072] Step 4: Use an ultrasonic atomizer to spray the second electrolyte slurry onto the first electrolyte membrane with a spraying thickness of 3 um, dry it in a vacuum at 50°C for 4 hours, and then roll it to obtain a composite solid electrolyte membrane after peeling off the substrate.
[0073] Example 2
[0074] Step 1: Place PEO / LiTFSI in a sample bottle at a mass ratio of 8:1, add a small amount of DMF solvent, stir at 500 rpm for 12 hours in a 60°C water bath to form a stable and transparent mother liquor; weigh a certain amount of LATP electrolyte, add DMF to immerse it, ultrasonically disperse it for 5 minutes, and then add the dispersed LATP to the mother liquor. After sealing, stir at 1000 rpm for 2 hours in a 60°C water bath to obtain a first electrolyte slurry; wherein the mass percentage of LATP in the first electrolyte slurry is 20%, the mass percentage of PEO and LiTFSI is 5%, and the balance is DMF.
[0075] Step 2: Use a small tape casting machine to tape cast the first electrolyte slurry on the substrate to form a film, and after drying, form a 50 μm first electrolyte membrane;
[0076] Step 3: Mix diethyl carbonate and LiFSI in a mass ratio of 3:1 and stir evenly, then add monomer ethylene glycol diacrylate and initiator benzoyl peroxide, and stir at room temperature for 20 minutes to obtain a second electrolyte slurry, wherein the mass percentage of ethylene glycol diacrylate in the second electrolyte slurry is 5%, and the mass of benzoyl peroxide is 1% of the mass of ethylene glycol diacrylate.
[0077] Step 4: Use an ultrasonic atomizer to spray the second electrolyte slurry onto the first electrolyte membrane with a spraying thickness of 10 um, dry it in a vacuum at 50° C. for 4 hours, and then roll it to obtain a composite electrolyte membrane after peeling off the substrate.
[0078] Example 3
[0079] Step 1: Mix and stir the PVDF binder and NMP until they are clear, uniform and free of bubbles, and prepare a glue solution with a PVDF concentration of 10%; add it to the LLZAO and NMP mixed solution after particle size refinement, mix and stir for 1 hour until uniform, and adjust the oxide solid content to 15% and the binder to 1% by adding glue solution and solvent NMP to prepare the first electrolyte slurry;
[0080] Step 2: Use a small coating machine to coat the first electrolyte slurry on the substrate, and form a 60 μm first electrolyte membrane after drying;
[0081] Step 3: Ethylene carbonate and LiFSI are mixed and stirred evenly in a mass ratio of 1:1, and then monomer triethylene glycol dimethacrylate and initiator azobisisobutyronitrile are added, and stirred at room temperature for 40 minutes to obtain a second electrolyte slurry, wherein the mass percentage of triethylene glycol dimethacrylate in the second electrolyte slurry is 12%, the mass of azobisisobutyronitrile is 8% of the mass of triethylene glycol dimethacrylate, and the remainder is ethylene carbonate and LiFSI;
[0082] Step 4: Use an ultrasonic atomizer to spray the second electrolyte slurry onto the first electrolyte membrane with a spraying thickness of 1 um, and then roll it after drying in a vacuum at 50°C for 4 hours. After peeling off the substrate, a composite electrolyte membrane is obtained.
[0083] Example 4
[0084] Step 1: PEO / LiTFSI is placed in a sample bottle at a mass ratio of 8:1, a small amount of DMF solvent is added, and the mixture is stirred at 500 rpm for 12 hours in a 60°C water bath to form a stable and transparent mother liquor; a certain amount of LLZAO electrolyte is weighed, and DMF is added to immerse the mixture, and ultrasonic dispersion is performed for 5 minutes. The dispersed LLZAO is then added to the mother liquor, and the mixture is sealed and stirred at 1000 rpm for 2 hours in a 60°C water bath to obtain a first electrolyte slurry, wherein the mass percentage of LATP in the first electrolyte slurry is 20%, the mass percentage of PEO and LiTFSI is 5%, and the balance is DMF;
[0085] Step 2: Using a small tape casting machine to tape cast the first electrolyte slurry on the substrate to form a film, and after drying, a 100 μm first electrolyte membrane is formed;
[0086] Step 3: Mix diethyl carbonate and LiFSI in a mass ratio of 3:1 and stir evenly, then add monomer ethylene glycol diacrylate and initiator benzoyl peroxide, and stir at room temperature for 20 minutes to obtain a second electrolyte slurry, wherein the mass percentage of ethylene glycol diacrylate in the second electrolyte slurry is 15%, and the mass of benzoyl peroxide is 10% of the mass of ethylene glycol diacrylate.
[0087] Step 4: Use an ultrasonic atomizer to spray the second electrolyte slurry onto the first electrolyte membrane with a spraying thickness of 50 um, dry it in a vacuum at 50° C. for 4 hours, and then roll it to obtain a composite electrolyte membrane after peeling off the substrate.
[0088] Comparative Example 1
[0089] The difference from Example 1 is that the spraying thickness of the second electrolyte slurry in step 4 is 70 μm.
[0090] Comparative Example 2
[0091] The difference from Example 2 is that the spraying thickness of the second electrolyte slurry in step 4 is 100 μm.
[0092] Comparative Example 3
[0093] PVDF binder and NMP are prepared into a glue solution in a mass ratio of 1:15, and pneumatically stirred until it is clear, uniform and free of bubbles; it is added into a mixture of LATP and NMP after particle size refinement, and mechanically stirred at room temperature for 1 hour, and the content of oxide electrolyte is adjusted to 25% and the content of binder to 3% by adding glue solution and solvent NMP; it is coated on a substrate using a small coating machine, and vacuum dried at 50°C for 12 hours to obtain an oxide electrolyte membrane.
[0094] Comparative Example 4
[0095] The difference from Comparative Example 3 is that the oxide solid electrolyte in step 1 is replaced with LLZAO.
[0096] Performance Testing
[0097] 1. The solid electrolyte membranes prepared in Examples 1 to 4 and Comparative Examples 1-4 were tested for ion conductivity. The test structure is shown in Table 1.
[0098] 2. The solid electrolyte membranes obtained in Examples 1-4 and Comparative Examples 1-4 were prepared into solid-state batteries, and cycle life tests were performed on each solid-state battery. The positive electrode material of the solid-state battery used NCM811 (the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese ternary positive electrode material is 8:1:1), and the negative electrode used graphite. The button battery was prepared. The assembly method of the solid-state battery can refer to the conventional battery assembly method in the field, which will not be described here. The cycle performance of the battery was tested, and the test results are shown in Table 2.
[0099] Table 1: Ionic conductivity of solid electrolyte membranes prepared in Examples 1 to 4 and Comparative Examples 1-4 at 25°C
[0100] Example / Comparative Example <![CDATA[Ionic conductivity (*10 -4 )]]> Example 1 0.68 Example 2 0.72 Example 3 0.64 Example 4 0.70 Comparative Example 1 0.50 Comparative Example 2 0.53 Comparative Example 3 0.72 Comparative Example 4 0.78
[0101] Table 2: Cyclic performance of solid-state batteries after 100 charge and discharge cycles at 0.1C
[0102]
[0103]
[0104] From the test results in Table 1 and Table 2, the composite solid electrolyte membrane prepared in this application not only has a high ionic conductivity, but also remains stable to the positive high nickel ternary or quaternary positive electrode material, and the capacity is maintained at more than 90% after 100 cycles. Although the comparative example also has a high ionic conductivity, its cycling performance is poor and cannot meet the application of power batteries.
[0105] The present invention sprays the high nickel resistant positive electrode material polymer electrolyte slurry onto the oxide electrolyte membrane by atomization spraying, and realizes in-situ polymerization of polymer monomers while removing the solvent through a subsequent drying process, improves the interface contact between the polymer electrolyte layer and the oxide electrolyte layer, and improves the density of the composite solid electrolyte. The above method can achieve the adaptation of the composite solid electrolyte membrane and the high voltage positive electrode material, reduce the amount of low ionic conductivity polymer, avoid the increase of the internal resistance of the battery, and improve the ability of the composite solid electrolyte membrane to inhibit the growth of lithium dendrites, thereby effectively improving the capacity and safety of the battery. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.
[0106] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a composite solid electrolyte membrane, characterized in that: At least the following steps are included: Preparing a first electrolyte slurry, wherein the first electrolyte slurry is an inorganic oxide electrolyte slurry or an inorganic-organic composite electrolyte slurry; The first electrolyte slurry is coated on a substrate to form a film and dried to obtain a first electrolyte membrane; Evenly mixing the polymer monomer, the initiator, the lithium salt and the organic solvent to prepare the second electrolyte slurry; Applying the second electrolyte slurry on the first electrolyte membrane by atomizing spraying, and forming a second electrolyte membrane on the first electrolyte membrane after in-situ curing; peeling off the substrate to obtain a composite solid electrolyte membrane; During the atomization spraying, the spraying distance is controlled to be 5-10 cm, and the spraying speed is 1-2 cm / s to form a uniform thin film layer on the first electrolyte membrane; the thickness of the atomization spraying is 1-50 μm.
2. The preparation method according to claim 1, characterized in that: In the inorganic oxide electrolyte slurry, the mass percentage of the oxide electrolyte is 15-35%, the mass percentage of the binder is 1-5%, and the rest is an organic solvent; in the inorganic-organic composite electrolyte slurry, the mass percentage of the oxide electrolyte is 12-25%, and the rest is a mixture of a polymer electrolyte, a lithium salt and an organic solvent, wherein the mass of the polymer electrolyte and the lithium salt is 2-5% of the mass of the mixture, and the mass ratio of the polymer electrolyte to the lithium salt is 7:1-20:
1.
3. The preparation method according to claim 2, characterized in that: The inorganic oxide electrolyte includes any one of LLZO, LLZAO, LLZTO, LLZNO, LATP, LAGP, LZSPO, SiO2 or Al2O3, or a combination of at least two of them; the organic solvent includes any one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, acetonitrile or acetone, or a combination of at least two of them; the lithium salt includes one or more combinations of lithium perchlorate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium trifluoromethanesulfonate and lithium dioxalatoborate.
4. The preparation method according to claim 1, characterized in that: The first electrolyte slurry is formed into a film by casting or coating, and the thickness of the first electrolyte film is 1-100 μm.
5. The preparation method according to claim 1, characterized in that: When preparing the first electrolyte membrane, after the drying process is completed, a hot pressing process is further included, and the hot pressing parameters of the hot pressing process are a temperature of 40-80° C., a pressure of 30-60 MPa, and a time of 10-80 min.
6. The preparation method according to claim 1, characterized in that: The preparation of the second electrolyte slurry comprises: adding the lithium salt to the organic solvent at room temperature and mixing and stirring evenly; then adding the polymer monomer and the initiator, and magnetically stirring at room temperature for 20 to 40 minutes; wherein, in the second electrolyte slurry, the mass percentage of the polymer monomer is 5 to 15%, the mass of the initiator is 1 to 10% of the mass of the polymer monomer, and the ratio of the organic solvent to the lithium salt is 1:1 to 3:
1.
7. The preparation method according to claim 6, characterized in that: The organic solvent in the second electrolyte slurry is a carbonate or carbonate-containing organic solvent, including one or more of ethylene carbonate, diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate; the polymer monomer includes one or a combination of triethylene glycol dimethacrylate, ethylene glycol diacrylate, and polyethylene glycol monomethyl ether methacrylate; the initiator is azobisisobutyronitrile or benzoyl peroxide.
8. The preparation method according to claim 1, characterized in that: The atomization spraying comprises: injecting the second electrolyte slurry into an ultrasonic atomization generator, and spraying the second electrolyte slurry onto the first electrolyte membrane after being atomized by the ultrasonic atomization generator.
9. A composite solid electrolyte membrane, characterized in that: The preparation method according to claim 1 is used for preparation.
10. A lithium-ion solid-state battery, characterized in that: A composite solid electrolyte membrane prepared by the preparation method according to claim 1.
Citation Information
Patent Citations
Composite solid electrolyte, and preparation method and application thereof
CN109244537A
Electrode sheet, all-solid battery, manufacturing method for electrode sheet, and manufacturing method for all-solid battery
CN110383560A
Organic / inorganic composite electrolyte membrane for solid-state sodium ion battery, preparation and application thereof
CN111628213A
Preparation method of positive plate or negative plate for solid-state battery, positive plate or negative plate for solid-state battery and solid-state battery
CN111799514A
In-situ formed sulfide composite solid electrolyte and preparation method thereof
CN112909322A